Outdoor glass cement with excellent weather resistance and preparation method thereof
By using branched polyether modified silicone oil and cerium dioxide-supported hindered phenolic anti-aging agent in glass sealant, the problem of insufficient weather resistance of outdoor glass sealant under extreme climates is solved, the bonding strength and anti-aging performance are improved, and it is suitable for outdoor engineering applications.
Patent Information
- Application Number
- CN202511798310.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-02
- Publication Date
- 2026-05-01
AI Technical Summary
Existing outdoor glass sealants lack sufficient weather resistance under extreme climatic conditions, and their bonding adaptability and environmental friendliness need to be improved. Furthermore, they are prone to aging during long-term use.
Branched polyether-modified silicone oil was used as a dispersant, and cerium dioxide-supported hindered phenolic anti-aging agent was added. The branched structure improved the interfacial compatibility and anti-aging performance, forming a synergistic anti-aging effect.
It significantly improves the weather resistance and bonding strength of glass sealant, extends its service life, and enhances its adaptability to bonding with a variety of materials and its environmental friendliness.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of adhesive technology, specifically relating to an outdoor glass adhesive with excellent weather resistance and its preparation method. Background Technology
[0002] Glass sealant is a functional material specifically designed for bonding and sealing glass with other substrates. It is widely used in building curtain walls, door and window installation, interior decoration, and industrial manufacturing. Based on chemical composition and performance characteristics, glass sealants on the market can be mainly divided into two categories: silicone sealants and polyurethane sealants (PU). Silicone sealants are based on organosilicon polymers and form a flexible elastomer after curing, exhibiting excellent adhesion and elasticity. Polyurethane sealants, on the other hand, use polyurethane prepolymers as their main component, possessing excellent mechanical properties, good abrasion resistance, and good oil resistance, but have certain limitations in hydrolysis resistance and weather resistance.
[0003] For outdoor applications, such as building exterior wall joints, roof glass caulking, and outdoor billboard encapsulation, silicone sealants are exposed to complex atmospheric environments for extended periods, facing challenges from UV radiation, high temperatures, rain, oxidation, and temperature cycling. Therefore, these applications typically require silicone sealants to possess excellent weather resistance, UV resistance, high and low temperature resistance, and long-term anti-aging stability. Among the many types of silicone sealants, silicone sealants exhibit superior UV resistance and heat resistance due to the stable silicon-oxygen bonds (Si–O–Si) in their molecular structure. They are less prone to yellowing, chalking, or cracking from prolonged exposure to sunlight, making them suitable for long-term outdoor use.
[0004] However, despite the excellent weather resistance of silicone sealants, some technical bottlenecks remain in their practical applications. These include limited adhesion to certain substrates, curing speed significantly affected by ambient temperature and humidity, and poor surface finish. Furthermore, the service life of existing standard silicone sealants under extreme climatic conditions (such as prolonged exposure to strong ultraviolet radiation and alternating periods of high temperature and humidity) still has room for improvement. Therefore, there is an urgent need to develop new modified silicone sealants or composite sealing materials that, while maintaining their excellent weather resistance, further enhance their adhesion to various materials, environmental friendliness, and long-term durability to meet the increasing demands of outdoor engineering applications. Summary of the Invention
[0005] The purpose of this invention is to provide an outdoor glass sealant with excellent weather resistance and its preparation method, so as to solve the problem of insufficient weather resistance of glass sealants.
[0006] The objective of this invention can be achieved through the following technical solutions: An outdoor glass sealant with excellent weather resistance comprises, by weight, 100 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of dimethyl silicone oil, 80-120 parts of filler, 6-12 parts of crosslinking agent, 0.05-0.2 parts of organotin catalyst, 0.5-2 parts of aminosilane coupling agent, 5-8 parts of cerium dioxide-supported hindered phenolic anti-aging agent, and 10-12 parts of branched polyether modified silicone oil.
[0007] In some possible implementations, the filler is one of calcium carbonate, silica, alumina, and aluminum hydroxide; the appropriate filler type is selected according to the different application scenarios.
[0008] The crosslinking agent is at least one of methyl tributanone oxime silane and vinyl tributanone oxime silane; The aminosilane coupling agent is at least one of γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane and γ-aminopropyltrimethoxysilane; The organotin catalyst is at least one of dibutyltin dilaurate, dioctyltin dilaurate, and stannous octoate.
[0009] In some possible implementations, the branched polyether-modified silicone oil is prepared by the following steps: End-epoxy polyether silicone oil and diethylenetriamine were added to isopropanol and stirred for 3-4 hours under nitrogen protection and at a temperature of 75-80℃. After the reaction was completed, branched polyether modified silicone oil was obtained by removing low-boiling substances such as isopropanol by vacuum distillation.
[0010] In some possible implementations, the mass ratio of terminal epoxy polyether silicone oil to diethylenetriamine is 120-130:1; the amount of isopropanol added is 25% to 35% of the total mass of terminal epoxy polyether silicone oil and diethylenetriamine.
[0011] In some possible implementations, the terminal epoxy polyether silicone oil is prepared by hydrosilylation of terminal hydrogen silicone oil and allyl epoxy polyether: Hydrogen-terminated silicone oil and allyl epoxy polyether were added to isopropanol, followed by chloroplatinic acid. The mixture was stirred and reacted at 75-80℃ for 5-6 hours. The solvent, isopropanol, was removed by vacuum distillation to obtain the terminal epoxy polyether silicone oil. The molecular weight of the terminal hydrogen silicone oil was 6000, and that of the allyl epoxy polyether was 1500. The molar ratio of the terminal hydrogen silicone oil to the allyl epoxy polyether was 1:2. The amount of chloroplatinic acid added as a catalyst was 0.1%-0.3% of the total mass of the terminal hydrogen silicone oil and allyl epoxy polyether. The amount of isopropanol added as a solvent was 15%-20% of the total mass of the terminal hydrogen silicone oil and allyl epoxy polyether.
[0012] Glass sealants typically incorporate large amounts of fillers to achieve good reinforcement and weather resistance; however, excessive filler can lead to poor dispersibility, hindering overall performance improvement. Therefore, this invention adds branched polyether-modified silicone oil as a dispersant. The polyether segments in this branched polyether-modified silicone oil can form hydrogen bonds with the hydroxyl groups on the filler surface. Furthermore, the structure of the branched polyether-modified silicone oil includes siloxane segments that are identical or highly similar to those in glass sealant, enabling excellent entanglement and compatibility with the matrix silicone rubber, forming a uniform phase interface. This solves the problem of agglomeration or poor dispersibility caused by interfacial incompatibility between the filler and the matrix silicone rubber.
[0013] Polyether segments are highly hydrophilic polar segments. The introduction of polyether segments into the branched polyether-modified silicone oil of this invention constructs a stable interfacial layer between the filler and the matrix silicone rubber, which is beneficial for improving the interfacial compatibility between the filler and the matrix silicone rubber, indirectly enhancing the mechanical properties after curing. The polarity of the polyether segments allows them to form stronger hydrogen bonds with hydroxyl and carboxyl groups on the surface of the substrate (metals, glass, etc., are generally polar), and even partially participate in coordination bonds, thereby significantly improving adhesion. However, because polyether segments are themselves highly hydrophilic polar segments, they have poor water resistance, low bond energy, and much lower thermal stability than organosilicon segments. Therefore, they are prone to oxidation and degradation, leading to molecular chain breakage and a decrease in mechanical properties. Therefore, this invention prepares branched polyether-modified silicone oil with a branched structure. The branched structure has a lower degree of freedom of movement compared to linear molecular chain segments, making it less prone to migration and not affecting compatibility. The branched structure can promote the formation of smaller and more uniform "microphase separation" regions between polyether segments and organosilicon segments, improving the mechanical properties of the material. The branched structure can improve the "utilization efficiency" of polyether segments, allowing for better adhesion and dispersion effects with only a small amount of polyether segments, thereby indirectly reducing damage to aging resistance. Moreover, the branched structure of the branched polyether-modified silicone oil can, to a certain extent, "shield" or "embed" polyether segments, delaying the process of thermal oxidative degradation and fully leveraging the role of the branched polyether-modified silicone oil.
[0014] In some possible implementations, cerium dioxide-supported hindered phenolic anti-aging agents are prepared via the following steps: Aminated cerium dioxide was added to toluene and ultrasonically dispersed. Then, 3,5-bis(tert-butyl)4-hydroxyphenylpropionyl chloride was added under nitrogen protection, followed by triethylamine. The mixture was stirred and reacted at 30-60°C for 16-20 hours. After the reaction, the product was filtered, washed, and dried to obtain a cerium dioxide-supported hindered phenol anti-aging agent. This cerium dioxide-supported hindered phenol anti-aging agent exhibits better anti-aging effects than a direct mixture of cerium dioxide and hindered phenol antioxidants. This is because the cerium dioxide is chemically "anchored" to cerium dioxide, greatly limiting its physical migration and volatilization. This ensures the long-term stability and durability of the anti-aging component in the matrix. After capturing free radicals, the hindered phenol structure transforms into phenoloxy radicals. The phenoloxy radicals closely adjacent to cerium dioxide can potentially gain electrons or hydrogen from the cerium dioxide surface, achieving a precise reaction. This regeneration mechanism can significantly extend the lifespan of the hindered phenol, enabling it to capture more free radicals and thus improve anti-aging efficiency.
[0015] This invention incorporates a cerium dioxide-supported hindered phenol anti-aging agent. The hindered phenol is immobilized by cerium dioxide, resulting in a synergistic anti-aging effect. In this cerium dioxide-supported hindered phenol anti-aging agent, the cerium dioxide structure contains Ce. 4+ and Ce 3+ The reversible conversion between these components efficiently eliminates free radicals in this cycle. When hindered phenols are loaded onto cerium dioxide, a synergistic anti-aging mechanism is formed. Cerium dioxide itself directly scavenges superoxide radicals and hydrogen peroxide through valence state changes; simultaneously, hindered phenols provide hydrogen atoms to scavenge other free radicals such as alkyl radicals. After cerium dioxide scavenges superoxide radicals and hydrogen peroxide, it provides a more "milder" environment for hindered phenols, reducing the consumption pressure on hindered phenols and thus extending the effective lifespan of the entire anti-aging system.
[0016] In some possible implementations, the ratio of aminated cerium dioxide, 3,5-bis(tert-butyl)4-hydroxyphenylpropionyl chloride, and triethylamine is 5 g: 2-3 g: 4-6 mL.
[0017] In some possible implementations, aminated cerium dioxide is prepared via the following steps: Cerium dioxide was added to 20% hydrogen peroxide and oxidized at 50-60℃ for 5-6 hours. After oxidation, the oxidized cerium dioxide was washed and dried to obtain hydroxylated cerium dioxide. Hydroxylated cerium dioxide and an aminosilane coupling agent were added to ethanol and reacted at 50-60℃ under a nitrogen atmosphere for 5-6 hours. After the reaction, the oxidized cerium dioxide was obtained by filtration, washing, and vacuum drying. The ratio of cerium dioxide, aminosilane coupling agent, and ethanol was 1 g: 0.2-0.3 g: 20-30 mL.
[0018] In some possible implementations, the aminosilane coupling agent is one of γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, and γ-aminopropyltrimethoxysilane.
[0019] The second aspect of this application provides a method for preparing an outdoor glass sealant with excellent weather resistance, comprising the following steps: Hydroxy-dimethylsiloxane, dimethyl silicone oil and filler are mixed evenly, heated to 110-120℃, vacuum dehydrated for 120-150 min, cooled to 30-40℃, crosslinking agent, organotin catalyst, aminosilane coupling agent, cerium dioxide supported hindered phenol anti-aging agent and branched polyether modified silicone oil are added and stirred evenly to obtain outdoor glass sealant with excellent weather resistance.
[0020] The beneficial effects of this invention are: This invention provides an outdoor glass sealant with excellent weather resistance and its preparation method. The glass sealant contains cerium dioxide-supported hindered phenol anti-aging agent. The hindered phenol is supported by cerium dioxide to form a synergistic anti-aging effect. Phenoxy radicals closely adjacent to cerium dioxide may obtain electrons or hydrogen from the cerium dioxide surface to achieve precise reaction. This regeneration mechanism can significantly extend the service life of hindered phenol, enabling it to capture more free radicals, thereby improving anti-aging efficiency.
[0021] The glass adhesive of this invention also contains branched polyether modified silicone oil as a dispersant, which solves the problem of agglomeration or poor dispersibility caused by interfacial incompatibility between filler and matrix silicone rubber. The introduction of polyether segments in the branched polyether modified silicone oil constructs a stable interfacial layer between the filler and matrix silicone rubber, which is beneficial to improving the interfacial compatibility between the filler and matrix silicone rubber and indirectly improving the mechanical properties after curing. The polarity of the polyether segments enables them to form stronger hydrogen bonds with hydroxyl and carboxyl groups on the surface of the substrate, and even participate in coordination bonds in some cases, thereby significantly improving the adhesion. Detailed Implementation
[0022] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0023] The following is a detailed description of an outdoor glass adhesive with excellent weather resistance and its preparation method, based on embodiments of this application.
[0024] The following is a detailed description with reference to specific examples.
[0025] Example 1 This embodiment provides an outdoor glass sealant with excellent weather resistance, which is prepared through the following steps: By weight, 100 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of dimethyl silicone oil and 100 parts of calcium carbonate are mixed evenly, heated to 110°C, vacuum dehydrated for 150 min, cooled to 30°C, and then 6 parts of methyl tributanone oxime silane, 0.1 parts of dibutyltin dilaurate, 1 part of γ-aminopropyltriethoxysilane, 5 parts of cerium dioxide-supported hindered phenolic anti-aging agent and 10 parts of branched polyether modified silicone oil are added and stirred evenly to obtain an outdoor glass sealant with excellent weather resistance.
[0026] The branched polyether modified silicone oil is prepared through the following steps: Hydrogen-terminated silicone oil and allyl epoxy polyether were added to isopropanol, followed by chloroplatinic acid. The mixture was stirred and reacted at 80°C for 5 hours. The solvent, isopropanol, was removed by vacuum distillation to obtain the terminal epoxy polyether silicone oil. The molecular weight of the terminal hydrogen silicone oil was 6000, and the molecular weight of the allyl epoxy polyether was 1500. The molar ratio of the terminal hydrogen silicone oil to the allyl epoxy polyether was 1:2. The amount of chloroplatinic acid added was 0.3% of the total mass of the terminal hydrogen silicone oil and allyl epoxy polyether, and the amount of isopropanol added was 20% of the total mass of the terminal hydrogen silicone oil and allyl epoxy polyether.
[0027] Terminal epoxy polyether silicone oil and diethylenetriamine were added to isopropanol and stirred for 3 hours under nitrogen protection and at 80°C. After the reaction was completed, branched polyether modified silicone oil was obtained by distillation under reduced pressure to remove low-boiling substances such as isopropanol. The mass ratio of terminal epoxy polyether silicone oil to diethylenetriamine was 120:1. The amount of isopropanol added was 30% of the total mass of terminal epoxy polyether silicone oil and diethylenetriamine.
[0028] The cerium dioxide-supported hindered phenolic anti-aging agent is prepared through the following steps: Cerium dioxide was added to 20% hydrogen peroxide and oxidized at 60°C for 5 hours. After oxidation, the oxidized cerium dioxide was washed and dried to obtain hydroxylated cerium dioxide. Hydroxylated cerium dioxide and an aminosilane coupling agent were added to ethanol and reacted at 50°C for 6 hours under a nitrogen atmosphere. After the reaction, the oxidized cerium dioxide was obtained by filtration, washing, and vacuum drying. The ratio of cerium dioxide, aminosilane coupling agent, and ethanol was 1 g:0.2 g:20 mL; the aminosilane coupling agent was γ-aminopropyltriethoxysilane.
[0029] Aminated cerium dioxide was added to toluene and ultrasonically dispersed. Then, 3,5-bis(tert-butyl)4-hydroxyphenylpropionyl chloride was added under nitrogen protection, followed by triethylamine. The mixture was stirred and reacted at 30°C for 16 hours. After the reaction was completed, the cerium dioxide-supported hindered phenolic anti-aging agent was obtained by filtration, washing, and drying. The ratio of aminated cerium dioxide, 3,5-bis(tert-butyl)4-hydroxyphenylpropionyl chloride, and triethylamine was 5 g: 2 g: 4 mL.
[0030] Example 2 This embodiment provides an outdoor glass sealant with excellent weather resistance, which is prepared through the following steps: By weight, 100 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of dimethyl silicone oil and 80 parts of calcium carbonate are mixed evenly, heated to 110°C, vacuum dehydrated for 150 min, cooled to 30°C, and then 6 parts of methyl tributanone oxime silane, 0.1 parts of dibutyltin dilaurate, 1 part of γ-aminopropyltriethoxysilane, 5 parts of cerium dioxide-supported hindered phenolic anti-aging agent and 10 parts of branched polyether modified silicone oil are added and stirred evenly to obtain outdoor glass sealant with excellent weather resistance.
[0031] Among them, the branched polyether modified silicone oil is the same as in Example 1; the cerium dioxide-supported hindered phenol anti-aging agent is the same as in Example 1.
[0032] Example 3 This embodiment provides an outdoor glass sealant with excellent weather resistance, which is prepared through the following steps: By weight, 100 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of dimethyl silicone oil and 100 parts of calcium carbonate are mixed evenly, heated to 110°C, vacuum dehydrated for 150 min, cooled to 30°C, and then 12 parts of methyl tributanone oxime silane, 0.1 parts of dibutyltin dilaurate, 1 part of γ-aminopropyltriethoxysilane, 5 parts of cerium dioxide-supported hindered phenolic anti-aging agent and 10 parts of branched polyether modified silicone oil are added and stirred evenly to obtain an outdoor glass sealant with excellent weather resistance.
[0033] Among them, the branched polyether modified silicone oil is the same as in Example 1; the cerium dioxide-supported hindered phenol anti-aging agent is the same as in Example 1.
[0034] Example 4 This embodiment provides an outdoor glass sealant with excellent weather resistance, which is prepared through the following steps: By weight, 100 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of dimethyl silicone oil and 100 parts of calcium carbonate are mixed evenly, heated to 110°C, vacuum dehydrated for 150 min, cooled to 30°C, and then 6 parts of methyl tributanone oxime silane, 0.1 parts of dibutyltin dilaurate, 2 parts of γ-aminopropyltriethoxysilane, 5 parts of cerium dioxide-supported hindered phenolic anti-aging agent and 10 parts of branched polyether modified silicone oil are added and stirred evenly to obtain an outdoor glass sealant with excellent weather resistance.
[0035] Among them, the branched polyether modified silicone oil is the same as in Example 1; the cerium dioxide-supported hindered phenol anti-aging agent is the same as in Example 1.
[0036] Example 5 This embodiment provides an outdoor glass sealant with excellent weather resistance, which is prepared through the following steps: By weight, 100 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of dimethyl silicone oil and 100 parts of calcium carbonate are mixed evenly, heated to 110°C, vacuum dehydrated for 150 min, cooled to 30°C, and then 6 parts of methyl tributanone oxime silane, 0.1 parts of dibutyltin dilaurate, 1 part of γ-aminopropyltriethoxysilane, 8 parts of cerium dioxide-supported hindered phenolic anti-aging agent and 10 parts of branched polyether modified silicone oil are added and stirred evenly to obtain an outdoor glass sealant with excellent weather resistance.
[0037] Among them, the branched polyether modified silicone oil is the same as in Example 1; the cerium dioxide-supported hindered phenol anti-aging agent is the same as in Example 1.
[0038] Example 6 This embodiment provides an outdoor glass sealant with excellent weather resistance, which is prepared through the following steps: By weight, 100 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of dimethyl silicone oil and 100 parts of calcium carbonate are mixed evenly, heated to 110°C, vacuum dehydrated for 150 min, cooled to 30°C, and then 6 parts of methyl tributanone oxime silane, 0.1 parts of dibutyltin dilaurate, 1 part of γ-aminopropyltriethoxysilane, 5 parts of cerium dioxide-supported hindered phenolic anti-aging agent and 12 parts of branched polyether modified silicone oil are added and stirred evenly to obtain an outdoor glass sealant with excellent weather resistance.
[0039] Among them, the branched polyether modified silicone oil is the same as in Example 1; the cerium dioxide-supported hindered phenol anti-aging agent is the same as in Example 1.
[0040] Example 7 This embodiment provides an outdoor glass sealant with excellent weather resistance, which is prepared through the following steps: By weight, 100 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of dimethyl silicone oil and 100 parts of calcium carbonate are mixed evenly, heated to 110°C, vacuum dehydrated for 150 min, cooled to 30°C, and then 6 parts of methyl tributanone oxime silane, 0.1 parts of dibutyltin dilaurate, 1 part of γ-aminopropyltriethoxysilane, 5 parts of cerium dioxide-supported hindered phenolic anti-aging agent and 10 parts of branched polyether modified silicone oil are added and stirred evenly to obtain an outdoor glass sealant with excellent weather resistance.
[0041] The branched polyether modified silicone oil is the same as in Example 1. The cerium dioxide-supported hindered phenolic anti-aging agent is prepared through the following steps: Cerium dioxide was added to 20% hydrogen peroxide and oxidized at 50°C for 5 hours. After oxidation, the oxidized cerium dioxide was washed and dried to obtain hydroxylated cerium dioxide. Hydroxylated cerium dioxide and an aminosilane coupling agent were added to ethanol and reacted at 50°C for 5 hours under a nitrogen atmosphere. After the reaction, the oxidized cerium dioxide was obtained by filtration, washing, and vacuum drying. The ratio of cerium dioxide, aminosilane coupling agent, and ethanol was 1 g:0.2 g:30 mL; the aminosilane coupling agent was N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane.
[0042] Aminated cerium dioxide was added to toluene and ultrasonically dispersed. Then, 3,5-bis(tert-butyl)4-hydroxyphenylpropionyl chloride was added under nitrogen protection, followed by triethylamine. The mixture was stirred and reacted at 30-60℃ for 16-20 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain cerium dioxide-supported hindered phenolic anti-aging agent. The ratio of aminated cerium dioxide, 3,5-bis(tert-butyl)4-hydroxyphenylpropionyl chloride, and triethylamine was 5 g: 2 g: 4 mL.
[0043] Example 8 This embodiment provides an outdoor glass sealant with excellent weather resistance, which is prepared through the following steps: By weight, 100 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of dimethyl silicone oil and 100 parts of calcium carbonate are mixed evenly, heated to 110°C, vacuum dehydrated for 150 min, cooled to 30°C, and then 6 parts of methyl tributanone oxime silane, 0.1 parts of dibutyltin dilaurate, 1 part of γ-aminopropyltriethoxysilane, 5 parts of cerium dioxide-supported hindered phenolic anti-aging agent and 10 parts of branched polyether modified silicone oil are added and stirred evenly to obtain an outdoor glass sealant with excellent weather resistance.
[0044] The branched polyether modified silicone oil is prepared through the following steps: Hydrogen-terminated silicone oil and allyl epoxy polyether were added to isopropanol, followed by chloroplatinic acid. The mixture was stirred and reacted at 80°C for 5 hours. The solvent, isopropanol, was removed by vacuum distillation to obtain the terminal epoxy polyether silicone oil. The molecular weight of the terminal hydrogen silicone oil was 6000, and the molecular weight of the allyl epoxy polyether was 1500. The molar ratio of the terminal hydrogen silicone oil to the allyl epoxy polyether was 1:2. The amount of chloroplatinic acid added as a catalyst was 0.2% of the total mass of the terminal hydrogen silicone oil and allyl epoxy polyether. The amount of isopropanol added as a solvent was 20% of the total mass of the terminal hydrogen silicone oil and allyl epoxy polyether.
[0045] Terminal epoxy polyether silicone oil and diethylenetriamine were added to isopropanol and stirred for 4 hours under nitrogen protection and at 75°C. After the reaction was completed, low-boiling substances such as isopropanol were removed by vacuum distillation to obtain branched polyether modified silicone oil. The mass ratio of terminal epoxy polyether silicone oil to diethylenetriamine was 130:1. The amount of isopropanol added was 30% of the total mass of terminal epoxy polyether silicone oil and diethylenetriamine.
[0046] The cerium dioxide-supported hindered phenol anti-aging agent is the same as in Example 1.
[0047] Comparative Example 1 The difference between this comparative example and Example 1 is that the cerium dioxide-supported hindered phenolic antioxidant is replaced with cerium dioxide and antioxidant 1010, with a mass ratio of cerium dioxide to antioxidant 1010 of 5:2. All other raw materials and preparation processes remain the same as in Example 1.
[0048] Comparative Example 2 The difference between this comparative example and Example 1 is that cerium dioxide in the cerium dioxide-supported hindered phenolic anti-aging agent is replaced with titanium dioxide. The specific preparation steps are as follows: Titanium dioxide and an aminosilane coupling agent were added to ethanol and reacted at 50°C for 6 hours under a nitrogen atmosphere. After the reaction, the mixture was filtered, washed, and vacuum dried to obtain aminated titanium dioxide. The ratio of titanium dioxide, aminosilane coupling agent, and ethanol was 1 g:0.2 g:20 mL; the aminosilane coupling agent was γ-aminopropyltriethoxysilane.
[0049] Aminated titanium dioxide was added to toluene and ultrasonically dispersed. Then, 3,5-bis(tert-butyl)4-hydroxyphenylpropionyl chloride was added under nitrogen protection, followed by triethylamine. The mixture was stirred and reacted at 30°C for 16 hours. After the reaction was completed, the mixture was filtered, washed, and dried. The ratio of aminated titanium dioxide, 3,5-bis(tert-butyl)4-hydroxyphenylpropionyl chloride, and triethylamine was 5 g: 2 g: 4 mL.
[0050] The remaining raw materials and preparation process are the same as in Example 1.
[0051] Comparative Example 3 The difference between this comparative example and Example 1 is that branched polyether modified silicone oil is not added, but dimethyl silicone oil is used instead. The other raw materials and preparation process are the same as in Example 1.
[0052] Comparative Example 4 The difference between this comparative example and Example 1 is that the branched polyether modified silicone oil is replaced with a polyether modified silicone oil prepared by the following method: Terminal epoxy polyether silicone oil (same as in Example 1) and 1,3-propanediamine were added to isopropanol and stirred for 3 hours under nitrogen protection and at 80°C. After the reaction was completed, low-boiling substances such as isopropanol were removed by vacuum distillation to obtain branched polyether modified silicone oil. The mass ratio of terminal epoxy polyether silicone oil to 1,3-propanediamine was 120:1. The amount of isopropanol added was 30% of the total mass of terminal epoxy polyether silicone oil and 1,3-propanediamine.
[0053] The remaining raw materials and preparation process are the same as in Example 1.
[0054] The weather resistance of the samples prepared in Examples 1-8 and Comparative Examples 1-4 was tested; thermal aging: the samples cured at room temperature were placed in a constant temperature and humidity chamber at 85°C and 85% relative humidity for 1000 hours, and then the tensile strength was tested. Photoaging: Under a 20W UV lamp emitting short-wave UV light with a characteristic wavelength of 253.7nm, the UV irradiance at 20cm vertically from the lamp center is 1400μW / cm². 2 The test sample is placed parallel to the light source in a fixed position for ultraviolet aging testing. Ensure that each sample receives the same amount of ultraviolet radiation during the test. The ultraviolet aging time is 1000 hours, and tensile strength is tested. Tensile strength was tested according to standard GB / T 528-2009, and the results are shown in Table 1: Table 1 As shown in Table 1, in Examples 1-8 of this invention, cerium dioxide was added to immobilize the hindered phenol anti-aging agent. The hindered phenol was immobilized by cerium dioxide, resulting in a synergistic anti-aging effect. The tensile strength decreased by approximately 30% after aging. Compared to direct mixing (the tensile strength of the sample in Comparative Example 1 decreased by approximately 35%), the method of immobilizing the hindered phenol with cerium dioxide in this invention can fully utilize the effect of the cerium dioxide-immobilized hindered phenol anti-aging agent. Compared to other anti-aging agents such as titanium dioxide (the tensile strength of the sample in Comparative Example 2 decreased by more than 35%), the cerium dioxide in this application can form a more stable anti-aging effect with the hindered phenol. Titanium dioxide has photocatalytic activity and can trigger photodegradation of the resin. The hindered phenol can provide hydrogen atoms to counteract the photodegradation effect, but it also counteracts the effect of the hindered phenol to some extent. In the system of this application, the utilization rate of the hindered phenol is higher and its consumption is slower. Therefore, the effective life of this system is longer, making it particularly suitable for applications requiring high durability and reliability. Compared to Example 1, which did not add branched polyether modified silicone oil, Comparative Example 4 used linear polyether modified silicone oil, which directly affected the dispersion performance of fillers (such as calcium carbonate) and indirectly affected the aging resistance.
[0055] The bonding performance of the samples prepared in Example 1 and Comparative Examples 1-4 was tested: Plastic and metal parts were bonded to a fiberglass surface and cured at room temperature for 24 hours. Then, using a pull gauge with a hook, the plastic and metal parts were pulled forcefully until they detached. The pulling force at the point of detachment was recorded. The results are shown in Table 2 below. Table 2 To further optimize the performance of the silicone sealant, this invention incorporates polyether segments from branched polyether-modified silicone oil as a dispersant. The polyether segments in the branched polyether-modified silicone oil, being identical or highly similar to the siloxane segments in the silicone sealant, can effectively intertwine and become compatible with the matrix silicone rubber, forming a uniform phase interface. This solves the problem of agglomeration or poor dispersibility caused by interfacial incompatibility between the filler and the matrix silicone rubber. Furthermore, the polarity of the polyether segments in the branched polyether-modified silicone oil allows them to form stronger hydrogen bonds with hydroxyl and carboxyl groups on the surface of the substrate (metals, glass, etc., which are generally polar), and even partially participate in coordination bonds, thereby significantly improving adhesion. Additionally, the introduction of branched segments weakens the negative impact of the polyether segments on aging resistance.
[0056] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0057] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. An outdoor glass sealant with excellent weather resistance, characterized in that, By weight, it includes 100 parts of hydroxyl-terminated polydimethylsiloxane, 10 parts of dimethyl silicone oil, 80-120 parts of filler, 6-12 parts of crosslinking agent, 0.05-0.2 parts of organotin catalyst, 0.5-2 parts of aminosilane coupling agent, 5-8 parts of cerium dioxide-supported hindered phenol anti-aging agent, and 10-12 parts of branched polyether modified silicone oil.
2. The outdoor glass sealant with excellent weather resistance according to claim 1, characterized in that, The branched polyether modified silicone oil is prepared through the following steps: End-epoxy polyether silicone oil and diethylenetriamine were added to isopropanol and stirred for 3-4 hours under nitrogen protection and at a temperature of 75-80℃ to obtain branched polyether modified silicone oil.
3. The outdoor glass sealant with excellent weather resistance according to claim 2, characterized in that, The mass ratio of terminal epoxy polyether silicone oil to diethylenetriamine is 120-130:1; the amount of isopropanol added is 25% to 35% of the total mass of terminal epoxy polyether silicone oil and diethylenetriamine.
4. The outdoor glass sealant with excellent weather resistance according to claim 2, characterized in that, The terminal epoxy polyether silicone oil is prepared by hydrosilylation of terminal hydrogen silicone oil and allyl epoxy polyether.
5. The outdoor glass sealant with excellent weather resistance according to claim 1, characterized in that, Cerium dioxide-supported hindered phenolic anti-aging agents are prepared through the following steps: Aminated cerium dioxide was added to toluene and ultrasonically dispersed. Then, 3,5-bis(tert-butyl)4-hydroxyphenylpropionyl chloride was added under nitrogen protection, followed by triethylamine. The mixture was stirred and reacted at 30-60℃ for 16-20 h to obtain cerium dioxide-supported hindered phenol anti-aging agent.
6. The outdoor glass sealant with excellent weather resistance according to claim 5, characterized in that, The ratio of aminated cerium dioxide, 3,5-bis(tert-butyl)4-hydroxyphenylpropionyl chloride and triethylamine is 5g:2-3g:4-6mL.
7. The outdoor glass sealant with excellent weather resistance according to claim 5, characterized in that, Aminated cerium dioxide is prepared by the following steps: Cerium dioxide was added to 20% hydrogen peroxide and oxidized at 50-60℃ for 5-6 hours. After oxidation, the oxidized cerium dioxide was washed and dried to obtain hydroxylated cerium dioxide. The hydroxylated cerium dioxide and aminosilane coupling agent were added to ethanol and reacted at 50-60℃ under a nitrogen atmosphere for 5-6 hours. After the reaction, the oxidized cerium dioxide was obtained by filtration, washing, and vacuum drying. The ratio of cerium dioxide, aminosilane coupling agent and ethanol was 1g:0.2-0.3g:20-30mL.
8. The outdoor glass sealant with excellent weather resistance according to claim 1, characterized in that, The filler is one of calcium carbonate, silica, alumina, and aluminum hydroxide; The crosslinking agent is at least one of methyl tributanone oxime silane and vinyl tributanone oxime silane; The organotin catalyst is at least one of dibutyltin dilaurate, dioctyltin dilaurate, and stannous octoate.
9. The outdoor glass sealant with excellent weather resistance according to claim 1 or 7, characterized in that, The aminosilane coupling agent is at least one selected from γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, and γ-aminopropyltrimethoxysilane.
10. A method for preparing an outdoor glass sealant with excellent weather resistance, used to prepare the outdoor glass sealant according to any one of claims 1-9, characterized in that, Includes the following steps: Hydroxy-dimethylsiloxane, dimethyl silicone oil and filler are mixed evenly, heated to 110-120℃, vacuum dehydrated for 120-150 min, cooled to 30-40℃, crosslinking agent, organotin catalyst, aminosilane coupling agent, cerium dioxide supported hindered phenol anti-aging agent and branched polyether modified silicone oil are added and stirred evenly to obtain outdoor glass sealant with excellent weather resistance.