Graphene carbon nano tube composite conductive paste for high-voltage electrode and preparation method of graphene carbon nano tube composite conductive paste

By combining carboxylated carbon nanotubes and fluorinated graphene with ionic liquid dispersants, the problems of easy oxidation and unstable dispersion of traditional conductive agents under high pressure were solved, thus achieving stable conductivity and long lifespan of high-voltage electrodes.

CN120878324APending Publication Date: 2025-10-31江苏希诚新材料科技有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202511068428.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-31
Publication Date
2025-10-31

AI Technical Summary

Technical Problem

Traditional conductive agents are prone to oxidation under high pressure, leading to increased electrode resistance, battery expansion and failure. Carbon nanotubes are prone to aggregation and have poor dispersion stability. Graphene sheet stacking leads to increased sedimentation rate and insufficient high-pressure compatibility.

Method used

By combining carboxylated single-walled carbon nanotubes and fluorinated modified graphene with ultrafine carbon black, ionic liquid dispersants, and rheology modifiers, a uniform conductive network is formed through high-shear dispersion and homogenization treatment, which suppresses electrochemical oxidation and electric field distortion.

Benefits of technology

It significantly improves the dispersion stability and high-voltage compatibility of conductive pastes, reduces resistance increase, extends battery life, and prevents battery swelling and failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of conductive agents, and particularly discloses graphene carbon nanotube composite conductive paste for a high-voltage electrode and a preparation method of the graphene carbon nanotube composite conductive paste. The graphene carbon nanotube composite conductive paste for the high-voltage electrode is prepared from the following raw materials in parts by weight: 2 to 6 parts of carboxylated single-walled carbon nanotube powder, 1 to 3 parts of fluorinated modified graphene powder, 0.6 to 1.2 parts of superfine carbon black, 2 to 4 parts of an ionic liquid dispersing agent, 0.2 to 0.4 part of a rheology modifier and 80 to 100 parts of N-methyl pyrrolidone. According to the graphene carbon nanotube composite conductive paste for the high-voltage electrode, the breakdown field strength can be remarkably improved, partial discharge is inhibited, and high conductivity is kept while the high-voltage service life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of conductive agent technology, and more specifically, to a graphene-carbon nanotube composite conductive paste for high-voltage electrodes and its preparation method. Background Technology

[0002] With the increasing demand for energy density in new energy vehicles, high-voltage cathode materials have become a key development direction for the industry. However, traditional conductive agents such as acetylene black and Ketjen black are prone to electrochemical oxidation under high voltages >4.3V, leading to degradation of the conductive network and a significant increase in electrode resistance after 100 cycles. Simultaneously, the oxidation decomposition generates CO2, causing battery swelling. Furthermore, metallic impurities such as Fe / Cu in carbon black can catalyze electrolyte decomposition, leading to battery failure. Graphene and carbon nanotube composite slurries are gradually replacing traditional conductive agents, but the following technical drawbacks still exist: Carbon nanotubes are prone to aggregation and have poor dispersion stability, requiring strong surfactants. The stacking of graphene sheets leads to an increased sedimentation rate, and the oxidation potential of the oxygen-containing groups (-OH / -C=O) at the edge of graphene is only 4.2V, resulting in insufficient high-voltage compatibility. Summary of the Invention

[0003] To address the shortcomings of existing technologies, the present invention aims to provide a graphene-carbon nanotube composite conductive paste for high-voltage electrodes and its preparation method.

[0004] To achieve the above objectives, the present invention provides the following technical solution: A graphene-carbon nanotube composite conductive paste for high-voltage electrodes comprises, by weight, 2-6 parts of carboxylated single-walled carbon nanotube powder, 1-3 parts of fluorinated modified graphene powder, 0.6-1.2 parts of ultrafine carbon black, 2-4 parts of ionic liquid dispersant, 0.2-0.4 parts of rheology modifier, and 80-100 parts of N-methylpyrrolidone.

[0005] Furthermore, the preparation method of the carboxylated single-walled carbon nanotube powder includes the following steps: Single-walled carbon nanotube powder, ammonium persulfate, and deionized water were mixed at a mass ratio of 1:5 to 10:100 and stirred in a water bath at 70 to 80°C for 6 to 12 hours. The lower solid layer was collected by centrifugation and washed 5 to 7 times with 10% to 20% hydrochloric acid, followed by 3 to 5 times with deionized water. The mixture was then vacuum dried at 50 to 60°C and -0.08 MPa to -0.06 MPa for 10 to 12 hours to obtain carboxylated single-walled carbon nanotube powder.

[0006] Furthermore, the diameter of the single-walled carbon nanotube powder is 1~3 nm.

[0007] Furthermore, the preparation method of the fluorinated modified graphene powder includes the following steps: S1. Weigh 2-4 parts graphene powder, 0.6-0.8 parts ethylenediamine, 0.4-0.6 parts perfluorooctyl sulfonyl fluoride, 0.1-0.3 parts triethylamine, and 80-100 parts N,N-dimethylformamide by weight. S2. Graphene powder is dispersed in N,N-dimethylformamide, ethylenediamine is added, and the mixture is reacted at 60~70℃ for 1~2 hours to obtain a mixed dispersion. S3. Add perfluorooctyl sulfonyl fluoride and ethylamine to the mixed dispersion, purge with nitrogen, and react at 50-60℃ for 6-12 hours. Centrifuge, remove the lower solid layer, clean it with anhydrous ethanol 3-5 times, and dry it to obtain fluorinated modified graphene powder.

[0008] Furthermore, the graphene powder has a sheet diameter of 0.6~1.2μm and 2~5 layers.

[0009] Furthermore, the particle size of the ultrafine carbon black is 20~30nm.

[0010] Furthermore, the ionic liquid dispersant includes at least one of 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, 1-ethyl-3-methylimidazolium tetrafluoroborate, and trihexyltetradecylphosphonium bis(trifluoromethanesulfonyl)imide salt.

[0011] Furthermore, the rheology modifier includes at least one of hydroxypropyl methylcellulose, ethylcellulose, polyethylene oxide, and polyethylene glycol.

[0012] Furthermore, the preparation method of the graphene-carbon nanotube composite conductive paste for the high-voltage electrode includes the following steps: (1) Weigh each component according to its weight percentage; (2) Add carboxylated single-walled carbon nanotube powder and 1 / 2 ionic liquid dispersant to 1 / 2 N-methylpyrrolidone, stir and wet at 300~500 rpm for 10~20 min, and then place it in a high shear disperser and disperse at 2000~4000 rpm for 30~60 min to obtain a pre-dispersed carbon nanotube slurry. (3) Place the pre-dispersed carbon nanotube slurry in a sand mill and grind and disperse it for 30-40 minutes at a linear speed of 8-15 m / s using zirconium beads with a particle size of 0.3-0.5 mm. Repeat the process 2-4 times to obtain a carbon nanotube pre-dispersion liquid. (4) Add the fluorinated modified graphene powder and the remaining 1 / 2 ionic liquid dispersant to the remaining 1 / 2 N-methylpyrrolidone, stir and wet at 300~500 rpm for 10~20 min, and then place it in a high shear disperser and disperse at 1500~3000 rpm for 30~60 min to obtain graphene pre-dispersion. (5) Add the graphene pre-dispersion to the carbon nanotube pre-dispersion at a rate of 15-30 ml / min, and stir continuously at a speed of 500-1000 rpm for 30-60 min. At the same time, add ultrafine carbon black and rheology modifier, and then place it in a high-pressure micro-jet homogenizer for homogenization and dispersion at a pressure of 10000-20000 psi. Repeat the cycle 3-8 times, and stir and degas in a vacuum degassing tank at a pressure of -0.08--0.06 MPa for 30-60 min to obtain graphene carbon nanotube composite conductive paste for high-voltage electrodes.

[0013] In summary, this application includes at least the following beneficial effects: (1) This invention prepares a conductive paste for high-voltage electrodes by modifying carbon nanotubes and graphene in the conductive phase. Carboxylation of carbon nanotubes can effectively improve dispersion stability and interfacial compatibility. Carboxylation significantly improves the dispersibility of carbon nanotubes in polar solvents, reduces electric field concentration points formed by agglomerates, and at the same time, carboxyl groups can form hydrogen bonds with electrode current collectors and ionic liquid dispersants, producing weak chemical interactions, improving the adhesion between the conductive agent and the electrode, and reducing the risk of interfacial delamination. Furthermore, well-dispersed carbon nanotubes form a more uniform, low-resistance conductive network, reducing local Joule heating when current passes through and avoiding thermal runaway-induced breakdown. The uniformly dispersed carbon nanotube network acts as a highly efficient conductive pathway, while avoiding local field distortion caused by agglomeration.

[0014] Fluorination modification of graphene can effectively construct dielectric barriers and suppress discharge. Perfluoroalkyl chains are strongly hydrophobic groups with extremely low dielectric constants and extremely high bond energies. Fluorinated graphene sheets act as high-dielectric-strength barriers in conductive networks, physically blocking adjacent conductors and lengthening the discharge path. The insulating properties of fluorinated graphene make it difficult for charge to accumulate on its surface, helping to smooth the electric field distribution and avoid excessively high local field strength, thus homogenizing the electric field distribution. The ultra-low surface energy of the perfluoroalkyl chains makes the graphene surface highly hydrophobic and oleophobic, significantly reducing surface charge adsorption and migration, suppressing surface discharge. The CF bonds impart excellent thermal stability, making it less prone to decomposition and gas generation under high-voltage arcs or local overheating. Therefore, fluorinated graphene constructs distributed insulating barriers in conductive networks, physically blocking the development path of electrical trees, and suppressing charge accumulation and discharge through surface properties, significantly improving the intrinsic dielectric strength of the conductive agent.

[0015] (2) This invention uses ionic liquid as a dispersant to prepare a conductive slurry for high-voltage electrodes. Ionic liquid has no vapor pressure and will not volatilize and generate air gaps under a high-voltage electric field. The strong Coulomb forces between the cations and anions in the ionic liquid result in extremely low migration rates under a strong electric field, avoiding concentration polarization, interface degradation, and increased leakage current caused by ion migration. At the same time, ionic liquid can effectively wet carbon materials and electrode substrates, forming a stable interface layer and reducing contact resistance and interface defects. Ionic liquid can form a passivation film on the surface of metal current collectors, inhibiting electrolyte corrosion. Ionic liquid is the key to high-voltage compatible dispersion media. Its ultra-low volatility and high stability prevent air gap formation, its low ion migration characteristics ensure long-term dielectric integrity under high voltage, and interface optimization reduces the risk of delamination. Detailed Implementation

[0016] It should be noted that, where there is no conflict, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.

[0017] It should be noted that, unless otherwise specified, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.

[0018] This invention provides a method for preparing a graphene-carbon nanotube composite conductive paste for high-voltage electrodes, comprising the following steps: (1) Mix single-walled carbon nanotube powder with a diameter of 1~3 nm, ammonium persulfate and deionized water at a mass ratio of 1:5~10:100, stir and react in a water bath at 70~80℃ for 6~12h, collect the lower solid by centrifugation, wash with hydrochloric acid with a mass fraction of 10%~20% 5~7 times, wash with deionized water 3~5 times, and vacuum dry at a temperature of 50~60℃ and a pressure of -0.08MPa~-0.06MPa for 10~12h to obtain carboxylated single-walled carbon nanotube powder.

[0019] (2) Weigh 2-4 parts of graphene powder with a diameter of 0.6-1.2 μm and 2-5 layers, 0.6-0.8 parts of ethylenediamine, 0.4-0.6 parts of perfluorooctyl sulfonyl fluoride, 0.1-0.3 parts of triethylamine, and 80-100 parts of N,N-dimethylformamide by weight.

[0020] (3) Graphene powder is dispersed in N,N-dimethylformamide, ethylenediamine is added, and the mixture is reacted at 60~70℃ for 1~2h to obtain a mixed dispersion.

[0021] (4) Add perfluorooctyl sulfonyl fluoride and ethylamine to the mixed dispersion, purge with nitrogen gas, react at 50-60℃ for 6-12 hours, centrifuge, take the lower solid layer, clean it with anhydrous ethanol 3-5 times, dry it, and obtain fluorinated modified graphene powder.

[0022] (5) Weigh 2-6 parts by weight of carboxylated single-walled carbon nanotube powder, 1-3 parts of fluorinated modified graphene powder, 0.6-1.2 parts of ultrafine carbon black with a particle size of 20-30 nm, 2-4 parts of ionic liquid dispersant, 0.2-0.4 parts of rheology modifier, and 80-100 parts of N-methylpyrrolidone; (6) Add carboxylated single-walled carbon nanotube powder and 1 / 2 ionic liquid dispersant to 1 / 2 N-methylpyrrolidone, stir and wet at 300~500 rpm for 10~20 min, and then place it in a high shear disperser and disperse at 2000~4000 rpm for 30~60 min to obtain a preliminarily dispersed carbon nanotube slurry. (7) Place the pre-dispersed carbon nanotube slurry in a sand mill and grind and disperse it for 30-40 minutes at a linear speed of 8-15 m / s using zirconium beads with a particle size of 0.3-0.5 mm. Repeat the process 2-4 times to obtain a carbon nanotube pre-dispersion liquid. (8) Add the fluorinated modified graphene powder and the remaining 1 / 2 ionic liquid dispersant to the remaining 1 / 2 N-methylpyrrolidone, stir and wet at 300~500 rpm for 10~20 min, and then place it in a high shear disperser and disperse at 1500~3000 rpm for 30~60 min to obtain graphene pre-dispersion. (9) Add the graphene pre-dispersion to the C carbon nanotube pre-dispersion at a rate of 15-30 ml / min and stir continuously at 500-1000 rpm for 30-60 min. At the same time, add ultrafine carbon black and rheology modifier, and then place it in a high-pressure micro-jet homogenizer at a pressure of 10000-20000 psi for homogenization and dispersion. Repeat the cycle 3-8 times, and stir and degas in a vacuum degassing tank at a pressure of -0.08--0.06 MPa for 30-60 min to obtain graphene carbon nanotube composite conductive paste for high-voltage electrodes.

[0023] The ionic liquid dispersant includes at least one of 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, 1-ethyl-3-methylimidazolium tetrafluoroborate, and trihexyltetradecylphosphonium bis(trifluoromethanesulfonyl)imide salt; the rheology modifier includes at least one of hydroxypropyl methylcellulose, ethylcellulose, polyethylene oxide, and polyethylene glycol.

[0024] The technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0025] Example 1 The preparation method of the graphene-carbon nanotube composite conductive paste for high-voltage electrodes in this embodiment includes the following steps: (1) Mix single-walled carbon nanotube powder with a diameter of 1 nm, ammonium persulfate and deionized water in a mass ratio of 1:5:100, stir and react for 6 h in a water bath at 70 °C, collect the lower solid by centrifugation, wash 5 times with 10% hydrochloric acid, wash 3 times with deionized water, and vacuum dry for 10 h at 50 °C and -0.08 MPa pressure to obtain carboxylated single-walled carbon nanotube powder.

[0026] (2) Weigh out 2 parts of graphene powder with a diameter of 0.6 μm and 2 layers, 0.6 parts of ethylenediamine, 0.4 parts of perfluorooctyl sulfonyl fluoride, 0.1 parts of triethylamine, and 80 parts of N,N-dimethylformamide by weight.

[0027] (3) Graphene powder was dispersed in N,N-dimethylformamide, ethylenediamine was added, and the mixture was reacted at 60°C for 1 h to obtain a mixed dispersion.

[0028] (4) Add perfluorooctyl sulfonyl fluoride and ethylamine to the mixed dispersion, purge with nitrogen gas for protection, react at 50°C for 6 hours, centrifuge, take the lower solid layer, clean it with anhydrous ethanol 3-5 times, dry it, and obtain fluorinated modified graphene powder.

[0029] (5) Weigh out 2 parts by weight of carboxylated single-walled carbon nanotube powder, 1-3 parts of fluorinated modified graphene powder, 0.6 parts of ultrafine carbon black with a particle size of 20 nm, 2 parts of 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, 0.2 parts of hydroxypropyl methylcellulose, and 80 parts of N-methylpyrrolidone; (6) Add carboxylated single-walled carbon nanotube powder and 1 / 2 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt to 1 / 2 N-methylpyrrolidone, stir and wet at 300 rpm for 10 min, and then place it in a high-shear disperser and disperse at 2000 rpm for 30 min to obtain a preliminarily dispersed carbon nanotube slurry. (7) Place the pre-dispersed carbon nanotube slurry in a sand mill and grind and disperse it for 30 minutes at a linear speed of 8 m / s using zirconium beads with a particle size of 0.3 mm. Repeat the process twice to obtain a carbon nanotube pre-dispersion liquid. (8) Add the fluorinated modified graphene powder and the remaining 1 / 2 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt to the remaining 1 / 2 N-methylpyrrolidone, stir and wet at 300 rpm for 10 min, and then place it in a high shear disperser and disperse at 1500 rpm for 30 min to obtain a graphene pre-dispersion. (9) Add the graphene pre-dispersion to the C carbon nanotube pre-dispersion at a rate of 15 ml / min and stir continuously at 500 rpm for 30 min. At the same time, add ultrafine carbon black and hydroxypropyl methylcellulose. Then place it in a high-pressure micro-jet homogenizer and homogenize it at a pressure of 10000 psi. Repeat the cycle 3 times. Stir and degas in a vacuum degassing tank at a pressure of -0.08 MPa for 30~60 min to obtain graphene carbon nanotube composite conductive paste for high-voltage electrodes.

[0030] Example 2 This embodiment describes a method for preparing a graphene-carbon nanotube composite conductive paste for high-voltage electrodes, comprising the following steps: (1) Mix single-walled carbon nanotube powder with a diameter of 2 nm, ammonium persulfate and deionized water in a mass ratio of 1:7:100, stir and react for 9 h in a water bath at 75 °C, collect the lower solid by centrifugation, wash 6 times with 15% hydrochloric acid, wash 4 times with deionized water, and vacuum dry for 11 h at 55 °C and -0.076 MPa pressure to obtain carboxylated single-walled carbon nanotube powder.

[0031] (2) Weigh out 3 parts of graphene powder with a diameter of 0.9 μm and 3 layers, 0.7 parts of ethylenediamine, 0.5 parts of perfluorooctyl sulfonyl fluoride, 0.2 parts of triethylamine, and 90 parts of N,N-dimethylformamide by weight.

[0032] (3) Graphene powder was dispersed in N,N-dimethylformamide, ethylenediamine was added, and the mixture was reacted at 65°C for 1.5 h to obtain a mixed dispersion.

[0033] (4) Add perfluorooctyl sulfonyl fluoride and ethylamine to the mixed dispersion, purge with nitrogen gas for protection, react at 55°C for 9 h, centrifuge, take the lower solid layer, clean it 4 times with anhydrous ethanol, dry it, and obtain fluorinated modified graphene powder.

[0034] (5) Weigh out 4 parts by weight of carboxylated single-walled carbon nanotube powder, 2 parts of fluorinated modified graphene powder, 0.9 parts of ultrafine carbon black with a particle size of 25 nm, 3 parts of 1-ethyl-3-methylimidazolium tetrafluoroborate, 0.3 parts of ethyl cellulose, and 90 parts of N-methylpyrrolidone. (6) Add carboxylated single-walled carbon nanotube powder and 1 / 2 1-ethyl-3-methylimidazolium tetrafluoroborate to 1 / 2 N-methylpyrrolidone, stir and wet at 400 rpm for 15 min, and then place in a high shear disperser and disperse at 3000 rpm for 45 min to obtain a preliminarily dispersed carbon nanotube slurry. (7) Place the pre-dispersed carbon nanotube slurry in a sand mill and grind and disperse it for 35 minutes at a linear speed of 12 m / s using zirconium beads with a particle size of 0.4 mm. Repeat the process 3 times to obtain a carbon nanotube pre-dispersion liquid. (8) Add the fluorinated modified graphene powder and the remaining 1 / 2 1-ethyl-3-methylimidazolium tetrafluoroborate to the remaining 1 / 2 N-methylpyrrolidone, stir and wet at 400 rpm for 15 min, and then place it in a high shear disperser and disperse at 1800 rpm for 45 min to obtain a graphene pre-dispersion. (9) Add the graphene pre-dispersion to the C carbon nanotube pre-dispersion at a rate of 24 ml / min and stir continuously at 700 rpm for 45 min. At the same time, add ultrafine carbon black and ethyl cellulose, and then place it in a high-pressure micro-jet homogenizer for homogenization and dispersion at a pressure of 15000 psi. Repeat the cycle 5 times, and stir and degas in a vacuum degassing tank at a pressure of -0.07 MPa for 45 min to obtain graphene carbon nanotube composite conductive paste for high-voltage electrodes.

[0035] Example 3 This embodiment describes a method for preparing a graphene-carbon nanotube composite conductive paste for high-voltage electrodes, comprising the following steps: (1) Mix single-walled carbon nanotube powder with a diameter of 3 nm, ammonium persulfate and deionized water in a mass ratio of 1:10:100, stir and react for 12 h in a water bath at 80 °C, collect the lower solid by centrifugation, wash 7 times with 20% hydrochloric acid, wash 5 times with deionized water, and vacuum dry for 12 h at 60 °C and -0.06 MPa pressure to obtain carboxylated single-walled carbon nanotube powder.

[0036] (2) Weigh out 4 parts of graphene powder with a diameter of 1.2 μm and 5 layers, 0.8 parts of ethylenediamine, 0.6 parts of perfluorooctyl sulfonyl fluoride, 0.3 parts of triethylamine, and 100 parts of N,N-dimethylformamide by weight.

[0037] (3) Graphene powder was dispersed in N,N-dimethylformamide, ethylenediamine was added, and the mixture was reacted at 70°C for 2 hours to obtain a mixed dispersion.

[0038] (4) Add perfluorooctyl sulfonyl fluoride and ethylamine to the mixed dispersion, purge with nitrogen gas for protection, react at 60°C for 12 h, centrifuge, take the lower solid layer, clean it 5 times with anhydrous ethanol, dry it, and obtain fluorinated modified graphene powder.

[0039] (5) Weigh out 6 parts by weight of carboxylated single-walled carbon nanotube powder, 3 parts of fluorinated modified graphene powder, 1.2 parts of ultrafine carbon black with a particle size of 30 nm, 4 parts of trihexyltetradecylphosphonium bis(trifluoromethanesulfonyl)imide salt, 0.4 parts of polyethylene oxide, and 100 parts of N-methylpyrrolidone. (6) Add carboxylated single-walled carbon nanotube powder and 1 / 2 trihexyltetradecylphosphonium bis(trifluoromethanesulfonyl)imide salt to 1 / 2 N-methylpyrrolidone, stir and wet at 500 rpm for 20 min, and then place it in a high-shear disperser and disperse at 4000 rpm for 60 min to obtain a pre-dispersed carbon nanotube slurry. (7) Place the pre-dispersed carbon nanotube slurry in a sand mill and grind and disperse it for 40 minutes at a linear speed of 15 m / s using zirconium beads with a particle size of 0.5 mm. Repeat the process 4 times to obtain a carbon nanotube pre-dispersion liquid. (8) Add the fluorinated modified graphene powder and the remaining 1 / 2 trihexyltetradecylphosphonium bis(trifluoromethanesulfonyl)imide salt to the remaining 1 / 2 N-methylpyrrolidone, stir and wet at 500 rpm for 20 min, and then place it in a high shear disperser and disperse at 3000 rpm for 60 min to obtain a graphene pre-dispersion. (9) Add the graphene pre-dispersion to the C carbon nanotube pre-dispersion at a rate of 30 ml / min and stir continuously at 1000 rpm for 60 min. At the same time, add ultrafine carbon black and polyethylene oxide. Then place it in a high-pressure micro-jet homogenizer and homogenize it at a pressure of 20000 psi. Repeat the cycle 8 times. Stir and degas in a vacuum degassing tank at a pressure of -0.06 MPa for 60 min to obtain graphene carbon nanotube composite conductive paste for high-voltage electrodes.

[0040] Comparative Example 1 The preparation method of the graphene-carbon nanotube composite conductive paste for the high voltage electrode in this comparative example is basically the same as that in Example 1, except that the graphene in this comparative example is not modified.

[0041] Comparative Example 2 The preparation method of the graphene-carbon nanotube composite conductive paste for the high voltage electrode in this comparative example is basically the same as that in Example 1, except that the ionic liquid dispersant in this comparative example is replaced with polyvinylpyrrolidone dispersant.

[0042] Experimental Example Conductive slurry samples from Examples 1-3 and Comparative Examples 1-2 were selected for various performance tests, including: dielectric strength testing (standard: IEC 60243-1 (Test Method for Electrical Strength of Solid Insulating Materials)); partial discharge initiation voltage testing (standard: IEC 60270 (Partial Discharge Measurement of High Voltage Equipment)); high-voltage accelerated aging testing (standard: IEC 61251 (Guideline for Evaluation of Electrical Aging Resistance of Insulating Materials)); and volume resistivity and surface resistivity determination (standard: ASTM D257 (Test of DC Resistance of Insulating Materials)). Specific results are shown in Table 1.

[0043] Table 1: Performance Test Results of Conductive Paste Samples from Examples and Comparative Examples

[0044] As shown in Table 1, the breakdown field strength of Comparative Example 1 is significantly lower than that of Example 1, proving that the insulating barrier effect of fluorinated graphene significantly lengthens the discharge path. Comparative Example 2 has the lowest breakdown strength due to the residual gas gaps from polyvinylpyrrolidone volatilization and weak interfacial bonding. The partial discharge initiation voltage of Example 1 is much higher than that of Comparative Example 1. This is because the superhydrophobic surface of fluorinated graphene inhibits charge accumulation, and the ionic liquid eliminates gas gaps, avoiding electric field distortion. In contrast, in Comparative Example 2, due to the volatilization of polyvinylpyrrolidone and the presence of numerous gas gaps, discharge occurs even at low field strengths. Furthermore, in Example 1, fluorinated graphene blocks electrical dendrite formation, the ionic liquid resists migration, and the thermal stability maintains structural integrity, thus resulting in a lifetime greater than 500 hours. Example 1 maintains high conductivity, proving that the fluorination modification of graphene does not sacrifice the conductive network, while the polyvinylpyrrolidone insulating coating in Comparative Example 2 increases the resistance. Example 1 is a conductive slurry sample prepared using the method of this invention. By combining fluorinated graphene insulation with an ionic liquid stabilizing medium through a synergistic design, the withstand voltage and lifespan are effectively improved while maintaining high conductivity.

[0045] Therefore, the preparation method of graphene-carbon nanotube composite conductive paste for high voltage electrodes provided by the present invention can significantly improve the breakdown field strength, suppress partial discharge, extend the high voltage life while maintaining high conductivity, and has good performance and broad application prospects.

[0046] Based on the above-described preferred embodiments of the present invention, and through the foregoing description, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.

Claims

1. A graphene-carbon nanotube composite conductive paste for high-voltage electrodes, characterized in that, The raw materials, by weight, include: 2-6 parts carboxylated single-walled carbon nanotube powder, 1-3 parts fluorinated modified graphene powder, 0.6-1.2 parts ultrafine carbon black, 2-4 parts ionic liquid dispersant, 0.2-0.4 parts rheology modifier, and 80-100 parts N-methylpyrrolidone.

2. The graphene-carbon nanotube composite conductive paste for high-voltage electrodes according to claim 1, characterized in that, The method for preparing the carboxylated single-walled carbon nanotube powder includes the following steps: Single-walled carbon nanotube powder, ammonium persulfate, and deionized water were mixed at a mass ratio of 1:5 to 10:100 and stirred in a water bath at 70 to 80°C for 6 to 12 hours. The lower solid layer was collected by centrifugation and washed 5 to 7 times with 10% to 20% hydrochloric acid, followed by 3 to 5 times with deionized water. The mixture was then vacuum dried at 50 to 60°C and -0.08 MPa to -0.06 MPa for 10 to 12 hours to obtain carboxylated single-walled carbon nanotube powder.

3. The graphene-carbon nanotube composite conductive paste for high-voltage electrodes according to claim 2, characterized in that, The diameter of the single-walled carbon nanotube powder is 1~3nm.

4. The graphene-carbon nanotube composite conductive paste for high-voltage electrodes according to claim 1, characterized in that, The preparation method of the fluorinated modified graphene powder includes the following steps: S1. Weigh 2-4 parts graphene powder, 0.6-0.8 parts ethylenediamine, 0.4-0.6 parts perfluorooctyl sulfonyl fluoride, 0.1-0.3 parts triethylamine, and 80-100 parts N,N-dimethylformamide by weight. S2. Graphene powder is dispersed in N,N-dimethylformamide, ethylenediamine is added, and the mixture is reacted at 60~70℃ for 1~2 hours to obtain a mixed dispersion. S3. Add perfluorooctyl sulfonyl fluoride and ethylamine to the mixed dispersion, purge with nitrogen, and react at 50-60℃ for 6-12 hours. Centrifuge, remove the lower solid layer, clean it with anhydrous ethanol 3-5 times, and dry it to obtain fluorinated modified graphene powder.

5. The graphene-carbon nanotube composite conductive paste for high-voltage electrodes according to claim 4, characterized in that, The graphene powder has a sheet diameter of 0.6~1.2μm and 2~5 layers.

6. The graphene-carbon nanotube composite conductive paste for high-voltage electrodes according to claim 1, characterized in that, The particle size of the ultrafine carbon black is 20~30nm.

7. The graphene-carbon nanotube composite conductive paste for high-voltage electrodes according to claim 1, characterized in that, The ionic liquid dispersant includes at least one of 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, 1-ethyl-3-methylimidazolium tetrafluoroborate, and trihexyltetradecylphosphonium bis(trifluoromethanesulfonyl)imide salt.

8. The graphene-carbon nanotube composite conductive paste for high-voltage electrodes according to claim 1, characterized in that, The rheology modifier includes at least one of hydroxypropyl methylcellulose, ethylcellulose, polyethylene oxide, and polyethylene glycol.

9. A method for preparing a graphene-carbon nanotube composite conductive paste for high-voltage electrodes as described in any one of claims 1 to 8, characterized in that, Includes the following steps: (1) Weigh each component according to its weight percentage; (2) Add carboxylated single-walled carbon nanotube powder and 1 / 2 ionic liquid dispersant to 1 / 2 N-methylpyrrolidone, stir and wet at 300~500 rpm for 10~20 min, and then place it in a high shear disperser and disperse at 2000~4000 rpm for 30~60 min to obtain a pre-dispersed carbon nanotube slurry. (3) Place the pre-dispersed carbon nanotube slurry in a sand mill and grind and disperse it for 30-40 minutes at a linear speed of 8-15 m / s using zirconium beads with a particle size of 0.3-0.5 mm. Repeat the process 2-4 times to obtain a carbon nanotube pre-dispersion liquid. (4) Add the fluorinated modified graphene powder and the remaining 1 / 2 ionic liquid dispersant to the remaining 1 / 2 N-methylpyrrolidone, stir and wet at 300~500 rpm for 10~20 min, and then place it in a high shear disperser and disperse at 1500~3000 rpm for 30~60 min to obtain graphene pre-dispersion. (5) Add the graphene pre-dispersion to the carbon nanotube pre-dispersion at a rate of 15-30 ml / min, and stir continuously at a speed of 500-1000 rpm for 30-60 min. At the same time, add ultrafine carbon black and rheology modifier, and then place it in a high-pressure micro-jet homogenizer for homogenization and dispersion at a pressure of 10000-20000 psi. Repeat the cycle 3-8 times, and stir and degas in a vacuum degassing tank at a pressure of -0.08--0.06 MPa for 30-60 min to obtain graphene carbon nanotube composite conductive paste for high-voltage electrodes.

Citation Information

Cited By

  • High-voltage-resistant carbon nanomaterial composite conductive paste and preparation method thereof

    CN121709621A