Waterproof coating composition, waterproof coating, its preparation method and application

By introducing polyetheramine and double-ended epoxy polyether silicone oil to form a three-dimensional network structure and using modified fillers to enhance interfacial forces, the problem of easy cracking of waterproof coatings under freeze-thaw cycles was solved, and a waterproof coating with high elongation and excellent freeze-thaw resistance was achieved.

CN120554904BActive Publication Date: 2026-11-10STATE GRID BEIJING ELECTRIC POWER CO +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202510614109.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-05-13
Publication Date
2026-11-10
Estimated Expiration
2045-05-13

AI Technical Summary

Technical Problem

Existing waterproof coatings have a high polymer-to-ash ratio, require a large amount of polymer, have low elongation, and are prone to cracking or peeling under freeze-thaw cycles, resulting in a decline in waterproof performance.

Method used

The coating utilizes a liquid material comprising acrylate emulsion, polyetheramine, double-ended epoxy polyether silicone oil, and water-reducing agent, along with a powder material comprising silicate cement and modified filler. By forming a three-dimensional network structure and modifying with an aminosilane coupling agent, the fatigue resistance and freeze-thaw resistance of the coating are improved.

Benefits of technology

It improves the elongation and freeze-thaw resistance of the waterproof coating, inhibits cracking or interface peeling during freeze-thaw cycles, maintains the integrity and waterproof effect of the coating, and provides more durable and reliable waterproof protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005400486710000101
    Figure BDA0005400486710000101
  • Figure BDA0005400486710000113
    Figure BDA0005400486710000113
Patent Text Reader

Abstract

This invention provides a waterproof coating composition, a waterproof coating layer, its preparation method, and its application. The waterproof coating composition comprises a liquid component and a powder component; wherein the liquid component includes an acrylic emulsion, a polyetheramine, a double-ended epoxy polyether silicone oil, and a water-reducing agent; the powder component includes silicate cement and a modified filler, wherein the modified filler is a filler modified with an aminosilane coupling agent. The polyetheramine and the double-ended epoxy polyether silicone oil can chemically bond and intertwine with the polymer network formed by the acrylic emulsion, forming a three-dimensional network structure, thereby improving the fatigue resistance and elongation of the waterproof coating and preventing cracking; the amino groups on the surface of the modified filler can react with the epoxy groups in the double-ended epoxy polyether silicone oil, enhancing the interfacial forces between the inorganic filler and the organic polymer in the liquid component, reducing the interfacial peeling rate of the waterproof coating, and inhibiting cracking or interfacial peeling during freeze-thaw cycles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coating technology, and more specifically, to a waterproof coating composition, a waterproof coating, its preparation method, and its application. Background Technology

[0002] Waterproofing materials are protective building materials used to protect certain parts of a building from the erosion of groundwater, domestic water, rainwater, and moisture in the air. They are fundamental to ensuring the quality of a building.

[0003] Polymer cement-based waterproof coating (JS waterproof coating, where J represents polymer and S represents cement) is a two-component water-based waterproof coating consisting of liquid (polymer emulsion and additives) and powder (cement, inorganic fillers, and auxiliaries). After the coating is applied to the substrate, as the dispersion medium evaporates, polymer particles approach, contact, and deform under pressure, agglomerating to form a continuous and dense film. This film embeds the inorganic fillers, auxiliaries, and cement hydration products, thus forming a waterproof coating. Polymer emulsions mainly include three categories: polyvinyl acetate-ethylene copolymer emulsions, styrene-butadiene latex emulsions, and acrylic emulsions. Among these, acrylic emulsions, by adjusting the types and proportions of soft monomers, hard monomers, and functional monomers, can achieve excellent mechanical and waterproof properties, making them the preferred choice for preparing polymer cement-based waterproof coatings.

[0004] Existing literature (publication number CN104591599A) discloses a polymer cement-based waterproof coating, comprising: a liquid component, which, by weight, contains 55-60 parts of acrylic emulsion, 7-10 parts of dispersant, 7-10 parts of film-forming aid, 2-6 parts of leveling agent, 2-6 parts of drying agent, 3-7 parts of preservative, 3-7 parts of water and 2-6 parts of defoamer; and a powder component, which, by weight, contains 40-45 parts of cement, 20-25 parts of quartz powder, 5-12 parts of corundum, 2-7 parts of modified montmorillonite, 3-7 parts of plasticizer and 3-7 parts of fiber.

[0005] Existing literature (CN116004073A) discloses a polymer cement waterproof coating comprising liquid and powder. By weight, the liquid comprises 100 parts of modified acrylic emulsion; by weight, the powder comprises 35-60 parts of silicate cement, 10-25 parts of filler, and 2-15 parts of tannic acid. The modified acrylic emulsion is prepared by reacting methyl acrylate, butyl acrylate, and terminal alkenyl epoxy resin in a mass ratio of 10:(20-30):(5-15).

[0006] The aforementioned polymer cement-based waterproof coatings have been widely used in waterproofing and leak repair projects for toilets, kitchens, exterior walls, roofs, underground engineering, and liquid storage tanks. However, existing waterproof coatings generally suffer from a high polymer-to-cement ratio (i.e., a high weight ratio of polymer to cement) but low elongation. For example, the polymer-to-cement ratio is usually (1-2):1, but the elongation of the coating is only 150-250%.

[0007] In northern winters, buildings are frequently subjected to severe freeze-thaw cycles. When the aforementioned waterproof coatings are applied to sealing holes for pipes and cables, or to walls with embedded pipes and cables that are subject to periodic stress or vibration, the waterproof coating will repeatedly expand and contract during the freeze-thaw cycle. At the same time, due to the compatibility of polymers and cement, stress concentration is easily generated, causing fatigue of the waterproof coating. This leads to severe damage to its ductility, making it unable to effectively cope with deformation caused by temperature changes, resulting in cracking or interface peeling. This accelerates the penetration of moisture into the coating, leading to a decrease in the coating's waterproof performance.

[0008] In summary, the research and development of a waterproof coating composition with high elongation and excellent fatigue resistance, a waterproof coating and its preparation method are of great significance for improving the freeze-thaw resistance of waterproof coatings. Summary of the Invention

[0009] The main objective of this invention is to provide a waterproof coating composition, a waterproof coating, its preparation method, and its application, in order to solve the problems of existing waterproof coatings having a high polymer-to-ash ratio, high polymer content, and low elongation of the waterproof coating obtained from them, as well as the severe damage to the extensibility of the coating under freeze-thaw cycles, which easily leads to cracking or peeling, thereby resulting in a decline in waterproof performance.

[0010] To achieve the above objectives, the present invention provides a waterproof coating composition comprising a liquid and a powder; wherein the liquid comprises an acrylic emulsion, a polyetheramine, a double-ended epoxy polyether silicone oil, and a water-reducing agent; and the powder comprises silicate cement and a modified filler, wherein the modified filler is a filler modified with an aminosilane coupling agent.

[0011] Further, by weight, the liquid component comprises: 100 parts acrylate emulsion, 0.5-1 parts polyetheramine, 10-30 parts double-ended epoxy polyether silicone oil, and 0.3-0.5 parts water-reducing agent; the powder component comprises: 40-50 parts silicate cement and 10-30 parts modified filler; preferably, by weight, the liquid component comprises: 100 parts acrylate emulsion, 0.5-0.8 parts polyetheramine, 15-20 parts double-ended epoxy polyether silicone oil, and 0.3-0.5 parts water-reducing agent; the powder component comprises: 40-50 parts silicate cement and 10-20 parts modified filler.

[0012] Furthermore, the weight ratio of liquid to powder is (0.8-1.5):1, preferably (0.8-1.2):1.

[0013] Furthermore, the polyetheramine has a functionality of 2–3, an amine value of 6–7 meq / g, and a molar mass of 300–440 g / mol.

[0014] Further, the polyetheramine is selected from one or more of the group consisting of polyoxyethylene diamine, polyoxyethylene triamine, polyoxypropylene diamine, polyoxypropylene triamine, polyoxybutylene diamine, polyoxybutylene triamine, poly(1,2)-dimethyloxyethylene diamine, and poly(1,2)-dimethyloxyethylene triamine.

[0015] Furthermore, the epoxy value of the double-ended epoxy polyether silicone oil is 0.15–0.2 mmol / g.

[0016] Furthermore, the acrylate emulsion includes polymer particles, the solid content of the acrylate emulsion is 45-60 wt%, and the solvent of the acrylate emulsion is water.

[0017] Furthermore, the average particle size of the polymer particles in the acrylate emulsion is 0.1–0.5 μm.

[0018] Furthermore, the film-forming temperature of the acrylate emulsion is ≥12℃, preferably 12~30℃.

[0019] Furthermore, the water-reducing agent is selected from polycarboxylate water-reducing agents and / or aminosulfonate water-reducing agents.

[0020] Furthermore, the average particle size of the modified filler is 500–1000 mesh.

[0021] Furthermore, the aminosilane coupling agent is selected from one or more of the group consisting of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane.

[0022] Furthermore, the average particle size of the filler is 500-800 mesh. Preferably, the filler is selected from one or more of the group consisting of silica, heavy calcium carbonate, quartz powder, mica powder and microsilica powder.

[0023] Furthermore, the strength grade of silicate cement is 42.5 to 52.5.

[0024] To achieve the above objectives, another aspect of the present invention provides a waterproof coating, which is obtained by coating and curing the waterproof coating composition provided in this application.

[0025] Another aspect of the present invention provides a method for preparing the above-mentioned waterproof coating provided in this application. The method includes: step S1, mixing acrylate emulsion, polyetheramine, double-ended epoxy polyether silicone oil and water-reducing agent to obtain a liquid; step S2, mixing silicate cement and modified filler to obtain a powder; step S3, mixing the liquid and powder to obtain a waterproof coating; and step S4, applying the waterproof coating to one side surface of the substrate and curing it to obtain a waterproof coating.

[0026] Furthermore, the thickness of the waterproof coating is 1–3 mm.

[0027] Furthermore, the coating is applied 1 to 3 times; preferably, at least two coatings are applied, and the interval between two adjacent coatings is 10 to 24 hours.

[0028] Furthermore, the curing process is a static setting process, with a static temperature of 23–28°C and a time of 96–120 hours.

[0029] Furthermore, the base is a wall.

[0030] Furthermore, the preparation method of the modified filler includes: mixing an aminosilane coupling agent, a filler and a solvent to obtain a mixture; subjecting the mixture to heat treatment, filtration, washing and drying in sequence to obtain the modified filler.

[0031] Furthermore, the weight ratio of aminosilane coupling agent, filler and solvent is (3-5):100:(400-500).

[0032] Furthermore, the solvent is selected from one or more of the group consisting of methanol, ethanol, and isopropanol.

[0033] Furthermore, the heat treatment temperature is 50–60°C, and the time is 5–6 hours.

[0034] The fourth aspect of the present invention also provides an application of the above-mentioned waterproof coating composition provided in this application, or the above-mentioned waterproof coating provided in this application, in the field of waterproofing and leak repair of building structures.

[0035] By applying the technical solution of this invention, this application introduces polyetheramine and double-ended epoxy polyether silicone oil into the liquid component of the waterproof coating composition. The amino groups in the polyetheramine can chemically bond with the epoxy groups in the double-ended epoxy polyether silicone oil and intertwine with the polymer network formed by the acrylate emulsion to form a three-dimensional network structure, thereby improving the fatigue resistance and elongation of the waterproof coating. Simultaneously, the oxygen atoms in the polyetheramine and double-ended epoxy polyether silicone oil can form hydrogen bonds with water molecules, thereby lowering the crystallization temperature of water molecules, inhibiting the formation and growth of ice crystals, delaying the freeze-thaw process, and acting as an antifreeze agent. This further improves the freeze-thaw resistance of the waterproof coating and inhibits cracking or interfacial peeling during freeze-thaw cycles. Introducing a water-reducing agent into the liquid component can, on the one hand, reduce the amount of water used while maintaining good fluidity of the waterproof coating, thereby inhibiting the decrease in mechanical strength of the waterproof coating due to excessive water content and improving the durability of the waterproof coating. On the other hand, it can enhance the interfacial bonding force between the liquid and powder components, inhibiting cracks at the interface. When the liquid and powder components are mixed, the silicate cement in the powder undergoes a hydration reaction upon contact with water. The resulting hydration products form an inorganic skeleton, which, together with the three-dimensional network structure of the polymer in the liquid component, creates a denser composite system, thereby improving the hardness, mechanical strength, and impermeability of the waterproof coating. Introducing aminosilane coupling agent-modified fillers into the powder component of the waterproof coating composition allows the amino groups on their surface to react with the epoxy groups in the double-ended epoxy polyether silicone oil, thereby enhancing the interfacial forces between the inorganic filler and the organic polymer in the liquid component, reducing the interfacial peeling rate of the waterproof coating, and thus inhibiting cracking or interfacial peeling during freeze-thaw cycles.

[0036] In summary, the waterproof coating prepared using the waterproof coating described in this application has a high elongation rate and excellent freeze-thaw resistance. When applied to the field of waterproofing and repair of building structures, even under frequent freeze-thaw cycles in the north, the waterproof coating can maintain its integrity and excellent waterproofing effect, providing buildings with more durable and reliable waterproof protection. Detailed Implementation

[0037] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.

[0038] As described in the background section, existing waterproof coatings suffer from problems such as high polymer-to-ash ratio, high polymer content, and low elongation of the resulting waterproof coating. Furthermore, the coating's ductility is severely damaged under freeze-thaw cycles, leading to cracking or peeling and consequently reduced waterproof performance. To address these technical problems, this application provides a waterproof coating composition comprising a liquid and a powder. The liquid comprises an acrylic emulsion, polyetheramine, double-ended epoxy polyether silicone oil, and a water-reducing agent. The powder comprises silicate cement and a modified filler, wherein the modified filler is an aminosilane coupling agent-modified filler.

[0039] This application introduces polyetheramine and double-ended epoxy polyether silicone oil into the liquid component of a waterproof coating composition. The amino groups in the polyetheramine can chemically bond with the epoxy groups in the double-ended epoxy polyether silicone oil and intertwine with the polymer network formed by the acrylate emulsion to form a three-dimensional network structure, thereby improving the fatigue resistance and elongation of the waterproof coating. Simultaneously, the oxygen atoms in the polyetheramine and double-ended epoxy polyether silicone oil can form hydrogen bonds with water molecules, thereby lowering the crystallization temperature of water molecules, inhibiting the formation and growth of ice crystals, delaying the freeze-thaw process, and acting as an antifreeze agent. This further enhances the freeze-thaw resistance of the waterproof coating and inhibits cracking or interfacial peeling during freeze-thaw cycles. Introducing a water-reducing agent into the liquid component can, on the one hand, reduce the amount of water used while maintaining good fluidity of the waterproof coating, thereby inhibiting the decrease in mechanical strength of the waterproof coating due to excessive water content and improving the durability of the waterproof coating. On the other hand, it can enhance the interfacial bonding force between the liquid and powder components, inhibiting cracks at the interface. When the liquid and powder components are mixed, the silicate cement in the powder undergoes a hydration reaction upon contact with water. The resulting hydration products form an inorganic skeleton, which, together with the three-dimensional network structure of the polymer in the liquid component, creates a denser composite system, thereby improving the hardness, mechanical strength, and impermeability of the waterproof coating. Introducing aminosilane coupling agent-modified fillers into the powder component of the waterproof coating composition allows the amino groups on their surface to react with the epoxy groups in the double-ended epoxy polyether silicone oil, thereby enhancing the interfacial forces between the inorganic filler and the organic polymer in the liquid component, reducing the interfacial peeling rate of the waterproof coating, and thus inhibiting cracking or interfacial peeling during freeze-thaw cycles.

[0040] In summary, the waterproof coating prepared using the waterproof coating described in this application has a high elongation rate and excellent freeze-thaw resistance. When applied to the field of waterproofing and repair of building structures, even under frequent freeze-thaw cycles in the north, the waterproof coating can maintain its integrity and excellent waterproofing effect, providing buildings with more durable and reliable waterproof protection.

[0041] In a preferred embodiment, the liquid component, by weight, comprises: 100 parts acrylate emulsion, 0.5-1 part polyetheramine, 10-30 parts double-ended epoxy polyether silicone oil, and 0.3-0.5 parts water-reducing agent; the powder component comprises: 40-50 parts silicate cement and 10-30 parts modified filler. The weight percentages of each component in the liquid and powder components include, but are not limited to, the ranges described above. Limiting these percentages to the ranges facilitates the synergistic effect of the components, promotes the formation of a denser three-dimensional network structure, and thus improves the elongation and freeze-thaw resistance of the waterproof coating, suppressing cracking or interfacial peeling during freeze-thaw cycles. The use of an appropriate amount of polyetheramine is particularly important. Compared to other ranges, limiting the weight percentage of polyetheramine to the ranges described above improves the elongation at break of the waterproof coating, reduces the loss of elongation at break during freeze-thaw cycles, and simultaneously prevents a decrease in the mechanical strength of the waterproof coating due to excessive polyetheramine.

[0042] To further enhance the synergistic effect of each component and form a denser three-dimensional network structure, thereby further improving the elongation and freeze-thaw resistance of the waterproof coating and further suppressing cracking or interface peeling during freeze-thaw cycles, preferably, by weight, the liquid component includes: 100 parts of acrylic emulsion, 0.5-0.8 parts of polyetheramine, 15-20 parts of double-ended epoxy polyether silicone oil, and 0.3-0.5 parts of water-reducing agent; the powder component includes: 40-50 parts of silicate cement and 10-20 parts of modified filler.

[0043] In a preferred embodiment, the weight ratio of liquid to powder is (0.8–1.5):1. The weight ratio of liquid to powder includes, but is not limited to, the above range. Limiting it to this range is beneficial for improving the rheological properties of the waterproof coating, facilitating its application to different substrate surfaces, forming a more uniform and dense waterproof coating, and simultaneously improving the elongation, fatigue resistance, hardness, and mechanical strength of the waterproof coating. It also reduces the elongation loss rate of the waterproof coating during freeze-thaw cycles, thereby helping to suppress cracking or interfacial peeling during freeze-thaw cycles.

[0044] To further improve the rheological properties of the waterproof coating, form a more uniform and dense waterproof coating, further enhance the elongation, fatigue resistance, hardness, and mechanical strength of the waterproof coating, and further suppress cracking or interfacial delamination during freeze-thaw cycles, preferably, the weight ratio of liquid to powder is (0.8–1.2):1. Specifically, the weight ratio of liquid to powder can be 0.8:1, 0.9:1, 1:1, 1.1:1, or 1.2:1.

[0045] In a preferred embodiment, the polyetheramine has a functionality of 2-3, an amine value of 6-7 meq / g, and a molar mass of 300-440 g / mol. The functionality, amine value, and weight-average molecular weight of the polyetheramine include, but are not limited to, the above ranges. Limiting them to these ranges is beneficial for improving the compatibility of the components in the liquid, and for enabling the polyetheramine to chemically bond with the double-ended epoxy polyether silicone oil to form a cross-linked network. This, in turn, helps to improve the mechanical strength and elongation of the waterproof coating, reduces the elongation loss rate of the waterproof coating during freeze-thaw cycles, and also improves the freeze-thaw resistance of the waterproof coating, inhibiting cracking or interfacial peeling during freeze-thaw cycles.

[0046] It should be noted that the amine value of the polyetheramine mentioned above in this application was determined by the method described in the national standard GB / T6365-2006 "Determination of free alkalinity or free acidity of surfactants by titration".

[0047] In a preferred embodiment, the polyetheramine includes, but is not limited to, one or more of the following groups: polyoxyethylene diamine, polyoxyethylene triamine, polyoxypropylene diamine, polyoxypropylene triamine, polyoxybutylene diamine, polyoxybutylene triamine, poly(1,2)-dimethyloxyethylene diamine, and poly(1,2)-dimethyloxyethylene triamine. Compared to other types, using the above-mentioned types of polyetheramines is beneficial for improving the compatibility of the components in the liquid, and for chemically bonding with the double-ended epoxy polyether silicone oil to form a three-dimensional network structure with a higher crosslinking density. This further improves the mechanical strength and elongation of the waterproof coating, reduces the elongation loss rate of the waterproof coating during freeze-thaw cycles, and further enhances the freeze-thaw resistance of the waterproof coating, suppressing cracking or interfacial peeling during freeze-thaw cycles.

[0048] In a preferred embodiment, the epoxy value of the dual-terminated epoxy polyether silicone oil is 0.15–0.2 mmol / g. The epoxy value of the dual-terminated epoxy polyether silicone oil includes, but is not limited to, the above range. Limiting it to this range is beneficial for improving the compatibility of the dual-terminated epoxy polyether silicone oil with other components in the liquid, allowing the dual-terminated epoxy polyether silicone oil to chemically bond with the polyether amine to form a cross-linked network. This, in turn, helps improve the mechanical strength and elongation of the waterproof coating, reduces the elongation loss rate of the waterproof coating during freeze-thaw cycles, and also improves the freeze-thaw resistance of the waterproof coating, inhibiting cracking or interfacial peeling during freeze-thaw cycles.

[0049] It should be noted that the epoxy value of the double-ended epoxy polyether silicone oil mentioned above in this application was measured using the method described in the national standard GB / T1677-2008 "Determination of Epoxy Value of Plasticizers".

[0050] Acrylic emulsion is an aqueous dispersion prepared by emulsion polymerization technology, containing tiny polymer particles mainly composed of acrylate monomers polymerized and stably dispersed in water to form an acrylic emulsion. In a preferred embodiment, the acrylic emulsion includes polymer particles, has a solid content of 45-60 wt%, and uses water as the solvent. The solid content of the acrylic emulsion includes, but is not limited to, the above range. Limiting it within this range is beneficial for improving the film-forming properties of the acrylic emulsion, forming a uniform and dense waterproof coating, and improving the elongation, mechanical properties, and durability of the waterproof coating, while inhibiting cracking or interfacial peeling during freeze-thaw cycles.

[0051] To further improve the film-forming properties of acrylic emulsions, form a more uniform and dense waterproof coating, further improve the elongation, mechanical properties and durability of the waterproof coating, and further suppress cracking or interfacial peeling during freeze-thaw cycles, preferably, the average particle size of the polymer particles in the acrylic emulsion is 0.1 to 0.5 μm.

[0052] The waterproof coating composition of this application can cure into a film at a relatively low temperature. In order to form a more uniform and stable waterproof coating, further improve the film quality of the waterproof coating, and further suppress cracking or interfacial peeling during freeze-thaw cycles, preferably, the film-forming temperature of the acrylic emulsion is ≥12°C, more preferably 12-30°C.

[0053] In a preferred embodiment, the water-reducing agent includes, but is not limited to, polycarboxylate water-reducing agents and / or aminosulfonate water-reducing agents. Compared to other types, using the above-mentioned types of water-reducing agents is beneficial in two ways: firstly, it improves the dispersibility of the liquid material, which helps to reduce the amount of water used while maintaining good fluidity of the waterproof coating, thereby inhibiting the decrease in mechanical strength of the waterproof coating due to excessive water content and improving the durability of the waterproof coating; secondly, it also helps to enhance the interfacial bonding force between the liquid material and the powder material, and inhibits the appearance of cracks at the interface.

[0054] In a preferred embodiment, the average particle size of the modified filler is 500-1000 mesh. The average particle size of the modified filler includes, but is not limited to, the above range. Limiting it to this range helps to enhance the interfacial interaction between the inorganic filler and the organic polymer in the liquid, improve the hardness and mechanical strength of the waterproof coating, and reduce its interfacial peeling rate. This, in turn, helps to suppress cracking or interfacial peeling of the waterproof coating during freeze-thaw cycles.

[0055] To further improve the interfacial bonding strength between the inorganic filler and the organic polymer in the liquid, further reduce the interfacial peeling rate of the waterproof coating, and simultaneously form a modified filler with superior performance, thereby further improving the elongation, fatigue resistance and mechanical strength of the waterproof coating, preferably, the aminosilane coupling agent includes, but is not limited to, one or more of the group consisting of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane.

[0056] To further improve the interfacial bonding strength between the inorganic filler and the organic polymer in the liquid, further reduce the interfacial peeling rate of the waterproof coating, and improve the rheological properties of the waterproof coating, the filler preferably has an average particle size of 500-800 mesh.

[0057] To further improve the interfacial bonding strength between the inorganic filler and the organic polymer in the liquid, and to further improve the elongation, fatigue resistance and mechanical strength of the waterproof coating, preferably, the filler includes, but is not limited to, one or more of the group consisting of silica, heavy calcium carbonate, quartz powder, mica powder and microsilica powder.

[0058] It should be noted that the aforementioned heavy calcium carbonate in this application refers to a powdered inorganic filler made from ground natural carbonate minerals (such as calcite, marble, and limestone). Microsilica powder is produced by collecting and treating the flue gas emitted with the exhaust gas during the high-temperature smelting of industrial silicon and ferrosilicon in industrial electric furnaces using a special collection device.

[0059] In a preferred embodiment, the strength grade of the silicate cement is 42.5 to 52.5. The strength of the silicate cement includes, but is not limited to, the above range. Limiting it to this range is beneficial for improving the hardness, mechanical strength, and impermeability of the waterproof coating, thereby improving the waterproof performance and durability of the waterproof coating.

[0060] The second aspect of this application also provides a waterproof coating, which is obtained by coating and curing the aforementioned waterproof coating composition provided in this application. This application introduces polyetheramine and double-ended epoxy polyether silicone oil into the liquid component of the waterproof coating composition, and simultaneously introduces an aminosilane coupling agent-modified filler into the powder component of the waterproof coating composition. The waterproof coating obtained by coating and curing the aforementioned waterproof coating composition provided in this application has high elongation and excellent freeze-thaw resistance, with a low elongation loss rate during freeze-thaw cycles. When applied to the field of waterproofing and leak repair in building structures, even under frequent freeze-thaw cycles in northern regions, the aforementioned waterproof coating can maintain the integrity and waterproofing effect of the coating, without cracking or interface peeling. It can provide more durable and reliable waterproof protection for buildings, thereby reducing maintenance costs and improving the safety, comfort, and overall durability of the living and use environment.

[0061] A third aspect of this application also provides a method for preparing the above-mentioned waterproof coating provided in this application. The method includes: step S1, mixing acrylate emulsion, polyetheramine, double-ended epoxy polyether silicone oil and water-reducing agent to obtain a liquid; step S2, mixing silicate cement and modified filler to obtain a powder; step S3, mixing the liquid and powder to obtain a waterproof coating; and step S4, applying the waterproof coating to one side surface of the substrate and curing it to obtain a waterproof coating.

[0062] In the preparation method provided in this application, step S1 introduces polyetheramine and double-ended epoxy polyether silicone oil into the liquid material, which can interact with the acrylate emulsion to form a three-dimensional network structure, thereby improving the fatigue resistance and elongation of the waterproof coating. Step S2 introduces modified filler into the powder, whose surface amino groups can react with the epoxy groups in the double-ended epoxy polyether silicone oil, thereby enhancing the interfacial interaction between the inorganic filler and the organic polymer in the liquid material, reducing the interfacial peeling rate of the waterproof coating, and thus inhibiting cracking or interfacial peeling during freeze-thaw cycles. Step S4 coats the waterproof coating obtained in step S3 onto the surface of the substrate, and after curing, a waterproof coating is obtained. The waterproof coating prepared by the above-described method of this application has high elongation and excellent freeze-thaw resistance. The elongation loss rate is low during freeze-thaw cycles. When applied to the field of waterproofing and repair of building structures, even under frequent freeze-thaw cycles in the north, the above-described waterproof coating can maintain the integrity of the coating and the waterproof effect without cracking or peeling. It can provide more durable and reliable waterproof protection for buildings, thereby reducing maintenance costs and improving the safety, comfort and overall durability of the living and use environment.

[0063] The waterproof coating provided in this application is suitable for waterproofing projects on the walls of various buildings, effectively inhibiting water penetration and protecting the wall surface from damage. In a preferred embodiment, the substrate is a wall surface. Specifically, the wall surface can be a sealing surface for holes of pipes penetrating the wall, a sealing surface for holes of cables penetrating the wall, or a wall surface with embedded pipes or cables.

[0064] In a preferred embodiment, the thickness of the waterproof coating is 1–3 mm. The thickness of the waterproof coating includes, but is not limited to, the above range; limiting it within this range is beneficial for improving the waterproof performance, mechanical strength, and freeze-thaw resistance of the waterproof coating.

[0065] In order to obtain a waterproof coating of suitable thickness and further improve the film-forming quality of the waterproof coating, thereby further improving the waterproof performance, elongation, mechanical strength and freeze-thaw resistance of the waterproof coating, in a preferred embodiment, the coating is applied 1 to 3 times.

[0066] To further improve the film quality of the waterproof coating, the next coating should be applied only after the previous coating has completely dried. Preferably, at least two coatings are applied, with an interval of 10 to 24 hours between adjacent coatings.

[0067] This application does not limit the amount of waterproof coating applied to the substrate surface, as long as the waterproof coating of the thickness described above can be obtained after curing.

[0068] In order to promote the curing of the waterproof coating and form a denser and more stable waterproof coating, thereby improving the elongation, mechanical strength and freeze-thaw resistance of the waterproof coating, in a preferred embodiment, the curing process is a static process with a static temperature of 23-28°C and a time of 96-120 hours.

[0069] In a preferred embodiment, the modified filler preparation method includes: mixing an aminosilane coupling agent, a filler, and a solvent to obtain a mixture; and sequentially subjecting the mixture to heat treatment, filtration, washing, and drying to obtain the modified filler. Heat treatment promotes the reaction between the aminosilane coupling agent and the active groups on the filler surface, improving the bonding between the aminosilane coupling agent and the filler, thereby obtaining the modified filler. This enhances the interfacial interaction between the inorganic filler and the organic polymer in the liquid, reduces the interfacial peeling rate of the waterproof coating, and thus inhibits cracking or interfacial peeling during freeze-thaw cycles.

[0070] In a preferred embodiment, the weight ratio of the aminosilane coupling agent, filler, and solvent is (3-5):100:(400-500). The weight ratio of the aminosilane coupling agent, filler, and solvent includes, but is not limited to, the above range. Limiting it to this range is beneficial for improving the modification efficiency of the aminosilane coupling agent on the filler surface, and for ensuring sufficient modification of the filler to obtain a modified filler with superior performance.

[0071] To improve the dispersibility of aminosilane coupling agents and fillers, in a preferred embodiment, the solvent includes, but is not limited to, one or more of the group consisting of methanol, ethanol, and isopropanol.

[0072] In a preferred embodiment, the heat treatment temperature is 50–60°C, and the time is 5–6 hours. The heat treatment temperature and time include, but are not limited to, the above range. Limiting them to the above range is beneficial to improving the modification efficiency, ensuring that the filler is fully modified, and at the same time, it is beneficial to suppress insufficient modification caused by uneven local heating.

[0073] The fourth aspect of this application also provides an application of the above-mentioned waterproof coating composition or waterproof coating provided in this application in the field of waterproofing and leak repair of building structures. The above-mentioned waterproof coating has high elongation and excellent freeze-thaw resistance, with a low elongation loss rate during freeze-thaw cycles. When applied to the field of waterproofing and leak repair of building structures, even under frequent freeze-thaw cycles in northern regions, the above-mentioned waterproof coating can maintain the integrity and waterproofing effect of the coating, without cracking or interface peeling. It can provide more durable and reliable waterproof protection for buildings, thereby reducing maintenance costs and improving the safety, comfort, and overall durability of the living and use environment.

[0074] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.

[0075] Example 1

[0076] A method for preparing a waterproof coating includes the following steps:

[0077] (1) Preparation of modified filler: 1 kg of heavy calcium carbonate (Jiangxi Guangyuan Chemical Co., Ltd., CC-800, average particle size of 800 mesh), 0.05 kg of 3-aminopropyltrimethoxysilane and 5 kg of ethanol were mixed to obtain a mixture; the mixture was heated to 60℃ and reacted for 6 h. After the reaction was completed, the mixture was filtered, and then the filter cake was washed with water 3 times and dried at 60℃ to constant weight to obtain the modified filler.

[0078] (2) Preparation of liquid material: 1000g of acrylate emulsion, 8g of polyoxypropylene triamine, 200g of double-ended epoxy polyether silicone oil and 5g of polycarboxylate superplasticizer are placed in a disperser and mixed evenly to obtain liquid material;

[0079] The acrylate emulsion was purchased from BASF, model Acronal PA 237ap, with a solid content of 48 wt%, an average particle size of 0.1 μm, and a minimum film-forming temperature of 13 °C; the polyoxypropylene triamine was purchased from Huntsman, model T403, with a functionality of 3, an amine value of 6.6 meq / g, and a molar mass of 440 g / mol; the double-ended epoxy polyether silicone oil was purchased from Anhui Aiyota Silicone Oil Co., Ltd., model IOTA-EO9000, with an epoxy value of 0.2 mmol / g; and the polycarboxylate superplasticizer was purchased from BASF, model RHEOPLUS420.

[0080] (3) Preparation of powder: Mix 500g of silicate cement (Anhui Conch Cement Co., Ltd., PO42.5, strength grade 42.5) and 200g of modified filler obtained in step (1) evenly to obtain powder;

[0081] (4) Preparation of waterproof coating: The liquid material obtained in step (2) and the powder material obtained in step (3) are mixed at a weight ratio of 1.2:1 to obtain the waterproof coating;

[0082] (5) Apply the waterproof coating obtained in step (4) to the surface of the hole sealing surface of the through-wall cable in three layers. The next layer of coating should be applied after the previous layer has dried completely. The interval between two adjacent layers of coating is 12 hours. After the coating is completed, cure it for 96 hours at 23°C and 50% relative humidity to obtain a waterproof coating with a thickness of 1.5 mm.

[0083] Example 2

[0084] The difference from Example 1 is that in step (2), an equal amount of double-ended epoxy polyether silicone oil of type IOTA-EO14000 (purchased from Anhui Aiyota Silicone Oil Co., Ltd., with a functionality of 2 and an epoxy value of 0.15 mmol / g) is used to replace the double-ended epoxy polyether silicone oil of type IOTA-EO9000 in Example 1, and the remaining steps are the same as in Example 1.

[0085] Examples 3 to 6

[0086] The difference from Example 1 is that, based on 100 parts by weight of acrylate emulsion, the amount of each component of the liquid in step (2) and the amount of each component of the powder in step (3) are different from those in Example 1, as shown in Table 1. The remaining steps are the same as those in Example 1.

[0087] Table 1

[0088]

[0089] Example 7

[0090] The difference from Example 1 is that in step (2), an equal amount of polyoxyethylene diamine (purchased from Shanghai Xuanya Biotechnology Co., Ltd., with a functionality of 2 and an amine value of 6 meq / g) is used to replace the polyoxypropylene triamine in Example 1. In step (3), the weight of the modified filler is 150g, and in step (4), the liquid and powder are mixed at a weight ratio of 0.8:1 to obtain the waterproof coating. The remaining steps are the same as in Example 1.

[0091] Comparative Example 1

[0092] The difference from Example 1 is that in step (2), polyoxypropylene triamine was not introduced when preparing the liquid, that is, polyetheramine was not introduced. The remaining steps are the same as in Example 1.

[0093] Comparative Example 2

[0094] The difference from Example 1 is that in step (2), no double-ended epoxy polyether silicone oil was introduced when preparing the liquid material, that is, no double-ended epoxy polyether silicone oil was introduced. The remaining steps are the same as in Example 1.

[0095] Comparative Example 3

[0096] The difference from Example 1 is that in step (2), polyoxypropylene triamine and double-ended epoxy polyether silicone oil were not introduced when preparing the liquid material, that is, polyetheramine and double-ended epoxy polyether silicone oil were not introduced. The remaining steps are the same as in Example 1.

[0097] Comparative Example 4

[0098] The difference from Example 1 is that step (1) is omitted, and no modified filler is introduced in step (3). An equal amount of heavy calcium carbonate is used to replace the modified filler in Example 1. The remaining steps are the same as in Example 1.

[0099] The waterproof coatings obtained in Examples 1 to 7 and Comparative Examples 1 to 4 of this application were subjected to the following performance tests:

[0100] (1) Initial tensile strength and initial elongation at break: measured according to the methods described in the national standard GB / T16777-2008 "Test Methods for Waterproof Coatings for Buildings";

[0101] (2) Freeze-thaw cycle test: Place the coating at -20℃ for 4 hours, then raise the temperature to 18℃ and place it at that temperature for 4 hours to complete one freeze-thaw cycle. Repeat the above freeze-thaw cycle 700 times. Visually inspect the surface of the waterproof coating for cracking. Then test the tensile strength and elongation at break of the waterproof coating after the freeze-thaw cycle according to the method described in the national standard GB / T16777-2008. Calculate the tensile strength loss rate according to formula (I). Where T is the initial tensile strength, and T' is the tensile strength after freeze-thaw cycles; the elongation at break loss rate is calculated according to formula (II). Where ε is the initial elongation at break and ε' is the elongation at break after freeze-thaw cycles.

[0102] The test results are shown in Table 2.

[0103] Table 2

[0104]

[0105] As can be seen from the above description, the embodiments of the present invention achieve the following technical effects:

[0106] Comparing Example 1 with Comparative Examples 1 to 3, it can be seen that introducing polyetheramine and double-ended epoxy polyether silicone oil into the liquid component of the waterproof coating composition can work together with the acrylic emulsion to form a three-dimensional network structure, improving the fatigue resistance and elongation of the waterproof coating. At the same time, the oxygen atoms in the polyetheramine and double-ended epoxy polyether silicone oil can form hydrogen bonds with water molecules, thereby lowering the crystallization temperature of water molecules, inhibiting the formation and growth of ice crystals, delaying the freeze-thaw process, and acting as an antifreeze agent. This improves the freeze-thaw resistance of the waterproof coating and inhibits cracking or interfacial peeling during freeze-thaw cycles.

[0107] Comparing Example 1 and Comparative Example 4, it can be seen that when an aminosilane coupling agent is introduced into the powder of the waterproof coating composition, the amino groups on its surface can react with the epoxy groups in the double-ended epoxy polyether silicone oil, thereby enhancing the interfacial force between the inorganic filler and the organic polymer in the liquid, reducing the interfacial peeling rate of the waterproof coating, and thus inhibiting the cracking or interfacial peeling phenomenon during freeze-thaw cycles.

[0108] Comparing Examples 1 and 2, it can be seen that, compared to other ranges, limiting the epoxy value of the double-ended epoxy polyether silicone oil to the range described above in this application is beneficial to improving the compatibility of the double-ended epoxy polyether silicone oil with other components in the liquid material, enabling the double-ended epoxy polyether silicone oil to chemically bond with the polyether amine to form a cross-linked network. This is beneficial to improving the mechanical strength and elongation of the waterproof coating, reducing the elongation loss rate of the waterproof coating during freeze-thaw cycles, and also improving the freeze-thaw resistance of the waterproof coating, suppressing cracking or interface peeling during freeze-thaw cycles.

[0109] Comparing Examples 1, 3, and 4, it can be seen that, compared to other ranges, limiting the weight parts of polyoxypropylene triamine and double-ended epoxy polyether silicone oil within the above range is beneficial to the synergistic effect of the two, forming a denser three-dimensional network structure, which is beneficial to improving the elongation and freeze-thaw resistance of the waterproof coating, and suppressing the phenomenon of cracking or interface peeling during freeze-thaw cycles.

[0110] Comparing Examples 1, 4 to 6, it can be seen that the amount of polyoxypropylene triamine used in Examples 5 and 6 is outside the preferred range. The waterproof coatings prepared in Examples 5 and 6 cracked after freeze-thaw cycle testing, and the loss rates of tensile strength and elongation at break were significantly higher than those in Examples 1 and 4. Therefore, compared to other ranges, limiting the weight fraction of polyetheramine within the above range is beneficial in two ways: firstly, it helps to suppress the decrease in mechanical strength of the waterproof coating due to excessive polyetheramine, improves the elongation at break of the waterproof coating, and reduces the loss of elongation at break during freeze-thaw cycles; secondly, it facilitates the formation of appropriate amounts of hydrogen bonds between oxygen atoms in the polyetheramine and water molecules, thereby lowering the crystallization temperature of water molecules, inhibiting the formation and growth of ice crystals, delaying the freeze-thaw process, and acting as an antifreeze agent. This, in turn, helps to improve the freeze-thaw resistance of the waterproof coating and inhibits cracking or interfacial peeling during freeze-thaw cycles.

[0111] Comparing Examples 1 and 7, it can be seen that, compared to other ranges, limiting the functionality, amine value, and molar mass of polyetheramine within the above-mentioned ranges is beneficial to improving the compatibility of the components in the liquid material, and to enabling polyetheramine to form a cross-linked network through chemical bonding with the double-ended epoxy polyether silicone oil. This improves the mechanical strength and elongation of the waterproof coating, reduces the elongation loss rate of the waterproof coating during freeze-thaw cycles, and also improves the freeze-thaw resistance of the waterproof coating, suppressing cracking or interfacial peeling during freeze-thaw cycles.

[0112] It should be noted that the terms "first," "second," etc., used in the specification and claims of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such terms can be used interchangeably where appropriate so that the embodiments of this application described herein can be implemented, for example, in a sequence other than those described herein.

[0113] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A waterproof coating composition, characterized in that, The waterproof coating composition comprises a liquid component and a powder component; wherein, the liquid component comprises an acrylic emulsion, a polyetheramine, a double-ended epoxy polyether silicone oil, and a water-reducing agent; the powder component comprises silicate cement and a modified filler, wherein the modified filler is a filler modified with an aminosilane coupling agent. By weight, the liquid component comprises: 100 parts acrylate emulsion, 0.5-0.8 parts polyetheramine, 15-20 parts double-ended epoxy polyether silicone oil, and 0.3-0.5 parts water-reducing agent; the powder component comprises: 40-50 parts silicate cement and 10-20 parts modified filler.

2. The waterproof coating composition according to claim 1, characterized in that, The weight ratio of the liquid to the powder is (0.8-1.5):

1.

3. The waterproof coating composition according to claim 2, characterized in that, The weight ratio of the liquid to the powder is (0.8 to 1.2):

1.

4. The waterproof coating composition according to claim 1, characterized in that, The polyetheramine has a functionality of 2-3, an amine value of 6-7 meq / g, and a molar mass of 300-440 g / mol.

5. The waterproof coating composition according to claim 1, characterized in that, The polyetheramine is selected from one or more of the group consisting of polyoxyethylene diamine, polyoxyethylene triamine, polyoxypropylene diamine, polyoxypropylene triamine, polyoxybutylene diamine, polyoxybutylene triamine, poly(1,2)-dimethyloxyethylene diamine, and poly(1,2)-dimethyloxyethylene triamine.

6. The waterproof coating composition according to claim 1, characterized in that, The epoxy value of the double-ended epoxy polyether silicone oil is 0.15 to 0.2 mmol / g.

7. The waterproof coating composition according to any one of claims 1 to 3, characterized in that, The acrylate emulsion comprises polymer particles, the solid content of the acrylate emulsion is 45-60 wt%, and the solvent of the acrylate emulsion is water; The average particle size of the polymer particles in the acrylate emulsion is 0.1–0.5 μm; The film-forming temperature of the acrylate emulsion is ≥12℃; The water-reducing agent is selected from polycarboxylate water-reducing agents and / or aminosulfonate water-reducing agents.

8. The waterproof coating composition according to claim 7, characterized in that, The film-forming temperature of the acrylate emulsion is 12–30°C.

9. The waterproof coating composition according to any one of claims 1 to 3, characterized in that, The average particle size of the modified filler is 500-1000 mesh; The aminosilane coupling agent is selected from one or more of the group consisting of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane and N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane; The average particle size of the filler is 500-800 mesh, and the filler is selected from one or more of the group consisting of silica, heavy calcium carbonate, quartz powder, mica powder and microsilica powder. The strength grade of the silicate cement is 42.5 to 52.

5.

10. A waterproof coating, characterized in that, The waterproof coating is obtained by coating and curing the waterproof coating composition according to any one of claims 1 to 9.

11. A method for preparing the waterproof coating according to claim 10, characterized in that, The preparation method includes: Step S1: Mix acrylate emulsion, polyetheramine, double-ended epoxy polyether silicone oil and water-reducing agent to obtain liquid material; Step S2: Mix silicate cement and modified filler to obtain powder; Step S3: Mix the liquid and the powder to obtain a waterproof coating; Step S4: Apply the waterproof coating to one side of the substrate and cure to obtain the waterproof coating.

12. The method for preparing the waterproof coating according to claim 11, characterized in that, The thickness of the waterproof coating is 1-3 mm; The coating is applied 1 to 3 times; The curing process is a static setting process, and the static setting temperature is 23-28°C for 96-120 hours. The base is a wall.

13. The method for preparing the waterproof coating according to claim 12, characterized in that, The coating is applied at least twice, with an interval of 10 to 24 hours between each two coating applications.

14. The method for preparing the waterproof coating according to claim 11, characterized in that, The method for preparing the modified filler includes: mixing an aminosilane coupling agent, a filler, and a solvent to obtain a mixture; and sequentially subjecting the mixture to heat treatment, filtration, washing, and drying to obtain the modified filler. The weight ratio of the aminosilane coupling agent, the filler, and the solvent is (3-5):100:(400-500). The solvent is selected from one or more of the group consisting of methanol, ethanol and isopropanol; The heat treatment is performed at a temperature of 50–60°C for 5–6 hours.

15. The application of a waterproof coating composition according to any one of claims 1 to 9 or the waterproof coating according to claim 10 in the field of waterproofing and repair of building structures.

Citation Information

Patent Citations

  • Polymer cement-based waterproof coating

    CN104591599A

  • Polymer cement waterproof coating

    CN116004073A

  • Heavy-duty anti-corrosion and anti-rust finish paint for ships and preparation method thereof

    CN115521687A