A filtration aid method to improve the filtration efficiency of monazite slag.
By adding the composite reducing agents sodium sulfite and thiourea during the solid-liquid separation process of monazite slag, a sulfate double salt precipitate that is easy to filter is generated, which solves the problem of poor filtration performance of monazite slag and achieves high-efficiency filtration speed and low water content, making it suitable for large-scale production.
Patent Information
- Application Number
- CN202510922881.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-04
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-07-04
AI Technical Summary
The existing technology for monazite slag has poor filtration performance, slow filtration speed, high water content, and mud-like substances adhering to the filter cloth, which affects subsequent applications and cannot meet the needs of large-scale production.
By adding the composite reducing agents sodium sulfite and thiourea during the solid-liquid separation process, controlling the pH value to 4-4.5, and stirring the reaction for 0.5-2 hours, an easily filterable double sulfate precipitate is generated. The moisture content of the filter residue and the filtration speed are adjusted, and a plate and frame filter press is used for filtration.
It improves the filtration speed and moisture content of monazite slag, reduces the moisture content of the filter cake, simplifies the operating temperature requirements, and enhances filtration efficiency and product quality.
Smart Images

Figure CN120905547B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of monazite processing technology, and in particular to a filter aid method for improving the filtration efficiency of monazite slag. Background Technology
[0002] Currently, monazite is a phosphate rare earth mineral and one of the main raw materials for rare earth production. The processing of monazite rare earth concentrate first involves alkaline decomposition and acid dissolution to generate alkali cake. Then, the monazite alkali cake is further processed to obtain highly soluble residue. The existing alkali cake processing involves acid dissolution of the alkali cake, adding alkali slurry to adjust the pH to 4-4.5, and then filtering. The filtered residue is then washed with water to form a slurry. The slurry is then mixed for solid-liquid separation. The water washing and solid-liquid separation process is repeated, usually 2-3 times. The final solid residue is highly soluble residue. However, during the washing process, the solid-liquid separation speed slows down with each wash. As the reaction proceeds, the final highly soluble residue has a water content of 50-80%. Furthermore, a layer of fine mud-like material adheres to the filter cloth after filtration, making the filter cake unformed and inconvenient for subsequent applications.
[0003] An existing invention patent with publication number CN114107661A provides a method for improving the filtration performance of monazite slurry. This method involves adding hydrochloric acid to the monazite slurry to obtain a leachate suspension. Based on the rich content of valuable elements such as rare earth elements, uranium, and thorium in this suspension, a certain amount of oxalic acid is added. By controlling the reaction temperature, time, residual acid, and the amount of oxalic acid added, thorium in the suspension is fully precipitated, along with other impurities in the monazite slurry. While this method improves filtration performance, it suffers from significant rare earth loss, a high temperature dependence due to forced operation above 70°C, and a low filtration rate resulting in a long filtration cycle, making it unsuitable for large-scale production. Summary of the Invention
[0004] The main objective of this invention is to provide a filter aid method to improve the filtration efficiency of monazite slurry, aiming to solve the technical problem of poor filtration performance of existing monazite slurry made from alkali cake.
[0005] To achieve the above objectives, the present invention provides a filter aid method for improving the filtration efficiency of monazite dissolved residue, the method comprising the following steps:
[0006] Step 1: The mixed slurry after the alkali cake is rehydrated and adjusted is subjected to solid-liquid separation to obtain filter residue 1 and filtrate 1;
[0007] Step 2: Add water to filter residue 1 and mix and stir at a liquid-to-solid ratio of 1-2.5:1 for 0.5-2 hours. Separate the slurry after reaction to obtain filter residue 2 and filtrate 2.
[0008] Step 3, if the slurry filtration rate in step 2 is less than 20 L / (m2 If the moisture content of filter residue 2 is greater than 60%, repeat step 2 with the filter residue, adding a predetermined mass of composite reducing agent during the mixing and stirring reaction and stirring for 2 hours, until the moisture content of the corresponding filter residue is less than or equal to 60% or the slurry filtration rate during plate and frame filtration is greater than or equal to 20 L / (m²). 2 *h);
[0009] In step 3, the mass ratio of the added composite reducing agent to the original dry residue is (5-50) kg: 1 t. The composite reducing agent includes sodium sulfite and thiourea in a mass ratio of 1 to 2:1.
[0010] Optionally, in steps 2 and 3, the temperature of the stirring reaction is 25–40°C.
[0011] Optionally, in steps 1-3, the solid-liquid separation is performed using a plate and frame filter press with a filtration pressure of 0.4-0.8 MPa.
[0012] Optionally, the method further includes aging the filtrate 1 obtained in step 1 to oxidize ferrous iron to form ferric hydroxide precipitate and remove it.
[0013] Optionally, before step 1, the process further includes leaching the alkali cake with hydrochloric acid, then adding alkali slurry and mixing, and controlling the pH of the mixture to 4-4.5 so that the tetravalent cerium in the alkali cake forms hydroxide precipitate and the trivalent iron hydrolyzes to form ferric hydroxide precipitate. The alkali slurry is a mixture of alkali cake and water.
[0014] Optionally, in step 3, the addition of the composite reducing agent reduces tetravalent cerium and trivalent iron in the slurry to trivalent cerium and divalent iron, respectively, and causes thiourea and sodium sulfite to be oxidized to form a sulfate double salt precipitate.
[0015] Optionally, if the slurry filtration rate in step 2 is less than 20 L / (m 2 If *h), add water and composite reducing agent to filter residue 2 and mix and stir at a liquid-to-solid ratio of 1-2.5:1 for 2 hours. Then, perform solid-liquid separation on the slurry after the reaction to obtain corresponding filter residue 3 and filtrate 3. The slurry filtration rate is ≥20 L / (m²). 2 *h);
[0016] Continue to separate the obtained filter residue 3 into solid and liquid components until a filter cake with a thickness of ≥15mm and a moisture content of ≤45% is obtained.
[0017] Optionally, if the moisture content of the filter residue 2 obtained in step 2 is greater than 60%, then water and composite reducing agent are added to the filter residue 2 and mixed and stirred at a liquid-solid ratio of 1 to 2.5:1 for 2 hours. The slurry after the reaction is then subjected to solid-liquid separation to obtain the corresponding filter residue 3 and filtrate 3.
[0018] If the moisture content of filter residue 3 is still greater than 60%, continue to add water and composite reducing agent to filter residue 3 and mix and stir at a liquid-solid ratio of 1-2.5:1 for 2 hours. Then, perform solid-liquid separation on the slurry after the reaction to obtain the corresponding filter residue 4 and filtrate 4.
[0019] If the moisture content of filter residue 4 is less than or equal to 60%, the obtained filter residue 4 will continue to undergo solid-liquid separation to obtain a filter cake with a thickness of ≥15mm and a moisture content of ≤45%.
[0020] Optionally, if the moisture content of the filter residue in step 2 is less than or equal to 60% or the slurry filtration rate is greater than or equal to 20 L / (m²), the filter residue can be filtered further. 2 If *h), then the corresponding filter residue will continue to undergo solid-liquid separation until a filter cake with a thickness ≥15mm and a moisture content ≤45% is obtained.
[0021] Optionally, the filtrate obtained in step 3 can be returned to step 2 for mixing and pulping.
[0022] Beneficial effects:
[0023] In this invention, by detecting whether the moisture content of the filter residue obtained after the previous solid-liquid separation and the filtration speed of the slurry meet the preset requirements, it is determined whether to add a composite reducing agent in the next water washing and stirring reaction. The corresponding slurry filtration speed or the moisture content of the filtered residue is also detected, thereby effectively controlling the timing of adding the composite reducing agent. The addition of the composite reducing agent can reduce the tetravalent cerium and trivalent iron in the original filter residue to trivalent cerium and divalent iron. At pH 4 to 4.5, both trivalent cerium and divalent iron are soluble. The sulfate ions generated after the oxidation of thiourea and sodium sulfite form sulfate double salt precipitates with thorium, iron and other ions. The sulfate double salt precipitates have large particles and low moisture content, making them easier to filter than cerium hydroxide and ferric hydroxide, thus achieving the control of the optimal slurry filtration efficiency. Attached Figure Description
[0024] Figure 1 This is a schematic flowchart of the first embodiment of a filter aid method for improving the filtration efficiency of monazite slag.
[0025] Figure 2 for Figure 1 The corresponding process flow diagram for secondary pulping and washing and the addition of composite reducing agent;
[0026] Figure 3 for Figure 1 The flowchart of the corresponding three pulping and washing processes and the addition of composite reducing agent;
[0027] Figure 4 for Figure 1 The flowcharts for the corresponding secondary and tertiary pulping and washing processes, and the addition of composite reducing agents.
[0028] The realization of the objective, functional features and advantages of the present invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation
[0029] It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.
[0030] See Figure 1-4 This invention provides a filter aid method for improving the filtration efficiency of monazite slag, the method comprising the following steps:
[0031] Step 1 involves solid-liquid separation of the mixed slurry after the alkali cake has been properly dissolved and adjusted, yielding filter residue 1 and filtrate 1. Specifically, the alkali cake comprises rare earth hydroxides, undecomposed monazite, phosphates, Th / U compounds, and light rare earth (cerium group) oxides. The soluble hydroxides are easily leached by acid. Therefore, the mixed slurry can be leached by adding hydrochloric acid to the alkali cake, followed by mixing with the alkali slurry, and adjusting the pH of the mixed slurry to 4-4.5. The purpose is to cause tetravalent cerium in the mixed slurry to form hydroxide precipitates, thorium to form thorium hydroxide precipitates, and trivalent iron to hydrolyze to form ferric hydroxide precipitates. The resulting filter residue 1 contains Th(OH)4, Ce(OH)4, and Fe(OH)3. Filtrate 1 undergoes a radioactive aging treatment to remove the radioactive element radium and reduce the radioactivity of the rare earth chloride solution.
[0032] Step 2: Add water to filter residue 1 and mix and stir at a liquid-to-solid ratio of 1-2.5:1 for 0.5-2 hours. Separate the solid and liquid components of the slurry after the reaction to obtain filter residue 2 and filtrate 2. Filtrate 2 still contains some radioactive elements and requires radioactive removal and aging treatment.
[0033] Step 3, if the slurry filtration rate in step 2 is less than 20 L / (m 2 If the moisture content of filter residue 2 is greater than 60%, then repeat step 2 with the filter residue and add a preset mass of composite reducing agent during the mixing and stirring reaction and stir for 2 hours; specifically, the mass ratio of the added composite reducing agent to the original dry residue is (5-50) kg: 1 t, preferably (6-17) kg: 1 t.
[0034] Furthermore, the composite reducing agent includes sodium sulfite and thiourea in a mass ratio of 1–2:1. Thiourea and sodium sulfite, acting as reducing agents, can reduce tetravalent cerium and trivalent iron to trivalent cerium and divalent iron. At pH 4–4.5, both trivalent cerium and divalent iron are soluble. The sulfate ions generated after the oxidation of thiourea and sodium sulfite form sulfate double salt precipitates with thorium and iron ions. These sulfate double salt precipitates have large particles and low water content, making them easier to filter than cerium hydroxide, ferric hydroxide, and thorium hydroxide. The resulting filtrate is returned to the primary washing and pulping process in step 2. After plate and frame filtration, the divalent iron in the filtrate is oxidized during the aging process (removing radioactive radium to reduce the radioactivity of rare earth chloride solution), forming ferric hydroxide precipitate, which is then filtered out along with the radium residue. Therefore, the addition of the composite reducing agent can reduce insoluble tetravalent cerium, increasing the cerium recovery rate and improving the filtration speed. However, adding too much reducing agent can introduce impurities such as sulfate and ammonia, affecting the quality of rare earth chloride products. Therefore, the amount of composite reducing agent added needs to be strictly controlled.
[0035] Furthermore, the stirring reaction temperature of the above pulping and washing process is 25–40°C, which is at room temperature and does not require heating, thus solving the dependence on temperature in the prior art.
[0036] Furthermore, plate and frame filter presses are used in all the above solid-liquid separation operations, with a filtration pressure of 0.4 to 0.8 MPa.
[0037] Furthermore, the aging time of the reduced ferrous iron in the impurity removal process can be extended; the aging time can also be shortened by adding a small amount of hydrogen peroxide, so that the oxidized ferric iron can form a precipitate and be filtered out together with the impurity removal residue.
[0038] Furthermore, the alkali slurry in step 1 is a mixture made from alkali cake and water.
[0039] Furthermore, such as Figure 2 As shown, if the slurry filtration rate in step 2 is less than 20 L / (m²), 2 *h), then add water and a preset amount of composite reducing agent to filter residue 2, mix and stir at a liquid-to-solid ratio of 1-2.5:1 for 2 hours, and then perform solid-liquid separation on the slurry after the reaction to obtain the corresponding filter residue 3 and filtrate 3, wherein the slurry filtration rate is ≥20L / (m 2 *h);
[0040] Continue to separate the obtained filter residue 3 into solid and liquid components until a filter cake with a thickness of ≥15mm and a moisture content of ≤45% is obtained.
[0041] Furthermore, such as Figure 4As shown, if the moisture content of the filter residue 2 obtained in step 2 is greater than 60%, then water and a preset amount of composite reducing agent are added to the filter residue 2 and mixed and stirred for 2 hours at a liquid-solid ratio of 1 to 2.5:1. The slurry after the reaction is then subjected to solid-liquid separation to obtain the corresponding filter residue 3 and filtrate 3.
[0042] If the moisture content of filter residue 3 is still greater than 60%, continue to add water and a preset amount of composite reducing agent to filter residue 3 and mix and stir for 2 hours at a liquid-solid ratio of 1-2.5:1. Then, perform solid-liquid separation on the slurry after the reaction to obtain the corresponding filter residue 4 and filtrate 4.
[0043] If the moisture content of filter residue 4 is less than or equal to 60%, the obtained filter residue 4 is further subjected to solid-liquid separation to obtain a filter cake with a thickness of ≥15mm and a moisture content of ≤45%.
[0044] Furthermore, if the moisture content of the filter residue in step 2 is less than or equal to 60% or the slurry filtration rate is greater than or equal to 20 L / (m²), 2 If *h), then the corresponding filter residue is further separated into solid and liquid components until a filter cake with a thickness ≥15mm and a moisture content ≤45% is obtained.
[0045] Furthermore, if the moisture content of the filter residue obtained after secondary plate and frame filtration with added water and corresponding filter residue is greater than 60%, or the slurry filtration rate during plate and frame filtration is less than 20 L / (m²), then... 2 If *h), then during the third addition of water for washing, a preset amount of composite reducing agent is also added to perform solid-liquid separation on the reacted slurry, obtaining the corresponding filter residue and filtrate. The moisture content of the filter residue must be less than or equal to 60%, or the slurry filtration rate during plate and frame filtration must be greater than or equal to 20 L / (m²). 2 If *h), then the corresponding filter residue is further separated into solid and liquid components until a filter cake with a thickness ≥15mm and a moisture content ≤45% is obtained. A specific schematic diagram is shown below. Figure 3 As shown.
[0046] In addition to the above-described contents, it can also be detected that if the slurry filtration rate in step 1 is less than 20 L / (m³),... 2 If the moisture content of filter residue 1 is greater than 60%, then a predetermined mass of composite reducing agent is added to the mixing and stirring reaction in step 2 and the reaction is stirred for 2 hours to obtain the corresponding filtrate 2' and filter residue 2'. The moisture content of filter residue 2' and the slurry filtration rate are then monitored. If the moisture content of filter residue 2' is less than or equal to 60% and the slurry filtration rate is greater than 20 L / (m²), the reaction proceeds. 2 *h), then continue solid-liquid separation on the obtained filter residue 2' until a filter cake with a thickness ≥15mm and a moisture content ≤45% is obtained; however, if the slurry filtration rate is still below 20L / (m 2If the moisture content of filter residue 2' is greater than 60%, repeat step 2 with filter residue 2', adding a preset mass of composite reducing agent during the mixing and stirring reaction and stirring for 2 hours until the moisture content of the corresponding filter residue is less than or equal to 60% or the slurry filtration rate is greater than or equal to 20 L / (m). 2 *h).
[0047] In summary, this invention determines whether to add a composite reducing agent in the next water washing and stirring reaction by detecting whether the moisture content of the filter residue obtained after the previous solid-liquid separation and the filtration speed of the slurry meet the preset requirements. It also detects the corresponding slurry filtration speed or the moisture content of the filtered residue, thereby effectively controlling the timing of adding the composite reducing agent. Furthermore, adding the composite reducing agent can reduce tetravalent cerium and trivalent iron in the original filter residue to trivalent cerium and divalent iron. At pH 4-4.5, both trivalent cerium and divalent iron are soluble. The sulfate ions generated after the oxidation of thiourea and sodium sulfite form sulfate double salt precipitates with thorium and iron ions. These sulfate double salt precipitates have large particles and low moisture content, making them easier to filter than cerium hydroxide and ferric hydroxide, thus achieving the control of optimal slurry filtration efficiency.
[0048] Furthermore, to better illustrate the process operation of the present invention, specific embodiments are described below.
[0049] Example 1
[0050] Using Rio Tinto monazite ore as the raw material, the concentrate was alkali-decomposed to obtain the corresponding monazite alkali cake, which was then leached with hydrochloric acid. The pH was adjusted to 4 by adding alkali slurry. The resulting mixed slurry underwent solid-liquid separation to obtain filter residue 1 and filtrate 1. Water was added to filter residue 1 and mixed at a liquid-to-solid ratio of 2:1, and the mixture was stirred for 2 hours. The resulting slurry was then subjected to plate and frame filtration to obtain filter residue 2 and filtrate 2. Filter residue 2 was a slurry with a thickness of approximately 5 mm, and its moisture content was measured to be 76%. The filtration velocity was 8 L / (m²). 2 *h), and the slag in the slurry weighed approximately 3t. Then, water, 33kg of sodium sulfite, and 17kg of thiourea were added to filter residue 2, and the mixture was stirred and reacted for 2 hours while maintaining a liquid-to-solid ratio of 2:1. The resulting slurry was then subjected to plate and frame filtration, and the filtration rate was measured to be 30L / (m²). 2 *h) Plate and frame filtration is then continued, resulting in a filter cake thickness of approximately 18 mm. The filter cake is relatively hard and has a moisture content of 45%. A schematic diagram of the reaction process can be found here. Figure 2 .
[0051] Example 2
[0052] Monazite ore was used as a low-terbium dysprosium ore. After alkali decomposition of the concentrate, the corresponding monazite alkali cake was obtained. This cake was then leached with hydrochloric acid, and the pH was adjusted to 4 by adding alkali slurry. The resulting mixed slurry underwent solid-liquid separation to obtain filter residue 1 and filtrate 1. Water was added to filter residue 1 and mixed at a liquid-to-solid ratio of 1.5:1, stirring for 0.5 hours. The resulting slurry was then filtered using a plate and frame filter press to obtain filter residue 2 and filtrate 2. If the water content of filter residue 2 was found to be less than or equal to 60%, water was added again and the mixture was stirred for 2 hours at a liquid-to-solid ratio of 1.5:1. The resulting slurry was then filtered using a plate and frame filter press to obtain filter residue 3 and filtrate 3. Filter residue 3 was a slurry approximately 10 mm thick, with a water content of 31%, and the filtration rate was 10 L / (m²). 2 *h), and the slag in the slurry weighs about 3t. Then, water, 15kg of sodium sulfite, and 15kg of thiourea are added to the filter residue 3, and the liquid-to-solid ratio is controlled at 1.5:1. The mixture is stirred and reacted for 2 hours. The slurry after the reaction is then filtered using a plate and frame filter press to obtain filter residue 4 and filtrate 4. The filtration rate is measured to be 24L / (m). 2 *h) Plate and frame filtration is then continued, resulting in a filter cake thickness of approximately 15 mm and a moisture content of 42%. A schematic diagram of the reaction process can be found here. Figure 3 .
[0053] Example 3
[0054] Monazite ore was used as a low-terbium dysprosium ore. After alkali decomposition of the concentrate, the corresponding monazite alkali cake was obtained. This cake was then leached with hydrochloric acid, and the pH was adjusted to 4 by adding alkali slurry. The resulting mixed slurry underwent solid-liquid separation to obtain filter residue 1 and filtrate 1. Water was added to filter residue 1 and mixed at a liquid-to-solid ratio of 1:1, with stirring for 0.5 hours. The resulting slurry was then filtered using a plate and frame filter press to obtain filter residue 2 and filtrate 2. If the water content of filter residue 2 was found to be less than or equal to 60%, water was added again and the mixture was stirred for another 0.5 hours at a liquid-to-solid ratio of 1:1. The resulting slurry was then filtered using a plate and frame filter press to obtain filter residue 3 and filtrate 3. Filter residue 3 was a slurry approximately 10 mm thick, with a water content of 48%, and the filtration velocity was 18 L / (m²). 2 *h), and the slag in the slurry weighs about 3t. Then, water, 9kg of sodium sulfite, and 9kg of thiourea are added to the filter residue 3, and the liquid-to-solid ratio is controlled at 1:1. The mixture is stirred and reacted for 2 hours. The slurry after the reaction is then filtered using a plate and frame filter press to obtain filter residue 4 and filtrate 4. The filtration rate is measured to be 25L / (m). 2 *h) Plate and frame filtration is then continued, resulting in a filter cake thickness of approximately 16 mm and a moisture content of 40%. A schematic diagram of the reaction process can be found here. Figure 3 .
[0055] It should be noted that, in this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or system that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or system. Unless otherwise specified, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or system that includes that element.
[0056] The sequence numbers of the above embodiments of the present invention are for descriptive purposes only and do not represent the superiority or inferiority of the embodiments.
[0057] The above are merely preferred embodiments of the present invention and do not limit the scope of the patent. Any equivalent structural or procedural transformations made based on the description and drawings of the present invention, or direct or indirect applications in other related technical fields, are similarly included within the scope of patent protection of the present invention.
Claims
1. A filter aid method for improving the filtration efficiency of monazite slag, characterized in that, The method includes the following steps: Step 1: The mixed slurry after the alkali cake is rehydrated and adjusted is subjected to solid-liquid separation to obtain filter residue 1 and filtrate 1; Step 2: Add water to filter residue 1 and mix at a liquid-to-solid ratio of 1-2.5:
1. Stir and react at 25-40℃ for 0.5-2 hours. Separate the solid and liquid components of the slurry after reaction to obtain filter residue 2 and filtrate 2. Step 3, if the slurry filtration rate in Step 2 is less than 20 L / (m 2 If the moisture content of filter residue 2 is greater than 60%, then repeat step 2 with filter residue 2, adding a predetermined mass of composite reducing agent during the mixing and stirring reaction, and stirring at 25-40℃ for 2 hours to obtain the filter residue after repeating the step; if the moisture content of the filter residue in the repeated step 2 operation is less than or equal to 60% or the slurry filtration rate during plate and frame filtration is greater than or equal to 20 L / (m 2 If *h), the corresponding filter residue will continue to be separated into solid and liquid components until a final filter cake with a thickness ≥15mm and a moisture content ≤45% is obtained; In step 3, the mass ratio of the added composite reducing agent to the original dry slag is (5-50) kg: 1 t. The composite reducing agent includes sodium sulfite and thiourea in a mass ratio of 1 to 2:
1. The addition of the composite reducing agent reduces tetravalent cerium and trivalent iron in the slurry to trivalent cerium and divalent iron, respectively, and causes thiourea and sodium sulfite to be oxidized to form sulfate double salt precipitates. Before step 1, the process also includes leaching the alkali cake with hydrochloric acid, then adding alkali slurry and mixing, and controlling the pH of the mixed slurry to be 4-4.5, so that the tetravalent cerium in the alkali cake forms hydroxide precipitate and the trivalent iron hydrolyzes to form ferric hydroxide precipitate. The alkali slurry is a mixture of alkali cake and water.
2. The filter aid method for improving the filtration efficiency of monazite slag as described in claim 1, characterized in that, In steps 1-3, solid-liquid separation is performed using a plate and frame filter press with a filtration pressure of 0.4-0.8 MPa.
3. The filter aid method for improving the filtration efficiency of monazite slag as described in claim 1, characterized in that, The method further includes aging the filtrate 1 obtained in step 1 to oxidize ferrous iron to form ferric hydroxide precipitate, which is then removed.
4. The filter aid method for improving the filtration efficiency of monazite slag as described in claim 1, characterized in that, If the slurry filtration rate in step 2 is less than 20 L / (m 2 If *h), add water and composite reducing agent to filter residue 2 and mix and stir at a liquid-to-solid ratio of 1-2.5:1 for 2 hours. Then, perform solid-liquid separation on the slurry after the reaction to obtain corresponding filter residue 3 and filtrate 3. The slurry filtration rate is ≥20 L / (m²). 2 *h); Continue to separate the obtained filter residue 3 into solid and liquid components until a filter cake with a thickness of ≥15mm and a moisture content of ≤45% is obtained.
5. The filter aid method for improving the filtration efficiency of monazite slag as described in claim 1, characterized in that, If the moisture content of filter residue 2 obtained in step 2 is greater than 60%, then add water and composite reducing agent to filter residue 2 and mix and stir at a liquid-solid ratio of 1 to 2.5:1 for 2 hours. Then, perform solid-liquid separation on the slurry after the reaction to obtain the corresponding filter residue 3 and filtrate 3. If the moisture content of filter residue 3 is still greater than 60%, continue to add water and composite reducing agent to filter residue 3 and mix and stir at a liquid-solid ratio of 1-2.5:1 for 2 hours. Then, perform solid-liquid separation on the slurry after the reaction to obtain the corresponding filter residue 4 and filtrate 4. If the moisture content of filter cake 4 is less than or equal to 60%, continue to separate the solid and liquid components of the obtained filter cake 4 until a filter cake with a thickness of ≥15mm and a moisture content of ≤45% is obtained.
6. The filter aid method for improving the filtration efficiency of monazite slag as described in any one of claims 1 to 5, characterized in that, The filtrate obtained in step 3 is returned to step 2 for mixing and pulping.
Citation Information
Patent Citations
Method for improving filtering performance of high-quality monazite slag
CN114107661A
Method for leaching valuable resources from selective solution slag
CN112760485A
Method for treating xenotime
CN118563133A