Multicomponent metal oxide photomagnetic material, its preparation method and application

By preparing multi-component metal oxide photomagnetic materials and treating lanthanum source, titanium source and M compound with high-temperature solid-state method, the problem of insufficient photo-controlled magnetism in the existing technology is solved, and efficient and fast photo-controlled magnetic response is achieved, which is applicable to fields such as sensing, optical communication and optical storage technology.

CN120527111BActive Publication Date: 2025-11-07JILIN UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511012963.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-23
Publication Date
2025-11-07
Estimated Expiration
2045-07-23

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve efficient photo-controlled magnetism in a single material, failing to meet the demands of spintronics for highly efficient photo-controlled magnetic response materials.

Method used

Multicomponent metal oxide optomagnetic materials were prepared with the chemical formula LaxTi1-yMyO3, where 0.60≤x≤1.0, 0

Benefits of technology

It achieves good material uniformity, high purity, and small particle size, with a maximum magnetic moment change of no less than 25% and a response time of no more than 0.1 s. It possesses fast response and high-intensity photomagnetic phenomena, and is suitable for fields such as sensing, optical communication, and optical storage technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120527111B_ABST
    Figure CN120527111B_ABST
Patent Text Reader

Abstract

The present application is suitable for the field of information material technology, and provides a multi-component metal oxide photomagnetic material, a preparation method and application thereof. The method is simple, feasible, green and environmentally friendly, is suitable for industrial production, and the prepared material has good uniformity, high purity and small particle size. The material presents obvious and stable negative photomagnetic response, and the maximum change of magnetic moment is not less than 25%. Taking the photomagnetic material La 0.9 Ti 0.5 Ni 0.5 O3 as an example, under the conditions of 2 K response temperature, 50 mW laser power irradiation and 1 T magnetic field, the photomagnetic response is negative, the response time is not higher than 0.1 s, and the maximum change of magnetic moment reaches 37.2%, realizing the photomagnetic phenomenon of fast response and continuous high-intensity response. The present application provides a new idea for constructing high-efficiency and low-energy consumption composite quantum transport devices, and has good application prospects in the fields of sensing, optical communication and optical storage technology, and the like.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application belongs to the technical field of information materials, and particularly relates to a multi-component metal oxide magneto-optical material and a preparation method and application thereof. BACKGROUND

[0002] With the rapid development of information technology, the society's demand for high-density, low-energy storage and computing is increasingly urgent. Traditional semiconductor devices based on electric charge are gradually approaching the limit of Moore's law, while spintronics using electron spin for information processing is expected to break through this bottleneck. Compared with the operation mode of traditional spin regulation scheme relying on large current or strong magnetic field, the manipulation of spin and magnetism by light field can not only significantly reduce energy consumption, but also greatly improve the speed of information storage and processing. However, how to realize efficient light-controlled magnetism in a single material is still a big challenge for spintronics.

[0003] Transition metal oxides are prone to form complex quantum orders due to the coupling between lattice, spin, charge and orbital and the symmetry breaking of surface / interface, and thus exhibit rich quantum effects. Titanium-based perovskite materials exhibit a wide range of physical and chemical properties due to their structural and elemental composition diversity, as well as excellent light response ability and structural stability: in terms of electrical properties, it can range from insulator to semiconductor, semimetal, metal, and even superconductor; magnetic interaction can be from antiferromagnetic to ferrimagnetic, ferromagnetic and different types of magnetic frustration; optical response wavelength can cover the high wavelength range of ultraviolet-infrared. By adjusting the lattice structure and coordination environment of metal ions through vacancy regulation of A site of titanium-based perovskite and introducing cations with different radii and valence states at B site, the local electronic state behavior dominated by charge, spin, orbital and lattice degrees of freedom is realized, such as lattice distortion, spin polarization, charge and orbital hybridization, etc. These characteristics ultimately lay the foundation for building high-efficiency, low-energy consumption quantum devices, and help to realize unconventional high-efficiency light-controlled magnetic response performance.

[0004] However, the technology of realizing high-efficiency light-controlled magnetism in inorganic functional materials has not yet matured, and the existing technology cannot fully meet the demand of spintronics for high-efficiency light-controlled magnetic response materials. In view of this, the present application proposes a multi-component metal oxide magneto-optical material and a preparation method and application thereof. SUMMARY

[0005] The purpose of the present application is to provide a multi-component metal oxide magneto-optical material and a preparation method and application thereof, aiming to solve the problems raised in the above background.

[0006] The purpose of the present application is realized by the following technical solutions:

[0007] A multi-component metal oxide photomagnetic material, the photomagnetic material is a titanium-based perovskite oxide, chemical formula is La x Ti 1-y M y O3, wherein 0.60≤x≤1.0, 0<y≤0.5. The photomagnetic material can be used in the fields of sensing, optical communication and optical storage technology, and the like.

[0008] Further, the photomagnetic response of the photomagnetic material is negative, and the magnetic moment change is not less than 25%.

[0009] A preparation method of the multi-component metal oxide photomagnetic material according to the above, comprising the following steps:

[0010] Step S1: calcining a commercial lanthanum source at 900 DEG C for 10 h; heating a commercial titanium source and an M compound at 200 DEG C for 10 h.

[0011] Step S2: weighing the treated commercial lanthanum source, the commercial titanium source and the M compound, adding water, anhydrous ethanol or a mixture of water and anhydrous ethanol, and forming a uniform mixture through constant temperature stirring and ultrasonic dispersion;

[0012] Step S3: calcining the mixture in a crucible;

[0013] Step S4: grinding and tabletting the calcined product, and repeatedly calcining by a solid phase method to obtain the multi-component metal oxide photomagnetic material.

[0014] Further, in the step S2, the lanthanum source is any one or a combination of at least two of lanthanum oxide (La2O3), lanthanum nitrate (La(NO3)3), lanthanum carbonate (La2(CO3)3) and lanthanum oxalate (La2(C2O4)3). Preferably, the lanthanum source is La2O3.

[0015] Further, in the step S2, the titanium source is titanium dioxide (TiO2).

[0016] Further, in the step S2, the particle size of the M compound is nanoscale; the M compound is any one or a combination of at least two of Sc, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Mg, Mo, Al and Zr. Preferably, it is any one or a combination of at least two of Co, Ni, Cr and Fe; the Co source is any one or a combination of at least two of CoO, Co2O3 and Co3O4; the Ni source is any one or a combination of at least two of NiO, Ni2O3 and Ni3O4; the Cr source is any one or a combination of at least two of CrO2 and Cr2O3; and the Fe source is any one or a combination of at least two of FeO, Fe2O3 and Fe3O4.

[0017] Furthermore, in step S3, the pretreatment calcination temperature is 900~1100℃, and the calcination time is 6~12 h. Preferably, the calcination temperature is 1000℃, the heating rate is 5℃ / min, and the calcination time is 10 h.

[0018] Furthermore, in step S4, the calcination temperature is not higher than the volatilization temperature of compound M, the calcination time is 18-24 h, and the oxygen partial pressure in the calcination atmosphere is 20-22 kPa. Preferably, the calcination temperature is 1200-1400℃; the calcination time is 24 h; the oxygen partial pressure in the calcination atmosphere is 5-21.2 kPa; and the solid phase is repeatedly ground, compressed, and calcined a total of 3 times.

[0019] Compared with the prior art, the beneficial effects of the present invention are:

[0020] This invention successfully prepared multi-component metal oxide photomagnetic materials via a high-temperature solid-state method. This method is simple, feasible, environmentally friendly, and suitable for industrial production. The resulting materials exhibit good uniformity, high purity, and small particle size, all displaying a significant and stable negative photomagnetic response, with maximum magnetic moment changes not less than 25%. The photomagnetic material La... 0.9 Ti 0.5 Ni 0.5 Taking O3 as an example, under the conditions of a response temperature of 2 K, irradiation with 50 mW laser power, and a magnetic field of 1 T, its photomagnetic response is negative, the response time is no higher than 0.1 s, and the maximum change in magnetic moment reaches 37.2%, realizing the photomagnetic phenomenon of rapid response and sustained high-intensity response. Compared with existing metal / non-metal and other organic photomagnetic response materials, this invention provides a new approach for constructing high-efficiency, low-energy-consumption composite quantum transport devices, and has good application prospects in fields such as multi-field synergistic control and intelligent integration in sensing, optical communication, and optical storage technologies. Attached Figure Description

[0021] Figure 1 La, a photomagnetic material 0.9 Ti 0.5 Ni 0.5 O3, La 0.9 Ti 0.5 Ni 0.45 Co 0.05 O3, La 0.67 Ti 0.9 Fe 0.1 O3, La 0.67 Ti 0.9 Cr 0.1 XRD pattern of O3.

[0022] Figure 2 La, a photomagnetic material 0.9 Ti 0.5 Ni 0.5The powder SEM image (left) and the tablet SEM image (right) of O3.

[0023] Figure 3 La 0.9 Ti 0.5 Ni 0.5 O3, La 0.9 Ti 0.5 Ni 0.45 Co 0.05 O3, La 0.67 Ti 0.9 Fe 0.1 O3, La 0.67 Ti 0.9 Cr 0.1 The change of the light response magnetic moment of O3 at 2 K temperature under the applied magnetic field.

[0024] Figure 4 La 0.9 Ti 0.5 Ni 0.5 The zero-field cooling curve of the photo-magnetic response of O3.

[0025] Figure 5 La 0.9 Ti 0.5 Ni 0.5 The photo-magnetic response M-H (magnetic moment-magnetic field) curve of O3, with the M-t (magnetic moment-time) curve attached. DETAILED DESCRIPTION

[0026] In order to have a clearer understanding of the technical features, objectives and beneficial effects of the present application, the technical solutions of the present application will be described in detail below, but it should not be understood as limiting the scope of the present application.

[0027] The specific implementation of the present application will be described in detail below in combination with specific embodiments.

[0028] Example 1: A multi-component metal oxide photo-magnetic material La 0.9 Ti 0.5 Ni 0.5 The preparation method of O3 comprises the following steps:

[0029] Step S1: calcine the commercial raw material La2O3 at 900℃ high temperature for 10 h; heat the commercial raw materials TiO2 and NiO at 200℃ high temperature for 10 h.

[0030] Step S2: Take the high-temperature treated commercial raw materials La2O3 1.223 g, TiO2 0.333 g and NiO 0.312 g, and stir uniformly in anhydrous ethanol at a constant temperature, and use a high-power ultrasonic cell crusher to ultrasonicize.

[0031] Step S3: Slowly inject the ultrasonicized uniform mixture into a crucible, and heat to 1000°C at a rate of 5°C / min, and calcine for 10 h.

[0032] Step S4: Grind and tabletize the pretreated product, and calcine at 1400°C for 24 h in an oxygen partial pressure calcination atmosphere of 21 KPa, and repeat tabletization and calcination three times to obtain La 0.9 Ti 0.5 Ni 0.5 O3 multi-component metal oxide photomagnetic material.

[0033] Step S5: Take 20 mg of the powder sample, and press into a 3 mm diameter wafer under a pressure of 0.5 MPa.

[0034] Step S6: At a response temperature of 2 K, use a laser power of 50 mW to irradiate the sample, and apply a response magnetic field of 1 T, and the maximum change in magnetic moment is 37.2% (M / M0). Figure 3 ).

[0035] Figure 2 The powder SEM image (left) and the tablet SEM image (right) of the photomagnetic material La 0.9 Ti 0.5 Ni 0.5 O3 are shown. As can be seen from the figure, the La 0.9 Ti 0.5 Ni 0.5 O3 photomagnetic material has a powder sample particle size of 200-500 nm, and an average particle size of 344.43±87.66 nm; the crystal grain boundaries in the tablet sample are tight and regular, and there are no defects such as pores.

[0036] Figure 4 The zero-field cooling curve of the photomagnetic response of the photomagnetic material La 0.9 Ti 0.5 Ni 0.5 O3 under the condition of applying a magnetic field of 1000 Oe (0.1 T) is shown. As can be seen from the figure, within the temperature range of 2-10 K in the photomagnetic response range and under the condition of applying a magnetic field of 0.1 T, the zero-field cooling curves of the photomagnetic material La 0.9 Ti 0.5 Ni 0.5 O3 before and after light application show different trends, which reflects the photomagnetic response characteristics thereof.

[0037] Figure 5The photomagnetic material La 0.9 Ti 0.5 Ni 0.5 O3 exhibits a photomagnetic response M-H (magnetic moment-magnetic field) curve, with an attached M-t (magnetic moment-time) curve. As can be seen from the figure, the photomagnetic material La 0.9 Ti 0.5 Ni 0.5 O3 exhibits a negative response of magnetic moment under a 1 T magnetic field, and the material has a reversible photomagnetic response under switching light conditions, and the response time is not higher than 0.1 s, which indicates that the material can realize fast information writing and reading.

[0038] Embodiment 2: A multi-component metal oxide photomagnetic material La 0.9 Ti 0.5 Ni 0.45 Co 0.05 O3, comprising the following steps:

[0039] Step S1: calcine the commercial raw material La2O3 at 900 DEG C for 10 h; heat the commercial raw materials TiO2, NiO and CoO at 200 DEG C for 10 h.

[0040] Step S2: weigh the high-temperature treated commercial raw materials La2O3 1.291 g, TiO2 0.333 g, NiO 0.281 g and CoO 0.00312 g, uniformly stir in anhydrous ethanol and use a high-power ultrasonic cell crusher to ultrasonically refine.

[0041] Step S3: slowly inject the ultrasonically mixed mixture into a crucible, heat to 1000 DEG C at a rate of 5 DEG C / min, and calcine for 10 h.

[0042] Step S4: fully grind and press the pre-processed product, calcine at 1300 DEG C for 24 h under a 21 KPa oxygen partial pressure calcination atmosphere, and repeatedly press and calcine 3 times to obtain a La 0.9 Ti 0.5 Ni 0.45 Co 0.05 O3 multi-component metal oxide photomagnetic material.

[0043] Step S5: weigh 20 mg of the powder sample and press it into a 3 mm diameter wafer under a pressure of 0.5 MPa.

[0044] Step S6: irradiate the sample with a 50 mW laser power at a response temperature of 2 K, and apply a 1 T response magnetic field, and the maximum change in magnetic moment is 31.5% (Mmax / M0). Figure 3 ).

[0045] Embodiment 3: A multi-component metal oxide photomagnetic material La0.67 Ti 0.9 Fe 0.1 A method for preparing O3, comprising the following steps:

[0046] Step S1: calcining commercial raw material La2O3 at 900°C for 10 h; heating commercial raw materials TiO2 and Fe2O3 at 200°C for 10 h.

[0047] Step S2: weighing 0.507 g of high-temperature treated commercial raw material La2O3, 0.333 g of TiO2 and 0.037 g of Fe2O3, uniformly stirring in anhydrous ethanol and using a high-power ultrasonic cell crusher for ultrasonic refinement.

[0048] Step S3: slowly injecting the uniformly mixed mixture after ultrasonic treatment into a crucible, increasing the temperature to 1000°C at a rate of 5°C / min, and calcining for 10 h.

[0049] Step S4: fully grinding and tabletting the pretreated product, calcining at 1300°C for 24 h in an oxygen partial pressure calcination atmosphere of 21 KPa, and repeatedly tabletting and calcining 3 times to obtain La 0.67 Ti 0.9 Fe 0.1 O3 multi-component metal oxide optical magnetic material.

[0050] Step S5: weighing 20 mg of the powder sample and pressing into a 3 mm diameter wafer under a pressure of 0.5 MPa.

[0051] Step S6: using a 50 mW laser power to irradiate the sample at a 2 K response temperature, applying a 0.7 T response magnetic field, and detecting a maximum magnetic moment change of 35.5% (M / M0). Figure 3

[0052] Example 4: a multi-component metal oxide optical magnetic material La 0.67 Ti 0.9 Cr 0.1 A method for preparing O3, comprising the following steps:

[0053] Step S1: calcining commercial raw material La2O3 at 900°C for 10 h; heating commercial raw materials TiO2 and Cr2O3 at 200°C for 10 h.

[0054] Step S2: weighing 0.507 g of high-temperature treated commercial raw material La2O3, 0.333 g of TiO2 and 0.0352 g of Cr2O3, uniformly stirring in anhydrous ethanol and using a high-power ultrasonic cell crusher for ultrasonic refinement.

[0055] ​Step S3: The homogenized mixture after ultrasonic treatment was slowly injected into a crucible, and the temperature was raised to 1000℃ at a rate of 5℃ / min, and calcined for 10 h.

[0056] Step S4: The pretreated product was thoroughly ground and pressed into a tablet, and calcined at 1400℃ for 24 h in an oxygen partial pressure calcination atmosphere of 21 KPa, and the tablet was repeatedly pressed and calcined for 3 times, to obtain La 0.67 Ti 0.9 Cr 0.1 O3 multi-component metal oxide photomagnetic material.

[0057] Step S5: 20 mg of the powder sample was weighed and pressed into a 3 mm diameter wafer under a pressure of 0.5 MPa.

[0058] Step S6: The sample was irradiated with a laser power of 50 mW at a response temperature of 2 K, and a response magnetic field of 0.7 T was applied, and the maximum change in magnetic moment was 28.5% (M / M0=28.5%) (M0: initial magnetic moment, M: magnetic moment after irradiation). Figure 3 )。

[0059] From Figure 1 It can be seen that the XRD patterns of the photomagnetic materials prepared in Examples 1-4 all exhibit characteristic peaks of perovskite material structure, and the peak type is clear and obvious. This indicates that after element multi-component doping, the material still maintains the perovskite crystal structure, and the element multi-component doping does not change the crystal structure of the material.

[0060] Performance test:

[0061] 20 mg of comparative material nano-Fe3O4 (Adv. Electron. Mater. 2018, 4, 1700661), Ni / BaTiO3 (ACS Appl. Mater. Interfaces 2023, 15, 18391-18401), [Mn(H4tetac)]2[W(CN)8]·4H2O (Angew. Chem. 2017, 129, 13468-13472), [Cu(H4tetac)]2[W(CN)8]·4H2O (https: / / doi.org / 10.1021 / acs.inorgchem.4c05576), and CsMnCl3 (J. Phys. Chem. Lett. 2020, 11, 9587-9595) were weighed, respectively, and pressed into a 3 mm diameter wafer under a pressure of 0.5 MPa, and the sample was irradiated with a laser power of 50 mW at a response temperature of 2 K, and a response magnetic field of 1 T was applied, and the maximum change in magnetic moment was detected, and compared with the maximum change in magnetic moment of the photomagnetic materials prepared in Examples 1-4. The results are shown in Table 1:

[0062] Table 1 Comparative results

[0063]

[0064] As shown in Table 1, the photomagnetic materials prepared in Examples 1-4 of this invention all exhibit obvious and stable negative photomagnetic responses, among which La 0.9 Ti 0.5 Ni 0.5 O3, La 0.9 Ti 0.5 Ni 0.45 Co 0.05 O3, La 0.67 Ti 0.9 Fe 0.1 O3, La 0.67 Ti 0.9 Cr 0.1 The maximum magnetic moment changes of O3 were 37.2%, 31.5%, 35.5%, and 28.5%, respectively, all significantly higher than those of the negative response comparison material nano-Fe3O4 (1.2%). Compared with the positive response comparison materials (Ni / BaTiO3, [Mn(H4tetac)]2[W(CN)8]·4H2O, [Cu(H4tetac)]2[W(CN)8]·4H2O, CsMnCl3), the photomagnetic materials prepared in Examples 1-4 of this invention exhibit unique negative photomagnetic response characteristics, breaking through the physical limitations of traditional positive response. This opens up a new path for the high environmental stability and functional complementarity of photomagnetic control technology, demonstrating significant performance advantages in the field of negative photomagnetic response, and possessing unique application value and potential.

[0065] The above are merely preferred embodiments of the present invention. It should be noted that those skilled in the art can make several modifications and improvements without departing from the concept of the present invention, and these should also be considered within the scope of protection of the present invention. These modifications and improvements will not affect the effectiveness of the implementation of the present invention or the practicality of the patent.

Claims

1. A multi-component metal oxide photomagnetic material, characterized by, The photo-magnetic material is a titanium-based perovskite oxide, chemical formula is La x Ti 1-y M y O3, wherein 0.60≤x≤1.0, 0<y≤0.5; The photomagnetic response of the photomagnetic material is negative, and the change of magnetic moment is not less than 25 %; In the photomagnetic material, the lanthanum source is any one or at least two combinations of lanthanum oxide, lanthanum nitrate, lanthanum carbonate and lanthanum oxalate; the titanium source is titanium dioxide; the particle size of the M compound is nanoscale, and the M compound is any one or at least two combinations of Co, Ni, Cr and Fe; wherein the Co source is any one or at least two combinations of CoO, Co2O3 and Co3O4; the Ni source is any one or at least two combinations of NiO, Ni2O3 and Ni3O4; the Cr source is any one or at least two combinations of CrO2 and Cr2O3; and the Fe source is any one or at least two combinations of FeO, Fe2O3 and Fe3O4.

2. A method of producing a multi-component metal oxide photomagnetic material according to claim 1, characterized by, The method comprises the following steps: Step S1: calcining the lanthanum source at 900 DEG C for 10 h; heating the titanium source and the M compound at 200 DEG C for 10 h; Step S2: weighing the treated lanthanum source, titanium source and M compound, adding water, anhydrous ethanol or a mixture of water and anhydrous ethanol, and stirring and ultrasonic dispersing to form a uniform mixture; Step S3: calcining the mixture in a crucible; Step S4: grinding and tabletting the calcined product, and repeatedly calcining by solid phase method to obtain the multi-component metal oxide photomagnetic material.

3. The preparation method according to claim 2, characterized in that, In step S3, the calcination temperature of the pretreated product is 900-1100 DEG C, the heating rate is 5 DEG C / min, and the calcination time is 6-12 h.

4. The preparation method according to claim 2, characterized in that, In step S4, the calcination temperature is not higher than the volatilization temperature of the M compound, the calcination time is 18-24 h, and the oxygen partial pressure of the calcination atmosphere is 20-22 KPa.

Citation Information

Patent Citations

  • Oxide of A-site vacancy alkaline-earth-element-free titanium-based perovskite structure and preparation and application thereof

    CN112824326A

  • Mn PERVOSKITE-TYPE OXIDE