A polyamide / polyphenylene ether alloy material and its manufacturing method
By introducing a core-shell structured silicone-coated aluminum diethylphosphinate flame retardant and gamma-ray pre-irradiation treatment into polyamide/polyphenylene ether alloy materials, combined with tetra-needle zinc oxide whiskers and CTI synergist, the flame retardancy and insulation problems of ultra-thin materials are solved, ensuring long-term performance stability and insulation reliability under high voltage conditions.
Patent Information
- Application Number
- CN202512027037.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-29
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-12-29
AI Technical Summary
Existing polyamide/polyphenylene ether alloy materials cannot simultaneously meet the requirements of UL94 V-0 flame retardancy, CTI≥700V high insulation, low precipitation (<0.1%) and high performance retention (>90%) after long-term damp heat aging, even at an ultra-thin thickness of 0.6mm. Furthermore, they suffer from problems such as flame retardant migration and poor interfacial compatibility.
A core-shell structure silicone-coated aluminum diethylphosphinic acid flame retardant, gamma-ray pre-irradiated polyphenylene ether resin, and maleic anhydride-grafted high-impact polystyrene compatibilizer are combined with tetra-needle zinc oxide whiskers and CTI synergist. Through gamma-ray irradiation treatment and vacuum drying, extrusion, and vacuum annealing processes, the interfacial compatibility and physical isolation effect of the flame retardant are improved.
It achieves UL94 V-0 flame retardancy at a thickness of 0.6mm, with a CTI value as high as 735V. After long-term damp heat aging, the CTI retention rate is >90%, the exudate content is <0.05%, and the material has high performance stability, making it suitable for high-voltage electrical insulation components.
Smart Images

Figure CN121574550B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of high-performance engineering plastics technology, and in particular to a polyamide / polyphenylene ether alloy material and its manufacturing method. Background Technology
[0002] Polyamide / polyphenylene oxide alloys (PA / PPO alloys) are considered ideal materials for high-voltage electrical insulation components due to their excellent mechanical properties, heat resistance, and electrical insulation.
[0003] However, traditional high glass fiber reinforced PA / PPO alloy materials present an inherent contradiction in achieving high flame retardancy (UL94 V-0) and high tracking index (CTI≥600V): Achieving UL94 V-0 requires the addition of large amounts of flame retardants, which (especially phosphorus-nitrogen based ones) are prone to migration and precipitation, leading to a severe decrease in CTI value. As described in patent CN114085522A, the CTI is typically only 200-400V. Existing similar solutions mostly focus on optimizing flame retardant formulations or adding special fillers. For example, while adding aniline black material in patent CN119899522A improves CTI, aniline black material is an organic pigment that is easily precipitated after high-temperature and high-humidity aging. In patent CN118546524A, the strength retention rate is >70% after aging at 130℃ for 1500 hours, but damp heat aging only assesses the material's appearance and cannot guarantee the retention rate of CTI and other properties, thus failing to meet long-term reliability requirements.
[0004] In summary, the shortcomings of existing technologies can be mainly attributed to three points:
[0005] 1. Flame retardant migration and precipitation: Traditional small molecule phosphorus and bromine-based flame retardants have poor compatibility with polymer matrices and are prone to migrate to the material surface under high temperature and high humidity environments. This not only leads to the deterioration of electrical properties such as CTI, but may also corrode precision electronic components.
[0006] 2. The contradiction between ultra-thin and high flame retardancy: When the material thickness is reduced to below 0.8mm, the difficulty of maintaining V-0 flame retardancy increases dramatically. Usually, the amount of flame retardant used needs to be greatly increased, which in turn aggravates the precipitation problem and damages mechanical properties.
[0007] 3. Poor interfacial compatibility: PA and PPO are thermodynamically incompatible systems. Poor compatibility at high filler levels leads to phase separation, resulting in stress concentration, decreased impact strength, and reduced flame retardant efficiency. The root cause of these drawbacks lies in the failure to innovatively design the flame retardant structure to prevent migration and the lack of effective means to simultaneously improve the interfacial compatibility of multiple components.
[0008] The challenge in solving these problems lies in finding a comprehensive solution that can simultaneously encapsulate flame retardants, reduce flame retardant exudation, improve the compatibilization interface, and enhance CTI without significantly increasing costs. Summary of the Invention
[0009] This invention discloses a polyamide / polyphenylene ether alloy material and its manufacturing method, which solves the technical problem that existing polyamide / polyphenylene ether alloy materials cannot simultaneously meet the requirements of UL94 V-0 flame retardancy, CTI≥700V high insulation, low precipitation (<0.1%) and high performance retention rate (>90%) after long-term damp heat aging, with an ultra-thin thickness of 0.6mm.
[0010] The present invention provides a polyamide / polyphenylene ether alloy material, which comprises the following components by weight:
[0011] 55-75 parts of polyamide 66 resin;
[0012] 25-45 parts of polyphenylene ether resin pre-irradiated with gamma rays;
[0013] 10-20 parts of core-shell structured silicone-coated aluminum diethylphosphinic acid flame retardant;
[0014] 5-10 parts of maleic anhydride grafted high-impact polystyrene compatibilizer pre-irradiated with gamma rays; 20-30 parts of hydrolysis-resistant glass fiber with surface treated with silane coupling agent.
[0015] 3-8 parts of tetrane-shaped zinc oxide whiskers;
[0016] CTI synergist 2-5 parts;
[0017] 1-2 parts of anti-precipitation agent.
[0018] Optionally, the polyphenylene ether resin pre-irradiated with gamma rays is specifically a polyphenylene ether resin pre-irradiated with gamma rays at a dose of 0.5-1.2 mgy.
[0019] Optionally, the maleic anhydride-grafted high-impact polystyrene compatibilizer pre-irradiated with gamma rays is specifically a maleic anhydride-grafted high-impact polystyrene compatibilizer pre-irradiated with gamma rays at a dose of 0.5-1.2 mgy.
[0020] Optionally, the core-shell structured silicone-coated aluminum diethylphosphinate flame retardant specifically uses aluminum diethylphosphinate as the core and fumed silica as the shell.
[0021] The shell thickness is 100-200 nm, and the coverage rate is ≥95%.
[0022] Optionally, the CTI synergist is linear low-density polyethylene-g-acrylic acid.
[0023] Optionally, the anti-exudant is a hyperbranched polyester amide.
[0024] The present invention provides a method for manufacturing a polyamide / polyphenylene ether alloy material, comprising the following steps:
[0025] Irradiation treatment: Polyphenylene ether resin and maleic anhydride-grafted high-impact polystyrene compatibilizer were respectively irradiated with γ-rays at doses of 0.5-1.2 mgy;
[0026] Vacuum drying: The polyamide 66 resin is vacuum dried at a first preset temperature until the moisture content is ≤500ppm;
[0027] Mixing and Extrusion: The dried polyamide 66 resin, gamma-ray pre-irradiated polyphenylene ether resin, core-shell silicone-coated aluminum diethylphosphinate flame retardant, gamma-ray pre-irradiated maleic anhydride-grafted high-impact polystyrene compatibilizer, CTI synergist, and anti-exudation agent are mixed at high speed; then the mixture is fed into the extruder through the main feed port, and hydrolysis-resistant glass fibers and tetra-needle zinc oxide whiskers with silane coupling agent surface treatment are added through the side feed port; after melt blending, extrusion, water cooling, and pelletizing, the composite material is obtained;
[0028] Vacuum annealing: The composite material is treated in a vacuum environment at a second preset temperature for a first preset time to obtain a polyamide / polyphenylene ether alloy material.
[0029] Optionally, in the mixing and extrusion steps, the extruder is a twin-screw extruder, wherein the twin-screw extruder adopts a three-stage variable diameter screw and zone temperature control: zone one temperature is 215-225℃, zone two temperature is 250-260℃, and zone three temperature is 235-245℃.
[0030] Optionally, in the vacuum drying step, the first preset temperature is 100-130℃.
[0031] Optionally, in the vacuum annealing step, the second preset temperature is 100-130℃, and the first preset time is 3-5 hours.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The polyamide / polyphenylene ether alloy material of the present invention comprises, by weight, the following components: 55-75 parts of polyamide 66 resin; 25-45 parts of polyphenylene ether resin pre-irradiated with gamma rays; 10-20 parts of core-shell structured silicone-coated aluminum diethylphosphinic acid flame retardant; 5-10 parts of maleic anhydride-grafted high-impact polystyrene compatibilizer pre-irradiated with gamma rays; 20-30 parts of hydrolysis-resistant glass fiber with a surface treated with a silane coupling agent; 3-8 parts of tetraneedle-shaped zinc oxide whiskers; 2-5 parts of CTI synergist; and 1-2 parts of anti-exudation agent.
[0034] In the above design, the core-shell structure silicone-coated aluminum diethylphosphinate flame retardant fundamentally and physically blocks the migration and precipitation of the flame retardant. The pre-irradiated polyphenylene ether resin and the pre-irradiated maleic anhydride-grafted high-impact polystyrene compatibilizer generate active free radicals on their molecular chains, greatly improving interfacial compatibility and grafting efficiency during subsequent melt blending. The whisker charge traps constructed by the tetra-needle zinc oxide whiskers and the CTI enhancer effectively improve CTI. The anti-precipitation agent enhances the long-term reliability of the alloy material, effectively inhibiting changes in the internal structure of the material over time due to small molecule migration, maintaining the mechanical property stability of the alloy, and extending the service life of the product.
[0035] Through the above design, the polyamide / polyphenylene ether alloy material of the present invention has the following advantages:
[0036] Ultra-thin and highly flame-retardant: Polyamide / polyphenylene ether alloy material that can pass UL94 V-0 certification at a thickness of 0.6mm makes lightweight component design possible;
[0037] Ultra-high insulation reliability: The CTI value is as high as 735V, and after 1000 hours of humid heat aging at 85℃ / 85%RH, the CTI retention rate is >90% and the exudate content is <0.05%, completely eliminating the risk of insulation failure under high voltage.
[0038] Green and long-lasting performance: halogen-free flame retardant, non-corrosive, with extremely low performance degradation throughout the material's lifespan, ensuring the safety of the battery system throughout its entire life cycle.
[0039] In summary, this polyamide / polyphenylene oxide alloy material can effectively solve the technical problems of existing polyamide / polyphenylene oxide alloy materials being unable to simultaneously meet the requirements of UL94 V-0 flame retardancy, CTI≥700V high insulation, and low precipitation (<0.1%) and high performance retention (>90%) after long-term damp heat aging, with an ultra-thin thickness of 0.6mm. Attached Figure Description
[0040] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0041] Figure 1 A flowchart illustrating a method for manufacturing a polyamide / polyphenylene ether alloy material provided by the present invention. Detailed Implementation
[0042] This invention discloses a polyamide / polyphenylene ether alloy material and its manufacturing method, which solves the technical problem that existing polyamide / polyphenylene ether alloy materials cannot simultaneously meet the requirements of UL94 V-0 flame retardancy, CTI≥700V high insulation, low precipitation (<0.1%) and high performance retention rate (>90%) after long-term damp heat aging, with an ultra-thin thickness of 0.6mm.
[0043] To enable those skilled in the art to better understand the present invention, the invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. Obviously, the described embodiments are merely some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0044] On the one hand, the polyamide / polyphenylene ether alloy material provided by the present invention comprises the following components by mass:
[0045] 55-75 parts of polyamide 66 resin;
[0046] 25-45 parts of polyphenylene ether resin pre-irradiated with gamma rays;
[0047] 10-20 parts of core-shell structured silicone-coated aluminum diethylphosphinic acid flame retardant;
[0048] 5-10 parts of maleic anhydride-grafted high-impact polystyrene compatibilizer pre-irradiated with gamma rays;
[0049] 20-30 parts of hydrolysis-resistant glass fiber with surface treated with silane coupling agent;
[0050] 3-8 parts of tetrane-shaped zinc oxide whiskers;
[0051] CTI synergist 2-5 parts;
[0052] 1-2 parts of anti-precipitation agent.
[0053] It should be noted that the viscosity of the polyamide 66 resin mentioned above is 2.4-2.7 Pa·s, and it can be sourced from the manufacturer Pingdingshan Shenma. The dosage can be 55 parts, 56 parts, 60 parts, 70 parts, or 75 parts.
[0054] The polyphenylene ether resin mentioned above has a weight-average molecular weight Mw=50,000 and can be sourced from the manufacturer Lanxing Group. Its dosage can be 25 parts, 28 parts, 30 parts, 40 parts, or 45 parts.
[0055] The amount of core-shell structured silicone-coated aluminum diethylphosphinic acid flame retardant can be 10 parts, 15 parts, 18 parts, or 20 parts.
[0056] The amount of maleic anhydride-grafted high-impact polystyrene compatibilizer can be 5 parts, 6 parts, 8 parts, or 10 parts.
[0057] Hydrolysis-resistant glass fiber with surface treated with silane coupling agent, specifically, hydrolysis-resistant glass fiber treated with silane coupling agent, wherein the glass fiber can be sourced from the manufacturer Jushi Group, and the amount used can be 20 parts, 22 parts, 25 parts, 28 parts, or 30 parts.
[0058] Four needle-like zinc oxide whiskers, with a length of 10-50μm, can be sourced from the manufacturer Tianyou Jingchuang, and the dosage can be 3 parts, 5 parts, 6 parts, or 8 parts.
[0059] CTI synergist enhances the surface resistance to electro-tracking in polyamide / polyphenylene ether alloys, ensuring their long-term safety and reliability in harsh electrical environments. Specifically, linear low-density polyethylene-g-acrylic acid can be selected, with an acrylic acid grafting rate of 1.0%, sourced from Dow Chemical, and the dosage can be 2 parts, 3 parts, or 5 parts.
[0060] Anti-precipitation agents can enhance the long-term reliability of alloy materials, effectively inhibiting changes in the internal structure of the material over time caused by the migration of small molecules, maintaining the mechanical property stability of the alloy, and extending the service life of the product. Specifically, hyperbranched polyesteramide, sourced from Weihai Chenyuan, can be used in dosages of 1 part, 1.2 parts, 1.5 parts, or 2 parts.
[0061] In the above design, the core-shell structure silicone-coated aluminum diethylphosphinate flame retardant fundamentally and physically blocks the migration and precipitation of the flame retardant. The pre-irradiated polyphenylene ether resin and the pre-irradiated maleic anhydride-grafted high-impact polystyrene compatibilizer generate active free radicals on their molecular chains, greatly improving interfacial compatibility and grafting efficiency during subsequent melt blending. The whisker charge traps constructed by the tetra-needle zinc oxide whiskers and the CTI enhancer effectively improve CTI. The anti-precipitation agent enhances the long-term reliability of the alloy material, effectively inhibiting changes in the internal structure of the material over time due to small molecule migration, maintaining the mechanical property stability of the alloy, and extending the service life of the product.
[0062] Through the above design, the polyamide / polyphenylene ether alloy material of the present invention has the following advantages:
[0063] Ultra-thin and highly flame-retardant: Polyamide / polyphenylene ether alloy material that can pass UL94 V-0 certification at a thickness of 0.6mm makes lightweight component design possible;
[0064] Ultra-high insulation reliability: The CTI value is as high as 735V, and after 1000 hours of humid heat aging at 85℃ / 85%RH, the CTI retention rate is >90% and the exudate content is <0.05%, completely eliminating the risk of insulation failure under high voltage.
[0065] Green and long-lasting performance: halogen-free flame retardant, non-corrosive, with extremely low performance degradation throughout the material's lifespan, ensuring the safety of the battery system throughout its entire life cycle.
[0066] In summary, this polyamide / polyphenylene oxide alloy material can effectively solve the technical problems of existing polyamide / polyphenylene oxide alloy materials being unable to simultaneously meet the requirements of UL94 V-0 flame retardancy, CTI≥700V high insulation, and low precipitation (<0.1%) and high performance retention (>90%) after long-term damp heat aging, with an ultra-thin thickness of 0.6mm.
[0067] Furthermore, in this embodiment, the polyphenylene ether resin pre-irradiated with gamma rays is specifically polyphenylene ether resin pre-irradiated with gamma rays at a dose of 0.5-1.2 mgy.
[0068] It should be noted that the polyphenylene ether resin pre-irradiated with gamma rays generates active free radicals on its molecular chain, which greatly improves the interfacial compatibility and grafting efficiency during subsequent melt blending. The gamma ray dose can be 0.5 mgy, 1.0 mgy, 1.1 mgy, etc., and this embodiment does not impose any limitations on this.
[0069] Furthermore, in this embodiment, the maleic anhydride-grafted high-impact polystyrene compatibilizer pre-irradiated with gamma rays is specifically a maleic anhydride-grafted high-impact polystyrene compatibilizer pre-irradiated with gamma rays at a dose of 0.5-1.2 MGy.
[0070] It should be noted that the maleic anhydride-grafted high-impact polystyrene compatibilizer, pre-irradiated with gamma rays, generates active free radicals on its molecular chain, which greatly improves the interfacial compatibility and grafting efficiency during subsequent melt blending. The gamma ray dose can be 0.5 mgy, 1.0 mgy, 1.1 mgy, etc., and this embodiment does not impose any limitations on this.
[0071] Furthermore, in this embodiment, the core-shell structure silicone-coated aluminum diethylphosphinate flame retardant specifically uses aluminum diethylphosphinate as the core and fumed silica as the shell.
[0072] The shell thickness is 100-200nm, specifically 100nm, 130nm, 160nm, 200nm, etc., with a coverage rate of ≥95%.
[0073] It should be noted that, through the above design, fumed silica acts as a shell to encapsulate the aluminum diethylphosphinate core, fundamentally physically blocking the migration and precipitation of flame retardants, ensuring that the subsequent polyamide / polyphenylene ether alloy material has high flame retardant performance, enabling the alloy material to meet the UL94 V-0 flame retardant rating.
[0074] Please see Figure 1Secondly, the present invention provides a method for manufacturing a polyamide / polyphenylene ether alloy material, comprising the following steps:
[0075] S1. Irradiation treatment: Polyphenylene ether resin and maleic anhydride-grafted high-impact polystyrene compatibilizer are respectively irradiated with γ-rays at a dose of 0.5-1.2 mgy;
[0076] S2. Vacuum drying: Vacuum dry the polyamide 66 resin at 100-130℃ until the moisture content is ≤500ppm;
[0077] S3. Mixing and Extrusion: The dried polyamide 66 resin, gamma-ray pre-irradiated polyphenylene ether resin, core-shell silicone-coated aluminum diethylphosphinate flame retardant, gamma-ray pre-irradiated maleic anhydride-grafted high-impact polystyrene compatibilizer, CTI synergist, and anti-exudation agent are mixed at high speed; then the mixture is added to the extruder through the main feed port, and hydrolysis-resistant glass fibers and tetra-needle zinc oxide whiskers with silane coupling agent surface treatment are added through the side feed port; after melt blending, extrusion, water cooling, and pelletizing, the composite material is obtained.
[0078] S4. Vacuum annealing: The composite material is treated in a vacuum environment at 100-130℃ for a first preset time of 3-5 hours to obtain a polyamide / polyphenylene ether alloy material.
[0079] Specifically, in the mixing and extrusion steps, the extruder is a twin-screw extruder, wherein the twin-screw extruder employs a three-stage variable diameter screw with zoned temperature control: zone one temperature is 215-225℃ (which can be 215℃, 220℃, 223℃, 225℃, etc.), zone two temperature is 250-260℃ (which can be 251℃, 252℃, 256℃, 260℃, etc.), and zone three temperature is 235-245℃ (which can be 235℃, 240℃, 242℃, 245℃, etc.).
[0080] It should be noted that in the aforementioned vacuum annealing process, internal stress is eliminated through thermal relaxation, phase structure is optimized, and volatiles are removed, thereby improving the dimensional stability, mechanical properties, and long-term reliability of the polyamide / polyphenylene ether alloy material. This step is crucial for ensuring the performance of alloy products in high-end fields such as precision electronics and automotive parts.
[0081] It should be further noted that the products made from the polyamide / polyphenylene ether alloy material obtained by the above manufacturing method achieve a UL94 V-0 rating, CTI≥700V performance at a thickness of 0.6mm, and exhibit low precipitation (<0.1%) and high performance retention rate (>90%) after long-term aging.
[0082] The numerical range described in this invention includes not only the point values listed above, but also any point values within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values included in the range.
[0083] The performance of this composite material will be verified through multiple examples and comparative examples, as follows:
[0084] Examples 1-3
[0085] Prepare the raw materials, including by weight:
[0086] Polyamide 66 resin, viscosity 2.4-2.7 Pa·s;
[0087] Polyphenylene ether resin pre-irradiated with gamma rays, with an irradiation dose of 0.8 mgy;
[0088] A core-shell structured silicone-coated aluminum diethylphosphinic acid flame retardant, wherein the shell thickness is 150±20nm and the coating rate is 96%;
[0089] Maleic anhydride grafted with high-impact polystyrene compatibilizer pre-irradiated with gamma rays, grafting rate 1.8%, irradiation dose 0.8 MGy;
[0090] Hydrolysis-resistant glass fiber with surface treated with silane coupling agent;
[0091] Four needle-like zinc oxide whiskers;
[0092] Linear low-density polyethylene-g-acrylic acid (CTI synergist), acrylic acid grafting rate 1.0%;
[0093] Hyperbranched polyester amide (anti-exudation agent).
[0094] Preparation method:
[0095] Polyamide 66 resin was vacuum dried at 120℃ for 6 hours. Each component (parts by weight) was weighed according to the formulation in Table 1. Polyamide 66 resin (PA66), pre-irradiated polyphenylene ether resin (PPO), core-shell silicone-coated aluminum diethylphosphinate flame retardant, pre-irradiated maleic anhydride-grafted high-impact polystyrene compatibilizer (MAH-g-HIPS), linear low-density polyethylene-g-acrylic acid (LLDPE-g-AA), and hyperbranched polyesteramide were poured into a high-speed mixer and mixed at 400 r / min for 5 minutes. The mixed material was fed into a co-rotating twin-screw extruder (screw diameter 40 mm, L / D = 44:1, equipped with a 16-unit static mixer at the end of the three zones) through the main feed port. Hydrolysis-resistant glass fiber and tetra-needle zinc oxide whiskers were added through the side feed port.
[0096] Extruder temperature settings: Zone 1 220℃, Zone 2 255℃, Zone 3 240℃, main extruder speed 300 r / min. After water cooling, pelletizing, and drying, the melt is annealed in a vacuum oven at 120℃ for 4 hours to obtain polyamide / polyphenylene ether alloy material.
[0097] Comparative Example 1
[0098] In Comparative Example 1, the specific components used differ from those in Examples 1-3 in that ordinary aluminum diethylphosphinate flame retardant was used, along with un-pre-irradiated PPO and MAH-g-HIPS. The preparation method was the same as in Examples 1-3.
[0099] Comparative Example 2
[0100] In Comparative Example 2, the specific components used differ from those in Examples 1-3 in that tetra-needle zinc oxide whiskers were not used. The preparation method was the same as in Examples 1-3.
[0101] The polyamide / polyphenylene ether alloy materials of the examples and comparative examples were injection molded into standard test strips for performance testing. The results are shown in Table 2.
[0102]
[0103] Table 1
[0104]
[0105] Table 2
[0106] Results analysis:
[0107] As can be seen from Examples 1-3, the polyamide / polyphenylene ether alloy materials prepared by this invention all achieve a V-0 flame retardant rating at an ultrathin thickness of 0.6 mm, with CTI values far exceeding 700V, and exhibit extremely high performance retention after long-term aging with very few precipitates. Comparative Example 1, which did not use a core-shell flame retardant or pre-irradiation process, showed a significant decrease in flame retardant rating, CTI value, and post-aging performance, with severe precipitation, demonstrating the necessity of these two technologies. Comparative Example 2, which did not use four-needle ZnO whiskers, showed a significantly lower CTI value and post-aging CTI retention rate than Examples 1-3, demonstrating the crucial role of whiskers in improving and maintaining high insulation performance.
[0108] The above provides a detailed description of a polyamide / polyphenylene ether alloy material and its manufacturing method provided by the present invention. For those skilled in the art, based on the ideas of the embodiments of the present invention, there will be changes in the specific implementation methods and application scope. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A polyamide / polyphenylene ether alloy material, characterized in that, The following components are included by weight: 55-75 parts of polyamide 66 resin; 25-45 parts of polyphenylene ether resin pre-irradiated with gamma rays; 10-20 parts of core-shell structured silicone-coated aluminum diethylphosphinic acid flame retardant; 5-10 parts of maleic anhydride-grafted high-impact polystyrene compatibilizer pre-irradiated with gamma rays; 20-30 parts of hydrolysis-resistant glass fiber with surface treated with silane coupling agent; 3-8 parts of tetrane-shaped zinc oxide whiskers; CTI synergist 2-5 parts; 1-2 parts of anti-precipitation agent; The polyphenylene ether resin pre-irradiated with gamma rays is specifically polyphenylene ether resin pre-irradiated with gamma rays at a dose of 0.5-1.2 mgy. The maleic anhydride-grafted high-impact polystyrene compatibilizer pre-irradiated with gamma rays is specifically a maleic anhydride-grafted high-impact polystyrene compatibilizer pre-irradiated with gamma rays at a dose of 0.5-1.2 MGy. The core-shell structured silicone-coated aluminum diethylphosphinate flame retardant specifically uses aluminum diethylphosphinate as the core and fumed silica as the shell. The shell thickness is 100-200nm, and the coverage rate is ≥95%.
2. The polyamide / polyphenylene ether alloy material according to claim 1, characterized in that, The CTI enhancer is linear low-density polyethylene-g-acrylic acid.
3. The polyamide / polyphenylene ether alloy material according to claim 1, characterized in that, The anti-exudate agent is hyperbranched polyester amide.
4. A method for manufacturing a polyamide / polyphenylene ether alloy material, characterized in that, Includes the following steps: Irradiation treatment: Polyphenylene ether resin and maleic anhydride-grafted high-impact polystyrene compatibilizer were respectively irradiated with γ-rays at doses of 0.5-1.2 mgy; Vacuum drying: The polyamide 66 resin is vacuum dried at a first preset temperature until the moisture content is ≤500ppm; Mixing and Extrusion: The dried polyamide 66 resin, gamma-ray pre-irradiated polyphenylene ether resin, core-shell silicone-coated aluminum diethylphosphinate flame retardant, gamma-ray pre-irradiated maleic anhydride-grafted high-impact polystyrene compatibilizer, CTI synergist, and anti-exudation agent are mixed at high speed; then the mixture is fed into the extruder through the main feed port, and hydrolysis-resistant glass fibers and tetra-needle zinc oxide whiskers with silane coupling agent surface treatment are added through the side feed port; after melt blending, extrusion, water cooling, and pelletizing, the composite material is obtained; Vacuum annealing: The composite material is treated in a vacuum environment at a second preset temperature for a first preset time to obtain a polyamide / polyphenylene ether alloy material.
5. The method for manufacturing the polyamide / polyphenylene ether alloy material according to claim 4, characterized in that, In the mixing and extrusion steps, the extruder is a twin-screw extruder, wherein the twin-screw extruder adopts a three-stage variable diameter screw and zone temperature control: zone one temperature is 215-225℃, zone two temperature is 250-260℃, and zone three temperature is 235-245℃.
6. The method for manufacturing the polyamide / polyphenylene ether alloy material according to claim 4, characterized in that, In the vacuum drying step, the first preset temperature is 100-130℃.
7. The method for manufacturing the polyamide / polyphenylene ether alloy material according to claim 4, characterized in that, In the vacuum annealing step, the second preset temperature is 100-130℃, and the first preset time is 3-5 hours.
Citation Information
Patent Citations
Halogen-free flame-retardant reinforced PPE / PA6 composition with high CTI value and preparation method thereof
CN119899522A
Environment-friendly and flame-retardant glass fiber reinforced PA (polyamide) 66 / PPO (polyphenylene oxide) alloy material with high CTI (comparative tracking index) value and high GWIT (glow-wire ignition temperature) value and preparation method thereof
CN102964829A
Compatilizer with high-content epoxy groups and preparation method of compatilizer
CN109293825A