Composite material, method for manufacturing the same, positive electrode sheet, secondary battery, and electric device
By using a composite material of lithium-containing compounds and catalysts with an average particle size ≤200nm in the battery, the problem of lithium ion consumption in the SEI film was solved, and the battery capacity was improved.
Patent Information
- Application Number
- CN202410346233.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-25
AI Technical Summary
In existing batteries, the formation of the SEI film during the first charge and discharge process consumes a large number of lithium ions, affecting battery capacity. How can a composite material be provided to better replenish lithium ions and improve battery capacity?
A composite material containing lithium compounds, catalysts, and conductive agents is used, wherein the average particle size of the lithium compounds is ≤200nm, and the catalysts include oxides of transition metals, etc. The lithium compounds are decomposed to replenish lithium ions in the battery and improve the conductivity.
It improves the lithium-ion transport and diffusion capabilities of the battery, enhances the battery's conductivity, and thus increases the battery's capacity.
Smart Images

Figure CN120709364B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and in particular to a composite material and its preparation method, a positive electrode sheet, a secondary battery, and an electrical device. Background Technology
[0002] With increasing environmental pollution, the new energy industry is attracting more and more attention. Within the new energy industry, battery technology is a crucial factor in its development.
[0003] The development of battery technology requires consideration of various design factors, such as capacity, energy density, cycle life, and reliability. During the initial charge and discharge of a single battery cell, a solid electrolyte interphase (SEI) film is formed on the surface of the negative electrode. The presence of the SEI film consumes a significant amount of lithium ions, affecting the battery's capacity. Therefore, providing a composite material that can replenish lithium ions more effectively, thereby improving battery capacity, is a pressing technical problem that needs to be solved. Summary of the Invention
[0004] This application is made in view of the above-mentioned issues, and its purpose is to provide a composite material to improve the capacity of a battery.
[0005] To achieve the above objectives, this application provides a composite material and its preparation method, a positive electrode sheet, a secondary battery, and an electrical device.
[0006] In a first aspect, a composite material is provided, comprising: a lithium-containing compound, a catalyst, and a conductive agent, wherein the lithium-containing compound comprises lithium, carbon, and oxygen; the catalyst comprises one or more of transition metal oxides, transition metal carbides, transition metal nitrides, or transition metal phosphides; and the average particle size D1 of the lithium-containing compound satisfies: D1 ≤ 200 nm.
[0007] In this embodiment, the lithium-containing compound can decompose to generate lithium ions, thereby replenishing the battery with lithium ions. The catalyst can catalyze the decomposition of the lithium-containing compound, making it easier for the compound to decompose and thus providing more lithium ions to the battery. The average particle size D1 of the lithium-containing compound satisfies: D1≤200nm. This is beneficial for increasing the contact area between the electrolyte and the lithium-containing compound, thereby facilitating the transport and diffusion of lithium ions. The composite material has a better lithium replenishment effect, which can improve the battery capacity. It also facilitates the contact between the conductive agent and the catalyst and the lithium-containing compound, promoting the catalytic decomposition of the lithium-containing compound and improving the conductivity of the composite material, thus increasing the battery capacity. Therefore, the technical solution of this embodiment can improve the battery capacity.
[0008] In one possible implementation, 20nm ≤ D1 ≤ 200nm. When the average particle size of the lithium-containing compound is greater than or equal to 20nm, it facilitates the preparation of the lithium-containing compound and helps to reduce the complexity of the preparation; when the average particle size of the lithium-containing compound is less than or equal to 200nm, it helps to improve the battery capacity.
[0009] In one possible implementation, 50nm ≤ D1 ≤ 150nm. This results in a more suitable average particle size for the lithium-containing compound, leading to a higher battery capacity.
[0010] In one possible implementation, the composite material further includes a sodium-containing compound, which comprises elemental sodium. During the preparation of the composite material, a sodium source is added to facilitate the preparation of primary lithium-containing compound particles with a smaller average particle size; therefore, the resulting composite material also includes elemental sodium.
[0011] In one possible implementation, the molar ratio W of sodium to lithium in the composite material satisfies: 0.005 ≤ W ≤ 0.12. Thus, in the composite material, a suitable molar content of sodium is beneficial for obtaining a lithium-containing compound with a suitable particle size; and a suitable molar content of lithium is also beneficial for obtaining a battery with high capacity.
[0012] In one possible implementation, 0.025 ≤ W ≤ 0.05. This is beneficial for obtaining lithium-containing compounds with a more suitable particle size, thereby improving battery capacity.
[0013] In one possible implementation, the lithium-containing compound has the chemical formula Li₂C. x O y Where 1≤x≤4, 3≤y≤6. Lithium-containing compounds that satisfy the above chemical formula can decompose into lithium ions and gases (such as carbon monoxide and carbon dioxide) under the action of voltage and catalyst. The lithium ions produced by decomposition can supplement lithium ions, which is beneficial to improving the battery capacity. The gases produced by decomposition will not remain in the positive electrode, and the residues produced by decomposition will not affect the long-term reliability and other performance of the battery cells.
[0014] In one possible implementation, the lithium-containing compound includes one or more of Li₂C₂O₄, Li₂CO₃, Li₂C₄O₄, Li₂C₃O₅, or Li₂C₄O₆. Under the influence of voltage and a catalyst, the aforementioned lithium-containing compound can decompose into lithium ions and gases (e.g., carbon monoxide, carbon dioxide). The lithium ions produced during decomposition can replenish lithium ions, which is beneficial for improving battery capacity. The gases produced during decomposition do not remain in the positive electrode, and the residues from decomposition do not affect the long-term reliability or other performance characteristics of the battery cells. Furthermore, the aforementioned lithium-containing compound exhibits good stability, remaining stable in air and organic solvents, and is compatible with the coating process of the positive electrode slurry.
[0015] In one possible implementation, the composite material has a secondary particle morphology. A lithium-containing compound, a conductive agent, and a catalyst are mixed together to form a composite material with a secondary particle morphology.
[0016] In one possible implementation, the lithium-containing compound is in the form of primary particles. On the one hand, this facilitates sufficient contact between the lithium-containing compound and the catalyst to achieve better catalytic effect, thereby reducing the decomposition voltage of the lithium-containing compound and increasing the battery capacity. On the other hand, the conductive agent is dispersed around the lithium-containing compound in the primary particles, which helps to improve the electronic conductivity of the lithium-containing compound, thereby helping to increase the battery capacity.
[0017] In one possible implementation, the volume average particle size Dv50 of the composite material satisfies: 2μm≤Dv50≤10μm.
[0018] When the volume average particle size Dv50 of the composite material is not less than 2 μm, the risk of composite material agglomeration and the difficulty of composite material preparation can be reduced. When the volume average particle size Dv50 of the composite material does not exceed 10 μm, the composite material has a suitable particle size, and the lithium ions extracted from the lithium-containing compound have a suitable diffusion distance, which is conducive to the lithium ion having a high transport rate and the extraction of more lithium ions, thereby improving the battery capacity.
[0019] In one possible implementation, 4μm ≤ Dv50 ≤ 8μm. This allows the battery to have a higher capacity.
[0020] In one possible implementation, based on the total mass of the composite material, the mass content A of the conductive agent satisfies: 1wt% ≤ A ≤ 40wt%.
[0021] When the mass content A of the conductive agent is not less than 1 wt%, the composite material has high conductivity and low resistivity; when the mass content A of the conductive agent is not more than 40 wt%, the conductive agent has a suitable mass ratio, the catalyst and lithium-containing compound also have suitable mass ratios, and the battery cell has a suitable capacity.
[0022] In one possible implementation, 2wt% ≤ A ≤ 20wt%. This results in a more suitable mass ratio of conductive agent and a higher battery capacity.
[0023] In one possible implementation, based on the total mass of the composite material, the mass content B of the catalyst satisfies: 0.5wt% ≤ B ≤ 20wt%.
[0024] When the mass content of catalyst B is not less than 0.5 wt%, the contact area between the catalyst and the lithium-containing compound is suitable, resulting in a better catalytic effect, which is beneficial for the decomposition of lithium-containing compounds and for improving battery capacity. When the mass content of catalyst B does not exceed 20 wt%, it is beneficial for adding more lithium-containing compounds to the composite material, which is beneficial for improving battery capacity.
[0025] In one possible implementation, 1wt% ≤ B ≤ 10wt%. This results in a more suitable mass ratio of catalyst and a higher battery capacity.
[0026] In one possible implementation, the chemical formula of the transition metal oxide is M. α O β Where 0 < α ≤ 3, 0 < β ≤ 5, and M includes one or more of Ni, Co, Fe, Mn, V, Cr, Cu, or Ti; optionally, M α O β These catalysts include one or more of NiO, Co3O4, Fe2O3, MoO3, or V2O5. These catalysts can lower the decomposition voltage of lithium-containing compounds, allowing them to decompose at lower voltages.
[0027] In one possible implementation, the transition metal carbide includes one or more of molybdenum carbide, vanadium carbide, tungsten carbide, titanium carbide, cobalt carbide, iron carbide, or nickel carbide; and / or, the transition metal nitride includes one or more of molybdenum nitride, vanadium nitride, titanium nitride, manganese nitride, cobalt nitride, iron nitride, or nickel nitride; and / or, the transition metal phosphide includes one or more of nickel phosphide, cobalt phosphide, manganese phosphide, tungsten phosphide, or molybdenum phosphide. The aforementioned transition metal carbides, transition metal nitrides, and transition metal phosphides exhibit good catalytic effects and can catalyze the decomposition of lithium-containing compounds.
[0028] In one possible implementation, the conductive agent comprises a carbon material; optionally, the conductive agent comprises a carbon-based conductive agent; optionally, the carbon-based conductive agent comprises one or more of the following: carbon nanotubes, carbon fibers, acetylene black, Ketjen black, conductive carbon black, C60, or graphene. Carbon materials have good electrical conductivity and are well compatible with other materials in the battery; including carbon materials in the composite material helps to reduce the resistivity of the composite material, improve the conductivity of the composite material, and increase the battery capacity.
[0029] In one possible implementation, the powder resistivity R of the composite material at 20 MPa satisfies: R ≤ 360 Ω·cm. This results in a low powder resistivity, which is beneficial for improving the conductivity of the composite material and thus increasing the battery capacity.
[0030] In one possible implementation, R ≤ 1 Ω·cm. This is beneficial for further improving the conductivity of the composite material, resulting in a battery with higher capacity.
[0031] Secondly, a method for preparing a composite material is provided, comprising: adding a lithium source, a catalyst, a conductive agent, and a sodium source to a solvent to obtain a slurry, wherein the catalyst comprises one or more of a transition metal oxide, a transition metal carbide, a transition metal nitride, or a transition metal phosphide; and drying the slurry to obtain the composite material. In the composite material prepared by this method, the lithium-containing compound has a smaller primary particle size, which is beneficial for improving battery capacity.
[0032] In one possible implementation, drying the slurry to obtain the composite material includes: drying the slurry by spray drying to obtain the composite material. Choosing spray drying facilitates the preparation of lithium-containing compounds with smaller particle sizes and the fabrication of the composite material.
[0033] In one possible implementation, the drying temperature T satisfies: 150℃ ≤ T ≤ 250℃; alternatively, 175℃ ≤ T ≤ 225℃. The drying temperature affects the growth and nucleation process of secondary particles in the composite material. By selecting a temperature within the above range, it is beneficial to obtain composite secondary particles with a suitable particle size.
[0034] In one possible implementation, based on the sum of the masses of the lithium source, the catalyst, the conductive agent, and the sodium source, the mass content C of the sodium source satisfies: 0.001 wt% ≤ C ≤ 0.25 wt%; alternatively, 0.02 wt% ≤ C ≤ 0.1 wt%. By selecting a sodium source mass content within the above range, it is advantageous to obtain primary particles of lithium-containing compounds with suitable particle size.
[0035] In one possible implementation, the lithium source includes one or more of Li₂C₂O₄, Li₂CO₃, Li₂C₄O₄, Li₂C₃O₅, Li₂C₄O₆, or LiOH. The lithium source can be soluble in a solvent and can provide lithium ions, thereby obtaining a slurry containing lithium ions, which facilitates the preparation of composite materials from the slurry.
[0036] In one possible implementation, the sodium source includes one or more of the following: NaOH, Na₂CO₃, NaCl, NaNO₃, Na₂SO₄, NaHSO₄, NaHCO₃, Na₂C₂O₄, Na₂C₄O₄, Na₂C₃O₅, and Na₂C₄O₆. The sodium source is soluble in a solvent, and during the drying process, it preferentially precipitates before the lithium source, thereby providing nucleation sites for the growth of lithium-containing compounds, facilitating the formation of lithium-containing compounds and obtaining lithium-containing compounds with smaller particle sizes.
[0037] Thirdly, a positive electrode sheet is provided, comprising a positive electrode active material; a composite material as described in the first aspect and any possible implementation thereof; and / or a composite material prepared by a method as described in the second aspect and any possible implementation thereof.
[0038] Fourthly, a secondary battery is provided, including the positive electrode sheet of the third aspect and any of its possible implementations.
[0039] In one possible implementation, the secondary battery is a pre-formation secondary battery.
[0040] Fifthly, an electrical device is provided, comprising the secondary battery described in the fourth aspect. Attached Figure Description
[0041] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.
[0042] Figure 1 This is a schematic diagram of a composite material preparation method according to an embodiment of this application;
[0043] Figure 2 This is a schematic diagram of a battery cell according to an embodiment of this application;
[0044] Figure 3 This is a schematic diagram of a battery according to an embodiment of this application;
[0045] Figure 4This is a schematic diagram of an electrical device according to an embodiment of this application;
[0046] Figure 5 This is a SEM image of a composite material according to an embodiment of this application;
[0047] Figure 6 This is a magnified SEM image of a composite material according to an embodiment of this application;
[0048] Figure 7 This is a SEM image of a proportional composite material of this application;
[0049] Figure 8 This is a SEM schematic diagram of a proportional composite material of this application. Detailed Implementation
[0050] The accompanying drawings provide a detailed description of the composite materials, preparation methods thereof, positive electrode sheets, secondary batteries, and embodiments of the electrical devices described in this application. However, unnecessary details may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0051] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0052] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0053] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0054] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0055] The development of battery technology requires consideration of various design factors, such as capacity, energy density, cycle life, and reliability. During the initial charge and discharge of a battery cell, a solid electrolyte interphase (SEI) film is formed on the surface of the negative electrode. The presence of the SEI film consumes a significant amount of lithium ions, affecting the battery's capacity. To improve battery capacity, lithium-containing compounds with high lithium content, such as lithium oxalate, are added to the positive electrode slurry to provide more lithium ions to the battery cell. However, lithium-containing compounds such as lithium oxalate require high potentials to decompose, and their poor conductivity limits their effectiveness in improving battery capacity. Therefore, providing a material that can improve battery capacity is a pressing technical problem that needs to be solved.
[0056] In view of this, embodiments of this application provide a composite material comprising a lithium-containing compound, a catalyst, and a conductive agent. The average particle size of the lithium-containing compound is less than or equal to 200 nm, which can increase the contact area between the electrolyte and the lithium-containing compound, thereby facilitating the transport and diffusion of lithium ions and improving the battery capacity. Furthermore, it also facilitates the contact between the conductive agent and the catalyst and the lithium-containing compound, promoting the catalytic decomposition of the lithium-containing compound, improving the conductivity of the composite material, and thus improving the battery capacity.
[0057] The composite material in this embodiment can be used as a lithium replenisher, that is, it can replenish the lithium ions consumed by the negative electrode. As an example, the composite material can be mixed with a positive electrode active material (such as lithium iron phosphate, ternary materials, etc.) to prepare a positive electrode slurry for use.
[0058] In this application's embodiments, the secondary battery can refer to either a single battery cell or a battery pack. A single battery cell can serve as the smallest unit of a battery pack. A single battery cell includes a positive electrode, a negative electrode, a separator, and an electrolyte, etc.
[0059] During the charging process of a lithium-ion secondary battery, lithium ions are released from the positive electrode active material, move and embed into the negative electrode material; while during the discharging process, lithium ions are released from the negative electrode material, move and embed into the positive electrode active material.
[0060] It should be understood that the “intercalation” process described in this application refers to the process in which lithium ions are intercalated in the positive electrode active material and the negative electrode material due to an electrochemical reaction, and the “deintercalation” and “deintercalation” processes described in this application refer to the process in which lithium ions are deintercalated in the positive electrode active material and the negative electrode material due to an electrochemical reaction.
[0061] [Composite Materials]
[0062] This application provides a composite material comprising a lithium-containing compound, a catalyst, and a conductive agent.
[0063] Lithium-containing compounds include lithium, carbon, and oxygen. They can include organic lithium compounds, such as lithium oxalate, or inorganic lithium compounds, such as lithium carbonate.
[0064] Lithium-containing compounds can refer to compounds that include lithium, carbon, and oxygen elements, such as lithium oxalate and lithium carbonate.
[0065] Lithium-containing compounds can decompose under voltage, breaking down into lithium ions and carbon oxides (such as CO and CO2). The lithium ions produced during decomposition can replenish the battery, thereby improving its capacity.
[0066] Catalysts include one or more of transition metal oxides, transition metal carbides, transition metal nitrides, or transition metal phosphides. Catalysts can reduce the decomposition voltage of lithium-containing compounds.
[0067] Transition metal carbides, transition metal nitrides, and transition metal phosphides can be obtained by processing transition metal oxides. Transition metal carbides can be molybdenum carbide or tungsten carbide, and transition metal nitrides can be molybdenum nitride or manganese nitride. Transition metal phosphides can be nickel phosphide, cobalt phosphide, manganese phosphide, tungsten phosphide, or molybdenum phosphide.
[0068] Transition metal oxides, transition metal carbides, transition metal nitrides, and transition metal phosphides not only have high electrical conductivity, but also possess abundant surface active sites and high specific surface area, which can catalyze the decomposition of lithium-containing compounds.
[0069] Oxides, carbides, nitrides, and phosphides of transition metals can catalyze the decomposition of lithium-containing compounds under voltage, that is, they can reduce the decomposition voltage of lithium-containing compounds.
[0070] As an example, the catalyst is an oxide of a transition metal, such as Ni. x O, where 0.67≤x≤1, and the embodiments of this application include but are not limited to this, as long as it can catalyze the decomposition of lithium-containing compounds.
[0071] A conductive agent is a material that can conduct electricity. For example, a conductive agent can be a carbon material.
[0072] In the composite material, the lithium-containing compound comes into contact with the catalyst and the conductive agent. In this way, the catalyst can catalyze the decomposition of the lithium-containing compound, and the conductive agent facilitates the transfer of electrons, thereby helping to reduce the decomposition voltage of the composite material and maximize its capacity.
[0073] The average particle size D1 of the lithium-containing compound satisfies: D1≤200nm. D1 can be 20nm, 50nm, 60nm, 80nm, 100nm, 120nm, 160nm, 200nm or any value within the above range.
[0074] When the average particle size of the lithium-containing compound is less than or equal to 200 nm, the smaller particle size shortens the lithium-ion extraction path and increases the contact area between the electrolyte and the lithium-containing compound, facilitating lithium-ion transport and diffusion during charging. The composite material exhibits better lithium replenishment performance, thus contributing to increased battery capacity. Furthermore, it promotes sufficient contact between the catalyst and the lithium-containing compound, facilitating the decomposition of the lithium-containing compound and reducing its decomposition voltage; it also facilitates sufficient contact between the conductive agent and the lithium-containing compound, promoting electron transport and further enhancing battery capacity.
[0075] As an example, the average particle size D1 is the average particle size of the primary particles of the lithium-containing compound.
[0076] In this embodiment, the lithium-containing compound can decompose to generate lithium ions and gas, thereby replenishing the battery with lithium ions. The catalyst can catalyze the decomposition of the lithium-containing compound, making it easier to decompose and thus providing more lithium ions to the battery. The average particle size D1 of the lithium-containing compound satisfies: D1≤200nm, which is beneficial for increasing the contact area between the electrolyte and the lithium-containing compound, thereby facilitating the transport and diffusion of lithium ions and improving the battery capacity. It also facilitates the contact between the conductive agent and the catalyst and the lithium-containing compound, promoting the catalytic decomposition of the lithium-containing compound, improving the conductivity of the composite material, and thus increasing the battery capacity. Therefore, the technical solution of this embodiment can improve the battery capacity.
[0077] In some embodiments, the average particle size D1 of the lithium-containing compound satisfies: 20nm ≤ D1 ≤ 200nm.
[0078] When the average particle size of lithium-containing compounds is greater than or equal to 20 nm, it facilitates the preparation of lithium-containing compounds and helps to reduce the complexity of preparation; when the average particle size of lithium-containing compounds is less than or equal to 200 nm, it helps to improve the capacity of the battery.
[0079] In some embodiments, the average particle size D1 of the lithium-containing compound satisfies: 50 nm ≤ D1 ≤ 150 nm.
[0080] D1 can be 50nm, 60nm, 70nm, 75nm, 80nm, 90nm, 115nm, 125nm, 135nm, 145nm, 150nm, or any value within the above range.
[0081] Within the 50nm to 150nm range, lithium-containing compounds have a more suitable primary particle size, which is beneficial for the preparation of lithium-containing compounds and allows the battery to have a higher capacity.
[0082] In some embodiments, the composite material further includes a sodium-containing compound, which comprises sodium, carbon, and oxygen. During the preparation of the composite material, a sodium source is added to facilitate the preparation of primary lithium-containing compound particles with a smaller average particle size; therefore, the resulting composite material also includes a sodium-containing compound.
[0083] As an example, sodium can be detected in composite materials.
[0084] As another example, the content of sodium-containing compounds in the composite material is very low, making it difficult to detect the presence of new phases (such as sodium oxalate), and only the presence of sodium element can be detected.
[0085] As an example, sodium-containing compounds can have similar chemical formulas to lithium-containing compounds. For instance, the chemical formula of a sodium-containing compound is Na₂C.x O y , 1≤x≤4, 3≤y≤6.
[0086] In the above embodiments, the composite material can also generate a small amount of sodium ions after decomposition, and the small amount of sodium ions can dissolve in the electrolyte.
[0087] In some embodiments, in the composite material, the molar ratio W of sodium to lithium satisfies: 0.005 ≤ W ≤ 0.12. For example, W can be 0.005, 0.006, 0.01, 0.02, 0.025, 0.03, 0.04, 0.05, 0.06, 0.08, 0.09, 0.1, 0.12, or any value within the above range.
[0088] As an example, to facilitate the representation of the molar ratio of sodium and lithium, sodium-containing compounds and lithium-containing compounds can be represented as Li b Na a C₂O₄, where 1 ≤ x ≤ 4, 3 ≤ y ≤ 6, a + b = 2, and 0.01 ≤ a ≤ 0.2. For example, a = 0.01, b = 1.99; a = 0.2, b = 1.8; a = 0.05, b = 1.95.
[0089] When W is greater than or equal to 0.005, a certain amount of sodium can inhibit the growth of primary particles of lithium-containing compounds during the preparation of composite materials, which is beneficial to obtaining primary particles with smaller particle sizes. When W is less than or equal to 0.12, the risk of reducing the lithium content in lithium-containing compounds due to excessive sodium can be reduced, thereby reducing the risk of less capacity improvement in the battery due to the reduced lithium content.
[0090] A suitable molar content of sodium is beneficial for obtaining lithium compounds with a suitable particle size; and a suitable molar content of lithium is beneficial for obtaining batteries with high capacity.
[0091] In some embodiments, 0.025 ≤ W ≤ 0.05. This results in a more suitable sodium content, which is beneficial for obtaining lithium compounds with smaller particle sizes and batteries with higher capacity.
[0092] In some embodiments, the lithium-containing compound has the chemical formula Li₂C. x O y , where 1≤x≤4, 3≤y≤6.
[0093] x and y satisfy the following relationship: x + y = 2n, 2 ≤ n ≤ 5. Where x can be 1, 2, 3, 4, or any value within the above range; y can be 3, 4, 5, 6, or any value within the above range; and n can be 2, 3, 4, 5, or any value within the above range. As an example, x, y, and n are all positive integers.
[0094] Lithium-containing compounds that meet the above chemical formulas can decompose into lithium ions and gases (such as carbon monoxide and carbon dioxide) under the action of voltage and catalyst. The lithium ions produced by decomposition can play a role in replenishing lithium ions, which is beneficial to improving the battery capacity. The gases produced by decomposition will not remain in the positive electrode, and the residues produced by decomposition will not affect the long-term reliability and other performance of the battery cells.
[0095] In some embodiments, the lithium-containing compound includes one or more of Li2C2O4, Li2CO3, Li2C4O4, Li2C3O5, or Li2C4O6.
[0096] Under the influence of voltage and a catalyst, the aforementioned lithium-containing compounds can decompose into lithium ions and gases (such as carbon monoxide and carbon dioxide). The lithium ions produced during decomposition can replenish lithium ions, which is beneficial for improving battery capacity. The gases produced during decomposition will not remain in the positive electrode sheet, and the residues from decomposition will not affect the long-term reliability and other performance characteristics of the battery cells. In addition, the aforementioned lithium-containing compounds have good stability and can exist stably in air and organic solvents, making them compatible with the coating process of positive electrode slurry.
[0097] As an example, the gases produced by the decomposition of lithium compounds can be extracted from battery cells during the formation process using tools such as suction nozzles.
[0098] In some embodiments, the composite material has a secondary particle morphology. A lithium-containing compound, a conductive agent, and a catalyst are mixed together to form a composite material with a secondary particle morphology.
[0099] Primary lithium-containing compound particles, conductive agents, and catalysts are mixed to form spherical or near-spherical composite materials. In this way, after the lithium-containing compound decomposes, the conductive agent and catalyst in the composite material retain the three-dimensional structure of the composite material. The pores or vacancies formed in the original positions of the lithium-containing compound are not directly present on the positive electrode, thus reducing the risk of damage to the conductive network of the positive electrode and minimizing the impact on electron and ion transport within the positive electrode, thereby improving battery capacity. Furthermore, the vacancies or pores left in the composite material after lithium-containing compound decomposition can enhance electrolyte wetting, and the electrolyte at these vacancies can provide channels for ion transport (e.g., lithium ions), which is beneficial for increasing battery capacity.
[0100] In some embodiments, the lithium-containing compound has the morphology of primary particles.
[0101] Primary particles can refer to unagglomerated particles, while secondary particles can refer to particles formed by the agglomeration of primary particles.
[0102] In the embodiments of this application, the primary particles containing lithium compounds have a rod-shaped or similar rod-shaped morphology, and the secondary particles of the composite material have a spherical or near-spherical morphology.
[0103] In the secondary particles of the composite material, the morphology of the lithium-containing compound is that of primary particles, or in other words, most of the lithium-containing compound particles are unaggregated. This has two advantages: firstly, it facilitates sufficient contact between the lithium-containing compound and the catalyst, leading to better catalytic performance and thus reducing the decomposition voltage of the lithium-containing compound, thereby increasing the battery capacity; secondly, the conductive agent dispersed around the lithium-containing compound in the primary particles helps improve the electronic conductivity of the lithium-containing compound, which in turn helps increase the battery capacity.
[0104] In some embodiments, the volume average particle size Dv50 of the composite material satisfies: 2μm≤Dv50≤10μm.
[0105] Dv50 can refer to the particle size corresponding to 50% of the cumulative particle size distribution number of a sample, which means that 50% of the particles are smaller than Dv50.
[0106] Dv50 can be 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm or any value within the above range.
[0107] The volume average particle size of a composite material can refer to the volume average particle size of the composite material powder or composite material particles.
[0108] When the volume average particle size Dv50 of the composite material is not less than 2 μm, the risk of composite material agglomeration and the difficulty of composite material preparation can be reduced. When the volume average particle size Dv50 of the composite material does not exceed 10 μm, the composite material has a suitable particle size, and the lithium ions extracted from the lithium-containing compound have a suitable diffusion distance, which is conducive to the lithium ion having a high transport rate and the extraction of more lithium ions, thereby improving the battery capacity.
[0109] In some embodiments, 4μm ≤ Dv50 ≤ 8μm. This results in a more suitable particle size for the composite material, which is beneficial for achieving higher battery capacity.
[0110] In some embodiments, based on the total mass of the composite material, the mass content A of the conductive agent satisfies: 1wt% ≤ A ≤ 40wt%.
[0111] A can be 1wt%, 5wt%, 10wt%, 15wt%, 25wt%, 30wt%, 35wt%, 40wt%, or any value within the above range.
[0112] When the mass content A of the conductive agent is not less than 1 wt%, the composite material has high conductivity and low resistivity; when the mass content A of the conductive agent is not more than 40 wt%, the conductive agent has a suitable mass ratio, the catalyst and lithium-containing compound also have suitable mass ratios, and the battery cell has a suitable capacity.
[0113] In some embodiments, 2wt% ≤ A ≤ 20wt%. This results in a more suitable mass ratio of conductive agent and a higher battery capacity.
[0114] In some embodiments, based on the total mass of the composite material, the mass content B of the catalyst satisfies: 0.5wt% ≤ B ≤ 20wt%.
[0115] B can be 0.5wt%, 1wt%, 5wt%, 8wt%, 10wt%, 15wt%, 20wt%, or any value within the above range.
[0116] When the mass content of catalyst B is not less than 0.5 wt%, the contact area between the catalyst and the lithium-containing compound is suitable, resulting in a better catalytic effect, which is beneficial for the decomposition of lithium-containing compounds and for improving battery capacity. When the mass content of catalyst B does not exceed 20 wt%, it is beneficial for adding more lithium-containing compounds to the composite material, which is beneficial for improving battery capacity.
[0117] In some embodiments, 1 wt% ≤ B ≤ 10 wt%. This results in a more suitable mass ratio of catalyst and a higher battery capacity.
[0118] In some embodiments, the chemical formula of the oxide of the transition metal is M. α O β Where 0 < α ≤ 3, 0 < β ≤ 5, and M includes one or more of Ni, Co, Fe, Mn, V, Cr, Cu, or Ti.
[0119] α can be 0.5, 1, 2, 3, or any value within the above range, and β can be 0.5, 1, 2, 3, 4, 5, or any value within the above range. In some examples, α and β are positive integers.
[0120] The catalysts described above can reduce the decomposition voltage of lithium-containing compounds, allowing them to decompose at lower voltages.
[0121] In some embodiments, M α O βIncluding one or more of NiO, Co3O4, Fe2O3, MoO3, or V2O5.
[0122] The catalysts described above can reduce the decomposition voltage of lithium-containing compounds, allowing them to decompose at lower voltages.
[0123] In some embodiments, the transition metal carbides include one or more of molybdenum carbide, vanadium carbide, tungsten carbide, titanium carbide, cobalt carbide, iron carbide, or nickel carbide; and / or, the transition metal nitrides include one or more of molybdenum nitride, vanadium nitride, titanium nitride, manganese nitride, cobalt nitride, iron nitride, or nickel nitride; and / or, the transition metal phosphides include one or more of nickel phosphide, cobalt phosphide, manganese phosphide, tungsten phosphide, or molybdenum phosphide. The aforementioned transition metal carbides, transition metal nitrides, and transition metal phosphides exhibit good catalytic effects and can catalyze the decomposition of lithium-containing compounds.
[0124] In some embodiments, the conductive agent includes a carbon material.
[0125] Optionally, the conductive agent includes a carbon-based conductive agent. For example, the conductive agent includes carbon-based materials. For example, the conductive agent can be conductive graphite, conductive carbon black, graphene, etc.
[0126] Optionally, the carbon-based conductive agent includes one or more of the following: carbon nanotubes, carbon fibers, acetylene black, Ketjen black, conductive carbon black, C60, or graphene.
[0127] Carbon materials have good electrical conductivity and are compatible with other materials in batteries. Including carbon materials in composite materials helps to reduce the resistivity of composite materials, improve their electrical conductivity, and increase battery capacity.
[0128] In some embodiments, the lithium-containing compound is chemically bonded to the conductive agent and to the catalyst in the composite material. For example, during the preparation of the composite material, the lithium-containing compound is grown in situ on the conductive agent and catalyst. This in-situ growth method, compared to physically mixing the lithium-containing compound with the conductive agent and catalyst, is beneficial for enhancing the bonding strength between the lithium-containing compound and the conductive agent and catalyst, ultimately improving the conductivity of the composite material, reducing its decomposition voltage, and enhancing its lithium replenishment effect and battery capacity.
[0129] In some embodiments, the powder resistivity R of the composite material at 20 MPa satisfies: R ≤ 360 Ω·cm. This results in a low powder resistivity, which is beneficial for improving the conductivity of the composite material and thus for increasing the battery capacity.
[0130] R can be 360Ω·cm, 350Ω·cm, 200Ω·cm, 100Ω·cm, 50Ω·cm, 10Ω·cm, 1Ω·cm, 0.5Ω·cm, or any value within the above range.
[0131] In some embodiments, R ≤ 1 Ω·cm. This is beneficial for further improving the conductivity of the composite material, resulting in a battery with higher capacity.
[0132] [Preparation methods for composite materials]
[0133] Figure 1 This is a schematic diagram of a method for preparing a composite material according to an embodiment of this application. This method can be used to prepare the composite material in any of the above embodiments. (In conjunction with...) Figure 1 As shown, method 100 includes the following steps.
[0134] Step 110: Add lithium source, catalyst, conductive agent and sodium source to solvent to obtain slurry.
[0135] The lithium source can be the lithium-containing compound in the above embodiments, or it can be lithium hydroxide, as long as it can be soluble in the solvent and provide lithium ions.
[0136] The solvent can be deionized water. As an example, a lithium-containing compound is dissolved in deionized water, followed by the addition of a conductive agent, a catalyst, and a sodium source, and the mixture is stirred to obtain a homogeneous slurry.
[0137] The sodium source is a substance containing the element sodium. For example, the sodium source is a sodium salt, such as a salt formed by the combination of sodium ions and acid radical ions. For example, Na₂CO₃. Another example is the sodium-containing compound mentioned in the above embodiments.
[0138] The lithium and sodium sources are soluble in the solvent, while the conductive agent and catalyst are insoluble in the solvent.
[0139] The catalyst can be one or more of the catalysts mentioned in the above embodiments. The catalyst includes one or more of transition metal oxides, transition metal carbides, transition metal nitrides, or transition metal phosphides.
[0140] Step 120: The slurry is dried to obtain a composite material.
[0141] During the drying process, sodium-containing compounds, including sodium, preferentially crystallize and nucleate around the conductive agent and catalyst. However, due to the low content of sodium source, the crystallized sodium-containing compounds are difficult or unable to grow rapidly. Due to the high content of lithium source, the lithium-containing compounds encounter already nucleated sodium sources during the crystallization and nucleation process, making it difficult for the lithium-containing compounds to grow further. This results in the production of primary lithium-containing compound particles with smaller particle sizes.
[0142] Drying can be a process performed at a specific temperature, i.e., drying is carried out while heating. For example, drying can be performed at a temperature of 150°C to 250°C.
[0143] The descriptions of lithium-containing compounds, catalysts, and conductive agents can be found in the examples of composite materials, and will not be repeated here.
[0144] In the embodiments of this application, the composite material prepared by method 100 has good performance, which is beneficial to improving the capacity of the battery body; and the method is simple to operate and facilitates the preparation of composite materials.
[0145] In some embodiments, drying the slurry to obtain a composite material includes: drying the slurry by spray drying to obtain the composite material. Choosing spray drying facilitates the preparation of lithium-containing compounds with smaller particle sizes and the preparation of composite materials.
[0146] As an example, a spray drying process is performed using a suitable apparatus. For instance, the slurry is fed into the apparatus through a feed inlet at a certain feed rate, and the drying temperature of the apparatus is set to perform spray drying on the slurry.
[0147] In some embodiments, the drying temperature T satisfies: 150℃≤T≤250℃.
[0148] During the spray drying process, hot air at a certain temperature is introduced at the outlet of the device to dry the slurry. In this embodiment, the drying temperature can be the temperature of the hot air.
[0149] T can be 150℃, 200℃, 250℃ or any value within the above range.
[0150] The drying temperature affects the growth and nucleation process of secondary particles in the composite material. By selecting a temperature within the aforementioned range, it is beneficial to obtain composite secondary particles of suitable particle size. The higher the drying temperature, the faster the secondary particles grow, and the larger the particle size of the resulting composite secondary particles.
[0151] Optionally, 175℃≤T≤225℃. By selecting a drying temperature within the above range, it is easier to obtain secondary composite particles with a more suitable particle size.
[0152] In some embodiments, based on the sum of the masses of the lithium source, catalyst, conductive agent, and sodium source, the mass content C of the sodium source satisfies: 0.001wt% ≤ C ≤ 0.25wt%; optionally, 0.02wt% ≤ C ≤ 0.1wt%.
[0153] C can be 0.001wt%, 0.01wt%, 0.02wt%, 0.5wt%, 0.1wt%, 0.2wt%, 0.25wt%, or any value within the above range.
[0154] As an example, the lithium source is lithium oxalate, and the mass content of the sodium source is set based on the sum of the masses of lithium oxalate, catalyst, conductive agent, and sodium source.
[0155] The mass content of sodium source affects the growth of primary particles of lithium-containing compounds. As the mass content of sodium source increases, the particle size of primary particles of lithium-containing compounds decreases, but this leads to a decrease in the lithium content in the composite material, resulting in a smaller increase in battery capacity.
[0156] By selecting a sodium source with a mass content that meets the above range, it is beneficial to balance the battery capacity and the particle size of the primary lithium compound particles.
[0157] In some embodiments, the mass content of the conductive agent is 1 wt% to 40 wt%, optionally 2 wt% to 20 wt%, based on the sum of the masses of the lithium source, catalyst, conductive agent and sodium source.
[0158] In some embodiments, the mass content of the catalyst is 0.5 wt% to 20 wt%, optionally 1 wt% to 10 wt%, based on the sum of the masses of the lithium source, catalyst, conductive agent and sodium source.
[0159] It should be noted that, in the embodiments of this application, parameters such as the drying temperature can also be set according to actual needs, and the embodiments of this application include, but are not limited to, this.
[0160] In some embodiments, the lithium source includes one or more of Li₂C₂O₄, Li₂CO₃, Li₂C₄O₄, Li₂C₃O₅, Li₂C₄O₆, or LiOH. The lithium source can be soluble in a solvent and can provide lithium ions, thereby obtaining a slurry containing lithium ions, which facilitates the preparation of composite materials from the slurry.
[0161] In some embodiments, the sodium source includes one or more of the following: NaOH, Na₂CO₃, NaCl, NaNO₃, Na₂SO₄, NaHSO₄, NaHCO₃, Na₂C₂O₄, Na₂C₄O₄, Na₂C₃O₅, and Na₂C₄O₆. The sodium source is soluble in a solvent. During the drying process, sodium-containing compounds, including sodium, preferentially precipitate out compared to lithium-containing compounds, thereby providing nucleation sites for the growth of lithium-containing compounds, facilitating the formation of lithium-containing compounds, and making it easier to obtain lithium-containing compounds with smaller particle sizes.
[0162] [Positive electrode plate]
[0163] This application provides a positive electrode sheet, comprising the composite material of any of the above embodiments, and / or the composite material prepared by the method of any of the above embodiments.
[0164] In some embodiments, the positive electrode sheet further includes a positive electrode active material. The positive electrode active material may be any known positive electrode active material for batteries. For example, the positive electrode active material may be lithium iron phosphate, ternary materials, lithium-rich manganese-based materials, etc.
[0165] The positive electrode includes a positive current collector and a positive electrode film layer disposed on the positive current collector.
[0166] The positive electrode current collector can be a metal foil or a composite current collector. For example, the positive electrode current collector can be an aluminum foil.
[0167] Composite current collectors may include a polymeric material substrate and a metal layer formed on at least one surface of the polymeric material substrate. Composite current collectors can be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymeric material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0168] The positive electrode film may include positive electrode active materials and composite materials, and the composite materials can be used as lithium supplements.
[0169] The positive electrode film layer may also optionally include a binder. As an example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resins.
[0170] The positive electrode film may optionally include a conductive material. The conductive material may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0171] [Negative electrode plate]
[0172] The negative electrode includes a negative current collector and a negative electrode film layer disposed on the negative current collector.
[0173] The negative electrode current collector can be a metal foil or a composite current collector. The negative electrode current collector can be copper foil. Composite current collectors can be formed by depositing metallic materials (copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys, etc.) onto a polymer substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0174] The negative electrode film layer includes a negative electrode active material. The negative electrode active material can be any negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material may include one or more of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. The silicon-based material may include one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may include one or more of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0175] The negative electrode film may optionally include a conductive material. The conductive material may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0176] [Electrolytes]
[0177] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific limitations on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel-like, or entirely solid.
[0178] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.
[0179] Electrolyte salts may include one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.
[0180] Solvents may include one or more of the following: ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0181] The electrolyte may also optionally include negative electrode film-forming additives, positive electrode film-forming additives, and performance additives that can improve certain battery performance, such as performance additives that improve battery overcharge performance, battery high temperature or low temperature performance, etc.
[0182] [Isolation membrane]
[0183] The separator is used to separate the positive electrode and the negative electrode. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.
[0184] The material of the separator membrane may include one or more of the following: glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator membrane can be a single-layer film or a multi-layer composite film; there are no particular restrictions. When the separator membrane is a multi-layer composite film, the materials of each layer can be the same or different; there are no particular restrictions.
[0185] Positive electrode, negative electrode and separator can be made into electrode assembly by winding process or stacking process.
[0186] [Rechargeable Battery]
[0187] This application provides a secondary battery, including the positive electrode sheet in the above embodiments.
[0188] In some embodiments, the secondary battery is a secondary battery before formation. Formation can be understood as the initialization of the secondary battery, the process of activating the active materials of the secondary battery; it can also be understood as a process of charging the secondary battery.
[0189] The secondary battery in this application embodiment can be a single battery cell, which can be a battery cell that has not undergone charging and discharging. For example, the battery cell is a newly assembled battery cell that has not been used. For example, the battery cell is a battery cell that has not undergone a formation process.
[0190] After the battery cells have been assembled and used for a period of time, the lithium-containing compounds in the composite material in the electrode of the battery cell decompose, and only a small amount or no lithium-containing compounds are present in the electrode; the mass of the catalyst in the composite material remains basically unchanged.
[0191] This application does not impose any particular limitation on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. The battery cell can be a lithium-ion battery, a lithium-sulfur battery, a sodium-ion battery, etc.
[0192] Figure 2 This is a schematic diagram of a battery cell according to an embodiment of this application. For example, as shown... Figure 2As shown, the battery cell 3 is a square battery cell. The battery cell 3 includes a housing 31, an end cap assembly 32, and an electrode assembly 33 disposed in the housing 31.
[0193] The electrode assembly 33 can be made from a positive electrode, a negative electrode, and a separator through a winding process or a stacking process.
[0194] End cap assembly 32 includes electrode terminals 322, for example, such as Figure 2 As shown, the end cap assembly 32 includes two electrode terminals 322, one of which is a positive electrode terminal and the other is a negative electrode terminal.
[0195] The battery cell 3 also includes a current collector 34, which is used to connect the tab 331 and the electrode terminal 322 of the electrode assembly 33. For example, in the case that the electrode 1 in this embodiment is a positive electrode, one current collector 34 is used to connect the positive electrode tab and the positive electrode terminal, and another current collector 34 is used to connect the negative electrode tab and the negative electrode terminal.
[0196] In some embodiments, individual battery cells can be assembled into a battery module. The number of individual battery cells contained in a battery module can be one or more, and the specific number can be selected by those skilled in the art based on the application and capacity of the battery module.
[0197] [Battery]
[0198] This application provides a battery, including the battery cell described in the above embodiments. Figure 3 This is a schematic diagram of a battery according to an embodiment of this application. Figure 3 As shown, battery 5 may include multiple battery cells (not shown in the figure).
[0199] Battery cells 3 can be directly assembled into battery 5, or they can be first assembled into battery modules, and then multiple battery modules can be assembled into battery 5.
[0200] [Electrical appliances]
[0201] This application provides an electrical device, including the battery described in the above embodiments.
[0202] Figure 4 This is a schematic diagram of an electrical device according to an embodiment of this application. Figure 4 As shown, this application provides an electrical device 6, which includes the battery in the above embodiment.
[0203] Alternatively, the electrical device may also be an energy storage device, a lighting device, a spacecraft, etc., as is the case in the embodiments of this application.
[0204] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0205] [Example]
[0206] Example 1
[0207] In Example 1, the composite material includes a lithium-containing compound, a catalyst, a conductive agent, and a small amount of a sodium-containing compound. The lithium-containing compound is Li₂C₂O₄, the catalyst is NiO, and the conductive agent is Ketjen Black (KB). In the composite material, the molar ratio W of sodium to lithium is approximately 0.025 (i.e., a ratio of 0.05 to 1.95). The lithium-containing compound and the sodium-containing compound can be represented as Li₂C₂O₄. 1.95 Na 0.05 C2O4. In the composite material, based on the total mass of the composite material, the mass content of the conductive agent A is 10 wt%, and the mass content of the catalyst B is 5 wt%. The volume average particle size Dv50 of the secondary particles in the composite material is 6 μm, and the average particle size D1 of the lithium-containing compound is 100 nm (where D1 is the average particle size of the primary particles of the lithium-containing compound).
[0208] In the preparation of the composite material of Example 1, the lithium source added was Li2C2O4, and the sodium source was Na2C2O4. Based on the total mass of the sodium source, lithium-containing compound, catalyst, and conductive agent, the mass content C of the sodium source was 0.06 wt%. During the spray drying process, the drying temperature T was 200°C.
[0209] Examples 2-5
[0210] The difference between Examples 2-5 and Example 1 is that the mass content A of the conductive agent is different.
[0211] Examples 6-9
[0212] The difference between Examples 6-9 and Example 1 is that the mass content B of the catalyst is different.
[0213] Examples 10-13
[0214] The difference between Examples 10-13 and Example 1 is that the drying temperature T is different. Consequently, the volume average particle size Dv50 of the secondary particles in the composite material is different.
[0215] Examples 14-17
[0216] The difference between Examples 14-17 and Example 1 is that the mass content of the sodium source is different. Accordingly, the average particle size D1 of the primary particles of the lithium-containing compound is different, and the molar content of sodium element is different.
[0217] Example 18
[0218] The difference between Example 18 and Example 1 is that the type of sodium source is different, and the mass content of the conductive agent and the catalyst is different.
[0219] Example 19
[0220] The difference between Example 19 and Example 1 is that the type and mass content of sodium source are different, the mass content of catalyst is different, and the volume average particle size of the secondary particles of the composite material and the average particle size of the primary particles of lithium-containing compound are different.
[0221] Example 20
[0222] The difference between Example 20 and Example 1 is that the type and mass content of sodium source are different, the mass content of conductive agent is different, and the volume average particle size of the secondary particles of the composite material is different.
[0223] Examples 21-23
[0224] The difference between Examples 21-23 and Example 1 is that the types of lithium-containing compounds added during the preparation of the composite materials are different.
[0225] Examples 24-28
[0226] The difference between Examples 24-28 and Example 1 is that the types of catalysts are different.
[0227] Example 29
[0228] The difference between Example 29 and Example 1 is that lithium iron phosphate was added as the positive electrode active material to prepare the battery cell. Based on the total mass of lithium iron phosphate and the composite material, the mass content of the composite material was 5 wt%, and the mass content of lithium iron phosphate was 95 wt%.
[0229] Comparative Example 1
[0230] The difference between Comparative Example 1 and Example 1 is that the material used is not a composite material, but only contains the lithium compound Li2C2O4.
[0231] Comparative Example 2
[0232] The difference between Comparative Example 2 and Example 1 is that the material is a mixture of lithium compound Li2C2O4 and a catalyst, without a conductive agent.
[0233] Comparative Example 3
[0234] The difference between Comparative Example 3 and Example 1 is that the material in Comparative Example 3 is a mixture of lithium compound Li2C2O4 and a conductive agent, without a catalyst.
[0235] Comparative Example 4
[0236] The difference between Comparative Example 4 and Example 1 is that no sodium source was added during the preparation process of the material in Comparative Example 4. The prepared composite material includes Li2C2O4, a conductive agent, and a catalyst, but does not contain sodium. In the composite material prepared in Comparative Example 4, the average particle size of the primary particles of Li2C2O4 is relatively large.
[0237] Comparative Examples 5-7
[0238] The difference between Comparative Examples 5-7 and Comparative Example 1 is that the lithium-containing compounds are Li2C4O4, Li2CO3, and Li2C4O6, respectively.
[0239] Comparative Example 8
[0240] The difference between Comparative Example 8 and Comparative Example 1 is that after obtaining compound Li2C2O4, the lithium-containing compound Li2C2O4 was subjected to sand milling. After sand milling, the average particle size of the primary particles of the lithium-containing compound Li2C2O4 was larger.
[0241] Comparative Example 9
[0242] The difference between Comparative Example 9 and Comparative Example 4 is that lithium iron phosphate was added as the positive electrode active material to prepare the battery cell. Based on the total mass of lithium iron phosphate and the composite material, the mass content of the composite material was 5 wt%, and the mass content of lithium iron phosphate was 95 wt%.
[0243] In Comparative Examples 1-8, no sodium source was added during the preparation of the slurry. Instead, the slurry was prepared from the corresponding raw materials and then spray-dried. Furthermore, it should be noted that in Comparative Example 1, the material used was a simple lithium-containing compound. Although spray-dried, this method makes it difficult to prepare the lithium-containing compound into spherical shapes.
[0244] Referring to Tables 1, 2, and 3, in Examples 1-28 and Comparative Examples 1-8, lithium-ion battery cells were prepared using only composite materials. Referring to Table 4, in Example 29 and Comparative Example 9, lithium-ion battery cells were prepared using composite materials as lithium supplementers and lithium iron phosphate as the positive electrode active material.
[0245] In Table 1, A represents the mass content of the conductive agent, B represents the mass content of the catalyst, D1 represents the average particle size of the primary particles of the lithium-containing compound, Dv50 represents the volume average particle size of the composite material powder, R represents the resistivity of the composite material powder, and W represents the molar ratio of sodium to lithium.
[0246] Table 1. Parameters of the composite materials of Examples 1-28 and Comparative Examples 1-8
[0247]
[0248]
[0249] Table 2. Parameters of the preparation methods of the composite materials in Examples 1-28 and Comparative Examples 1-8
[0250]
[0251]
[0252] Table 3. Experimental results of Examples 1-28 and Comparative Examples 1-8
[0253]
[0254] Table 4. Experimental results of Example 29 and Comparative Example 9
[0255]
[0256]
[0257] [Preparation of battery cells in Examples 1-28 and Comparative Examples 1-8]
[0258] (1) Preparation of the positive electrode sheet: The composite material, the binder polyvinylidene fluoride (PVDF), and the conductive agent (acetylene black) were dissolved in the solvent N-methylpyrrolidone (NMP) at a mass ratio of 97:2:1. After thorough mixing, a positive electrode slurry was prepared. The positive electrode slurry was uniformly coated onto the positive electrode current collector aluminum foil, and then dried, cold-pressed, and slit to obtain the positive electrode sheet. No other active materials were added during the preparation of this positive electrode sheet.
[0259] (2) Preparation of negative electrode sheet: The negative electrode active material artificial graphite, conductive agent acetylene black, binder styrene-butadiene rubber (SBR) and thickener sodium carboxymethyl cellulose (CMC-Na) are dissolved in deionized water at a mass ratio of 96:1.5:1.5:1.0 and mixed thoroughly to prepare a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector copper foil, and then dried, cold pressed and cut to obtain the negative electrode sheet.
[0260] (3) Separation membrane: A polypropylene membrane with a thickness of 13μm is used.
[0261] (4) Preparation of electrolyte: Ethyl carbonate (EC), methyl ethyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1. LiPF6 was then uniformly dissolved in the mixture to obtain the electrolyte. The concentration of LiPF6 in the electrolyte was 1 mol / L.
[0262] (5) Preparation of lithium-ion battery cell: The above positive electrode sheet, separator and negative electrode sheet are stacked and wound in sequence to obtain electrode assembly; the electrode assembly is placed in outer packaging, the electrolyte prepared above is added, and after encapsulation, standing, formation and aging processes, lithium-ion battery cell is obtained.
[0263] [Preparation of battery cells in Example 29 and Comparative Example 9]
[0264] (1) Preparation of the positive electrode sheet: The composite material, positive electrode active material lithium iron phosphate (LFP), binder polyvinylidene fluoride (PVDF), and conductive agent (acetylene black) are dissolved in solvent N-methylpyrrolidone (NMP) at a mass ratio of 97:2:1. After thorough stirring and mixing, a positive electrode slurry is prepared. The positive electrode slurry is uniformly coated on the positive electrode current collector aluminum foil, and then dried, cold-pressed, and slit to obtain the positive electrode sheet. In the preparation of this positive electrode sheet, the composite material is used as a lithium supplement agent.
[0265] (2) Preparation of negative electrode sheet: The negative electrode active material artificial graphite, conductive agent acetylene black, binder styrene-butadiene rubber (SBR) and thickener sodium carboxymethyl cellulose (CMC-Na) are dissolved in deionized water at a mass ratio of 96:1.5:1.5:1.0 and mixed thoroughly to prepare a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector copper foil, and then dried, cold pressed and cut to obtain the negative electrode sheet.
[0266] (3) Separation membrane: Polypropylene membrane is used.
[0267] (4) Preparation of electrolyte: Ethyl carbonate (EC), methyl ethyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1. LiPF6 was then uniformly dissolved in the mixture to obtain the electrolyte. The concentration of LiPF6 in the electrolyte was 1 mol / L.
[0268] (5) Preparation of lithium-ion battery: The above positive electrode sheet, separator and negative electrode sheet are stacked and wound in sequence to obtain electrode assembly; the electrode assembly is placed in outer packaging, the electrolyte prepared above is added, and after encapsulation, standing, formation and aging processes, a lithium-ion battery cell is obtained.
[0269] [First Charging Capacity Test]
[0270] The assembled lithium-ion battery was charged at a constant current rate of 0.1C to 4.25V, and left to stand for 5 minutes. The first charge capacity of the lithium-ion battery at this time was recorded. The first charge capacity of the lithium-ion battery was obtained by dividing the first charge capacity of the battery by the mass of the corresponding active material.
[0271] In Examples 1-25, the mass of the corresponding active material is the mass of the composite material; in Comparative Examples 1-7, the mass of the corresponding active material is the mass of the active material selected for the comparative examples, and the specific active materials can be found in the description above, which will not be repeated here. For Examples 26 and Comparative Example 8, the mass of the corresponding active material also includes the mass of lithium iron phosphate.
[0272] [Test of volume average particle size]
[0273] Volume average particle size can be determined using a particle size analyzer-laser diffraction method. Specifically, refer to standard GB / T19077-2016, using a laser diffraction scattering particle size analyzer, and measure according to the manufacturer's instructions. As an example, take an appropriate amount of composite material and test the volume average particle size of the material using a Malvern 2000 (MasterSizer 2000) laser particle size analyzer. Specifically, take an appropriate amount of the sample to be tested (the sample concentration should be 8-12% opacity), add 20 ml of deionized water, and simultaneously sonicate externally for 5 min (53 kHz / 120 W) to ensure complete dispersion of the sample. Then, measure the sample according to GB / T19077-2016 / ISO 13320:2009.
[0274] [Average particle size test]
[0275] The average particle size of lithium-containing compounds can be measured using the following method. As an example, the composite material is photographed using a scanning electron microscope. The lithium-containing compound, which has a rod-like shape, is located in the photograph. The lengths of the long and short sides of the rod-shaped lithium-containing compound are measured, and the average of these lengths is taken as the particle size of the lithium-containing compound. Specifically, the entire field of view at 30K magnification can be used, and 30 primary particles of the lithium-containing compound can be selected for measurement. The average particle size of the measured particles is then taken as the average particle size.
[0276] [Testing the Powder Resistivity of Composite Materials]
[0277] The powder of the composite material was dried, an appropriate amount of powder was weighed, and then the powder resistivity of the sample was determined by using a powder resistivity tester (ST2722 digital four-probe instrument, manufactured by Suzhou Jingge Electronics Co., Ltd.) according to GB / T 30835-2014. The test pressure was 20MPa.
[0278] [Testing the decomposed voltage]
[0279] The decomposition voltage of lithium-containing compounds is the average charging voltage during the first charge, i.e., the ratio of charging energy to charging capacity. Charging energy and charging capacity can be obtained using testing equipment connected to the lithium-ion battery.
[0280] [Testing of the mass content of conductive agents, catalysts, and lithium compounds in composite materials]
[0281] The components of a composite material and the mass content of each component can be determined in the following ways.
[0282] As an example, an appropriate amount of composite material powder was taken, and the elemental composition of the composite material was determined by energy dispersive spectroscopy. Then, the material and mass content of each component were determined by thermogravimetric analysis.
[0283] As an example, a suitable amount of composite material powder is taken and dissolved in deionized water (or a suitable solvent). Since lithium compounds are soluble in water, they can be separated from the composite material, and their weight can be measured to calculate the mass content. Next, the undissolved portion of the powder is added to another solvent that can dissolve the catalyst, and the weight of the catalyst is measured to calculate its mass content. Finally, a substance containing only the conductive agent is obtained, which can then be weighed to determine the mass content of the conductive agent.
[0284] In lithium-containing compounds, the content of doped sodium can be determined by inductively coupled plasma atomic emission spectrometry (ICP). As an example, the test can be performed using an ICAP 7400 spectrometer (e.g., Thermo Fisher Scientific ICAP 7400). An exemplary test method is as follows: 2g of the composite material is added to an acid solution (e.g., aqua regia) for digestion. Digestion can be carried out under stirring (e.g., mechanical stirring or microwave stirring) for 30 minutes. The digested solution is then added to an ICAP 4700 spectrometer for quantitative analysis of the chemical composition elements in the composite material. The mass of sodium is determined by the quantification of each element, and the molar mass of sodium is finally calculated.
[0285] It should be noted that the first-cycle charging capacity, volume average particle size, resistivity, decomposition voltage, mass content of conductive agent in composite material, mass content of catalyst, and mass content of lithium compound in the embodiments of this application are common knowledge in the art and have common meanings in the art. They can be measured by test methods and instruments known in the art.
[0286] In this embodiment, the battery capacity is represented by the first charge capacity of a single battery cell.
[0287] Figure 5 This is a SEM image of a composite material according to an embodiment of this application. Figure 6 This is a partially enlarged SEM image of a composite material according to an embodiment of this application. Figure 7 This is a SEM image of a proportional composite material of this application. Figure 8 This is a SEM schematic diagram of a proportional composite material of this application.
[0288] Combination Figure 5 As shown, the composite material in this embodiment has a secondary particle morphology, and the composite material is spherical or nearly spherical in shape. Combined with... Figure 6 As shown, multiple primary particles containing lithium compounds and multiple conductive agent particles (carbon material) can also be seen, and the lithium compound particles and conductive agent particles are in contact. The lithium compound particles are rod-shaped or nearly rod-shaped.
[0289] Combination Figure 7 As shown, Figure 7 The composite material prepared without the addition of a sodium source exhibits a relatively large primary particle size containing lithium compounds, with these particles being rhomboid or nearly rhomboid in shape. Figure 8 As shown, Figure 8 This is a SEM image of lithium oxalate after sand milling. Figure 8 As can be seen, the lithium oxalate particles after sand milling still have a relatively large average particle size, which is about 0.6 μm to 1.5 μm.
[0290] In conjunction with Examples 1-28 and Comparative Examples 1-8, the composite materials of the embodiments of this application can improve the first-cycle charging capacity of a single battery cell.
[0291] Combined with Comparative Example 1 and 5-7, lithium-containing compounds have higher decomposition voltage and larger resistivity, and batteries made using only lithium-containing compounds as active materials have lower first-charge capacity.
[0292] As shown in Comparative Example 2, by using only a mixture of lithium-containing compounds and catalysts, the resulting material exhibits high resistivity and low initial charge capacity of the battery.
[0293] As shown in Comparative Example 3, using only a mixture of carbon materials and lithium-containing compounds results in a high decomposition voltage of the lithium-containing compounds, which is detrimental to improving battery capacity. Although the resistivity of the composite material powder was reduced in Comparative Example 3 by using only a mixture of carbon and lithium-containing compounds, the high decomposition voltage of the lithium-containing compounds made it difficult to use normally.
[0294] As shown in Comparative Example 4, without adding a sodium source during the preparation of the composite material, the average particle size of the primary lithium-containing compound particles in the prepared composite material is larger, resulting in a lower first-cycle charging capacity of the battery.
[0295] As shown in Comparative Example 8, even after only milling lithium oxalate, the treated lithium oxalate still has a large average particle size, resulting in a low first-cycle charging capacity of the battery.
[0296] As shown in Examples 1-5, when the mass content of the conductive agent is set to 1wt% to 40wt%, the battery cell has a high first-cycle charging capacity and the composite material has a low powder resistivity; when the mass content of the conductive agent is set to 2wt% to 20wt%, the composite material has a low powder resistivity while the battery cell has a higher capacity.
[0297] As shown in Examples 6-9, when the mass content of the catalyst is set to 0.5wt% to 20wt%, the battery cell has a high capacity and the lithium compound has a low decomposition voltage; when the mass content of the catalyst is set to 1wt% to 10wt%, the lithium compound has a low decomposition voltage and the battery cell has a higher first-cycle charging capacity.
[0298] As shown in Examples 10-13, the particle size of the secondary particles in the composite material is related to the spray drying temperature. As the spray drying temperature increases, the secondary particles grow faster, making it easier to obtain secondary particles with larger particle sizes. When the spray drying temperature is in the range of 150℃ to 250℃, secondary particles of the composite material with a volume average particle size (Dv50) of 2μm to 10μm can be obtained. Furthermore, when the spray drying temperature is in the range of 175℃ to 225℃, secondary particles of the composite material with a volume average particle size (Dv50) of 4μm to 8μm can be obtained.
[0299] As shown in Examples 14-17, the size of the primary particles of the lithium-containing compound is related to the mass content of the sodium source. During the preparation of the composite material, a higher mass content of the sodium source is more conducive to obtaining primary particles of the lithium-containing compound with a smaller average particle size. When the mass content of the sodium source is in the range of 0.001 wt% to 0.25 wt%, the average particle size D1 of the primary particles of the lithium-containing compound is in the range of 20 nm to 200 nm, the composite material has a lower decomposition voltage, and the battery has a higher first-cycle charging capacity. Furthermore, when the mass content of the sodium source is in the range of 0.02 wt% to 0.1 wt%, the average particle size D1 of the primary particles of the lithium-containing compound is in the range of 50 nm to 100 nm, and the battery has an even higher first-cycle charging capacity.
[0300] As shown in Example 18, when the mass content of the conductive agent is 0.5 wt%, the mass content of the catalyst is 0.2 wt%, the volume average particle size of the secondary particles of the composite material is 6 μm, the average particle size of the primary particles of the lithium-containing compound is 100 nm, and the molar ratio of sodium to lithium in the lithium-containing compound is 0.025, the composite material has a high decomposition voltage and a high powder resistivity, but the improvement in the first charge capacity of the battery is limited.
[0301] As shown in Example 19, when the mass content of the conductive agent is 10 wt%, the mass content of the catalyst is 25 wt%, the volume average particle size of the secondary particles of the composite material is 15 μm, the average particle size of the primary particles of the lithium-containing compound is 300 nm, and the molar ratio of sodium to lithium in the lithium-containing compound is 0.0025, the improvement in the first charge capacity of the battery is limited.
[0302] As shown in Example 20, when the mass content of the conductive agent is 50 wt%, the mass content of the catalyst is 5 wt%, the volume average particle size of the secondary particles of the composite material is 1 μm, the average particle size of the primary particles of the lithium-containing compound is 100 nm, and the molar ratio of sodium to lithium in the lithium-containing compound is 0.025, the improvement in the first charge capacity of the battery is limited.
[0303] As shown in Examples 21-23, the embodiments of this application are applicable to a variety of different lithium-containing compounds, and composite materials containing different lithium-containing compounds have different capacities; as shown in Examples 24-28, the embodiments of this application are applicable to a variety of different catalysts.
[0304] In conjunction with Example 29 and Comparative Example 9, the battery cell prepared by mixing the composite material and the positive electrode active material lithium iron phosphate in this application embodiment has a high capacity.
[0305] Although only lithium iron phosphate is shown as the positive electrode active material in the embodiments, the composite material of this application is also applicable to battery cells with other active materials.
[0306] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A composite material, characterized in that, include: Lithium-containing compounds, catalysts, and conductive agents, in, The lithium-containing compound includes lithium, carbon, and oxygen. The catalyst comprises one or more of the following: oxides of transition metals, carbides of transition metals, nitrides of transition metals, or phosphides of transition metals. The average particle size D1 of the lithium-containing compound satisfies: D1≤200nm; The composite material further includes a sodium-containing compound, which includes sodium element, and the ratio W of the molar content of sodium element to the molar content of lithium element satisfies: 0.005≤W≤0.
12.
2. The composite material according to claim 1, characterized in that, 20nm≤D1≤200nm.
3. The composite material according to claim 1, characterized in that, 50nm≤D1≤150nm.
4. The composite material according to claim 1, characterized in that, 0.025≤W≤0.05。 5. The composite material according to any one of claims 1-4, characterized in that, The chemical formula of the lithium-containing compound is Li₂C. x O y , where 1≤x≤4, 3≤y≤6.
6. The composite material according to claim 5, characterized in that, The lithium-containing compounds include one or more of Li2C2O4, Li2CO3, Li2C4O4, Li2C3O5, or Li2C4O6.
7. The composite material according to any one of claims 1-4, characterized in that, The morphology of the composite material is secondary particles; and / or, the morphology of the lithium-containing compound is primary particles.
8. The composite material according to any one of claims 1-4, characterized in that, The volume average particle size Dv50 of the composite material satisfies: 2μm≤Dv50≤10μm.
9. The composite material according to claim 8, characterized in that, 4μm≤Dv50≤8μm.
10. The composite material according to any one of claims 1-4, characterized in that, Based on the total mass of the composite material, the mass content A of the conductive agent satisfies: 1wt%≤A≤40wt%.
11. The composite material according to claim 10, characterized in that, 2wt%≤A≤20wt%.
12. The composite material according to any one of claims 1-4, characterized in that, Based on the total mass of the composite material, the mass content B of the catalyst satisfies: 0.5wt%≤B≤20wt%.
13. The composite material according to claim 12, characterized in that, 1wt%≤B≤10wt%.
14. The composite material according to any one of claims 1-4, characterized in that, The chemical formula of the oxide of the transition metal is M. α O β Where 0 < α ≤ 3, 0 < β ≤ 5, and M includes one or more of Ni, Co, Fe, Mn, V, Cr, Cu, or Ti.
15. The composite material according to claim 14, characterized in that, M α O β Including one or more of NiO, Co3O4, Fe2O3, MoO3, or V2O5.
16. The composite material according to any one of claims 1-4, characterized in that, The transition metal carbides include one or more of molybdenum carbide, vanadium carbide, tungsten carbide, titanium carbide, cobalt carbide, iron carbide, or nickel carbide; and / or, the transition metal nitrides include one or more of molybdenum nitride, vanadium nitride, titanium nitride, manganese nitride, cobalt nitride, iron nitride, or nickel nitride; and / or, the transition metal phosphides include one or more of nickel phosphide, cobalt phosphide, manganese phosphide, tungsten phosphide, or molybdenum phosphide.
17. The composite material according to any one of claims 1-4, characterized in that, The conductive agent includes carbon materials.
18. The composite material according to claim 17, characterized in that, The conductive agent includes a carbon-based conductive agent.
19. The composite material according to claim 18, characterized in that, The carbon-based conductive agent includes one or more of the following: carbon nanotubes, carbon fibers, acetylene black, Ketjen black, conductive carbon black, C60, or graphene.
20. The composite material according to any one of claims 1-4, characterized in that, The powder resistivity R of the composite material at 20 MPa satisfies: R ≤ 360 Ω·cm.
21. The composite material according to claim 20, characterized in that, R≤1Ω·cm.
22. A method for preparing a composite material as described in any one of claims 1-21, characterized in that, include: A lithium source, a catalyst, a conductive agent, and a sodium source are added to a solvent to obtain a slurry. The catalyst includes one or more of the following: oxides of transition metals, carbides of transition metals, nitrides of transition metals, or phosphides of transition metals. The slurry is dried to obtain the composite material.
23. The preparation method according to claim 22, characterized in that, The process of drying the slurry to obtain the composite material includes: The slurry is dried by spray drying to obtain the composite material.
24. The preparation method according to claim 22, characterized in that, The drying temperature T satisfies the following condition: 150℃≤T≤250℃.
25. The preparation method according to claim 24, characterized in that, 175℃≤T≤225℃。 26. The preparation method according to any one of claims 22-25, characterized in that, Based on the sum of the masses of the lithium source, the catalyst, the conductive agent, and the sodium source, the mass content C of the sodium source satisfies: 0.001wt%≤C≤0.25wt%.
27. The preparation method according to claim 26, characterized in that, 0.02wt%≤C≤0.1wt%.
28. The preparation method according to any one of claims 22-25, characterized in that, The lithium source includes one or more of Li2C2O4, Li2CO3, Li2C4O4, Li2C3O5, Li2C4O6, or LiOH.
29. The preparation method according to any one of claims 22-25, characterized in that, The sodium source includes one or more of the following: NaOH, Na2CO3, NaCl, NaNO3, Na2SO4, NaHSO4, NaHCO3, Na2C2O4, Na2C4O4, Na2C3O5, or Na2C4O6.
30. A positive electrode plate, characterized in that, include: The composite material according to any one of claims 1-21, and / or the composite material obtained by the preparation method according to any one of claims 22-29.
31. A secondary battery, characterized in that, Including the positive electrode sheet as described in claim 30.
32. The secondary battery according to claim 31, characterized in that, The secondary battery is the secondary battery before formation.
33. An electrical appliance, characterized in that, Includes the secondary battery as described in claim 31 or 32.
Citation Information
Patent Citations
Positive electrode lithium supplementing material and preparation method and application thereof
CN116598443A
Positive electrode lithium supplementing material and preparation method and application thereof