Method for manufacturing resourceful product of waste plastic

By calculating the carbonization time in a coking oven using the relationship between maximum charging height and carbonization time, the problem of insufficient carbonization conditions for waste plastics in coking ovens was solved, thus realizing the efficient recycling of waste plastics and the generation of high-quality products.

CN120882837APending Publication Date: 2025-10-31NIPPON STEEL CORPORATION
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202480019989.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-20
Filing Date
2024-03-07
Publication Date
2025-10-31

AI Technical Summary

Technical Problem

Existing technologies have failed to effectively address the pyrolysis conditions when only waste plastics are pyrolyzed in coking ovens, resulting in low efficiency in the recycling of waste plastics.

Method used

Waste plastics are loaded into the coking oven at a maximum loading height exceeding half the oven width. The carbonization time is calculated using a predetermined formula relating the maximum loading height to the carbonization time. Carbonized products, tar, and gas are generated, and the carbonized products are discharged using an extruder.

Benefits of technology

It achieves efficient recycling of waste plastics, generating high-quality pyrolytes, tar, and gases, effectively utilizing coke ovens that are not loaded with coal, and realizing the recycling of large quantities of waste plastics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120882837A_ABST
    Figure CN120882837A_ABST
Patent Text Reader

Abstract

Provided is a method for producing a recycled product of waste plastic, which makes it possible to recycle a large amount of waste plastic. The manufacturing method comprises the following steps: charging waste plastics into a coke oven at a predetermined maximum charging height which is a height exceeding half of the oven width of the coke oven, and performing dry distillation for a predetermined dry distillation time to generate a dry distillation product, tar, light oil and gas; and taking out the dry retort from the coke oven by means of the extruder; the value of the predetermined dry distillation time is obtained by determining a relational expression between the maximum loading height of the waste plastic and the dry distillation time required for the completion of the dry distillation, and substituting the predetermined maximum loading height into the relational expression to calculate the predetermined dry distillation time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing recycled products from waste plastics using a coking oven. Background Technology

[0002] In recent years, from the perspective of efficient resource utilization and contributing to carbon neutrality, there has been a demand for the recycling of waste plastics. Among these methods, the dry distillation of waste plastics in a coking oven to obtain recycled products such as distillates, tar, light oil, and gases has advantages such as the ability to process large quantities of waste plastics and the effective utilization of existing coking ovens. However, insights into suitable dry distillation conditions for the recycling of waste plastics are still insufficient. Therefore, it is desirable to develop a method for predicting suitable dry distillation conditions for the recycling of waste plastics.

[0003] Patent Document 1 describes a method for manufacturing coke for blast furnaces, which involves first loading coke raw materials into the carbonization chamber of a coking furnace, and then loading waste plastics into the space at the top of the furnace. The method is characterized by pre-determining the relationship between the type and quantity of waste plastics and the thermal decomposition time of the waste plastics, and setting the type, quantity, loading time, and placement time of the waste plastics to be loaded, so that the thermal decomposition of the loaded waste plastics is completed before the coke is extruded.

[0004] Patent document 2 describes a method for producing fuel gas by combining plastics with raw coal or by dry distillation of a single component.

[0005] Existing technical documents Patent documents Patent Document 1: Japanese Patent Application Publication No. 2002-047494 Patent Document 2: Japanese Patent Application Publication No. 48-032902 Summary of the Invention

[0006] The problem that the invention aims to solve Patent Document 1 provides a method for pre-loading coke feedstock into the carbonization chamber of a coke oven before loading waste plastics, but it does not address the pyrolysis conditions when only waste plastics are pyrolyzed. As described in Patent Document 1, using coke feedstock may not be advantageous for large-scale processing of waste plastics. On the other hand, Patent Document 2 provides a method for pyrolyzing plastics as a single component. However, Patent Document 2 does not teach specific pyrolysis conditions when only plastics are pyrolyzed. In other words, a method for confirming the discharge of the pyrolyzed product from the coke oven after pyrolysis is completed when pyrolyzing a substance consisting essentially only of waste plastics in a coke oven kiln (hereinafter sometimes simply referred to as a coke oven for convenience) has not been established in the prior art.

[0007] One objective of this invention is to solve the aforementioned problems by providing a method for manufacturing recycled waste plastic products, which enables the recycling of large quantities of waste plastics by dry distilling a processed material consisting essentially only of waste plastics in a coking oven.

[0008] Methods for solving problems The gist of this invention is as follows.

[0009] [1] A method for manufacturing a recycled product from waste plastics, characterized in that: It is a method for manufacturing recycled products from waste plastics from coke ovens that have not been charged with coal, the method comprising: The waste plastic is loaded into the coking furnace at a height exceeding half the furnace width, i.e., a predetermined maximum loading height. It is then subjected to carbonization for a predetermined time derived from the predetermined maximum loading height, thereby generating carbonized distillate, tar, light oil, and gas as recycling products of the waste plastic; and The pyrolyte is discharged from the coking oven using an extruder; The predetermined distillation time is obtained through the following steps: Calculate in advance the relationship between the maximum loading height of waste plastics into the coking oven and the required carbonization time to complete the carbonization process, and Substitute the predetermined maximum loading height into the formula to calculate the predetermined distillation time.

[0010] [2] The method for manufacturing recycled products of waste plastics as described in [1] above is characterized in that: The dry distillation is carried out at a predetermined furnace temperature. The aforementioned formula represents the relationship between the maximum charging height, furnace temperature, and the time required to complete the dry distillation. Substitute the predetermined maximum loading height and the predetermined furnace temperature into the formula to calculate the predetermined dry distillation time.

[0011] Invention Effects According to one aspect of the present invention, a method for manufacturing recycled waste plastic products can be provided, which enables the recycling of large quantities of waste plastics by dry distilling a processed material consisting essentially only of waste plastics in a coking oven. Attached Figure Description

[0012] Figure 1 This is a schematic diagram illustrating a general example of the structure of a coking oven.

[0013] Figure 2 This is a schematic diagram illustrating a general example of the structure of a coking oven.

[0014] Figure 3This is a diagram showing the distillate produced when waste plastics are distilled in an experimental distillation furnace.

[0015] Figure 4 This is a graph showing the relationship between the maximum loading height of waste plastics in Example 1 and the measured required dry distillation time.

[0016] Figure 5 This is a graph showing the relationship between the estimated and measured values ​​of the required dry distillation time for waste plastics in Example 1.

[0017] Figure 6 This is a graph showing the relationship between the total amount of waste plastics loaded in Comparative Example 1 and the measured required dry distillation time.

[0018] Figure 7 This is a graph showing the relationship between the estimated and measured values ​​of the required dry distillation time for the waste plastics in Comparative Example 1.

[0019] Figure 8 This is a graph showing the relationship between the estimated and measured values ​​of the required dry distillation time for waste plastics in Example 2. Detailed Implementation

[0020] The present invention will now be described in an exemplary manner (sometimes referred to as the present embodiment in this disclosure), but the present invention is not limited to the following manner.

[0021] One aspect of the present invention provides a method for manufacturing recycled products of waste plastics using a coke oven without coal (i.e., a kiln without coal). Furthermore, "without coal" means that coal is not intentionally added. Therefore, a kiln where coal exists in the form of residues (e.g., deposits on the furnace walls) is also included in a kiln without coal. More specifically, "without coal" means that coal is not intentionally added throughout the entire process of manufacturing the recycled product. The method includes: loading waste plastics into the coke oven at a height exceeding half the width of the coke oven, i.e., a predetermined maximum loading height; performing carbonization for a predetermined carbonization time derived from the predetermined maximum loading height, thereby generating carbonized products, tar, light oil, and gas as recycled products of waste plastics; and removing the carbonized products from the coke oven using an extruder. The predetermined distillation time is obtained by the following steps: when loading waste plastic selected for testing into the coking oven selected for testing, the relationship between the maximum loading height and the distillation time required to complete the distillation is determined; and the predetermined distillation time is calculated by substituting the predetermined maximum loading height into the above relationship.

[0022] Figure 1 as well as Figure 2 This is a schematic diagram illustrating a simplified structure of a coking oven. (See reference...) Figure 1 as well as Figure 2A coking oven 100 typically has a configuration in which carbonization chambers 30 and combustion chambers 40 are alternately arranged above the regenerator 10, separated by a furnace wall 20. That is, each carbonization chamber is a kiln. The carbonization chamber 30 has a furnace width W, a furnace height H, and a furnace length L. Specifically, referring to... Figure 2 Waste plastic P is fed from hopper 50 into carbonization chamber 30 through loading holes a, b, c, d, and e. Multiple loading holes may exist in each carbonization chamber. Figure 2 The example shown has 5 loading holes per carbonization chamber, but the number of loading holes is not limited to this.

[0023] Specifically, refer to Figure 2 The loading height of the waste plastic is calculated from the bottom surface B of the carbonization chamber 30 to the upper surface h1 of the loaded waste plastic P, and is taken at each position along the furnace length L. Furthermore, the maximum loading height mh refers to the largest loading height calculated at each position along the furnace length. Typically, the loading height is as follows: Figure 2 As shown in the insertion heights ha, hb, hc, hd, and he, the heights rise directly below the insertion holes a, b, c, d, and e. Figure 2 The example shown illustrates a loading height hd where the maximum loading height mh is the maximum loading height. (See reference...) Figure 1 as well as Figure 2 Waste plastic P is carbonized in carbonization chamber 30 via heat transfer from combustion chamber 40, producing distillate, tar, light oil, and gas as recycled products. Specifically, refer to... Figure 2 The pyrolyte is extruded by the extruder 60 in the direction of furnace length L. Tar, light oil and gas flow out of the furnace from the carbonization chamber 30 through the riser pipe (not shown) and separate from each other.

[0024] When coal is charged into a coking oven for dry distillation, the dominance factor for the dry distillation time required to complete the dry distillation (required dry distillation time) is the coal charging height (e.g., Figure 2 The height (from bottom surface B to the upper surface h1 of waste plastic P) is greater than the width of the coking furnace (e.g., Figure 1When the furnace height is half the width (W) of the coking oven, heat transfer is typically along the furnace width direction. Furthermore, the required carbonization time (required carbonization time) refers to the time required from the start of carbonization until the carbonized material can be extruded. Additionally, the case where the coal charging height is greater than half the furnace width of the coking oven refers to a situation where the coal charging height is greater than the value obtained by dividing the furnace width at the maximum charging height (mh) of the coking oven by 2. However, the inventors have discovered that the heat conduction behavior when carbonizing waste plastics using a coking oven differs from that of coal. Specifically, in the carbonization of waste plastics, even when the charging height is greater than half the furnace width of the coking oven, the dominant factor for the required carbonization time is not heat transfer along the furnace width direction as in the carbonization of coal, but rather along the charging height direction. The inventors have further discovered that even when the total charging mass of waste plastics differs, the required carbonization time is the same if the maximum charging height is the same. The reason why heat transfer in the furnace width direction does not become a rate-controlling step in the carbonization of waste plastics is not yet clear, but it can be speculated that this is because the waste plastics near the furnace wall, which heats up rapidly immediately after being loaded, form extremely porous and low-heat-conductivity plate-like carbonized material, hindering heat transfer in the furnace width direction. The waste plastics that require the longest time to complete carbonization are those located at the position where the heat transfer distance in the furnace height direction is the greatest; therefore, the maximum loading height can be used as an indicator of the loading height.

[0025] The inventors further discovered that by considering furnace temperature in addition to the maximum charging height, the required distillation time can be estimated with higher accuracy. That is, the main factor affecting the required distillation time is the maximum charging height, and the secondary factor is the furnace temperature.

[0026] According to the method of this embodiment, waste plastics can be prevented from being discharged from the coke oven in a state of incomplete pyrolysis. Therefore, by utilizing the coke oven to pyrolyze the processed material, which is essentially composed only of waste plastics, a large amount of waste plastics can be recycled, and the recycled products, especially the hydrocarbon gases therein, can be recovered to the maximum extent. In addition, according to the method of this embodiment, waste plastics can be recycled effectively by utilizing coke ovens that have not been fed with coal, such as non-operating kilns or empty kilns, thus achieving both efficient utilization of the coke oven and large-scale recycling of waste plastics. Furthermore, "pyrolyzing the processed material, which is essentially composed only of waste plastics, in the coke oven" means that the material used is intentionally only waste plastics. For example, coal may also be present as residues (e.g., deposits on the furnace wall). One approach is to produce recycled waste plastic products without using coal.

[0027] <Waste Plastics> The recycled products manufactured using the method of this embodiment are products generated by recycling waste plastics (making them useful materials that can be used as resources). In the method of this embodiment, the waste plastics used for pyrolysis can be general waste or industrial waste, and their source is not limited. The waste plastics can originate from one or more of the following: bottles (e.g., PET bottles and bottles other than PET), bottle caps, packaging films, packaging materials (e.g., expanded polystyrene packaging materials), household appliances (e.g., appliance frames), logistics materials (e.g., pallets and containers), agricultural plastics, automotive parts, pipes, wire sheathing materials, etc. In one embodiment, the waste plastics can originate from a single type of raw material, such as waste plastics that are substantially derived only from PET bottles, or waste plastics that are substantially derived only from expanded polystyrene packaging materials, etc. The waste plastics can be composed of two or more polymer materials. The waste plastics can originate from two or more raw materials. According to the method of this embodiment, by reliably completing the pyrolysis, high-quality recycled products can be generated even if the properties of the processed material are diverse.

[0028] Waste plastics refer to various types of plastics that can be recycled as general waste or industrial waste. In one approach, waste plastics can meet the classification standards for plastics (such as PET bottles and plastic containers and packaging) that are subject to the revised Container and Packaging Recycling Law (a law that is part of the revised laws on the classification, collection, and promotion of the resale of containers and packaging, enacted in April 2007, Law No. 76 of June 15, 2008). Waste plastics that meet such classification standards have a more uniform material composition, which facilitates the manufacture of high-quality recycled products.

[0029] Waste plastics can include thermoplastic resins and / or thermosetting resins. Examples of thermoplastic resins include polyolefins (e.g., polyethylene and polypropylene), polyesters (e.g., polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate), acrylic resins, polyvinyl alcohol, polyvinyl chloride, polystyrene, polycarbonate, polyamide, polyacetal, and fluoropolymers. Examples of thermosetting resins include phenolic resins, melamine resins, urea-formaldehyde resins, polyurethane, epoxy resins, and unsaturated polyester resins.

[0030] From the perspective of distillation efficiency, in one approach, the moisture content of waste plastics can be less than 30% by mass, or less than 20% by mass, or less than 15% by mass, or less than 10% by mass.

[0031] The shape of the waste plastics fed into the coking oven is not limited; they can be in their original shape as waste for recycling, or they can be shaped after recycling. In one approach, the waste plastics can be fed into the coking oven as pellets. The waste plastics can undergo pretreatment before being fed into the coking oven after recycling. Examples of pretreatment include crushing, foreign matter removal, granulation, and moisture content adjustment based on dryness. Foreign matter removal can be achieved using a magnetic separator for metal removal, or a pneumatic separator for removing heavy objects. Crushing and granulation can be performed using, for example, compression, shearing, cutting, impact, or friction crushers.

[0032] <Dry distillation> In this embodiment, a non-operating kiln, an empty kiln, or other coking oven that is not loaded with coal is used. In other words, the coking oven is essentially only loaded with waste plastics. Therefore, large-scale processing of waste plastics is possible.

[0033] In this embodiment, the recycled products are generated as carbonized residues, tar, light oil, and gas. If waste plastics are thermally decomposed in the carbonization chamber of a coke oven, coke (carbon residue), tar, light oil, gas, and byproducts are generated as carbonized residues. In one approach, almost all of the waste plastics can be recovered as a useful component consisting of coke, hydrocarbon oils (in the form of tar or light oil), and gas (hydrocarbon gases, hydrogen, etc.). The coke can be used, for example, for sintering; the hydrocarbon oils can be used, for example, as raw materials for various chemicals; and the gas is recovered from the top of the coke oven and can be used, for example, as fuel for power generation. In a typical approach, the recycled product may have a composition of approximately 20% by mass of coke, approximately 40% by mass of oil, and approximately 40% by mass of gas.

[0034] In this embodiment, waste plastics are charged into a coke oven that is not loaded with coal, but the oven temperature can also be within the same range as that used for producing coke from coal. The oven temperature, for example, the oven bottom temperature, can be between 900°C and 1200°C in one embodiment. Generally, polymeric materials generally cease thermal decomposition below 500°C. For example, polyethylene (PE), polystyrene (PS), polyethylene terephthalate (PET), and polypropylene (PP), which are the mainstream types of recycled waste plastics, begin thermal decomposition at approximately 300°C and cease at approximately 420°C to 470°C. Furthermore, even polyvinyl chloride (PVC), which is sometimes included in waste plastics and can produce harmful gases when burned, undergoes a first thermal decomposition reaction at approximately 250°C and a second thermal decomposition reaction based on main chain scission at approximately 400°C. High-temperature dry distillation using a coking oven avoids the release of harmful substances into the environment even when the waste plastics contain recalcitrant organic matter that could become an environmental burden, due to the excellent thermal decomposition properties of waste plastics. This allows for the production of clean, recycled products containing various useful components. In particular, the method of this embodiment enables large-scale processing of waste plastics because the distillate is removed after the distillation is reliably completed.

[0035] Coke ovens typically have multiple loading ports. Waste plastics can be loaded into the coke oven through more than one loading port, for example, through two, three, four, or five loading ports. The maximum loading height is the largest of the loading heights from all the loading ports. The maximum loading height can be below the maximum loading height when coal is being loaded into the coke oven.

[0036] For example, in a coking oven with a furnace height of 5.5m, the maximum charging height can be 5.15m.

[0037] In the method of this embodiment, the required distillation time (required distillation time) can be determined using the indicators described below. In one embodiment, the required distillation time can be considered as the time from the start of distillation to the moment when black smoke stops escaping from the riser pipe when the loading port is opened. In another embodiment, the moment when black smoke stops escaping from the riser pipe when the loading port is opened can be determined as the moment when the gas exiting the riser pipe changes from a black level to a non-black level after the loading port is opened. The appearance of the gas exiting the riser pipe when the loading port is opened changes with the degree of distillation. In the stage where distillation is not yet complete, hydrocarbon gases are discharged as the waste plastic is distilled; due to the incomplete combustion of these hydrocarbon gases, the gas exiting the riser pipe is black. On the other hand, in the stage where distillation is complete, the gas exiting the riser pipe mainly consists of hydrogen and water vapor (i.e., the discharge of hydrocarbon gases has essentially ended), exhibiting a white appearance due to water vapor. Therefore, whether the gas exiting the riser pipe is black is a useful indicator for determining whether distillation has ended. The observation interval for the gas can be set according to the purpose, for example, every 6 minutes (i.e., 0.1 hours). From the viewpoint of maximizing the recovery of recycled products, especially hydrocarbon gases therein, it is preferable to perform dry distillation until black smoke stops being discharged from the riser pipe when the loading port is opened.

[0038] In this embodiment, a formula is pre-determined relating the maximum loading height of the waste plastic to the measured value of the required carbonization time (in one approach, the time from the start of carbonization to the moment when black smoke stops exiting from the riser pipe when the loading port is opened) when the waste plastic is carbonized. In the carbonization of waste plastic, either a fully operational coking furnace or a test carbonization furnace can be used. However, test carbonization furnaces tend to remove more heat than fully operational furnaces; therefore, from the viewpoint of more accurately estimating the required carbonization time, a fully operational coking furnace is preferred. The coking furnace used in the experiments deriving the formula and in the actual processing of the waste plastic can be the same or different.

[0039] The experimental waste plastics used for pyrolysis to derive the relationship preferably have the same or similar material composition as the waste plastics used for actual recycling. Examples of waste plastics used for actual recycling and experimental waste plastics having the same or similar material composition include cases where these waste plastics are recycled through the same waste collection method. The experimental waste plastics can also be a portion of the waste plastics extracted from the waste plastics used for actual recycling. When the waste plastics used for actual recycling and experimental waste plastics differ in the density of the granulated waste plastics, it is preferable to reselect the experimental waste plastics to make the density the same. The density can vary depending on the material composition, but it can also vary depending on the granulation method.

[0040] In one approach, for the waste plastic used in the experiment, a pyrolysis test is conducted under multiple pyrolysis conditions with at least varying maximum charge heights, and the required pyrolysis time is determined (in one approach, the time from the start of pyrolysis to the moment when black smoke stops escaping from the riser pipe when the charge port is opened). The aforementioned pyrolysis test can be conducted, for example, under multiple pyrolysis conditions with only varying maximum charge heights, or, for example, under multiple pyrolysis conditions with varying maximum charge heights and furnace temperatures. The furnace temperature can be, for example, the furnace bottom temperature.

[0041] <Derivation of Relational Expressions> Based on the measured values ​​of the required distillation time obtained from the above distillation experiments, a relationship between the maximum loading height and the required distillation time is derived. The method for deriving this relationship is not limited to this; for example, it could be a regression analysis with at least the maximum loading height as the explanatory variable and the required distillation time as the target variable.

[0042] In one approach, based on the measured values ​​of the required distillation time obtained through the above-mentioned distillation experiments under multiple distillation conditions with varying maximum loading heights, a relationship between the maximum loading height and the required distillation time is derived. The method for deriving this relationship is not limited to this; for example, it could be univariate regression analysis. The regression could be linear or nonlinear (e.g., multinomial regression), but in one approach it is linear regression. In univariate regression analysis, the maximum loading height can be used as the explanatory variable, and the required distillation time as the target variable. The regression is not limited to this; for example, it could be linear regression based on the least squares method. In this case, the following equation (1) can be obtained as the relationship.

[0043] (In the formula, a is the regression coefficient derived from the relationship between the maximum loading height of the waste plastics used in the test and the required dry distillation time, and c is the constant term derived from the relationship between the maximum loading height of the waste plastics used in the test and the required dry distillation time).

[0044] In another approach, based on the measured values ​​of the required distillation time obtained from the above-mentioned distillation experiments under multiple distillation conditions with varying maximum charge height and furnace temperature, a relationship between the maximum charge height, furnace temperature, and required distillation time is derived. The method for deriving this relationship is not limited to this; for example, it can be a multivariate analysis such as multiple regression analysis. The regression can be linear or nonlinear, but in one approach it is linear regression. In multiple regression analysis, the maximum charge height and furnace temperature can be used as explanatory variables, and the required distillation time as the target variable. There is no strong correlation between the maximum charge height and furnace temperature, so using them as explanatory variables may be advantageous in conducting statistically significant multiple regression analysis.

[0045] Regression is not limited to this; for example, it can be linear regression based on the least squares method. In this case, the following equation (2) is obtained as the relation.

[0046] (In the formula, a and b are regression coefficients derived from the relationship between the maximum loading height of the waste plastics used in the test and the furnace temperature and the required carbonization time, and c is a constant term derived from the relationship between the maximum loading height of the waste plastics used in the test and the furnace temperature and the required carbonization time.) Furthermore, in multiple regression analysis, standardization can be used to obtain a relationship where the intercept c (i.e., the constant term) is 0, but standardization is not required.

[0047] There are no particular limitations on the verification methods for whether univariate or multivariate regression analysis is effective; it can be tested using common methods. The significance level can be selected as needed, for example, it can be set to 5% or 1%.

[0048] Furthermore, in the above, the use of the maximum charging height or the maximum charging height and furnace temperature as explanatory variables for estimating the required carbonization time was explained. However, if other factors affect the required carbonization time, these other factors can also be used in addition to the maximum charging height and furnace temperature. Examples of these other factors include the material, particle size, and bulk density of the waste plastic. For example, in the above, the case of two explanatory variables was shown for multiple regression analysis, but three or more explanatory variables can also be set. As additional explanatory variables, one or more of the above-mentioned materials, particle size, and bulk density of the waste plastic can be used. As a relationship for multiple regression analysis using a total of four explanatory variables—maximum charging height, furnace temperature, the first additional explanatory variable, and the second additional explanatory variable—the following equation (3) can be listed.

[0049] (In the formula, a, b, α and β are regression coefficients derived from the relationship between the maximum loading height of the waste plastics used in the experiment, the furnace temperature, the first additional explanatory variable and the second additional explanatory variable and the required carbonization time, and c is a constant term derived from the relationship between the maximum loading height of the waste plastics used in the experiment, the furnace temperature, the first additional explanatory variable and the second additional explanatory variable and the required carbonization time).

[0050] <Calculation of the predetermined distillation time in actual recycling> By substituting the values ​​of the conditions used in actual recycling into the relationships derived through the steps illustrated above, an estimated value for the required carbonization time for actual recycling can be calculated. In one approach, the estimated value for the required carbonization time for actual recycling can be calculated by importing the maximum loading height in actual recycling into equation (1) above, or by substituting the values ​​of the maximum loading height and furnace temperature in actual recycling into equation (2) above. In actual recycling, the carbonization of waste plastics can be reliably completed by carbonizing according to a predetermined carbonization time set based on this estimated value. In a typical approach to actual recycling, waste plastics are loaded into the coking oven in a single operation.

[0051] Example The following examples further illustrate the illustrative aspects of the present invention, but the present invention is not limited to these examples in any way.

[0052] <Preparation of Waste Plastics> As waste plastic, it is packaged in containers. The waste plastic is granulated to form cylindrical granules with a diameter of approximately 35 mm and a length of approximately 30–100 mm. The bulk density of this waste plastic is 0.299 t / m³. 3 .

[0053] <Preliminary research> First, in order to study the behavior of waste plastics during pyrolysis, the aforementioned waste plastics were pyrolyzed at 1050℃ in an experimental pyrolysis furnace (furnace height 0.55m, furnace length 0.6m, furnace width 0.45m). Figure 3 This diagram shows the distillate produced when waste plastics are carbonized in a test carbonization furnace. The loading height of the waste plastics was set to 0.4m. The height of the distillate from the bottom of the furnace was approximately 20%–30% of the loading height (i.e., a loss on ignition of approximately 70–80%). The resulting distillate was then observed; the results show that the condition of the sample varied depending on its location. Figure 3 As shown, plate-like porous distillate forms near the furnace wall. Additionally, plate-like distillate also forms on the surface. On the other hand, samples ranging from flakes to powder can be seen in the central part, showing a tendency to become more powdery closer to the furnace bottom. It can be assumed that these differences in sample shape are caused by differences in heating rates. Here, it can be speculated that porous samples containing numerous large pores form particularly near the furnace wall where the heating rate is faster. In the distillation of waste plastics, the plate-like porous material adhering to this furnace wall hinders heat transfer in the width direction of the furnace, thus affecting the distillation rate in the height direction.

[0054] Based on the aforementioned preliminary research results, the relationship between the maximum loading height or total loading amount of waste plastics and the required carbonization time was studied using multiple actual coking ovens (i.e., multiple hearth groups). In the study, actual coking ovens with a height of 5.0–7.1 m (different for each hearth group), a length of 14.6–16.5 m (different for each hearth group), and a width of 0.45–0.46 m (different for each hearth group) were used, equipped with 4–5 loading holes arranged at equal intervals (different for each hearth group).

[0055] [Example 1: Estimation based on maximum loading height] Waste plastics with properties identical to those used in the aforementioned preliminary study were loaded into the actual coking oven for dry distillation according to loading conditions 1 to 11 shown in Table 1. Furthermore, due to rounding, the quantities in the tables may not always correspond to the total quantity at each loading hole; this should be noted. The required dry distillation time was evaluated from the start of dry distillation until the black smoke ceased to be emitted from the riser pipe when the loading hole was opened. Under each loading condition, waste plastics were loaded into one or more of four to five loading holes (loading holes 1 to 4 or 1 to 5) with the loading quantities and loading heights shown in Table 1. Furthermore, the maximum loading height was defined as the loading height at that loading hole when only one loading hole was used, and as the loading height at the loading hole with the highest loading height when two or more loading holes were used.

[0056] The moment when the black smoke stopped escaping from the riser pipe after the loading port was opened was defined as the point at which the loading port was opened. The observation was made at this point when the gas exiting the riser pipe changed from a black level to a non-black level. This observation was conducted every 6 minutes after opening the loading port. The results are shown in Table 1.

[0057] As shown in Table 1, even when the total amount of waste plastic loaded varies greatly, the measured required distillation time is also similar when the maximum loading height is the same (e.g., loading conditions 8 and 10). This result indicates that the measured required distillation time is not determined by the total amount of waste plastic loaded, but by the maximum loading height.

[0058] Figure 4 This is a graph showing the relationship between the maximum loading height of waste plastics in Example 1 and the measured required dry distillation time. Based on Figure 4 The curve shown was subjected to a univariate regression analysis with the maximum loading height as the explanatory variable and the required distillation time as the target variable. A linear regression based on least squares yielded a coefficient of determination of 0.9202, which is sufficiently high. Furthermore, the p-value for the maximum loading height used as the explanatory variable was 3.06 × 10⁻⁶. -6 Since it is sufficiently below 0.05, it can be determined that it can be used as an explanatory variable. The resulting regression equation is as follows.

[0059] Required distillation time (hours) = 6.3459 × maximum loading height (m) - 1.2913 As can be seen from the above, the maximum loading height and the measured required distillation time have a good linear correlation.

[0060] Next, the maximum loading height values ​​for loading conditions 1 to 11 are substituted into the maximum loading height in the above regression equation to calculate the estimated value of the required dry distillation time. The calculated estimated values ​​are shown in Table 1.

[0061] Figure 5 This is a graph showing the relationship between the estimated and measured values ​​of the required dry distillation time for the waste plastics in Example 1. The least squares method was used to... Figure 5 The curve shown is approximated by a straight line, and the result is R. 2 The value is 0.91, showing a good correlation between the measured and estimated values. This indicates that in the dry distillation of waste plastics, the heat transfer is not along the width of the furnace as in the typical coal dry distillation of coke production, but rather along the height of the furnace, which influences the distillation speed. Therefore, the required distillation time can be accurately estimated based on the maximum loading height.

[0062] [Comparative Example 1: Estimation based on total load] Based on the measured required dry distillation time obtained in Example 1, the relationship between the total amount of waste plastics loaded and the measured required dry distillation time was plotted. Figure 6 This is a graph showing the relationship between the total amount of waste plastic loaded in Comparative Example 1 and the measured required dry distillation time. Based on Figure 6 The curve shown was analyzed using a univariate regression analysis with the total loading amount as the explanatory variable and the required distillation time as the target variable. A linear regression based on least squares was performed, yielding a coefficient of determination of 0.8698, significantly lower than that of Example 1. Furthermore, the p-value for the total loading amount used as the explanatory variable was 2.83 × 10⁻⁶. -5 Since the value is sufficiently below 0.05, it can be determined that it can be used as an explanatory variable. The resulting regression equation is as follows.

[0063] Required distillation time (hours) = 5.2203 × total loading (tons) + 4.7726 As mentioned above, the results show that the correlation between total charge and measured required distillation time is greater than the correlation between maximum charge height and measured required distillation time (R0). 2 =0.9202) small.

[0064] Next, substitute the total loading values ​​for each of loading conditions 1 to 11 into the total loading value in the above regression equation to calculate the estimated value of the required distillation time. The calculated estimated values ​​are shown in Table 1.

[0065] Figure 7 This is a graph showing the relationship between the estimated and measured values ​​of the required dry distillation time for the waste plastics in Comparative Example 1. The least squares method was used to... Figure 7 The curve shown is approximated by a straight line, and the result is R. 2 The value is 0.60, which is less accurate compared to using the maximum loading height as a variable. This result indicates that the required distillation time cannot be accurately estimated based on the total loading volume.

[0066] [Example 2: Estimation based on maximum charge height and furnace temperature] As mentioned above Figure 4 As shown, in Example 1, the maximum charging height showed a good correlation with the measured required distillation time. However, in Example 2, in order to estimate the required distillation time with higher accuracy, a study was conducted that considered the furnace temperature in addition to the maximum charging height. Furthermore, the furnace bottom temperature was used as the furnace temperature.

[0067] Regarding the measured required dry distillation time obtained in Example 1, a multiple regression analysis was performed for charging conditions 1–11, using maximum charging height and furnace temperature as explanatory variables and required dry distillation time as the target variable. The coefficient of determination, adjusted for degrees of freedom, obtained through least squares-based linear regression, was 0.97, which is sufficiently high. Furthermore, the p-value distribution for maximum charging height and furnace temperature, used as explanatory variables, was 7.32 × 10⁻⁶. -8 Both 0.002 and 0.002 are sufficiently lower than 0.05, and can be considered as explanatory variables. The resulting regression equation is as follows.

[0068] Required distillation time (hours) = 6.6 × maximum charging height (m) - 0.042 × furnace temperature (°C) + 41.7 Next, the maximum charging height and furnace temperature values ​​for charging conditions 1 to 11 are substituted into the maximum charging height and furnace temperature values ​​in the above regression equation to calculate the estimated values ​​of the required dry distillation time. The calculated estimated values ​​are shown in Table 1.

[0069] Figure 8 This is a graph showing the relationship between the estimated and measured values ​​of the required dry distillation time for the waste plastics in Example 2. The least squares method was used to... Figure 8 The curve shown is approximated by a straight line, and the result is R. 2 The value is 0.98, showing a good correlation between the measured and estimated values. This result indicates that by considering furnace temperature in addition to the maximum loading height, a higher accuracy estimation can be achieved.

[0070] [Comparative Example 2] In Comparative Example 2, the study was conducted in the same manner as in Example 2, except that the total charge was considered instead of the maximum charge height. Regarding the measured required dry distillation time obtained in Example 1, a multiple regression analysis was performed for charge conditions 1–11, using the total charge and furnace temperature as explanatory variables and the required dry distillation time as the target variable. The coefficient of determination, adjusted for degrees of freedom, obtained through linear regression based on least squares, was reduced to 0.894. Furthermore, the p-value for the total charge and furnace temperature used as explanatory variables was 1.51 × 10⁻⁶. -5 The value of 0.07 indicates that the P-value of furnace temperature cannot be used as an explanatory variable.

[0071] The results show that the required distillation time cannot be accurately estimated based on the total charge and furnace temperature.

[0072]

Claims

1. A method for manufacturing a recycled product from waste plastics, characterized in that: It is a method for manufacturing recycled products from waste plastics from coke ovens that have not been charged with coal, the method comprising: The waste plastic is loaded into the coking furnace at a height exceeding half the furnace width, i.e., a predetermined maximum loading height. It is then subjected to carbonization for a predetermined time derived from the predetermined maximum loading height, thereby generating carbonized distillate, tar, light oil, and gas as recycling products of the waste plastic; and The pyrolyte is discharged from the coking oven using an extruder; The predetermined distillation time is obtained through the following steps: Calculate in advance the relationship between the maximum loading height of waste plastics into the coking oven and the required carbonization time to complete the carbonization process, and Substitute the predetermined maximum loading height into the formula to calculate the predetermined distillation time.

2. The method for manufacturing recycled products from waste plastics according to claim 1, characterized in that: The dry distillation is carried out at a predetermined furnace temperature. The aforementioned formula represents the relationship between the maximum charging height, furnace temperature, and the time required to complete the dry distillation. Substitute the predetermined maximum loading height and the predetermined furnace temperature into the formula to calculate the predetermined dry distillation time.

Citation Information

Patent Citations

  • JP1973032902A

  • Coke production method

    JP2002047494A