An ultrasonic dust removal head manufactured by extrusion molding and a preparation method thereof

The ultrasonic dust collector head manufacturing method, which combines extrusion molding and multi-step anodizing, solves the problems of material waste and consistency in traditional manufacturing methods, achieving efficient and low-cost dust collector head production, and improving the wear resistance and corrosion resistance of the product.

CN121491796BActive Publication Date: 2026-11-10DONGGUAN VILLO ENVIRONMENTAL PROTECTION INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202511963885.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-12-24
Publication Date
2026-11-10
Estimated Expiration
2045-12-24

AI Technical Summary

Technical Problem

Traditional ultrasonic dust removal head production methods suffer from serious material waste, high costs, low production efficiency, and difficulty in ensuring product consistency.

Method used

The ultrasonic dust removal head is manufactured by extrusion molding and its surface properties are improved by a two-step anodizing process, which includes the use of an anodizing bath solution with specific components and phosphoric acid intermediate treatment, combined with extrusion molding and a multi-step anodizing process.

Benefits of technology

It improves production efficiency and product consistency, while also enhancing the wear resistance and corrosion resistance of the ultrasonic dust removal head.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121491796B_ABST
    Figure CN121491796B_ABST
Patent Text Reader

Abstract

The application discloses an ultrasonic dust removal head manufactured by extrusion molding and a preparation method thereof, and belongs to the technical field of dust removal equipment manufacturing technology.The application comprises the following steps: S1, mold design and manufacturing: designing and manufacturing an extrusion mold with a corresponding cavity; S2, aluminum bar pretreatment: selecting a 6061 aluminum alloy bar, and performing heating and surface treatment; S3, extrusion molding: placing the pretreated aluminum bar in an extruder, and once extruding the aluminum bar into a profile with a continuous length through the extrusion mold; S4, precise cutting: performing high-precision cutting on the extruded profile to form a dust removal head monomer; and S5, subsequent finishing: performing necessary deburring, surface treatment and sonotrode assembly on the cut monomer.Through the above method, near-net forming of the ultrasonic dust removal head is realized, the production efficiency is improved, the manufacturing cost is reduced, and meanwhile, the consistency of product size precision and performance is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of dust removal equipment manufacturing technology, and particularly relates to an ultrasonic dust removal head manufactured by extrusion molding and its preparation method. Background Technology

[0002] The ultrasonic dust removal head is a core component of ultrasonic cleaning and dust removal equipment. Its function is to convert the high-frequency electrical signal generated by the ultrasonic generator into high-frequency mechanical vibration, and generate a strong cavitation effect in the medium (such as air or liquid), thereby achieving the purpose of removing dust and stains attached to the surface of the object.

[0003] Traditional ultrasonic dust collectors, especially those made of aluminum (such as 6061 aluminum alloy), are generally manufactured using either "integral machining" or "bar turning / milling" processes. Specifically, this involves purchasing a single aluminum alloy bar and then using CNC lathes, machining centers, and other equipment to perform numerous cutting, drilling, and milling processes to gradually remove excess material, ultimately forming a dust collector with a complex shape and internal structure.

[0004] However, this traditional machining method has the following significant drawbacks:

[0005] 1. Significant material waste and high costs: Machining is a "subtractive manufacturing" process, and a large amount of aluminum alloy material is wasted during the cutting process, turning into low-value metal chips, resulting in high material costs.

[0006] 2. Low production efficiency: Each dust collector head requires multiple independent processing steps, which takes a long time and makes it impossible to achieve rapid mass production, thus restricting production capacity.

[0007] 3. Difficulty in ensuring product consistency: Due to reliance on manual operation and multiple clamping, products processed by different batches and different operators vary in dimensional accuracy and surface finish, affecting the stability of product performance. Summary of the Invention

[0008] The purpose of this invention is to provide an ultrasonic dust removal head manufactured by extrusion molding, which aims to solve the technical problems of serious material waste, high cost, low production efficiency and difficulty in ensuring product consistency in the prior art.

[0009] To achieve the above objectives, the ultrasonic dust removal head manufactured by extrusion molding according to the embodiments of the present invention includes a dust removal head main shell and a positive pressure outer wall. Multiple sets of equidistantly distributed positive pressure pipes are fixedly connected to the upper end of the dust removal head main shell. The lower end of the positive pressure pipes is fixedly connected to the upper end of the positive pressure outer wall, and the positive pressure outer wall communicates with the positive pressure pipes. Multiple sets of equidistantly distributed negative pressure pipes are fixedly connected to the upper end of the dust removal head main shell. The negative pressure pipes and positive pressure pipes are staggered. Two sets of symmetrically distributed pressure collecting blocks are fixedly connected inside the positive pressure outer wall. A positive pressure head located at the lower end of the pressure collecting blocks is fixedly connected to the inner wall of the positive pressure outer wall. A negative pressure cavity is formed between the inner wall of the dust removal head main shell and the outer wall of the positive pressure outer wall. Two sets of symmetrically distributed negative pressure ports are opened between the lower end of the dust removal head main shell and the lower end of the positive pressure outer wall. A positive pressure cavity is formed between the inner wall of the positive pressure outer wall and the upper end of the pressure collecting blocks. A pressure collecting cavity is formed by the inner wall of the pressure collecting blocks. A positive pressure port is opened in the middle of the positive pressure head. An ultrasonic vibrator is installed inside the positive pressure pipe.

[0010] Before installing the ultrasonic vibrator, the ultrasonic dust removal head undergoes two steps of anodizing and phosphoric acid intermediate treatment. The anodizing bath solution A used in the first step of anodizing treatment includes the following components by weight: deionized water: 1000 parts, sulfuric acid: 160-190 parts, tartaric acid: 10-15 parts, succinic acid: 6-12 parts, nano alumina: 1-5 parts, dispersant: 1-3 parts, wetting agent: 0.1-0.5 parts.

[0011] The preparation process of the intermediate treatment solution used in the intermediate treatment of phosphoric acid is as follows: dissolve phosphoric acid in deionized water, add phytic acid and mix evenly, the amount of phytic acid added is 0.5-1.5% of the solution mass;

[0012] The anodizing bath solution B used in the second step of anodizing treatment includes the following components by weight: deionized water: 1000 parts, sulfuric acid: 150-180 parts, malic acid: 8-15 parts, sodium gluconate: 5-10 parts, aluminum sulfate: 15-25 parts, brightener: 0.5-2.0 parts, anti-chalking agent: 0.2-1.0 parts, acid mist inhibitor: 0.05-0.20 parts.

[0013] Furthermore, the opening of the positive pressure port is smaller than the opening of the negative pressure port.

[0014] Furthermore, the negative pressure pipe is connected to an external negative pressure generating device, and the positive pressure pipe is connected to an external blower.

[0015] To better achieve the objectives of this invention, this invention also provides a method for preparing an ultrasonic dust removal head manufactured by extrusion molding, comprising the following steps:

[0016] Step 1: Manufacture a mold according to the mechanism of the ultrasonic dust removal head;

[0017] Step 2: Preheat the raw materials;

[0018] Step 3: Extrude the preheated raw material into shape;

[0019] Step 4: The extruded profile is pulled to the cutting station for fixed-length cutting to obtain a single dust collector head blank.

[0020] Step 5: Perform a two-step anodizing process on the blank part:

[0021] (a) First step: Anodizing treatment

[0022] The blank is placed in anodizing bath A, which comprises the following components by weight:

[0023] Deionized water: 1000 parts, sulfuric acid: 160-190 parts, tartaric acid: 10-15 parts, succinic acid: 6-12 parts, nano alumina: 1-5 parts, dispersant: 1-3 parts, wetting agent: 0.1-0.5 parts;

[0024] (ii) Intermediate treatment of phosphoric acid

[0025] Phosphoric acid with a mass fraction of 85% is dissolved in deionized water at a volume ratio of 8-15% to obtain solution A. Phytic acid is added to solution A at a mass ratio of 0.5-1.5%. After mixing evenly, an intermediate treatment solution is obtained. The phosphoric acid intermediate treatment is carried out in the intermediate treatment solution. After the phosphoric acid intermediate treatment, the second step of anodizing treatment is carried out.

[0026] (III) Second step: Anodizing treatment:

[0027] The second step, anodizing, is carried out in anodizing bath B, which comprises the following components by weight: deionized water: 1000 parts, sulfuric acid: 150-180 parts, malic acid: 8-15 parts, sodium gluconate: 5-10 parts, aluminum sulfate: 15-25 parts, brightener: 0.5-2.0 parts, anti-chalking agent: 0.2-1.0 parts, and acid mist inhibitor: 0.05-0.20 parts.

[0028] The device is then washed with water, sealed with a nickel-free and fluorine-free sealing agent, and dried. Finally, an ultrasonic vibrator is installed at the positive pressure tube to obtain the ultrasonic dust removal head.

[0029] Furthermore, the specific process of step 2 is as follows:

[0030] Select a 6061 aluminum alloy round bar with a diameter of 80mm, place it in an induction heating furnace, and heat it to 420-480℃.

[0031] Furthermore, the specific process of the first step of anodizing is as follows:

[0032] The temperature is 5-15℃, the current density is 2.0-4.0A / dm2, the voltage is 40-60V, and the time is 40-80 minutes, eventually forming an oxide film with a thickness of 20-35 micrometers;

[0033] The dispersant used is ammonium polyacrylate, the wetting agent is acetylenic diol, and the particle size of the nano-alumina is 30-50nm.

[0034] Furthermore, the specific process of intermediate phosphoric acid processing is as follows:

[0035] The temperature is 30-45℃, the time is 10-25 minutes, and the stirring speed is 80-150 rpm.

[0036] Furthermore, the specific process of the second step, anodizing, is as follows:

[0037] The temperature is 18-25℃, the current density is 0.8-1.5A / dm2, the voltage is 8-16V, and the time is 15-30 minutes, eventually forming an oxide film with a thickness of 5-12 micrometers;

[0038] The brightener is made of high-grade fatty alcohol polyoxyethylene ether, the anti-chalking agent is made of polyvinyl alcohol, and the acid mist inhibitor is made of Span.

[0039] The ultrasonic dust removal head manufactured by extrusion molding according to the embodiments of the present invention has at least one of the following technical effects:

[0040] 1. By using extrusion molding, the production efficiency and product consistency of ultrasonic dust removal heads are improved;

[0041] 2. Through a multi-step anodizing process using a variety of acids, the wear resistance and corrosion resistance of the ultrasonic dust removal head surface are improved. Attached Figure Description

[0042] To more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0043] Figure 1 This is a process flow diagram of the ultrasonic dust removal head manufactured by extrusion molding according to the present invention.

[0044] Figure 2 The three-dimensional ultrasonic dust removal head manufactured by extrusion molding according to the present invention Figure 1 ;

[0045] Figure 3The three-dimensional ultrasonic dust removal head manufactured by extrusion molding according to the present invention Figure 2 ;

[0046] Figure 4 This is a front view of the ultrasonic dust removal head manufactured by extrusion molding according to the present invention;

[0047] Figure 5 For along Figure 2 A schematic diagram of the structure with part of it cut off in the AA direction.

[0048] The following are the labeling elements in the figure:

[0049] 11. Dust collector head main shell; 12. Negative pressure chamber; 13. Negative pressure port; 21. Positive pressure outer wall; 22. Pressure collecting block; 23. Positive pressure head; 24. Pressure collecting chamber; 25. Positive pressure chamber; 26. Positive pressure port; 3. Negative pressure pipe; 4. Positive pressure pipe. Detailed Implementation

[0050] Embodiments of the present invention are described in detail below. Examples of these embodiments are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the embodiments of the present invention, and should not be construed as limiting the present invention.

[0051] In the description of the embodiments of the present invention, it should be understood that the terms "length", "width", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the present invention.

[0052] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of embodiments of the present invention, "a plurality of" means two or more, unless otherwise explicitly specified.

[0053] In the embodiments of the present invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in the embodiments of the present invention according to the specific circumstances.

[0054] Example 1: The process flow diagram of the ultrasonic dust removal head is as follows. Figure 1 As shown, a method for preparing an ultrasonic dust removal head by extrusion molding includes the following specific steps:

[0055] 1. Mold design and manufacturing: based on Figures 2-5 The cross-sectional shape of the dust collector head was determined using CAD / CAM software, and an extrusion die was designed. The die cavity perfectly matches the cross-section of the dust collector head. The die material is high-strength heat-resistant die steel, and it is manufactured through precision machining and heat treatment.

[0056] 2. Raw material preparation and heating: Select 6061 aluminum alloy round bars with a diameter of 80mm, place them in an induction heating furnace, heat them to 420℃, and hold them at that temperature for 30 minutes to ensure uniform internal and external temperatures and achieve a good plastic state.

[0057] 3. Extrusion Molding: The heated aluminum rod is quickly transferred to a 2000-ton horizontal extrusion press. The extrusion press is started, and the extrusion bar pushes the aluminum rod through the die cavity at a constant speed. Under high temperature and pressure, the aluminum material undergoes plastic deformation and is "extruded" out of the die, forming a continuous aluminum alloy profile that perfectly matches the shape of the die cavity. This profile already possesses the basic shape of the dust collector head.

[0058] 4. Fixed-length cutting: The extruded profile is pulled to the cutting station and cut to a fixed length using a high-precision laser cutting machine according to the product drawing requirements (length is 150mm) to obtain a single dust collector head blank.

[0059] The cut end face is flat, and the dimensional tolerance is controlled within ±0.05mm.

[0060] 5. Follow-up processing:

[0061] (a) The blank is deburred, degreased, pickled and washed, and then subjected to two-step anodizing treatment.

[0062] (II) First step: Anodizing treatment:

[0063] The blank is placed in anodizing bath A, which comprises the following components by weight:

[0064] Deionized water: 1000 parts, sulfuric acid (98% by mass): 160 parts, tartaric acid: 15 parts, succinic acid: 6 parts, nano alumina (30nm): 5 parts, dispersant (ammonium polyacrylate): 1 part, wetting agent (acetylenic diol): 0.5 parts.

[0065] The process parameters for the first step of anodizing are as follows: temperature 5℃, current density 4.0A / dm³. 2 The voltage was 40V and the time was 80 minutes, which eventually formed an oxide film with a thickness of 20 micrometers.

[0066] (III) Intermediate treatment of phosphoric acid

[0067] After the first step of anodizing, the sample is washed with water, followed by intermediate phosphoric acid treatment. The intermediate phosphoric acid treatment is carried out in an intermediate treatment solution, and the preparation process of the intermediate treatment solution is as follows:

[0068] Phosphoric acid with a mass fraction of 85% was dissolved in deionized water at a volume ratio of 8% to obtain solution A. Phytic acid (1.5% of the solution mass) was added to solution A and mixed evenly to prepare the solution.

[0069] The process parameters for intermediate treatment of phosphoric acid are as follows: temperature is 30℃, time is 25 minutes, and stirring speed is 80 rpm.

[0070] After intermediate treatment with phosphoric acid, the mixture is washed with alkali and water, followed by a second step of anodizing.

[0071] (II) Second step: Anodizing treatment:

[0072] The second step, anodizing, is carried out in anodizing bath B, which comprises the following components by weight: deionized water: 1000 parts, sulfuric acid (98% by mass): 150 parts, malic acid: 15 parts, sodium gluconate: 5 parts, aluminum sulfate: 25 parts, brightener (high-grade fatty alcohol polyoxyethylene ether): 0.5 parts, anti-chalking agent (polyvinyl alcohol): 1.0 part, and acid mist inhibitor (Span): 0.05 parts.

[0073] The process parameters for the second step, anodizing, are as follows: temperature 18℃, current density 1.5A / dm³. 2 The voltage was 8V and the time was 30 minutes, which eventually formed an oxide film with a thickness of 5 micrometers.

[0074] The device is then washed with water, sealed with a nickel-free and fluorine-free sealing agent, and dried. Finally, an ultrasonic vibrator is installed at the positive pressure tube to obtain the ultrasonic dust removal head.

[0075] The specific structure of the ultrasonic dust removal head is as follows: In some embodiments, please refer to the accompanying drawings. Figures 2-5 An ultrasonic dust removal head manufactured by extrusion molding includes a dust removal head main shell 11 and a positive pressure outer wall 21. Multiple sets of equidistantly distributed positive pressure pipes 4 are fixedly connected to the upper end of the dust removal head main shell 11. The lower ends of the positive pressure pipes 4 are fixedly connected to the upper end of the positive pressure outer wall 21, and the positive pressure outer wall 21 communicates with the positive pressure pipes 4. Multiple sets of equidistantly distributed negative pressure pipes 3 are fixedly connected to the upper end of the dust removal head main shell 11. The negative pressure pipes 3 and positive pressure pipes 4 are staggered. Two sets of symmetrically distributed pressure collecting blocks 22 are fixedly connected inside the positive pressure outer wall 21. The positive pressure head 23 at the lower end of the block 22 is fixedly connected to the inner wall of the positive pressure outer wall 21. A negative pressure cavity 12 is formed between the inner wall of the dust collector head body shell 11 and the outer wall of the positive pressure outer wall 21. Two sets of negative pressure ports 13 are symmetrically distributed between the lower end of the dust collector head body shell 11 and the lower end of the positive pressure outer wall 21. A positive pressure cavity 25 is formed between the inner wall of the positive pressure outer wall 21 and the upper end of the pressure collecting block 22. A pressure collecting cavity 24 is formed between the inner wall of the pressure collecting block 22. A positive pressure port 26 is opened in the middle of the positive pressure head 23. The opening of the positive pressure port 26 is smaller than the opening of the negative pressure port 13.

[0076] The negative pressure pipe 3 is connected to an external negative pressure generating device, and the positive pressure pipe 4 is connected to an external blower. At the same time, an ultrasonic vibrator is installed in the positive pressure pipe 4. When the gas blown in by the blower passes through the positive pressure pipe 4 with the ultrasonic vibrator and reaches the positive pressure chamber 25 and the pressure collecting chamber 24 in sequence, and is blown out through the positive pressure port 26, the destructive power of the gas on the dust adhering to the surface can be further improved.

[0077] The ultrasonic vibrator is rigidly connected to the inner wall of the positive pressure pipe by means of flanges or threads and is strictly sealed to ensure that the vibration is effectively transmitted to the pipe wall and air passage, while preventing air leakage.

[0078] In this invention, clean air is blown into the positive pressure pipe 4 by a blower. The clean air is accelerated into the pressure collecting chamber 24 through the positive pressure chamber 25 and blown out through the positive pressure port 26. The blown gas can destroy the adhesion of dust on the part to be cleaned. At the same time, the external negative pressure generating device starts to work, and negative pressure adsorption force is generated in the negative pressure chamber 12. The blown dust is sucked into the negative pressure chamber 12 through the negative pressure port 13 and then discharged through the negative pressure pipe 3, thereby achieving the dust removal effect.

[0079] Example 2: A method for preparing an ultrasonic dust removal head by extrusion molding, the specific steps of which are as follows:

[0080] In the raw material preparation and heating process, 6061 aluminum alloy round bars with a diameter of 80mm are placed in an induction heating furnace, heated to 480℃, and held at that temperature for 30 minutes.

[0081] The specific steps for subsequent processing are as follows:

[0082] (a) The blank is deburred, degreased, pickled and washed, and then subjected to two-step anodizing treatment.

[0083] (II) First step: Anodizing treatment:

[0084] The blank is placed in anodizing bath A, which comprises the following components by weight:

[0085] Deionized water: 1000 parts, sulfuric acid (98% by mass): 190 parts, tartaric acid: 10 parts, succinic acid: 12 parts, nano alumina (50nm): 1 part, dispersant (ammonium polyacrylate): 3 parts, wetting agent (acetylenic diol): 0.1 parts.

[0086] The process parameters for the first step of anodizing are as follows: temperature 15℃, current density 2.0A / dm³. 2 The voltage was 60V and the time was 40 minutes, which eventually formed an oxide film with a thickness of 35 micrometers.

[0087] (III) Intermediate treatment of phosphoric acid

[0088] After the first step of anodizing, the sample is washed with water, followed by intermediate phosphoric acid treatment. The intermediate phosphoric acid treatment is carried out in an intermediate treatment solution, and the preparation process of the intermediate treatment solution is as follows:

[0089] Phosphoric acid with a mass fraction of 85% was dissolved in deionized water at a volume ratio of 15% to obtain solution A. Phytic acid (0.5% of the solution mass) was added to solution A and mixed evenly to prepare the solution.

[0090] The process parameters for intermediate treatment of phosphoric acid are as follows: temperature is 45℃, time is 10 minutes, and stirring speed is 150 rpm.

[0091] After intermediate treatment with phosphoric acid, the mixture is washed with alkali and water, followed by a second step of anodizing.

[0092] (II) Second step: Anodizing treatment:

[0093] The second step, anodizing, is carried out in anodizing bath B, which comprises the following components by weight: deionized water: 1000 parts, sulfuric acid (98% by mass): 180 parts, malic acid: 8 parts, sodium gluconate: 10 parts, aluminum sulfate: 15 parts, brightener (high-grade fatty alcohol polyoxyethylene ether): 2.0 parts, anti-chalking agent (polyvinyl alcohol): 0.2 parts, and acid mist inhibitor (Span): 0.20 parts.

[0094] The process parameters for the second step, anodizing, are as follows: temperature 25℃, current density 0.8A / dm³. 2The voltage was 16V and the time was 15 minutes, which eventually formed an oxide film with a thickness of 12 micrometers.

[0095] The remaining steps are the same as in Example 1.

[0096] Example 3: A method for preparing an ultrasonic dust removal head by extrusion molding, the specific steps of which are as follows:

[0097] In the raw material preparation and heating process, 6061 aluminum alloy round bars with a diameter of 80mm are placed in an induction heating furnace, heated to 450℃, and held at that temperature for 30 minutes.

[0098] The specific steps for subsequent processing are as follows:

[0099] (a) The blank is deburred, degreased, pickled and washed, and then subjected to two-step anodizing treatment.

[0100] (II) First step: Anodizing treatment:

[0101] The blank is placed in anodizing bath A, which comprises the following components by weight:

[0102] Deionized water: 1000 parts, sulfuric acid (98% by mass): 180 parts, tartaric acid: 12 parts, succinic acid: 10 parts, nano alumina (40nm): 3 parts, dispersant (ammonium polyacrylate): 2 parts, wetting agent (acetylenic diol): 0.3 parts.

[0103] The process parameters for the first step of anodizing are as follows: temperature 12℃, current density 3.5A / dm³. 2 The voltage was 50V and the time was 60 minutes, which eventually formed an oxide film with a thickness of 25 micrometers.

[0104] (III) Intermediate treatment of phosphoric acid

[0105] After the first step of anodizing, the sample is washed with water, followed by intermediate phosphoric acid treatment. The intermediate phosphoric acid treatment is carried out in an intermediate treatment solution, and the preparation process of the intermediate treatment solution is as follows:

[0106] Phosphoric acid with a mass fraction of 85% was dissolved in deionized water at a volume ratio of 10% to obtain solution A. Phytic acid (1% of the solution mass) was added to solution A and mixed evenly to prepare the solution.

[0107] The process parameters for intermediate treatment of phosphoric acid are as follows: temperature is 37℃, time is 18 minutes, and stirring speed is 100 rpm.

[0108] After intermediate treatment with phosphoric acid, the mixture is washed with alkali and water, followed by a second step of anodizing.

[0109] (II) Second step: Anodizing treatment:

[0110] The second step, anodizing, is carried out in anodizing bath B, which comprises the following components by weight: deionized water: 1000 parts, sulfuric acid (98% by mass): 160 parts, malic acid: 12 parts, sodium gluconate: 8 parts, aluminum sulfate: 20 parts, brightener (high-grade fatty alcohol polyoxyethylene ether): 1 part, anti-chalking agent (polyvinyl alcohol): 0.5 parts, and acid mist inhibitor (Span): 0.1 parts.

[0111] The process parameters for the second step, anodizing, are as follows: temperature 22℃, current density 1.2A / dm³. 2 The voltage was 14V and the time was 23 minutes, which eventually formed an oxide film with a thickness of 7 micrometers.

[0112] The remaining steps are the same as in Example 1.

[0113] Comparative Example 1:

[0114] Using the preparation method of Example 1, the production data of 100 products with a width of 1600mm were statistically analyzed and compared with traditional machining methods. The results are shown in the table.

[0115] Table 1. Cost Comparison of Extrusion Demolding and Pure Machining

[0116] Molding process pure machining Extrusion molding Product width (mm) 1600 1600 Quantity of products (units) 100 100 Product weight (kg / piece) 82.8 25 Price per unit of material 6061 (kg / piece) 21 21 Total processing time (h) 4.5 0.5 Comprehensive processing unit price (RMB / hour) 280 200 Demolding time (h) 0 0.05 Mold production unit price (RMB / hour) 0 30 Mold cost (RMB) 0 25000 Total cost (RMB) 299880 90500.05 Cost reduction rate (%) - 69.82

[0117] As shown in Table 1, using extrusion molding to manufacture ultrasonic dust removal heads reduces the cost of a single piece of material from RMB 2998.8 per piece (machined) to RMB 905 per piece. Simultaneously, the processing time per piece decreases from 4.5 hours per piece (machined) to 0.55 hours per piece (including cutting). Overall, the comprehensive manufacturing cost is reduced by approximately 69.82%. Furthermore, in terms of product consistency, the CPK (process capability index) of critical dimensions for batch products increases from 1.2 to over 1.8. Therefore, using extrusion molding to manufacture ultrasonic dust removal heads significantly improves both production costs and product quality compared to traditional machining methods.

[0118] Comparative Example 2: Compared with Example 3, the difference is that tartaric acid and succinic acid were not added to the anodizing bath solution A, and the nano alumina was replaced with an equal mass of aluminum sulfate.

[0119] Comparative Example 3: Compared with Example 3, the difference is that phytic acid is not added to the intermediate treatment solution, and malic acid and sodium gluconate are not added to the anodizing bath solution B. The amount of sulfuric acid is changed to 170 parts.

[0120] Comparative Example 4: Compared with Example 3, the difference is that tartaric acid and succinic acid are not added to the anodizing bath solution A, and the nano alumina is replaced with an equal mass of aluminum sulfate; in addition, phytic acid is not added to the intermediate treatment solution, and malic acid and sodium gluconate are not added to the anodizing bath solution B, and the amount of sulfuric acid is changed to 170 parts.

[0121] Experimental example:

[0122] The wear resistance and corrosion resistance of the ultrasonic dust removal heads prepared in Examples 1-3 and Comparative Examples 2-4 were tested.

[0123] Wear resistance test: The wear rate was calculated according to GB / T 12967.1-2020;

[0124] Corrosion resistance testing: The potentiodynamic polarization curve was measured using the traditional three-electrode method, with the potential scan rate set to 1 mV / s, and corrosion tests were conducted.

[0125] Table 2 Test results of wear resistance and corrosion resistance

[0126] project <![CDATA[Wear rate (mm 3 / Nm)]]> Corrosion potential (mV) <![CDATA[Corrosion current (µA / cm 2 )]]> Example 1 <![CDATA[2.2×10 -4 ]]> -563 1.21 Example 2 <![CDATA[2.5×10 -4 ]]> -567 1.18 Example 3 <![CDATA[1.9×10 -4 ]]> -559 1.12 Comparative Example 2 <![CDATA[8.9×10 -4 ]]> -671 2.10 Comparative Example 3 <![CDATA[9.2×10 -4 ]]> -689 2.13 Comparative Example 4 <![CDATA[5.0×10 -3 ]]> -858 3.01

[0127] As can be seen from Comparative Example 2 and Example 3, if tartaric acid and succinic acid are not added to the anodizing bath solution A, and the nano-alumina is replaced with an equal mass of aluminum sulfate, the wear resistance and corrosion resistance of the prepared ultrasonic dust removal head will decrease.

[0128] As can be seen from Comparative Example 3 and Example 3, if phytic acid is not added to the intermediate treatment solution, and malic acid and sodium gluconate are not added to the anodizing bath solution B, and the amount of sulfuric acid is changed to 170 parts, the wear resistance and corrosion resistance of the prepared ultrasonic dust removal head will decrease.

[0129] As can be seen from Comparative Example 4 and Example 3, the components of anodic oxidation bath solution A, intermediate treatment solution and anodic oxidation bath solution B, as well as the secondary anodic oxidation treatment, have a synergistic effect on the wear rate and corrosion potential of the prepared ultrasonic dust removal head.

[0130] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. An ultrasonic dust removal head manufactured by extrusion molding, comprising a dust removal head main body shell and a positive pressure outer wall, characterized in that: Multiple sets of equidistantly distributed positive pressure pipes are fixedly connected to the upper end of the dust collector head's main shell. The lower end of the positive pressure pipe is fixedly connected to the upper end of the positive pressure outer wall, and the positive pressure outer wall communicates with the positive pressure pipe. Multiple sets of equidistantly distributed negative pressure pipes are fixedly connected to the upper end of the dust collector head's main shell. The negative pressure pipes and positive pressure pipes are staggered. Two sets of symmetrically distributed pressure collecting blocks are fixedly connected inside the positive pressure outer wall. The positive pressure head located at the lower end of the pressure collecting block is fixedly connected to the inner wall of the positive pressure outer wall. A negative pressure cavity is formed between the inner wall of the dust collector head's main shell and the outer wall of the positive pressure outer wall. Two sets of symmetrically distributed negative pressure ports are opened between the lower end of the dust collector head's main shell and the lower end of the positive pressure outer wall. The inner wall of the positive pressure outer wall and the upper end of the pressure collecting block form a positive pressure cavity. The inner wall of the pressure collecting block forms a pressure collecting cavity. A positive pressure port is opened in the middle of the positive pressure head. An ultrasonic vibrator is installed inside the positive pressure pipe. Before installing the ultrasonic vibrator, the ultrasonic dust removal head undergoes two steps of anodizing and phosphoric acid intermediate treatment. The anodizing bath solution A used in the first step of anodizing treatment includes the following components by weight: deionized water: 1000 parts, sulfuric acid: 160-190 parts, tartaric acid: 10-15 parts, succinic acid: 6-12 parts, nano alumina: 1-5 parts, dispersant: 1-3 parts, wetting agent: 0.1-0.5 parts. The preparation process of the intermediate treatment solution used in the intermediate treatment of phosphoric acid is as follows: dissolve phosphoric acid in deionized water, add phytic acid and mix evenly, the amount of phytic acid added is 0.5-1.5% of the solution mass; The anodizing bath solution B used in the second step of anodizing treatment includes the following components by weight: deionized water: 1000 parts, sulfuric acid: 150-180 parts, malic acid: 8-15 parts, sodium gluconate: 5-10 parts, aluminum sulfate: 15-25 parts, brightener: 0.5-2.0 parts, anti-chalking agent: 0.2-1.0 parts, acid mist inhibitor: 0.05-0.20 parts.

2. The ultrasonic dust removal head manufactured by extrusion molding according to claim 1, characterized in that, The opening of the positive pressure port is smaller than the opening of the negative pressure port.

3. The ultrasonic dust removal head manufactured by extrusion molding according to claim 1, characterized in that, The negative pressure pipe is connected to an external negative pressure generating device, and the positive pressure pipe is connected to an external blower.

4. A method for preparing an ultrasonic dust removal head manufactured by extrusion molding according to any one of claims 1-3, characterized in that, Includes the following steps: Step 1: Manufacture a mold according to the mechanism of the ultrasonic dust removal head; Step 2: Preheat the raw materials; Step 3: Extrude the preheated raw material into shape; Step 4: The extruded profile is pulled to the cutting station for fixed-length cutting to obtain a single dust collector head blank. Step 5: Perform a two-step anodizing process on the blank part: (a) First step: Anodizing treatment The blank is placed in anodizing bath A, which comprises the following components by weight: Deionized water: 1000 parts, sulfuric acid: 160-190 parts, tartaric acid: 10-15 parts, succinic acid: 6-12 parts, nano alumina: 1-5 parts, dispersant: 1-3 parts, wetting agent: 0.1-0.5 parts; (ii) Intermediate treatment of phosphoric acid Phosphoric acid with a mass fraction of 85% is dissolved in deionized water at a volume ratio of 8-15% to obtain solution A. Phytic acid is added to solution A at a mass ratio of 0.5-1.5%. After mixing evenly, an intermediate treatment solution is obtained. The phosphoric acid intermediate treatment is carried out in the intermediate treatment solution. After the phosphoric acid intermediate treatment, the second step of anodizing treatment is carried out. (III) Second step: Anodizing treatment: The second step, anodizing, is carried out in anodizing bath B, which comprises the following components by weight: deionized water: 1000 parts, sulfuric acid: 150-180 parts, malic acid: 8-15 parts, sodium gluconate: 5-10 parts, aluminum sulfate: 15-25 parts, brightener: 0.5-2.0 parts, anti-chalking agent: 0.2-1.0 parts, and acid mist inhibitor: 0.05-0.20 parts. The device is then washed with water, sealed with a nickel-free and fluorine-free sealing agent, and dried. Finally, an ultrasonic vibrator is installed at the positive pressure tube to obtain the ultrasonic dust removal head.

5. The method for preparing the ultrasonic dust removal head by extrusion molding according to claim 4, characterized in that, The specific process of step 2 is as follows: Select a 6061 aluminum alloy round bar with a diameter of 80mm, place it in an induction heating furnace, and heat it to 420-480℃.

6. The method for preparing the ultrasonic dust removal head by extrusion molding according to claim 4, characterized in that, The specific process of the first step of anodizing is as follows: The temperature is 5-15℃, the current density is 2.0-4.0A / dm2, the voltage is 40-60V, and the time is 40-80 minutes, eventually forming an oxide film with a thickness of 20-35 micrometers; The dispersant used is ammonium polyacrylate, the wetting agent is acetylenic diol, and the particle size of the nano-alumina is 30-50nm.

7. The method for preparing the ultrasonic dust removal head by extrusion molding according to claim 4, characterized in that, The specific process of intermediate phosphoric acid processing is as follows: The temperature is 30-45℃, the time is 10-25 minutes, and the stirring speed is 80-150 rpm.

8. The method for preparing the ultrasonic dust removal head by extrusion molding according to claim 4, characterized in that, The specific process of the second step, anodizing, is as follows: The temperature is 18-25℃, the current density is 0.8-1.5A / dm2, the voltage is 8-16V, and the time is 15-30 minutes, eventually forming an oxide film with a thickness of 5-12 micrometers; The brightener is made of high-grade fatty alcohol polyoxyethylene ether, the anti-chalking agent is made of polyvinyl alcohol, and the acid mist inhibitor is made of Span.

Citation Information

Patent Citations

  • Aluminum profile anodic oxidation process applied to photovoltaic frame

    CN114214698A

  • Special-shaped end frame and forming method thereof

    CN114226969A