Cold press molding process for miniature radio frequency conical inductor magnetic core and module device
By using a vacuum mixer and a biaxial gradient pressure cold pressing process, combined with a specific cone-angle mold and high-temperature sintering, the demolding defects and performance fluctuations of miniature radio frequency cone inductor cores have been solved. This has resulted in high-density, low-defect-rate, and high-strength cores, improving inductor performance in the high-frequency band and meeting the needs of high-end applications.
Patent Information
- Application Number
- CN202511169532.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-20
- Publication Date
- 2025-11-25
AI Technical Summary
In the existing technology, the molding process of miniature radio frequency tapered inductor cores has problems such as demolding defects, insufficient strength and performance fluctuations, especially in the high-frequency band, which makes it difficult to meet the needs of high-end applications.
The magnetic core is uniformly mixed using a vacuum mixer, combined with a biaxial gradient pressure cold pressing process, a specific cone-angle mold and a precision mold design, and high-temperature sintering to achieve improved density uniformity and strength.
This technology achieves high density, low defect rate, and high strength in miniature RF tapered inductor cores, improving inductor performance in the high-frequency band, adapting to applications such as broadband RF power amplification and antenna matching, reducing production energy consumption, and improving production efficiency.
Smart Images

Figure CN121011448A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of magnetic core manufacturing, in particular to a micro radio frequency conical inductor magnetic core cold pressure forming process and module device. BACKGROUND
[0002] In the field of high-frequency electronic devices, ordinary inductors perform stably in a specific low-frequency band, but fail completely due to sharp self-resonance at high frequencies, and the effective bandwidth is relatively narrow; in contrast, a wideband conical inductor, through the revolutionary design of a conical magnetic core and a gradually changing winding structure, continuously and gradually changes the distributed parasitic capacitance and inductance value along the physical length, completely disperses the single resonance point, and thus maintains stable inductive reactance characteristics in an ultra-wide frequency band of several MHz to several GHz, and the core advantage lies in the absence of sudden self-resonance collapse - high-frequency performance is not suddenly lost, but smoothly transitions, so that it becomes an irreplaceable core component in high-end applications such as wideband radio frequency power amplification and antenna matching that require stable impedance in the entire frequency band.
[0003] From the perspective of material forming, when soft magnetic materials (such as iron-based and carbonyl soft magnetic powder) are mixed with a binder and a release agent, conventional mixing methods (such as mechanical stirring) are prone to air residues and uneven mixing, resulting in large density fluctuations (axial density deviation exceeding 5%) after the magnetic core is pressed, and the edges of the formed magnetic core are loose and the center is dense, which seriously affects the consistency of high-frequency eddy current loss and permeability. If the moisture control is not proper (such as a difference in moisture content of the raw materials > 1%) during the drying stage of mixing, it will cause local "over-wetting / over-drying" during the pressing process, resulting in cracking and insufficient strength of the magnetic core. Traditional processes lack sufficient control over drying temperature (usually 80-100℃), duration (about 24h) and moisture consistency, making it difficult to meet the high precision requirements of micro magnetic cores. SUMMARY
[0004] (I) Technical problems solved
[0005] In view of the deficiencies of the prior art, the present application provides a micro radio frequency conical inductor magnetic core cold pressure forming process and module device, which solves the problems of demolding defects, insufficient strength and performance fluctuations in the forming of existing ferrite magnetic cores.
[0006] (II) Technical solutions
[0007] To achieve the above-mentioned purpose, the present application provides the following technical solutions: a micro radio frequency conical inductor magnetic core cold pressure forming process and module device, comprising the following steps:
[0008] Mixing the soft magnetic material with 3-5wt% PVA and 0.2-0.5wt% zinc stearate, uniformly mixing by a vacuum mixer to obtain a uniform mixture, and expelling the internal air to make the density uniform and compact;
[0009] The magnetic core forming die comprises an upper punch, a lower punch and a female die assembly, the upper and lower punches are composed of powder steel, and the female die is a hollow special steel, the mixed material after mixing is injected into the female die, the upper punch is lowered to pressurize, the lower punch is synchronously moved reversely, the biaxial pressure makes the powder be directionally compressed along the tapered gradient to realize uniform distribution of density; in the demolding stage, the lower punch ejects the blank, the taper of the die is matched with the ejection mechanism to stably demold, and the magnetic core with uniform strength and smooth surface is obtained.
[0010] Preferably, the soft magnetic material, PVA and zinc stearate are baked at 105 DEG C for 36 hours, and the moisture is kept consistent and is lower than 1%.
[0011] Preferably, the mixing time of the uniform mixed material in the vacuum mixer is not less than 30 minutes, and the density is kept uniform.
[0012] Preferably, the cavity taper angle of the upper punch die and the lower punch die of the magnetic core forming die is 19.6 DEG + or - 0.1 DEG, and the cavity surface roughness is less than or equal to 1.6 microns; the die material is powder steel, the un-injection tolerance is + or - 0.1 mm, the un-injection chamfer is 0.5*45 DEG, and the countersunk hole adopts a right angle structure.
[0013] Preferably, the upper punch die and the lower punch die adopt double-axial synchronous reverse movement in the pressing process, the axial pressure range of the upper punch is 300 MPa-800 MPa, the lower punch is synchronously ejected to realize gradient compression of the tapered magnetic core, and the pressure maintaining time is 5-10 seconds.
[0014] Preferably, the die cavity surface is polished and is provided with an R0.5 round corner transition structure to avoid stress concentration in the powder pressing process of the magnetic core.
[0015] Preferably, the die assembly is matched with an automatic feeding system to realize quantitative filling of the magnetic powder and the binder, and the filling precision error is less than or equal to + or - 0.05 mm.
[0016] Preferably, the soft magnetic material is a mixture of iron-based soft magnetic material and carbonyl soft magnetic material, the iron-based soft magnetic material is Fe-Si-Al alloy powder, the carbonyl soft magnetic material is carbonyl iron powder, 0.5-2 wt% of polyvinyl alcohol is added as a binder after mixing, and the uniform mixing degree deviation is less than or equal to + or - 1.5%.
[0017] (Three) beneficial effects
[0018] Compared with the prior art, the present application provides a micro radio frequency tapered inductor magnetic core cold pressure forming process and die assembly, which has the following beneficial effects:
[0019] 1. In this invention, the "vacuum mixing + biaxial gradient pressing" process, combined with a 19.6°±0.1° conical mold, ensures that the axial density deviation of the magnetic core is ≤2% (compared to >5% for traditional single-axis pressing). Vacuum mixing eliminates the uneven porosity caused by air bubbles, and biaxial pressing compresses the powder along the tapered direction, solving the industry problem of "loose edges and dense center," thus laying the foundation for low-loss (eddy current loss 0.018-0.022) high-frequency inductors.
[0020] 2. In this invention, the mold adopts a 0.5mm rounded corner transition, a ≤1.6μm polished cavity, and a smooth ejection speed of 0.8mm / s-1.2mm / s, so that the surface defect rate of the magnetic core is ≤0.5% (the defect rate of traditional cold pressing demolding is mostly ≥3%). The ±0.1mm tolerance of the powder steel mold is matched with the special steel master mold to achieve a green blank size accuracy of ±0.05mm, which meets the requirements of "small size and high consistency" of miniature radio frequency inductors and reduces subsequent grinding / trimming processes.
[0021] 3. In this invention, after the magnetic core is sintered at 850℃-980℃, the porosity is ≤0.8% and the initial permeability μi@10kHz is ≥3000 (the μi of traditional cold-pressed magnetic cores is usually <2500). The high-density structure reduces the resistance to movement of magnetic domain walls, and the tapered gradient design optimizes the magnetic domain arrangement, thereby improving the Q value of the miniature RF inductor by 15% to 20% in the 10MHz-1000MHz frequency band, meeting the requirements of 5G base stations and millimeter-wave modules for "low-loss, high-Q" inductors.
[0022] 4. In this invention, cold pressing and high-temperature sintering work together to achieve a core bending strength of 22MPa-32MPa (the bending strength of traditional cold-pressed cores is mostly <20MPa). Biaxial pressing avoids "laminar cracking" defects, and sintering eliminates micropores, improving the core's resistance to vibration and thermal shock (-40℃-125℃ cyclic testing, inductance parameter drift ≤±3%), making it suitable for harsh environments such as automotive electronics and industrial control.
[0023] 5. In this invention, the mold is compatible with an automatic feeding system, and the vacuum mixing, biaxial cold pressing, and smooth demolding processes can be integrated into existing powder metallurgy production lines with low modification difficulty. The single-mold molding cycle is ≤20 seconds (pre-pressing + main pressing + demolding), and with a pressurization rate of 50MPa / s-100MPa / s, the hourly production capacity is increased by 25%, adapting to the needs of "small batch, multi-variety" RF inductor customization and "large-scale standardized" production.
[0024] 6. In this invention, the traditional "degreasing-pre-firing" process (which relies on a high-temperature furnace and has high energy consumption) is eliminated. By optimizing the binder (PVA is water-soluble and zinc stearate is easy to demold) and the mold design, "one-time cold pressing and direct sintering" is achieved, reducing energy consumption by more than 30%; the mold life (powder steel is wear-resistant) is increased to more than 50,000 cycles (the traditional mold life is often <30,000 cycles), further reducing production costs and meeting the industry's demand for cost reduction. Attached Figure Description
[0025] Figure 1 This is a flowchart of a cold pressing process for a miniature radio frequency tapered inductor core and a module device proposed in this invention;
[0026] Figure 2 This is a front view of a micro radio frequency tapered inductor core cold pressing process and module device proposed in this invention;
[0027] Figure 3 This is a detailed cross-sectional view of the core mold and molded part of a micro radio frequency conical inductor core cold pressing process and module device proposed in this invention.
[0028] Figure 4 The present invention provides a three-view diagram of a carrier board for a micro-RF tapered inductor core cold pressing process and module device.
[0029] Figure 5 Three-view drawings of a cold pressing process for a miniature radio frequency tapered inductor core and auxiliary tooling for a module device proposed in this invention;
[0030] Figure 6 This is a schematic diagram of the core module integration of a micro radio frequency tapered inductor core cold pressing process and module device proposed in this invention. Detailed Implementation
[0031] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0032] Please see Figure 1 - Figure 6 A cold-pressing process for a miniature radio frequency tapered inductor core and a module device, comprising the following steps:
[0033] The soft magnetic material is mixed with 3-5 wt% PVA and 0.2-0.5 wt% zinc stearate, and then uniformly mixed using a vacuum mixer to remove internal air and make it uniformly dense and compact.
[0034] The magnetic core forming die comprises an upper punch, a lower punch and a female die assembly, the upper and lower punches are composed of powder steel, and the female die is a hollow special steel. The mixed material is injected into the female die, the upper punch is pressed downward, the lower punch is synchronously moved in the opposite direction, the biaxial pressure makes the powder be directionally compressed along the tapered gradient, and uniform density distribution is realized. In the demolding stage, the lower punch ejects the embryo, the mold taper cooperates with the ejection mechanism to smoothly demold, and the magnetic core with uniform strength and smooth surface is obtained.
[0035] In this embodiment, the present application successfully realizes the high-density, high-strength and low-defect rate forming process of the micro radio frequency conical inductor magnetic core through multi-link precise control technology. In the pretreatment stage of the soft magnetic raw material, the soft magnetic material, 3-5wt% of PVA binder and 0.2-0.5wt% of zinc stearate release agent are mixed in a precise proportion. In order to ensure the dryness of the mixed material, the three are first subjected to high-temperature drying treatment at 105 DEG C for 36 hours, so that the water content is reduced to below 1%. Then, the dried mixed material is put into a vacuum mixer to mix at a speed of 200 rpm to 400 rpm, and the mixing time is not less than 30 minutes, and the vacuum degree is strictly controlled to be ≤0.08 MPa. This vacuum environment can effectively exhaust the air inside the mixed material, avoiding the formation of pores due to air bubble residues in the pressing process. In addition, the double-shaft planetary stirring mode is adopted to ensure that the material can be uniformly dispersed, and the mixing uniformity deviation is controlled to be ≤±1.2%. The PVA binder significantly enhances the bonding force of the material by coating the powder particles, and the zinc stearate effectively reduces the subsequent friction with the mold, laying a solid foundation for the forming strength and demolding performance. The uniformly mixed powder also needs to be screened through a 200-mesh screen to ensure that its Hall flow rate is ≤25 s / 50 g, and it has good fluidity to meet the needs of automatic filling.
[0036] The mold structure design is the core of realizing precise forming, the upper punch, the lower punch and the hollow special steel female die assembly are made of powder steel, the upper and lower punch cavity taper angles are accurately controlled to be 19.6±0.1°, which can guide the powder to be directionally compressed along the tapered gradient through fluid mechanics simulation optimization; the cavity surface roughness is ≤1.6 μm and is subjected to polishing treatment, cooperating with the R0.5 round corner transition structure, which can not only reduce the powder adhesion, but also disperse the pressing stress to avoid edge cracking; the mold tolerance is ±0.1 mm, which ensures the assembly accuracy and prevents the powder from remaining in the gap to cause "pressure relief"; in the demolding stage, the lower punch cooperates with the ejection mechanism to smoothly eject the embryo at a speed of 0.8-1.2 mm / s, and the mold taper and low-speed ejection are coordinated to reduce the internal stress release rate, so that the surface defect rate of the magnetic core is ≤0.5%.
[0037] The mold structure design is a core link for realizing precision molding. The upper punch, the lower punch and the hollow special steel mold assembly are made of powder steel. The taper angle of the upper punch and the lower punch is accurately controlled at 19.6±0.1°. The angle is optimized through fluid mechanics simulation, and can effectively guide the powder to be compressed along the taper gradient. The surface roughness of the cavity is controlled at ≤1.6μm, and is subjected to fine polishing treatment. The R0.5 round corner transition structure reduces the powder adhesion and effectively disperses the pressing stress, and avoids the edge cracking phenomenon. The un-injection tolerance of the mold is strictly controlled at ±0.1mm, so as to ensure the assembly accuracy and prevent the powder from being left in the gap to cause the pressure relief. In the demolding stage, the lower punch cooperates with the ejection mechanism to smoothly eject the blank body at the speed of 0.8-1.2mm / s. The taper of the mold and the low-speed ejection are cooperated to effectively reduce the release rate of the internal stress, so that the surface defect rate of the magnetic core is reduced to ≤0.5%.
[0038] The cold pressing forming process realizes the uniform distribution of the density through the stage pressurization. Firstly, the double axial pressure mode of the downward movement of the upper punch and the synchronous reverse movement of the lower punch is adopted. In the pre-pressing stage, the pressure is increased at the speed of 5MPa / s-10MPa / s to 50MPa-100MPa and is kept for 2-3 seconds, so as to fully discharge the air in the powder gap. Then, in the main pressing stage, the pressure is increased to 300MPa-800MPa and is kept for 5-10 seconds, so as to make the powder particles tightly combine under the double axial pressure. The green density is ≥3.5g / cm 3 , the axial density deviation is ≤2%, the magnetic core after forming is dried at 105℃ for 24 hours to remove the residual moisture, and then is sintered at 850℃-980℃, so as to realize further densification through the particle diffusion migration. The density after sintering is ≥4.8g / cm 3 , the porosity is ≤0.8%, the sintering process promotes the grain growth and the solid phase reaction at the same time, eliminates the micro defects, and finally makes the magnetic core obtain the bending strength of 22MPa-32MPa, the initial permeability (μi@10kHz) is increased to ≥3000, the high-frequency eddy current loss is reduced to 0.018-0.022, and the strict requirements of the micro radio frequency inductor on low loss and high stability are met.
[0039] The cold pressing forming process realizes the uniform distribution of the density through the stage pressurization. Firstly, the double axial pressure mode of the downward movement of the upper punch and the synchronous reverse movement of the lower punch is adopted. In the pre-pressing stage, the pressure is increased at the speed of 5MPa / s-10MPa / s to 50MPa-100MPa and is kept for 2-3 seconds, so as to fully discharge the air in the powder gap. Then, in the main pressing stage, the pressure is increased to 300MPa-800MPa and is kept for 5-10 seconds, so as to make the powder particles tightly combine under the double axial pressure. The green density is ≥3.5g / cm 3, axial density deviation is controlled to be ≤2%. After the molding, the magnetic core still needs to be dried at a high temperature of 105 DEG C for 24 hours to remove residual moisture, and then sintered at a high temperature of 850 DEG C to 980 DEG C. Through particle diffusion migration, further densification is realized, and the density after sintering reaches ≥4.8g / cm 3 , porosity is reduced to ≤0.8%. The sintering process not only promotes the growth of grains and solid phase reaction, but also eliminates micro defects, finally makes the magnetic core obtain the bending strength of 22MPa to 32MPa, the initial permeability (μi@10kHz) is improved to ≥3000, the high-frequency eddy current loss is reduced to 0.018 to 0.022, which fully meets the strict requirements of low loss and high stability of micro radio frequency inductors.
[0040] Overall, the uniformity control of pretreatment provides high-quality raw materials for molding, the precise structure of the mold provides directional space for powder compression, and the staged pressing and smooth demolding realize density uniformity and low defects. The three solve the problems of density unevenness, demolding difficulty and performance fluctuation in traditional cold pressing molding, and finally realize the synchronous optimization of the mechanical and electromagnetic properties of the magnetic core, and reach the high-standard indicators of industrial production.
[0041] Working principle, the present application realizes the high density, high strength and low defect rate of the micro radio frequency conical inductor magnetic core through multi-link precise control. In the pretreatment stage of the soft magnetic raw material, the soft magnetic material is mixed with 3-5wt% of PVA binder and 0.2-0.5wt% of zinc stearate demolding agent in proportion, the three are first dried at 105 DEG C for 36 hours to make the moisture less than 1%, then put into the vacuum mixer at a speed of 200rpm-400rpm for mixing for not less than 30 minutes, the vacuum degree is controlled to be ≤0.08MPa, the internal air of the mixed material is effectively discharged in the vacuum environment to avoid the formation of pores due to air bubbles remaining during pressing, and the biaxial planetary stirring ensures the uniform dispersion of the material, the mixing uniformity deviation is ≤±1.2%, the PVA enhances the bonding force by coating the powder particles, and the zinc stearate reduces the friction with the mold, which lays a foundation for the forming strength and demolding performance. The mixed powder is passed through a 200 mesh screen to ensure good flowability of the Hall flow rate ≤25s / 50g to meet the automatic filling demand.
[0042] The mold structure design is the core of realizing precision molding. The upper punch, the lower punch and the hollow special steel mold assembly are made of powder steel. The taper angle of the upper punch and the lower punch cavity is accurately controlled to be 19.6±0.1°. The angle optimized by fluid mechanics simulation can guide the powder to be compressed along the tapered gradient. The cavity surface roughness is ≤1.6μm and is polished. The R0.5 round corner transition structure can reduce powder adhesion and disperse pressing stress to avoid edge cracking. The mold is not injected with a tolerance of ±0.1mm to ensure assembly accuracy and prevent powder residue gap from causing “pressure relief”. In the demolding stage, the lower punch cooperates with the ejection mechanism to smoothly eject the embryo at a speed of 0.8-1.2mm / s. The synergy of the mold taper and low-speed ejection reduces the internal stress release rate, and the surface defect rate of the magnetic core is ≤0.5%.
[0043] The cold pressing forming process realizes uniform density distribution through staged pressing. Firstly, the biaxial pressure mode of the upper punch descending and the lower punch synchronous reverse motion is used. The pre-pressing stage is pressed at a rate of 5MPa / s-10MPa / s to 50MPa-100MPa and is kept for 2-3 seconds to fully discharge the air gap between the powders. Then, the main pressing stage is increased to 300MPa-800MPa and is kept for 5-10 seconds to make the powder particles tightly combined under the action of biaxial pressure. The green density is ≥3.5g / cm 3 , the axial density deviation is ≤2%, the formed magnetic core is dried at 105℃ for 24 hours to remove residual moisture, and then is sintered at 850℃-980℃ to realize further densification through particle diffusion migration. The density after sintering is ≥4.8g / cm 3 , the porosity is ≤0.8%, the sintering process promotes grain growth and solid phase reaction at the same time, eliminates micro defects, and finally makes the magnetic core obtain a bending strength of 22MPa-32MPa, an initial permeability (μi@10kHz) of ≥3000, and a high-frequency eddy current loss of 0.018-0.022, which meets the strict requirements of low loss and high stability of micro radio frequency inductors.
[0044] Overall, the uniformization control of pretreatment provides high-quality raw materials for molding, the precise structure of the mold provides a directional space for powder compression, and staged pressing and smooth demolding realize uniform density and low defects. The three work together to solve the problems of density unevenness, demolding difficulty and performance fluctuation in traditional cold pressing forming. Finally, the mechanical and electromagnetic properties of the magnetic core are optimized simultaneously to achieve industrial production indicators.
[0045] It is to be noted that, as used in this specification and the appended claims, the singular forms "a," "an" and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a component" can include a combination of two or more components. Similarly, the terms "one" and "the" do not exclude the presence of more than one item, unless the context clearly indicates otherwise. Further, the terminology "an" and "one" are used in the detailed description and claims only to mean one or more, at least one, or "at least one." Finally, the words "comprise," "comprises," and "comprising" and the like, are to be construed in their broadest, intended, and open ended form to encompass events that would otherwise prevent a process, method, article, or apparatus from being encompassed by the claim.
Claims
1. A cold-pressing process for a miniature radio frequency tapered inductor core and a module device, characterized in that: The method comprises the following steps: The soft magnetic material is mixed with 3-5wt% PVA and 0.2-0.5wt% zinc stearate, uniformly mixed by a vacuum mixer to form a uniform mixture, and the internal air is discharged to make the density uniform and compact; A magnetic core forming die is used, which comprises an upper punch, a lower punch and a female die assembly, the upper and lower punches are composed of powder steel, and the female die is a hollow special steel, the mixed mixture is injected into the female die, the lower punch is synchronously moved in the opposite direction by the downward pressure of the upper punch, and the biaxial pressure makes the powder be directionally compressed along the tapered gradient to realize uniform distribution of density; the lower punch ejects the blank in the demolding stage, and the die taper cooperates with the ejection mechanism to stably demold to obtain a magnetic core with uniform strength and smooth surface.
2. The micro radio frequency tapered inductor magnetic core cold press forming process and module device according to claim 1, characterized in that: The soft magnetic material, PVA and zinc stearate are dried at 105°C for 36h, and the moisture is kept consistent and lower than 1%.
3. The micro radio frequency tapered inductor magnetic core cold press forming process and module device according to claim 1, characterized in that: The mixing time of the uniform mixture in the vacuum mixer is not less than 30min, and the density is kept uniform.
4. The micro radio frequency (RF) conical inductor magnetic core cold press forming process and module device of claim 2, wherein: The cavity taper angle of the upper punch die and the lower punch die of the magnetic core forming die is 19.6°±0.1°, and the cavity surface roughness is ≤1.6μm; the die material is powder steel, the unmarked tolerance is ±0.1mm, the unmarked chamfer is 0.5×45°, and the countersunk hole adopts a right angle structure.
5. The micro radio frequency tapered inductor magnetic core cold press forming process and module device according to claim 4, characterized in that: The upper punch die and the lower punch die adopt double-axial synchronous reverse movement in the pressing process, the axial pressure range of the upper punch is 300MPa-800MPa, the lower punch is synchronously ejected to realize gradient compression of the tapered magnetic core, and the pressure maintaining time is 5-10s.
6. The micro radio frequency tapered inductor magnetic core cold press forming process and module device of claim 4, wherein: The die cavity surface is polished and provided with an R0.5 round corner transition structure to avoid stress concentration during the pressing of the magnetic core powder.
7. The micro radio frequency tapered inductor magnetic core cold press forming process and module device of claim 4, wherein: The die assembly cooperates with an automatic feeding system to realize quantitative filling of the magnetic powder and the binder, and the filling precision error is ≤±0.05mm.
8. The micro radio frequency tapered inductor magnetic core cold press forming process and module device of claim 4, wherein: The soft magnetic material is a mixture of iron-based soft magnetic material and carbonyl soft magnetic material, the iron-based soft magnetic material is Fe-Si-Al alloy powder, the carbonyl soft magnetic material is carbonyl iron powder, and 0.5-2wt% polyvinyl alcohol is added as a binder after mixing, and the uniformity deviation of the mixture is ≤±1.5%.
