A method for preparing alkali metal materials from halogenated alkali metal salts and high-calcium sodium.

By employing a displacement reaction between halogenated alkali metal salts and high-calcium sodium, along with a linked component design, the problem of complete recycling of high-calcium sodium was solved. This enabled the simultaneous processing of sodium and calcium, simplified the process, reduced costs, and improved the accuracy of detection and the durability of the temperature and humidity probe.

CN120738486BActive Publication Date: 2026-11-17INNER MONGOLIA XISHANGXI NEW MATERIAL TECH CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202510943353.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-09
Publication Date
2026-11-17
Estimated Expiration
2045-07-09

AI Technical Summary

Technical Problem

Existing technologies make it difficult to completely recycle high-calcium sodium, and the secondary slag and waste generated during the process result in high equipment costs and energy consumption. Furthermore, the thermometer and hygrometer are easily damaged in high-temperature environments, making it difficult to achieve reasonable linkage between the flipping structure and temperature and humidity acquisition.

Method used

The process employs a displacement reaction between halogenated alkali metal salts and high-calcium sodium. The displacement reaction is carried out in a high-temperature vacuum furnace under inert gas protection. Combined with drying and dehydration equipment and sodium slag crushing equipment, the chemical reaction between halogenated alkali metal salts and high-calcium sodium enables the simultaneous treatment of sodium and calcium. The linkage components enable the protection and detection of temperature and humidity probes.

Benefits of technology

It achieves complete recovery and utilization of sodium and calcium in high-calcium sodium, simplifies the post-processing process, reduces equipment and energy costs, increases product added value, and improves the accuracy and durability of detection by protecting the temperature and humidity probe through linkage components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120738486B_ABST
    Figure CN120738486B_ABST
Patent Text Reader

Abstract

This application discloses a method for preparing alkali metal materials from haloalkali metal salts and high-calcium sodium, relating to the field of alkali metal recovery and preparation technology. The method involves drying the haloalkali metal salt using a drying and dehydration device; crushing or dissociating the high-calcium sodium using a sodium slag crushing device; introducing the haloalkali metal salt from step S100 and the high-calcium sodium from step S200 into a high-temperature vacuum furnace and carrying out a displacement reaction under the protection of an inert gas; and storing the alkali metal material, as a product of the displacement reaction, in a storage tank by distillation. The technical advantages of this application are: the displacement reaction between the haloalkali metal salt and high-calcium sodium thoroughly removes impurities from the high-calcium sodium obtained from electrolytic sodium chloride, purifying not only sodium for subsequent applications but also treating calcium, the second largest component by mass, reducing post-processing steps and further improving economic efficiency; the equipment and energy costs required by this invention are reasonable, highly targeted, and safe to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of alkali metal recovery and preparation technology, and in particular to a method for preparing alkali metal materials from haloalkali metal salts and high-calcium sodium. Background Technology

[0002] In the process of producing metallic sodium through the molten electrolysis of sodium chloride, a certain amount of electrolytic tailings remains after the metallic sodium is separated from the electrolytic cell. This tailings are commonly known as high-calcium sodium, or secondary sodium. The amount of high-calcium sodium produced is approximately 3% of the metallic sodium yield. High-calcium sodium contains 60-80% sodium, 10-40% calcium, and small amounts of residual molten salts such as sodium chloride, calcium chloride, and oxide impurities such as sodium oxide and calcium oxide. High-calcium sodium is difficult to process, and long-term storage poses safety hazards. Extracting metallic sodium from high-calcium sodium not only improves economic efficiency but also allows for the recycling and reuse of hazardous waste, eliminating safety hazards and environmental pollution.

[0003] Common industrial methods for processing high-calcium sodium metal include: extrusion as mentioned in CN2846437Y and CN2846436Y; vacuum distillation as proposed in CN104294054A and CN102634671A; sub-boiling distillation using thermal radiation synergistic distillation as described in CN103757435A and CN203700465U; vacuum distillation as described in CN103667708A, CN111363922A, and CN212560390U; and CN1 The molten salt heating method in 07574318A; the molten electrolysis method mentioned in CN108048872B, CN203700555U, CN108624913A and "Research on the Purification of Metallic Sodium through Na•β—Al_2O_3 Membrane"; the direct heating filtration method adopted in patents CN206188863U, CN109136579B, and CN208378965U; and other treatment methods such as heating solvent filtration, cold trap method, chemical treatment method, and sedimentation method. Some of these methods do not completely remove impurities from the resulting products, while others introduce new substances that need to be separated, and the required equipment costs and energy consumption are relatively high. In addition, none of these methods solve the problem of treating calcium slag, which accounts for the second largest proportion of the mass in high-calcium sodium. Calcium slag is relatively hard and reactive, and collecting high-purity calcium products is difficult, except for vacuum distillation which requires certain equipment. In order to completely process high-calcium sodium, there is an urgent need for a method that can easily recover and reuse both sodium and calcium in high-calcium sodium. When drying and pretreating haloalkali metal salts, it is necessary to periodically turn the material over and collect temperature and humidity data. After the haloalkali metal salt material is evenly turned over, the temperature and humidity meter is manually inserted. This is difficult to do manually in high-temperature operations. Alternatively, the temperature and humidity meter can be directly embedded, but the fixed embedding height leads to inaccurate data collection, and the temperature and humidity meter is easily damaged by long-term exposure to high-temperature environments. How to achieve a reasonable linkage between the turning structure and temperature and humidity collection has also become a technical problem that needs to be solved by those skilled in the art. Summary of the Invention

[0004] To address the shortcomings of existing technologies, this invention provides a method for preparing alkali metal materials from halogenated alkali metal salts and high-calcium sodium. This method solves the technical problems of existing technologies, such as the difficulty in achieving reasonable recovery and full utilization of high-calcium sodium, and the generation of secondary slag waste. Furthermore, it enables the synthesis of high-value alkali metals to increase product added value. The specific implementation method is as follows: A method for preparing alkali metal materials from halogenated alkali metal salts and high-calcium sodium includes the following steps: S100. The alkali metal halide salt is dried and dehydrated using a drying and dehydration device. S200: High-calcium sodium is crushed or dissociated using sodium slag crushing equipment; S300: The haloalkali metal salt from step S100 and the high-calcium sodium from step S200 are introduced into a high-temperature vacuum furnace and subjected to a displacement reaction under the protection of an inert gas. The reaction principle of the displacement reaction in steps S400 and S300 is as follows: Na + Ca + MX → NaX + CaX2 + M Ca + Na₂O → CaO + Na Where M refers to one or more of lithium, sodium, potassium, rubidium, and cesium, and X refers to one or two of halogens, namely chlorine or fluorine; S500, the alkali metal material, which is the product of the substitution reaction, is introduced into the storage tank for storage by distillation.

[0005] Preferably, the halogenated alkali metal salt is one or more of fluorinated or chlorinated alkali metal salts; the main components of the high-calcium sodium are: 60-80% sodium, 10-40% calcium, and a small amount of residual molten salt such as sodium chloride, calcium chloride, and oxide impurities such as sodium oxide, calcium oxide, etc.

[0006] Preferably, the alkali metal material is one or more alkali metal elements or alkali metal alloys; the alkali metal is one or more of lithium, sodium, potassium, rubidium, and cesium; the alkali metal alloy is an alkali metal alloy composed of one or more of lithium, potassium, rubidium, and cesium and sodium in an appropriate proportion.

[0007] Based on the above technical solutions, a more thorough impurity removal process can be achieved through the displacement reaction of halogenated alkali metal salts with high-calcium sodium obtained from electrolytic sodium chloride. This process not only purifies sodium for subsequent applications but also simultaneously treats calcium, the second most abundant element, effectively shortening the post-processing steps. This technical approach improves sodium purity while further enhancing overall economic efficiency by simplifying the process chain.

[0008] Preferably, the ratio of the haloalkali metal salt to high-calcium sodium is 0.5-10:1.

[0009] Preferably, in step S100, calcium chloride is also added to the drying and dehydration equipment. The calcium chloride forms a mixed salt with the haloalkali metal salt, which is the reaction substrate, to lower the melting point of the desired mixture.

[0010] Preferably, the high-calcium sodium in step S200 is broken and dissociated in an inert gas environment, and the inert gas in steps S200 and S300 is argon.

[0011] Based on the above technical solutions, the dehydration of haloalkali metal salts can be achieved by one or more of the following technologies: vacuum high-temperature dehydration, microwave drying, azeotropic distillation, vibrating fluidized bed drying, and membrane separation.

[0012] Preferably, in step S200, the sodium slag disintegration equipment uses heating followed by the addition of a solvent, and utilizes the difference in density and complexation degree for layered filtration and separation. The solvent is one or more of the following: thermally conductive silicone oil, 2-methylnaphthalene, high-boiling-point saturated aliphatic hydrocarbons or aromatic hydrocarbons, ionic liquids, esters, ethers, and other density gradient liquids.

[0013] Based on the above technical solutions, the high-calcium sodium crushing and dissociation method can also be selected by using one or more of the following in an inert gas environment: a double spiral belt crusher, a hammer mill, or a toothed disc crusher, to crush by mechanical force.

[0014] Preferably, the temperature of the displacement reaction in step S300 is 600-900℃, the holding time is 3-12h, and the pressure inside the furnace is 0.05-0.5MPa.

[0015] Preferably, in step S600, the byproduct is separated by vacuum distillation or hot filtration, and the byproduct is a mixture of calcium chloride and sodium chloride composite salts used in the preparation of de-icing agents.

[0016] Based on the above technical solutions, after the required alkali metal or alkali metal alloy is prepared, the product and by-product need to be separated by separation methods such as vacuum distillation or hot filtration. The resulting by-products, such as a mixture of compound salts like calcium chloride and sodium chloride, can be further prepared into the main components of de-icing agents or treated in other ways.

[0017] An apparatus for preparing alkali metal materials from haloalkali metal salts and high-calcium sodium includes a drying and dehydration device for vacuum high-temperature dehydration in step S100. The drying and dehydration device includes a drying chamber and a heating base. A square isolation box is provided inside the drying chamber, and the haloalkali metal salts are C-shaped filled inside the drying chamber.

[0018] The square isolation box has a built-in linkage component, which includes a vertical closed-loop conveyor belt. Temperature and humidity probes and a flip plate are respectively installed at high and low positions on both sides of the conveyor belt. The overall outline of the flip plate matches the C-shaped layout of the drying box. A second opening is opened at the low position of the square isolation box, and the temperature and humidity probe communicates with the second opening when it is at the low position.

[0019] The square isolation box is also equipped with a vertical lifting component. The output end of the lifting component is connected to the flip plate. The lifting and lowering of the flip plate is transmitted to the temperature and humidity probe through the linkage component. The lifting and lowering directions of the flip plate and the temperature and humidity probe are opposite.

[0020] Based on the above technical solutions, when pretreating halogenated alkali metal salts in a high-temperature vacuum furnace, moisture can be effectively removed through a drying process. When detecting the degree of dryness, the temperature and humidity probe and the turning plate are linked: after the turning plate completes the material turning, the temperature and humidity probe is exposed for detection. This linkage mechanism not only ensures the uniformity of the test sample, but also protects the temperature and humidity probe during the material turning process, achieving a dual optimization of process reliability and detection accuracy.

[0021] In summary, this application includes the following beneficial technical effects: 1. This invention achieves a more thorough purification of high-calcium sodium obtained from electrolytic sodium chloride through a displacement reaction between a haloalkali metal salt and high-calcium sodium. Not only is sodium purified for subsequent applications, but calcium, which accounts for the second largest proportion by mass, is also treated, reducing the post-processing steps and further improving economic efficiency. 2. The equipment and energy required by this invention are cost-effective, the process is simple, it is highly targeted, and the operation is safe; 3. The present invention has a simple structure. By setting up a high-temperature vacuum furnace to pretreat halogenated alkali metal salts, water can be effectively removed through drying. When the degree of dryness is detected by the temperature and humidity probe, the flipping plate is linked with the temperature and humidity probe. After the flipping plate flips the material, the temperature and humidity probe is exposed for detection. This can improve the uniformity of the test sample and also protect the temperature and humidity probe. 4. In this invention, the flipping plate can be linked with the temperature and humidity probe, or it can independently flip the material, which reduces the exposure frequency of the temperature and humidity probe before drying is completed and further improves the durability of the temperature and humidity probe. Attached Figure Description

[0022] Figure 1 This is a schematic diagram of the process flow of the present invention; Figure 2 This is a schematic diagram of the structure of the present invention; Figure 3 This is an exploded structural diagram of the present invention; Figure 4 This is a cross-sectional view of the present invention after the cooling structure has been added; Figure 5 This is a cross-section of the structure of the present invention. Figure 1 ; Figure 6 This is a cross-section of the structure of the present invention. Figure 2 ; Figure 7 This is a cross-section of the structure of the present invention. Figure 3 ; Figure 8 This is an exploded structural diagram of the drying oven in this invention; Figure 9 This is a schematic diagram of the linkage component and the flip plate in this invention. Figure 1 ; Figure 10 In this invention Figure 9 Enlarged schematic diagram; Figure 11 This is a cross-section of the linkage component and the flip-plate structure in this invention; Figure 12 This is a schematic diagram of the linkage component and the flip plate in this invention. Figure 2 .

[0023] Explanation of reference numerals in the attached figures: 1. Drying oven; 2. Linkage assembly; 3. Flip plate; 4. Temperature and humidity probe; 5. Locking assembly; 6. Square isolation box; 7. Lifting platform; 8. Cooling tower; 9. Cooling unit; 10. Heating base; 11. Thermal liquid tank; 12. Liquid piping; 13. Opening and closing valve; 14. Temperature sensor; 15. Water pump; 16. Lifting assembly. 101. Feed inlet; 102. Top cover; 103. Bulk material conical head. 201. Conveyor belt; 202. Partition plate; 203. Elastic telescopic component; 204. Guide wheel; 205. Vertical guide groove; 206. Serrated; 207. Side plate. 301. Mounting base; 302. Angle-folded loose material plate; 303. Horizontal plate. 501. Handle; 502. Gear; 503. Synchronizing block; 504. Locking wheel. 601, First opening; 602, Second opening. Detailed Implementation

[0024] The specific embodiments of the present invention are described below with reference to the accompanying drawings and examples: It should be noted that the structures, proportions, sizes, etc. illustrated in the accompanying drawings of this specification are only used to complement the content disclosed in the specification, so that those skilled in the art can understand and read them, and are not intended to limit the conditions under which the present invention can be implemented. Any modifications to the structure, changes in the proportions, or adjustments to the size, without affecting the effects and objectives that the present invention can produce, should still fall within the scope of the technical content disclosed in the present invention.

[0025] Furthermore, the terms such as "upper," "lower," "left," "right," "middle," and "one" used in this specification are merely for clarity of description and are not intended to limit the scope of the invention. Any changes or adjustments to their relative relationships, without substantially altering the technical content, should also be considered within the scope of the invention.

[0026] The following is in conjunction with the appendix Figure 1-12 This application will be described in further detail.

[0027] This application discloses a method for preparing alkali metal materials from haloalkali metal salts and high-calcium sodium.

[0028] Example 1, referring to Figure 1 This embodiment discloses a method for preparing alkali metal materials from haloalkali metal salts and high-calcium sodium. This method is used to prepare refined sodium and includes the following steps: The first step is to place 100 kg of high-calcium sodium in a high-calcium sodium melting tank and turn on argon protection. Slowly heat it to above 120°C. After the high-calcium sodium has initially dissociated, turn on the stirring to accelerate the dissociation. The stirring speed should be gradually increased from slow to fast depending on the degree of dissociation, and then maintained at 50-300 rpm to obtain molten high-calcium sodium. The second step involves placing 105 kg of sodium chloride solid and 160 kg of calcium chloride solid in a high-temperature resistance furnace for vacuum high-temperature dehydration at 200°C under 10-100 Pa for 2 hours, so that the water content is no more than 0.1%.

[0029] The third step involves placing molten high-calcium sodium and dry sodium chloride, along with solid calcium chloride, into a high-temperature vacuum furnace at 600-800°C via pipelines and a feeding device for a displacement reaction. Under argon protection, metallic sodium and calcium chloride gradually form.

[0030] The fourth step involves maintaining the displacement reaction for two hours after the temperature stabilizes and no longer rises significantly or decreases slightly, and the detector shows that the amount of sodium vapor no longer changes. After the displacement reaction is complete, the resulting metallic sodium is distilled under a low vacuum of 0.1-1 Pa and stored in a sodium storage tank, yielding approximately 99.4 kg of sodium with a purity of approximately 99.9%. The final sodium is then die-cast into silvery-white cylindrical sodium ingots with a diameter of approximately 30 mm, a length of approximately 500 mm, and a weight of approximately 35 kg.

[0031] In the fifth step, after the reaction is complete, the remaining by-products in the high-temperature vacuum furnace are cooled and then removed by rotating through the liftable furnace chamber and rotating arm to obtain approximately 243 kg of calcium chloride and 17 kg of sodium chloride mixed white solid, with a very small amount of sodium oxide, calcium oxide and other small impurities. This product can be used in the preparation of de-icing agents.

[0032] Example 2, refer to Figure 1 Unlike the above embodiments, this embodiment also discloses a method for preparing alkali metal materials from haloalkali metal salts and high-calcium sodium. This method is used to prepare sodium-potassium alloys and includes the following steps: The first step involves crushing 100 kg of high-calcium sodium in an inert gas environment using a double-spiral belt crusher. The crusher's cutter shafts are made of high-wear-resistant stainless steel alloy, with staggered spiral cutters or toothed rollers arranged on the shafts. During operation, the two spiral shafts rotate in opposite directions. After the high-calcium sodium enters the crushing chamber, it is broken down into particles of 10-50 mm in size by the shearing and tearing forces of the spiral belt cutters.

[0033] The second step involves placing 150 kg of potassium chloride solid and 100 kg of calcium chloride solid in a vibrating fluidized bed for high-temperature dehydration under the following conditions: inlet air temperature of 150°C, air velocity of 0.5 m / s, amplitude of 1 mm, and residence time of 30 min, so that the moisture content is no more than 0.1%.

[0034] The third step involves placing high-calcium sodium granules and dry potassium chloride and calcium chloride solid in a high-temperature vacuum furnace at 600-800℃ via pipelines and a feeding device to carry out a displacement reaction. Under argon protection, metallic sodium-potassium alloy and calcium chloride and sodium chloride are gradually formed.

[0035] The fourth step involves maintaining the displacement reaction for two hours after the temperature stabilizes and no longer rises significantly or even decreases slightly, and the detector shows no further change in the amount of sodium vapor. After the displacement reaction is complete, the resulting sodium-potassium alloy is distilled under a low vacuum of 0.1-1 Pa and stored in an alloy storage tank, yielding approximately 137.5 kg of sodium-potassium alloy with a purity of approximately 99.9%. This alloy contains approximately 58.9 kg of sodium (42.8%) and approximately 78.6 kg of potassium (57.2%). The final sodium-potassium alloy has a melting point of approximately 19°C and a density of 0.89.

[0036] In the fifth step, after the reaction is complete, the remaining by-products in the high-temperature vacuum furnace are cooled and then removed by rotating through the liftable furnace chamber and rotating arm to obtain a white solid mixture of approximately 197.1 kg of calcium chloride and 58.5 kg of sodium chloride, containing a very small amount of impurities such as calcium oxide. This mixture can be used in the preparation of de-icing agents.

[0037] Example 3, referring to Figure 1 Unlike the above embodiments, this embodiment also discloses a method for preparing alkali metal materials from haloalkali metal salts and high-calcium sodium. This method is used to prepare metallic potassium and includes the following steps: First, add 100 kg of high-calcium sodium and 300 kg of 2-methylnaphthalene to a stirred tank, slowly heat to above 150°C, and slowly start stirring, gradually increasing the stirring speed from slow to 10-300 rpm. After the high-calcium sodium is completely dissociated, vacuum filter to obtain fragmented high-calcium sodium; The second step involves microwave infrared drying of 350 kg of potassium chloride solid and 150 kg of calcium chloride solid. The microwave power is 18 kW, the frequency is 2450 MHz, the working temperature is 120 ℃, the material layer thickness is 10 mm, the conveying speed is 1 m / min, the air volume is 2000 m³ / h, the far-infrared band is 3-10 μm, and the processing time is 6 h, so that the moisture content is no more than 0.2%.

[0038] The third step involves placing the crushed high-calcium sodium and dried potassium chloride, along with the solid calcium chloride, into a high-temperature vacuum furnace at 600-800°C via pipelines and a feeding device for a displacement reaction. Under argon protection, metallic potassium, calcium chloride, and sodium chloride are gradually formed.

[0039] The fourth step is to maintain the displacement reaction for two hours after the temperature stabilizes and no longer rises significantly or decreases slightly, and the detector shows that the amount of sodium vapor no longer changes. After the displacement reaction is completed, the resulting metallic potassium is distilled under a low vacuum of 0.1-1 Pa and enters a potassium storage tank, yielding approximately 178.5 kg of potassium with a purity of approximately 99.9%. Finally, the potassium is die-cast into silver-white cylindrical potassium ingots with a diameter of approximately 30 mm, a length of approximately 500 mm, and a weight of approximately 30 kg.

[0040] In the fifth step, after the reaction is complete, the remaining byproducts in the high-temperature vacuum furnace are cooled and then removed by rotating through the liftable furnace chamber and rotating arm, yielding a white solid mixture of approximately 247.1 kg of calcium chloride, 165.3 kg of sodium chloride, and 9.1 kg of potassium chloride, containing a very small amount of impurities such as calcium oxide. This mixture can be used in the preparation of de-icing agents.

[0041] Example 4, refer to Figures 2 to 12This embodiment discloses a drying and dehydration device for preparing alkali metal materials from halogenated alkali metal salts and high-calcium sodium. The drying and dehydration device includes a drying chamber 1 and a heating base 10. A square isolation box 6 is provided inside the drying chamber 1, and the halogenated alkali metal salts are filled in a C-shape within the drying chamber 1. A linkage component 2 is built into the square isolation box 6. The linkage component 2 includes a vertically arranged closed-loop conveyor belt 201. Temperature and humidity probes 4 and a tilting plate 3 are respectively installed at high and low positions on both sides of the conveyor belt 201. The overall outline of the tilting plate 3 conforms to the C-shaped layout of the drying chamber 1. A second opening 602 is provided at the low position of the enclosure 6. When the temperature and humidity probe 4 is at the low position, it communicates with the second opening 602. In this structure, a lifting component 16 is also vertically provided inside the square isolation enclosure 6. The output end of the lifting component 16 is connected to the flip plate 3. The lifting and lowering of the flip plate 3 is transmitted to the temperature and humidity probe 4 through the linkage component 2, and the lifting and lowering directions of the flip plate 3 and the temperature and humidity probe 4 are opposite. A wiping sponge can be built into the top of the square isolation enclosure 6. After the temperature and humidity probe 4 is lifted and hidden, it can be cleaned by wiping with the sponge to improve the sensitivity and accuracy of subsequent detection.

[0042] The linkage component 2 also includes a sealing plate 202 and a side plate 207 on both sides. Both of them have a vertical guide groove 205 on their inner side. A lifting seat 7 is slidably mounted on the vertical guide groove 205. The lifting seat 7 is connected to the temperature and humidity probe 4.

[0043] The top of the drying chamber 1 is provided with a top cover 102 with a feed inlet 101, and a material-dispersing cone head 103 is provided inside the feed inlet 101. In this structure, the haloalkali metal salt is pre-dispersed by the tip of the material-dispersing cone head 103 to improve the subsequent drying quality.

[0044] The flip plate 3 includes a mounting base 301 connected to the conveyor belt 201. The mounting base 301 has a folded material distribution plate 302 extending downwards through a horizontal plate 303. The folded material distribution plate 302 is horizontally designed as a narrowed, hollow shape from the inside out. A first opening 601 is provided on the side of the square isolation box 6 away from the second opening 602. The height of the first opening 601 is greater than that of the second opening 602. The second opening 602 is used for vertical sliding of the mounting base 301. A telescopic plate for sealing is fitted between the mounting base 301 and the second opening 602 to prevent materials from being introduced through the gap of the second opening 602. A corresponding telescopic plate can also be set between the first opening 601 and the temperature and humidity probe 4, so that the conveyor belt 201 is completely built into the square isolation box 6, improving the isolation effect.

[0045] The specific implementation process is as follows: the alkali halide metal salt is introduced through the feed inlet 101, and under the action of the bulk material conical head 103, the alkali halide metal salt is initially dispersed; when temperature and humidity detection is required, the lifting component 16, which acts as a cylinder, moves the flipping plate 3 upward, and the upward movement of the flipping plate 3 causes the alkali halide metal salt to be flipped; when the flipping plate 3 moves upward, the conveyor belt 201 causes the temperature and humidity probe 4 to move downward, and after the first opening 601 coincides with the temperature and humidity probe 4, the temperature and humidity probe 4 is exposed to begin the detection of drying effect.

[0046] Example 5, refer to Figure 4 Based on Example 4, this example discloses a drying and dehydration device for preparing alkali metal materials from halogenated alkali metal salts and high-calcium sodium. It includes a heat-conducting liquid tank 11 located on the side of the drying chamber 1. A liquid pipeline 12 is provided between the high and low positions of the heat-conducting liquid tank 11. Both the inlet and outlet of the liquid pipeline 12 are equipped with opening and closing valves 13. A temperature sensor 14, a water pump 15, and a cooling unit 9 are connected in series on the liquid pipeline 12. In this structure, the cooling unit 9 is connected to a cooling tower 8. During the heat preservation and drying state, both opening and closing valves 13 are closed, and the heat-conducting liquid tank 11 provides heat preservation. When rapid cooling of the drying chamber 1 is required after drying, both opening and closing valves 13 are opened, and the liquid in the liquid pipeline 12 is drawn from the top, cooled by the cooling unit 9, and then returned to the drying chamber 1 from the bottom. The heat-conducting liquid tank 11 preferentially draws out the liquid with the higher temperature at the top, which can improve heat dissipation efficiency.

[0047] Example 6, refer to Figures 8 to 12 Based on Example 4, this example discloses a drying and dehydration device for preparing alkali metal materials from halogenated alkali metal salts and high-calcium sodium. The linkage component 2 also includes guide wheels 204 and serrated 206 provided on the vertical guide groove 205. Each guide wheel 204 supports the conveyor belt 201 as a square frame, and the middle section of the conveyor belt 201 is provided with an elastic telescopic member 203, which is preferably a spring.

[0048] The locking assembly 5 includes a gear 502 and a locking wheel 504 that are rotatably mounted on the lifting seat 7. The gear 502 meshes with the sawtooth 206 on both sides. In this structure, the gear 502 is coaxially connected to a synchronizing block 503. The synchronizing block 503 has several arc surfaces equidistantly arranged along its circumference. The locking wheel 504 is coaxially connected to the handle 501. The locking wheel 504 can also be coaxially connected to the drive motor. The locking wheel 504 has a notch. The notch in the locking wheel 504 interacts with the arc surface of the synchronizing block 503.

[0049] The specific implementation process is as follows: the flipping plate 3 needs to be flipped up and down multiple times during drying, and the number of detections by the temperature and humidity probe 4 is less than the flipping frequency of the flipping plate 3; when the flipping plate 3 is flipped in the early stage, the temperature and humidity probe 4 needs to be locked; the flipping locking wheel 504 is turned so that the non-notch part of the locking wheel 504 is engaged with the arc surface on the synchronization block 503, at which time the gear 502 is locked on the vertical guide groove 205; the lifting component 16 drives the flipping plate 3 to move up and down to complete the vertical stirring of the halogenated alkali metal salt, and the elastic telescopic component 203 deforms to adapt to the position locking of the gear 502.

[0050] Comparative Example 1: Referring to CN103757435A, this comparative example relates to a method for purifying metallic sodium. Solid metallic sodium with a purity of 99.5% is placed in a distillation vessel, sealed with bolts, and mounted on a heating furnace. The solid sodium is heated by an infrared radiation lamp and a focusing tube. Under conditions of controlled temperature (240℃~260℃), vacuum degree ≤10Pa, heating time of 2 hours, and two intermediate applications of high-purity argon gas to carry impurities, the solid sodium is melted into a liquid state. Volatile impurities in the liquid metallic sodium evaporate and separate from the liquid sodium. A vacuum pump is used to remove the volatile impurities. The liquid sodium is then heated in the furnace to 400℃. Circulating cooling water is then introduced through a condenser tube, and external radiation-assisted distillation is applied. Thermal radiation raises the liquid surface temperature, accelerating the evaporation rate of sodium. Sodium vapor rapidly condenses into solid sodium upon contact with the condenser tube, thus achieving thermal radiation-assisted distillation purification of metallic sodium. This example requires a high content of raw materials, and the impurities are not completely removed. Only low-boiling-point impurities can be treated, and the remaining sodium slag cannot be completely processed.

[0051] Comparative Example 2: Referring to CN107574318A, this comparative example relates to a method for purifying and separating sodium slag and the purification equipment used. Molten salt, a mixture of sodium chloride, potassium chloride, and calcium chloride, is prepared in a molten salt melting furnace and heated to 600℃ to melt. Sodium slag with a sodium content of 65wt% and a calcium content of 24wt% is slowly added in batches to the sodium slag melting tank. After the sodium slag reaches its melting point, it flows into the molten salt melting furnace through a downcomer. After buffering, the sodium slag enters the molten salt liquid. Through the separation action of the molten salt liquid, the separated sodium floats to the surface of the molten salt liquid and is collected in a sodium collection device through a sodium recovery pipe. This example uses a mixed molten salt as a solvent to heat the sodium slag, but it essentially does not solve the problem of calcium recovery and utilization from the sodium slag.

[0052] Comparative Example 3: Referring to CN108624913A, this comparative example relates to a process for molten electrolytic purification of industrial sodium into high-purity sodium. The process involves filling a small sodium refinement container with sodium seeds. With the argon pressure in the electrolytic cell at 0.1 kPa, the small sodium refinement container is connected to the cathode tube. The electrolytic cell is heated to 180°C and held at this temperature to preheat the ceramic diaphragm tube. Then, heating of the small sodium refinement container and the cathode tube begins, and the temperature is maintained at 180°C. All the sodium seeds are injected into the ceramic diaphragm tube. The industrial sodium container, industrial sodium transition container, and electrolytic cell are heated to 180°C, held at this temperature, and argon gas is introduced. Then, the industrial sodium... Sodium is injected into the industrial sodium transition tank and then into the electrolytic cell. When the industrial sodium in the electrolytic cell reaches a specified amount, injection is stopped. When the industrial sodium transition tank is full of industrial sodium, injection is stopped again. Finally, the industrial sodium transition tank is heated to 260°C and kept at that temperature. After a period of time, the electrolysis current is set to 10A, and electrolysis begins. After a period of electrolysis, the current is increased. When the refined sodium production in the ceramic diaphragm tube reaches a specified amount, electrolysis is stopped. Using the argon gas pressure difference between the electrolytic cell and the refined sodium tank, the refined sodium in the ceramic diaphragm tube is forced into the refined sodium tank through the refined sodium pipeline. After sodium removal is completed, electrolysis is restarted. After multiple sodium removals, industrial sodium from the industrial sodium transition tank is injected into the electrolytic cell to replenish the industrial sodium. Then, industrial sodium from the industrial sodium tank is injected into the industrial sodium transition tank until it is full, at which point the injection stops. When the refined sodium in the refined sodium tank reaches the specified amount, the refined sodium in the refined sodium tank is discharged into a refined sodium storage tank that has been evacuated and heated to 110°C. This method uses complex equipment, is expensive, and cannot solve the problem of recovering and utilizing sodium slag calcium.

[0053] Many other changes and modifications can be made without departing from the concept and scope of this invention. It should be understood that this invention is not limited to the specific embodiments, and the scope of this invention is defined by the appended claims.

Claims

1. A method for preparing alkali metal materials from halogenated alkali metal salts and high-calcium sodium, characterized in that, Includes the following steps: S100. The alkali metal halide salt is dried and dehydrated using a drying and dehydration device. S200: High-calcium sodium is crushed or dissociated using sodium slag crushing equipment; S300: The haloalkali metal salt from step S100 and the high-calcium sodium from step S200 are introduced into a high-temperature vacuum furnace and subjected to a displacement reaction under the protection of an inert gas. The reaction principle of the displacement reaction in steps S400 and S300 is as follows: Na + Ca + MX → NaX + CaX2 + M Ca + Na₂O → CaO + Na Where M refers to one or more of lithium, sodium, potassium, rubidium, and cesium, and X refers to one or two of halogens, namely chlorine or fluorine; S500, the alkali metal material, which is the product of the substitution reaction, is introduced into the storage tank for storage by distillation; It also includes a drying and dehydration device used in step S100. The drying and dehydration device includes a drying box (1) and a heating base (10). The drying box (1) is provided with a square isolation box (6), and the haloalkali metal salt is filled in the drying box (1) in a C-shape. The square isolation box (6) has a built-in linkage component (2), which includes a vertical closed-loop conveyor belt (201). Temperature and humidity probes (4) and a flip plate (3) are respectively provided at high and low positions on both sides of the conveyor belt (201). The overall outline of the flip plate (3) matches the C-shaped layout of the drying box (1). A second opening (602) is provided at the low position of the square isolation box (6). When the temperature and humidity probe (4) is at the low position, it communicates with the second opening (602). The square isolation box (6) is also vertically equipped with a lifting component (16). The output end of the lifting component (16) is connected to the flip plate (3). The lifting and lowering of the flip plate (3) is transmitted to the temperature and humidity probe (4) through the linkage component (2). The lifting and lowering directions of the flip plate (3) and the temperature and humidity probe (4) are opposite. The top of the square isolation box (6) is equipped with a wiping sponge. After the temperature and humidity probe (4) is lifted and hidden, it is cleaned by the wiping sponge.

2. The method for preparing alkali metal materials from haloalkali metal salts and high-calcium sodium according to claim 1, characterized in that, The haloalkali metal salt is one or more of fluorinated or chlorinated alkali metal salts.

3. The method for preparing alkali metal materials from haloalkali metal salts and high-calcium sodium according to claim 2, characterized in that, The alkali metal material is one or more alkali metal elements or alkali metal alloys; The alkali metal is one or more of lithium, sodium, potassium, rubidium, and cesium; The alkali metal alloy is an alkali metal alloy composed of one or more alkali metals selected from lithium, potassium, rubidium, and cesium, and a mixture of sodium in appropriate proportions.

4. The method for preparing alkali metal materials from a haloalkali metal salt and high-calcium sodium according to claim 1, characterized in that, The mass ratio of the haloalkali metal salt to high-calcium sodium is 0.5-10:

1.

5. The method for preparing alkali metal materials from a haloalkali metal salt and high-calcium sodium according to claim 1, characterized in that, In step S100, calcium chloride is also added to the drying and dehydration equipment. The calcium chloride forms a mixed salt with the haloalkali metal salt, which is the reaction substrate, to lower the melting point of the desired mixture.

6. The method for preparing alkali metal materials from haloalkali metal salts and high-calcium sodium according to claim 1, characterized in that, The high-calcium sodium described in step S200 is broken down and dissociated in an inert gas environment.

7. The method for preparing alkali metal materials from a haloalkali metal salt and high-calcium sodium according to claim 6, characterized in that, The inert gas in step S200 is nitrogen or argon, and the inert gas in step S300 is argon.

8. The method for preparing alkali metal materials from haloalkali metal salts and high-calcium sodium according to claim 1, characterized in that, In step S300, the temperature of the displacement reaction is 600-900℃, the holding time is 3-12h, and the pressure inside the furnace is 0.05-0.5MPa.

Citation Information

Patent Citations

  • Device for continuously recovering metallic sodium from sodium slag

    CN102634671A

  • Method for purifying metallic sodium

    CN103757435A

  • Method and apparatus for recycling metal sodium and calcium from sodium slag or calcium slag

    CN104294054A

  • Sodium slag purifying separation method and purifying equipment adopted in same

    CN107574318A

  • Technology for purifying industrial sodium into high-purity sodium through fusion electrolysis

    CN108624913A