A concrete quick-setting agent and its preparation method

By preparing a concrete accelerator with a high aluminum-to-sulfur ratio of polyaluminum sulfate, an emulsion suspension stabilizer, and an organic alcohol amino ester polymer, the problems of alkali corrosion, shrinkage, durability, and compatibility of accelerators were solved, achieving the effects of being fluorine-free and chlorine-free, having ultra-early strength, low-temperature stability, and high cost-effectiveness.

CN122277140BActive Publication Date: 2026-11-10NAT ENG LAB FOR HIGH SPEED RAILWAY CONSTR +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202610746126.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-05-28
Publication Date
2026-11-10
Estimated Expiration
2046-05-28

AI Technical Summary

Technical Problem

Existing quick-setting agents have problems such as high alkali corrosion, large concrete shrinkage, low later strength, affecting concrete durability, fluoride poisoning and steel corrosion caused by fluorine and chlorine content, and are unstable and have poor compatibility with cement-based materials in low-temperature environments.

Method used

Using high-alumina-sulfur ratio polyaluminum sulfate, emulsion suspension stabilizers, and organic alcohol amino ester polymers, an alkali-free, fluorine-free, and chlorine-free concrete accelerator is prepared through a specific process, ensuring good compatibility with cement-based materials, stable storage, and ultra-early strength performance.

Benefits of technology

The prepared concrete accelerator is alkali-free and chlorine-free, possesses ultra-early strength, good durability, stability at low temperatures, high cost-effectiveness, good compatibility with cement-based materials, environmentally friendly production, and excellent construction performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122277140B_ABST
    Figure CN122277140B_ABST
Patent Text Reader

Abstract

This invention relates to the field of cement concrete admixtures, and more particularly to a concrete accelerator and its preparation method. The accelerator is prepared using this method. The method includes sequentially adding a main accelerator, a setting aid, a solubilizer, a complexing component, an early-strength component, a pH adjusting component, an emulsion suspension stabilizer, an organic alcohol amine ester polymer, an alcohol amine stabilizing component, a nanomaterial component, a thickening component, a surfactant component, and a water-reducing and defoaming component, followed by stirring to dissolve and obtain a seventh solution. The pH of the seventh solution is adjusted to 2-4.5 using an alkaline solution, and a eighth stirring treatment is performed to obtain the accelerator cooled to room temperature. This invention not only enables the preparation of an alkali-free, fluorine-free, and chlorine-free accelerator, but also enables the prepared accelerator to possess advantages such as ultra-early strength, durability, high cost-effectiveness, low-temperature storage stability, and good compatibility with cement-based materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of cement concrete admixtures, and more particularly to a concrete quick-setting agent and its preparation method. Background Technology

[0002] Accelerators for concrete are important admixtures in shotcrete construction. They accelerate the hardening and setting of cement slurry and effectively improve the early strength of shotcrete. They are widely used in shotcrete construction for tunnel engineering, geotechnical engineering, and subway projects, as well as in rapid construction applications such as emergency repairs and leak sealing. Liquid accelerators offer advantages such as high construction efficiency and low rebound rate, making them one of the leading accelerators currently available.

[0003] However, existing accelerators suffer from problems such as high alkali corrosion, large concrete shrinkage, low later-stage strength, and impaired concrete durability. Furthermore, some accelerators often use fluorine- or chloride-containing raw materials in their preparation, leading to fluorosis and chloride ion-induced steel reinforcement corrosion. To address these issues, GB / T35159-2017 "Accelerators for Shotcrete" and Q / CR 807-2020 "Liquid Alkali-Free Accelerators for Shotcrete in Tunnels" both specify limits on the content of alkali and chloride ions. Meanwhile, existing accelerators in some publicly disclosed products and patents still suffer from high prices, instability in low-temperature storage, and poor compatibility with cement-based materials. Examples include Chinese invention applications 201610390267.5 ("Low-Rebound Liquid Accelerator for Shotcrete and its Preparation Method") and 202110916790.8 ("An Ultra-Early-Strength Fluorine-Free and Alkali-Free Liquid Accelerator and its Preparation Method"). In addition, higher performance requirements have been put forward for shotcrete in large-scale engineering construction, such as the requirement for ultra-early strength, chlorine-free, fluorine-free, and alkali-free properties.

[0004] Therefore, it is necessary to provide a concrete accelerator and its preparation method to solve the problems caused by the presence of chlorine, fluorine and alkali in existing accelerators, as well as the problems of instability in low-temperature storage and poor compatibility with cement-based materials. Summary of the Invention

[0005] The purpose of this invention is to provide a concrete quick-setting agent and its preparation method, the specific technical solution of which is as follows: In a first aspect, the present invention provides a method for preparing a concrete quick-setting agent, comprising: Step S1: Add 35-60 parts by weight of the main coagulant to 40-60 parts by weight of water at a temperature of 60-90℃, and obtain a first solution that is completely dissolved after the first stirring treatment; Step S2: Add 0.01 to 3 parts by weight of the coagulant and 0.5 to 10 parts by weight of the solubilizer to the first solution, and then perform a second stirring process to obtain a completely dissolved second solution. Step S3: Add 0.5 to 2.5 parts by weight of the complexing component to the second solution, and then perform a third stirring process to obtain a completely dissolved third solution; Step S4: After the temperature of the third solution drops to 60~70℃, add 0.5~10 parts by weight of the early-strength component and 0.1~5 parts by weight of the pH-adjusting component to the third solution, and then stir to obtain a completely dissolved fourth solution. Step S5: After the temperature of the fourth solution drops to 50~60℃, add 0.1~5 parts by weight of emulsion suspension stabilizer and 0.1~3 parts by weight of organic alcohol amino ester polymer to the fourth solution, and then stir to obtain a completely dissolved fifth solution. Step S6: After the temperature of the fifth solution drops to 35~40℃, add 0.1~10 parts by weight of the amine stabilizing component and 0.001~3 parts by weight of the nanomaterial component to the fifth solution, and then stir to obtain a completely dissolved sixth solution. Step S7: Add 0.01 to 3 parts by weight of thickening agent, 0.0001 to 0.06 parts by weight of surfactant agent and 0.005 to 0.5 parts by weight of water-reducing and defoaming agent to the sixth solution, and then perform a seventh stirring treatment to obtain a completely dissolved seventh solution; Step S8: Adjust the pH of the seventh solution to 2~4.5 using an alkaline solution, and then perform an eighth stirring process to obtain the eighth solution, which is cooled to room temperature, i.e., concrete quick-setting agent.

[0006] Optionally, the main coagulating component includes high aluminum-to-sulfur ratio polyaluminum sulfate; The preparation method of the high alumina-to-sulfur ratio type polyaluminum sulfate includes: Step A1: Add 10-40 parts by weight of aluminum sulfate to 60-120 parts by weight of water, heat to 25-35°C, and control the stirring speed to 200-300 r / min, stirring until the aluminum sulfate is completely dissolved to obtain the first aluminum sulfate aqueous solution. Step A2: In the first aluminum sulfate aqueous solution, the stirring rate is controlled at 200~500 r / min, and 10~30 parts by weight of catalyst ammonia aqueous solution are added dropwise over a time of 20~30 min. The volume concentration of the ammonia aqueous solution is 10%~35%. Subsequently, the pH of the first aluminum sulfate aqueous solution is adjusted to 5.5~6.5, and hydrolysis is carried out at a temperature of 30~50℃ for 4~6 h to prepare an aluminum hydroxide colloidal solution. Step A3: After filtering and washing the aluminum hydroxide colloidal solution, place it under vacuum drying at 50~80℃ for more than 24 hours to obtain aluminum hydroxide colloid. Step A4: Grind the aluminum hydroxide colloid into a fine powder and pass it through a 200-mesh square-hole sieve to obtain aluminum hydroxide amorphous powder; add 10-40 parts by weight of aluminum sulfate to 60-120 parts by weight of water, control the stirring speed at 100-300 r / min and the temperature at 30-40℃, and stir until the aluminum sulfate is completely dissolved to obtain a second aluminum sulfate aqueous solution; then, add 10-25 parts by weight of the aluminum hydroxide amorphous powder to the second aluminum sulfate aqueous solution, heat to 60-90℃, stir at a stirring speed of 100-300 r / min for 1-3 hours until completely dissolved, and cool to room temperature to obtain a high aluminum-sulfur ratio polyaluminum sulfate solution; Step A5: The high aluminum-sulfur ratio polyaluminum sulfate solution is dried by vacuum suction drying for 24-72 hours to obtain high aluminum-sulfur ratio polyaluminum sulfate solid; then, the high aluminum-sulfur ratio polyaluminum sulfate solid is ground and passed through a 200-mesh square hole sieve to obtain powdered high aluminum-sulfur ratio polyaluminum sulfate.

[0007] Optionally, in step A5, the vacuum suction drying process uses a suction negative pressure of -0.08 to -0.1 MPa and a drying temperature of 60 to 90°C.

[0008] Optionally, the preparation method of the emulsion suspension stabilizer includes: Step B1: Mix 10-25 parts by weight of acrylamide and 60-120 parts by weight of water, purge with nitrogen for protection, and control the stirring speed at 100-200 r / min. Heat to 70-95℃ until the mixture is completely dissolved to obtain an aqueous solution of acrylamide. Step B2: Mix 5-15 parts by weight of acrylic acid, 3-5 parts by weight of methacrylic acid, 2-5 parts by weight of acrylamide, 2-10 parts by weight of ammonium persulfate solution, 4-10 parts by weight of mercaptoacetic acid, and 2-10 parts by weight of potassium hydrogen tartrate, and then add the acrylamide aqueous solution dropwise at a constant rate to obtain a reaction system; control the pH of the reaction system to be 5-6, the dropwise rate to be 1-3 mL / min, the dropwise time to be no more than 3 h, and after the dropwise addition, keep the reaction at a constant temperature of 40-60℃ for 2-6 h to obtain an emulsion; Step B3: Adjust the pH of the emulsion to 7-8, and cool it to room temperature to obtain an emulsion suspension stabilizer.

[0009] Optionally, the method for preparing the organic alcohol amino ester polymer includes: Step C1: Heat 60-120 parts by weight of ethanol to 30-40°C at a stirring rate of 50-200 r / min. Step C2: Add 30-60 parts by weight of gallic acid to the ethanol, control the stirring speed at 100-200 r / min, and continue stirring for 30-60 min to ensure complete dissolution, so as to obtain a gallic acid alcohol solution. Step C3: Add 80-120 parts by weight of an alcohol amine and 4-10 parts by weight of an acidic catalyst to the gallic acid alcohol solution, heat to 80-85°C, and keep at this temperature for 2-3 hours to remove ethanol; then heat to 130°C, control the stirring rate at 100-300 r / min, and continue stirring for at least 4 hours; after the reaction is complete, allow it to cool naturally to room temperature to obtain a viscous liquid, which is the organic alcohol amine ester polymer.

[0010] Optionally, the alkanolamines include at least one of diethanolamine, triethanolamine, and triisopropanolamine; The gallic acid compounds include at least one of gallic acid, octyl gallate, and octadecyl gallate; The acidic catalyst includes at least one of p-toluenesulfonic acid ethanol solution and methanesulfonic acid.

[0011] Optionally, the coagulant component includes at least one of calcium sulfate, calcium nitrite, and calcium nitrate; The solubilizing agent includes at least one of aluminum formate, aluminum nitrate, and methacrylic acid. The complexing component includes at least one of ethylenediaminetetraacetic acid and sodium ethylenediaminetetraacetic acid; The early strength component includes at least one of calcium formate, lithium carbonate, urea, lithium oxalate, lithium hydroxide, magnesium sulfate, and magnesium sulfate heptahydrate. The pH adjusting ingredients include at least one of phosphoric acid, oxalic acid, sulfuric acid, citric acid, salicylic acid, tartaric acid, maleic acid, formic acid, ascorbic acid, and lactic acid. The amine stabilizing component includes at least one of diethanolamine, triethanolamine, triisopropanolamine, and diethanol monoisopropanolamine; The nanomaterial composition includes at least one of nano-silica, graphene, nano-titanium dioxide, and nano-alumina; The thickening component is one or more of polyacrylamide and hydroxycellulose; The surfactant component includes at least one of sodium dodecylbenzenesulfonate and sodium dodecyl sulfate; The water-reducing and defoaming components include at least one of the following: tributyl phosphate, tributyl citrate, butyl acetate, polyether-modified silicone oil, polycarboxylate water-reducing agent, naphthalene-based water-reducing agent, and sulfonate water-reducing agent.

[0012] Optionally, the stirring rate used in the first stirring treatment is 100~200 r / min, and the stirring time is 0.5~1 h; The second stirring treatment uses a stirring rate of 150~300 r / min and a stirring time of 0.5~2 h; The third stirring process uses a stirring rate of 150~300 r / min and a stirring time of 10~45 min; The fourth stirring process uses a stirring rate of 200-300 r / min and a stirring time of 10-50 min. The fifth stirring process uses a stirring rate of 100~200 r / min and a stirring time of not less than 3 hours. The sixth stirring process uses a stirring rate of 300-400 r / min and a stirring time of 5-30 min. The seventh stirring process uses a stirring rate of 100~200 r / min and a stirring time of not less than 1 hour. The eighth stirring process uses a stirring rate of 100~200 r / min and a stirring time of not less than 3 h.

[0013] Optionally, the method for preparing the concrete accelerator may further include sealing and storing the prepared concrete accelerator.

[0014] In a second aspect, the present invention provides a concrete accelerator, which is prepared by the method described above.

[0015] The application of the technical solution of the present invention has at least the following beneficial effects: (1) The present invention provides a method for preparing a concrete accelerator, which not only produces an alkali-free, fluorine-free, and chlorine-free concrete accelerator, but also enables the prepared concrete accelerator to possess advantages such as ultra-early strength, durability, high cost-effectiveness, low-temperature storage stability, and good compatibility with cement-based materials. Specifically: Regarding the absence of alkali, fluorine, and chlorine, this invention uses alkali-free, fluorine-free, and chlorine-free raw materials, and no toxic substances are generated or emitted during the preparation process. It does not endanger human health or pollute the environment during production and use.

[0016] In terms of good compatibility and storage stability, the concrete accelerator prepared by this invention is compatible with conventional cement, admixtures and additives, and does not affect the workability and construction performance of on-site concrete. In addition, the concrete accelerator prepared by this invention can be stored stably for a long time in room temperature and low temperature environments without flocculation, precipitation and crystallization.

[0017] In terms of early-strength performance, durability, and cost-effectiveness, the concrete accelerator prepared by this invention can significantly shorten the setting time of cement-based materials, improve the early strength of concrete, significantly reduce the shrinkage rate of concrete, and effectively promote the durability of concrete. Furthermore, the raw materials used in this invention are readily available and inexpensive, greatly improving the cost-effectiveness of the concrete accelerator.

[0018] (2) The method for preparing a concrete quick-setting agent provided by the present invention is not only simple in process, but also has mild reaction conditions, which is convenient for industrial production.

[0019] (3) The high-alumina-to-sulfur ratio polyaluminum sulfate, the main coagulating component prepared in this invention, not only achieves rapid coagulation under the premise of "alkali-free and halogen-free", but also improves early strength, compatibility, and the retention of later strength. Specifically: In terms of rapid setting, the high aluminum-to-sulfur ratio polyaluminum sulfate prepared by this invention essentially forms a system in which high-aluminum / high-basicity polyaluminum species (polynuclear hydroxyl aluminum complex / polymer ions) coexist with sulfate ions. This system contains polymeric aluminum, which hydrolyzes faster than monomeric aluminum salt, generates more aluminum hydroxyl complexes, and has stronger charge neutralization / adsorption bridging on the negative potential points on the surface of cement particles. It is more likely to induce the rapid "bridging-flocculation-network formation" of cement paste structure, which manifests as rapid loss of plasticity and accelerated setting, thus achieving a rapid setting effect.

[0020] Regarding the improvement of early strength, the high alumina-to-sulfur ratio polyaluminum sulfate prepared in this invention essentially forms a system in which high alumina / high basicity polyaluminum species (polynuclear hydroxyaluminum complex / polymer ions) coexist with sulfate ions. This system can rapidly provide Al in the presence of sulfate ions. 3+ / Polyaluminum species, and Ca released during cement hydration 2+SO4 in solution 2- Together, they promote the early formation of ettringite and other crystal networks, thereby shortening the initial and final setting times and increasing the early strength development rate. Furthermore, high-alumina-sulfur ratio polyaluminum sulfate has a large specific surface area and high solubility / reactivity, which can further shorten the initial and final setting times and increase the early strength development rate.

[0021] In terms of improving compatibility, compared with conventional aluminum sulfate, the high aluminum-to-sulfur ratio polyaluminum sulfate prepared in this invention contains high-aluminum / high-basicity polyaluminum species, which makes its action in cement systems more stable and mild. It is less likely to cause sudden hydrolytic disturbance to cement paste, and can better adapt to different cement, admixture and additive systems, reducing abnormal flocculation, crystallization and fluctuations in construction performance. This improves the compatibility between concrete accelerators and cement-based materials and is beneficial to the maintenance of strength in the later stage.

[0022] In terms of maintaining strength in the later stages, compared with traditional high-alkali or fluorine / chlorine-containing systems, the high aluminum-to-sulfur ratio polyaluminum sulfate prepared by this invention is more likely to work at pH values ​​of 2 to 4.5, reducing alkali corrosion and adverse effects on cement systems, which is beneficial to the goals of strength retention and durability.

[0023] (4) The emulsion suspension stabilizer prepared by this invention can not only significantly improve the storage stability of concrete accelerators at room temperature / low temperature and inhibit flocculation, precipitation, gelation and crystallization, but also improve the dispersion uniformity of the concrete accelerator system, indirectly ensuring the acceleration efficiency and strength stability. Specifically: Regarding storage stability, emulsion suspension stabilizers contain carboxyl groups (-COO). - / -COOH) and amide group (-CONH) 2 (Ammonium salt form) The carboxyl sites of the suspension stabilizer can form a weak complexation / adsorption equilibrium with polyvalent metal ions, and the complexation components can capture excess free metal ions; the carboxyl sites of the suspension stabilizer can coordinate and buffer with the amine stabilizing components, making the aluminum species in the solution more stable and less prone to sudden hydrolysis and gelation, thereby improving storage stability and construction fluctuation control; the amide group can provide a hydration layer and hydrogen bonding, enhancing solvation stability; in the preparation of the emulsion suspension stabilizer, mercaptoacetic acid is used to regulate the emulsion suspension stabilizer to an appropriate molecular weight, avoiding excessive thickening / bridging flocculation caused by excessively high molecular weight, while ensuring sufficient stability and thickening capacity of the concrete accelerator; potassium hydrogen tartrate and pH value are used in the preparation of the emulsion suspension stabilizer to facilitate the maintenance of ionic environment and complexation balance of the concrete accelerator, ensuring sufficient storage stability of the concrete accelerator.

[0024] Regarding dispersion uniformity, the emulsion suspension stabilizer inhibits sedimentation / gelation of concrete accelerators through a triple mechanism of "electrostatic stabilization + steric hindrance + hydration layer," ensuring the uniform dispersion of the concrete accelerator. Specifically, the emulsion suspension stabilizer adsorbs onto the surface of colloidal / microparticles in the concrete accelerator, imparting a surface charge; it forms a polymer chain layer around the particles, providing steric hindrance; and it provides a strong hydration layer, reducing the probability of effective collision and adhesion between particles, thereby significantly reducing the possibility of flocculation, sedimentation, and gel formation, ensuring the uniform dispersion of the concrete accelerator.

[0025] (5) The organic alcohol amine ester polymer prepared in this invention can form a synergistic effect with high aluminum-to-sulfur ratio polyaluminum sulfate, alcohol amine stabilizing components, and calcium ions released during cement hydration, thereby taking into account the efficiency of setting, early strength development, and later strength retention. Specifically, the organic alcohol amine ester polymer molecule contains alcohol amine groups and ester structural units. The alcohol amine groups can coordinate and stabilize aluminum ions and other polyvalent metal ions, mitigate the local sudden hydrolysis of highly active aluminum species in the solution, reduce system fluctuations, and avoid excessive concentration of the setting reaction. The ester structural units can improve the distribution of the setting components on the surface of cement particles through adsorption, complexation, and interface regulation, making them participate more uniformly in the early hydration reaction of cement. Thus, the organic alcohol amine ester polymer not only helps to reduce the performance fluctuations of concrete accelerators during storage and use, improve system uniformity and construction stability, but also reduces the defects in the paste structure caused by localized excessively rapid setting, promotes the uniform generation of hydration products and the densification of the internal structure, thereby improving the compressive strength and strength retention rate of the sample.

[0026] In addition to the objectives, features, and advantages described above, the present invention has other objectives, features, and advantages. The invention will now be described in further detail with reference to the figures. Attached Figure Description

[0027] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.

[0028] Figure 1 This is a schematic flowchart of a method for preparing a concrete quick-setting agent in Example 1.

[0029] Figure 2 This is a schematic flowchart of the preparation method of high aluminum-to-sulfur ratio polyaluminum sulfate in Example 1.

[0030] Figure 3This is a schematic flowchart of the emulsion suspension stabilizer preparation method in Example 1.

[0031] Figure 4 This is a schematic flowchart of the method for preparing the organic alcohol amino ester polymer in Example 1. Detailed Implementation

[0032] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0033] Example 1: See Figure 1 A method for preparing a concrete quick-setting agent, comprising: Step S1: Add 40 parts by weight of the main coagulating component to 50 parts by weight of water at 70°C, and perform a first stirring treatment in a four-necked flask equipped with a mechanical stir bar to obtain a completely dissolved first solution (i.e., Figure 1 medium transparent solution); Step S2: Add 0.5 parts by weight of the coagulant and 1 part by weight of the solubilizer to the first solution, and then perform a second stirring process to obtain a completely dissolved second solution (i.e., Figure 1 (First clear solution) Step S3: Add two parts by weight of the complexing component to the second solution, and then perform a third stirring process to obtain a completely dissolved third solution (i.e., Figure 1 (Second clear solution); Step S4: After the temperature of the third solution drops to 60~70℃ (specifically 65℃), add 1.5 parts by weight of the early-strength component and 3.1 parts by weight of the pH-adjusting component to the third solution, and then perform a fourth stirring process to obtain a completely dissolved fourth solution (i.e., Figure 1 medium solution); Step S5: After the temperature of the fourth solution drops to 55°C, add 0.2 parts by weight of emulsion suspension stabilizer and 0.1 parts by weight of organic alcohol amino ester polymer to the fourth solution, and then perform a fifth stirring treatment to obtain a completely dissolved fifth solution (i.e. Figure 1 (The first clear emulsion in China). Step S6: After the temperature of the fifth solution drops to 40°C, add 5 parts by weight of the amine stabilizing component and 1 part by weight of the nanomaterial component to the fifth solution, and then perform a sixth stirring treatment to obtain a completely dissolved sixth solution (i.e., Figure 1(Second clear emulsion). Step S7: Add 0.2 parts by weight of thickening agent, 0.05 parts by weight of surfactant agent, and 0.04 parts by weight of water-reducing and defoaming agent to the sixth solution, and then perform a seventh stirring treatment to obtain a completely dissolved seventh solution (i.e. Figure 1 (Medium emulsion); Step S8: Adjust the pH of the seventh solution to 3 using an alkaline solution, and then perform an eighth stirring treatment to obtain the eighth solution, which is cooled to room temperature; this is the concrete accelerator. The prepared concrete accelerator is then sealed and stored (i.e., [the product is obtained]). Figure 1 (The quick-setting agent in the finished product).

[0034] The main coagulating component is high aluminum-to-sulfur ratio polyaluminum sulfate; See Figure 2 The preparation method of the high aluminum-to-sulfur ratio polyaluminum sulfate includes: Step A1: Add 34.2 parts by weight of aluminum sulfate to 100 parts by weight of water, heat to 30°C, and control the stirring speed at 200~300 r / min (specifically 300 r / min) until the aluminum sulfate is completely dissolved, to obtain the first aluminum sulfate aqueous solution (i.e. Figure 2 (a transparent solution); wherein, the reaction apparatus for obtaining the first aluminum sulfate aqueous solution is a four-necked flask equipped with a heater, a thermometer, and a stirrer; Step A2: In the first aluminum sulfate aqueous solution, the stirring speed is controlled at 200~500 r / min (specifically 400 r / min), and 20 parts by weight of ammonia solution are added dropwise over a time of 20~30 min (specifically 20 min). The volume concentration of the ammonia solution is 20%. Subsequently, the pH of the first aluminum sulfate aqueous solution is adjusted to 6, and hydrolysis is carried out at 40℃ for 5 h to prepare an aluminum hydroxide colloidal solution (i.e., Figure 2 (medium colloidal solution); Step A3: After filtering the aluminum hydroxide colloidal solution and washing it with water three times, place it under vacuum drying at 80°C for 24 hours to obtain aluminum hydroxide colloid. Step A4: Grind the aluminum hydroxide colloid using a mechanical grinding mill and pass it through a 200-mesh square-hole sieve to obtain amorphous aluminum hydroxide powder; add 34.2 parts by weight of aluminum sulfate to 100 parts by weight of water, control the stirring speed at 200 r / min, control the temperature at 30℃, and stir until the aluminum sulfate is completely dissolved to obtain a second aluminum sulfate aqueous solution (i.e. Figure 2The reaction apparatus for obtaining the second aluminum sulfate aqueous solution is a four-necked flask equipped with a heater, a thermometer, and a stirrer; then, 17.1 parts by weight of the amorphous aluminum hydroxide powder are added to the second aluminum sulfate aqueous solution, heated to 70°C, stirred at a stirring rate of 300 r / min for 2 hours until completely dissolved, and cooled to room temperature to obtain a high aluminum-sulfur ratio type polyaluminum sulfate solution; Step A5: The high alumina-to-sulfur ratio polyaluminum sulfate solution is dried using vacuum suction drying for 72 hours to obtain high alumina-to-sulfur ratio polyaluminum sulfate solid (i.e., Figure 2 The high-alumina-sulfur ratio polyaluminum sulfate solid was then ground finely using a mechanical grinding mill and passed through a 200-mesh square-hole sieve to obtain powdered high-alumina-sulfur ratio polyaluminum sulfate (i.e.,...). Figure 2 (Middle powder material).

[0035] In step A5, the vacuum suction drying process uses a suction negative pressure of -0.08 MPa and a drying temperature of 80°C.

[0036] See Figure 3 The preparation method of the emulsion suspension stabilizer includes: Step B1: Mix 20 parts by weight of acrylamide and 100 parts by weight of water, purge with nitrogen for protection, and control the stirring speed at 100-200 r / min (specifically 200 r / min). Heat to 85°C until completely dissolved, obtaining an aqueous solution of acrylamide (i.e., Figure 3 The reaction apparatus for obtaining an aqueous solution of acryloylammonium was a four-necked flask equipped with a temperature control device, a reflux condenser, and a stirrer; Step B2: Mix 10 parts by weight of acrylic acid, 4.3 parts by weight of methacrylic acid, 2 parts by weight of acryloylammonium, 5 parts by weight of ammonium persulfate solution (mass concentration of 2%), 4.6 parts by weight of mercaptoacetic acid, and 10 parts by weight of potassium hydrogen tartrate, and then add the acryloylammonium aqueous solution dropwise at a uniform rate to obtain a reaction system; control the pH of the reaction system to be 5-6 (specifically 5.5), the uniform dropping rate to be 1-3 mL / min, the uniform dropping time to be no more than 3 h, and after the dropping, keep the reaction at a constant temperature of 40 °C for 4 h to obtain an emulsion; Step B3: Adjust the pH of the emulsion to 7, and cool it to room temperature to obtain the emulsion suspension stabilizer. Transfer the emulsion suspension stabilizer to a sealed bottle for storage.

[0037] See Figure 4 The method for preparing the organic alcohol amino ester polymer includes: Step C1: Add 100 parts by weight of ethanol to a four-necked flask equipped with a stirrer, heating device, thermometer and reflux condenser, and heat to 30°C at a stirring rate of 50~200 r / min (specifically 100 r / min). Step C2: Add 50 parts by weight of gallic acid to the ethanol, and control the stirring speed at 100-200 r / min (specifically 200 r / min) for 30 min to ensure complete dissolution, thus obtaining a gallic acid alcohol solution (i.e., Figure 4 medium transparent solution); Step C3: Add 100 parts by weight of an alcohol amine and 6 parts by weight of an acidic catalyst to the gallic acid alcohol solution, heat to 80°C and keep warm for 2-3 hours (specifically 2.5 hours) to evaporate ethanol and obtain an emulsion solution; then heat to 130°C, control the stirring rate at 200 r / min, and continue stirring for more than 4 hours; after the reaction is completed, cool naturally to room temperature to obtain a viscous liquid, which is the organic alcohol amine ester polymer.

[0038] The alkanolamines include at least one of diethanolamine, triethanolamine, and triisopropanolamine, specifically triethanolamine; The gallic acid compounds include at least one of gallic acid, octyl gallate, and octadecyl gallate, specifically octadecyl gallate. The acidic catalyst includes at least one of p-toluenesulfonic acid ethanol solution and methanesulfonic acid, specifically a p-toluenesulfonic acid ethanol solution with a mass concentration of 50%.

[0039] The coagulant component includes at least one of calcium sulfate, calcium nitrite, and calcium nitrate, specifically calcium nitrate; The solubilizing component includes at least one of aluminum formate, aluminum nitrate, and methacrylic acid, specifically aluminum formate; The complexing component includes at least one of ethylenediaminetetraacetic acid (EDTA) and sodium EDTA, specifically EDTA. The early strength component includes at least one of calcium formate, lithium carbonate, urea, lithium oxalate, lithium hydroxide, magnesium sulfate, and magnesium sulfate heptahydrate, specifically calcium formate. The pH adjusting component includes at least one of phosphoric acid, oxalic acid, sulfuric acid, citric acid, salicylic acid, tartaric acid, maleic acid, formic acid, ascorbic acid, and lactic acid, specifically 0.1 parts by weight of phosphoric acid and 3 parts by weight of oxalic acid. The amine stabilizing component includes at least one of diethanolamine, triethanolamine, triisopropanolamine and diethanol monoisopropanolamine, specifically 3 parts by weight of diethanolamine, 1 part by weight of triethanolamine and 1 part by weight of diethanol monoisopropanolamine. The nanomaterial composition includes at least one of nano-silica, graphene, nano-titanium dioxide, and nano-alumina, specifically nano-silica; The thickening component is one or more of polyacrylamide and hydroxycellulose, specifically polyacrylamide; The surfactant includes at least one of sodium dodecylbenzenesulfonate and sodium dodecyl sulfate, specifically sodium dodecylbenzenesulfonate; The water-reducing and defoaming components include at least one of the following: tributyl phosphate, tributyl citrate, butyl acetate, polyether-modified silicone oil, polycarboxylate superplasticizer, naphthalene superplasticizer, and sulfonate superplasticizer, specifically 0.01 parts by weight of tributyl phosphate and 0.03 parts by weight of polycarboxylate superplasticizer.

[0040] The first stirring process uses a stirring rate of 100 r / min and a stirring time of 1 h; The second stirring treatment uses a stirring rate of 200 r / min and a stirring time of 1 h; The third stirring process uses a stirring rate of 200 r / min and a stirring time of 30 min. The fourth stirring process uses a stirring rate of 200 r / min and a stirring time of 30 min. The fifth stirring process uses a stirring rate of 100~200 r / min (specifically 100 r / min) and a stirring time of not less than 3 hours. The sixth stirring process uses a stirring rate of 300 r / min and a stirring time of 30 min. The seventh stirring process uses a stirring rate of 200 r / min and a stirring time of not less than 1 hour. The eighth stirring process uses a stirring rate of 100 r / min and a stirring time of not less than 3 h.

[0041] Example 2: Unlike Example 1, in step S1, the main coagulating component, high aluminum-to-sulfur ratio polyaluminum sulfate, has a weight ratio of 45 parts; in step S2, the solubilizing component, aluminum formate, has a weight ratio of 1.5 parts; and in step S4, the pH adjusting component, phosphoric acid, has a weight ratio of 0.5 parts.

[0042] Example 3: Unlike Example 1, the amount of triethanolamine used in the preparation of the organic alcohol amine ester polymer was 150 parts by weight.

[0043] Example 4: Unlike Example 1, in step S5 the organic alcohol amine ester polymer is 0.2 parts by weight; in step S6 the alcohol amine stabilizing components are 3.5 parts by weight of diethanolamine, 0.5 parts by weight of triethanolamine and 1.5 parts by weight of diethanol monoisopropanolamine.

[0044] Example 5: Unlike Example 1, in step S5 the emulsion suspension stabilizer is 0.3 parts by weight; in step S6 the nanomaterial component nano silica is 3 parts by weight.

[0045] Example 6: Unlike Example 1, in step S4, the early-strength component calcium formate is 2 parts by weight; in step S4, the pH-adjusting components are 0.6 parts by weight of phosphoric acid and 3.5 parts by weight of oxalic acid.

[0046] Comparative Example 1: Unlike Example 1, no pH adjustment component was used in step S4.

[0047] Comparative Example 2: Unlike Example 1, organic alcohol amino ester polymers were not used in step S5.

[0048] Comparative Example 3: Unlike Example 1, no emulsion suspension stabilizer was used in step S5.

[0049] Comparative Example 4: Unlike Example 1, no nanomaterials were used in step S6 and no thickening agents were used in step S7.

[0050] Comparative Example 5: Unlike Example 1, the early-strength component was not used in step S4.

[0051] Comparative Example 6: Unlike Example 1, the main coagulating component in step S1, high aluminum-to-sulfur ratio polyaluminum sulfate, is replaced with conventional aluminum sulfate.

[0052] The concrete accelerators prepared in Examples 1-6 and Comparative Examples 1-6 were subjected to performance tests, and the test results are shown in Table 1. The specific test methods are as follows: Appearance test method: The appearance is inspected in accordance with GB / T 8077-2023 "Test method for homogeneity of concrete admixtures", and the color, transparency and presence of layering, flocculation, precipitation or crystallization of the sample are recorded under the same lighting, background and container conditions.

[0053] pH value test method: According to GB / T 8077-2023. First, drop the concrete quick-setting agent solution to be tested onto pH test paper and let it stand for 3 minutes; then, compare it with the colorimetric card to determine the pH value.

[0054] Solid content test method: The solid content was determined according to GB / T 35159-2017 "Accelerating Agents for Shotcrete". First, the mass of the covered petri dish was measured as m0. Then, the accelerating agent to be tested was thoroughly shaken, and 10g was weighed using an analytical balance, obtaining the total mass of the petri dish and sample as m1. Finally, the petri dish containing the sample was opened and placed in an oven at 105℃ to dry. The petri dish was removed, covered, and placed in a desiccator to cool for 30 minutes before weighing. The above steps were repeated until a constant weight was obtained, yielding the mass as m2. The solid content S = (m2 - m0) / (m1 - m0) × 100%.

[0055] Density test method: The density is tested in accordance with GB / T 8077-2023 "Test method for homogeneity of concrete admixtures".

[0056] The testing methods for setting time, compressive strength, and strength retention rate were conducted according to GB / T 35159-2017 "Accelerating Agents for Shotcrete". Reference cement and standard sand were used as raw materials. The setting time of cement paste and the compressive strength of mortar were tested using a DL-AWK Vicat apparatus and a YAW-300 mortar pressure testing machine, respectively. The dosage of concrete accelerator was 6% of the cement mass. For the setting time test, the water-cement ratio of the cement paste was 0.35, the material temperature was controlled between (20±2)℃, and the ambient humidity was not less than 90%. For the mortar compressive strength test, the mortar mix ratio was water:cement:standard sand = 1:2:3, the specimen size was 40mm×40mm×160mm, the curing temperature was (20±2)℃, and the ambient humidity was not less than 90%. The compressive strength of the specimens was tested after 1 day and 28 days of curing. Simultaneously, specimens without concrete accelerator were molded for strength retention rate calculation. Three parallel samples were tested in each group, and the average value was taken.

[0057] Room temperature stability test method: After shaking the concrete accelerator to be tested evenly, pour it into a 100ml stoppered graduated cylinder, align it with the scale, and tighten the stopper. Place it at a temperature of 20±2℃, and measure the volume of the supernatant in the graduated cylinder at regular intervals (7d, 30d, 90d).

[0058] Low-temperature stability test method: The test is conducted in accordance with GB / T 8077-2023 "Test method for homogeneity of concrete admixtures". Visual inspection is conducted to observe whether the concrete accelerator exhibits stratification, crystallization or precipitation after standing at a low temperature (-5℃) for a specified time.

[0059] Table 1 Test Results

[0060] From the data in Table 1, we know that: Compared with Comparative Examples 1-6, the concrete accelerators prepared in Examples 1-6 of this invention have shorter setting time, higher compressive strength, better strength retention rate, and good room temperature and low temperature stability. Moreover, their performance meets the relevant requirements of GB / T 35159-2017 "Accelerators for Shotcrete".

[0061] Comparing Example 1 and Comparative Example 1, it is evident that the absence of a pH-adjusting component in Comparative Example 1 resulted in a prolonged setting time for the prepared concrete accelerator, and a decrease in the compressive strength and strength retention rate at all ages of the sample. This indicates that the use of a pH-adjusting component can effectively promote early cement hydration and impart stronger mechanical properties to the cement. Furthermore, the concrete accelerator prepared in Comparative Example 1 also exhibited a small amount of gel. This is because without the use of a pH-adjusting component, it is difficult to maintain the acidity and ion balance of the system within a suitable range, leading to more uneven hydrolysis and aggregation of highly reactive aluminum species in the local environment, further forming aluminum hydroxyl aggregates or colloids. Simultaneously, the coordination / complexation balance between various metal ions, complexing components, and alkanolamine stabilizing components in the system is disrupted, making the concrete accelerator more prone to local cross-linking and thickening during storage and mixing, thus producing a small amount of gel.

[0062] Comparing Example 1 and Comparative Example 2, it is evident that the absence of an organic alcohol amino ester polymer in Comparative Example 2 resulted in a shorter setting time and a decrease in compressive strength and strength retention rate of the concrete accelerator prepared in Comparative Example 2. This indicates that the use of an organic alcohol amino ester polymer can effectively regulate the release and action process of active aluminum species in the concrete accelerator, improve the uniformity of the accelerating reaction, and avoid the adverse effects of excessively rapid local setting on the paste structure, thereby improving the compressive strength and strength retention rate of the sample.

[0063] Comparing Example 1 and Comparative Example 3, it is evident that the absence of an emulsion suspension stabilizer in Comparative Example 3 resulted in decreased room temperature and low temperature stability of the concrete accelerator prepared in Comparative Example 3, leading to partial precipitation and gelation. This indicates that the use of an emulsion suspension stabilizer can significantly improve the storage stability of the concrete accelerator at room temperature / low temperature, inhibiting flocculation, precipitation, gelation, and crystallization.

[0064] Comparing Example 1 and Comparative Example 4, it is evident that the absence of nanomaterials and thickening agents in Comparative Example 4 resulted in a prolonged setting time and decreased compressive strength and strength retention rate in the concrete accelerator prepared in Comparative Example 4. This indicates that the use of nanomaterials and thickening agents can thicken the system, shorten the setting time, and improve compressive strength and strength retention rate. Furthermore, a small amount of gelation occurred in the concrete accelerator prepared in Comparative Example 4. This is because the absence of nanomaterials and thickening agents in Comparative Example 4 led to a decrease in the dispersion stability and suspension capacity of the concrete accelerator system. The active aluminum species in the main accelerator and their synergistic calcium and sulfate ion components were more prone to local aggregation and uneven reaction, resulting in the formation of a small amount of gel.

[0065] Comparing Example 1 and Comparative Example 5, it is evident that the absence of an early-strength component in Comparative Example 5 resulted in a prolonged setting time and a decrease in compressive strength and strength retention rate of the concrete accelerator prepared in Comparative Example 5. This indicates that the use of an early-strength component can effectively improve the early hardening rate of cement and promote the cement hydration reaction.

[0066] Comparing Example 1 and Comparative Example 6, it is evident that in Comparative Example 6, replacing the high-alumina-sulfur ratio polyaluminum sulfate as the main accelerator with conventional aluminum sulfate resulted in a prolonged setting time and a decrease in compressive strength and strength retention rate of the concrete accelerator prepared in Comparative Example 6. This indicates that using high-alumina-sulfur ratio polyaluminum sulfate as the main accelerator can still achieve rapid setting and improve early strength and later strength retention. Furthermore, the concrete accelerator prepared in Comparative Example 6 also exhibited significant crystallization / precipitation. This is because conventional aluminum sulfate has a lower degree of polymerization and poorer aluminum species stability, making it more prone to local hydrolysis and aggregation in the system, and precipitating under the influence of temperature and ionic environment changes, thus leading to significant crystallization / precipitation.

[0067] The above description is only a preferred embodiment of the present invention and does not limit the scope of the present invention. All equivalent structural transformations made under the inventive concept of the present invention using the contents of the present invention specification and drawings, or direct / indirect applications in other related technical fields, are included within the protection scope of the present invention.

Claims

1. A method for preparing a concrete quick-setting agent, characterized in that, include: Step S1: Add 35-60 parts by weight of the main coagulant to 40-60 parts by weight of water at a temperature of 60-90℃, and obtain a first solution that is completely dissolved after the first stirring treatment; Step S2: Add 0.01 to 3 parts by weight of the coagulant and 0.5 to 10 parts by weight of the solubilizer to the first solution, and then perform a second stirring process to obtain a completely dissolved second solution. Step S3: Add 0.5 to 2.5 parts by weight of the complexing component to the second solution, and then perform a third stirring process to obtain a completely dissolved third solution; Step S4: After the temperature of the third solution drops to 60~70℃, add 0.5~10 parts by weight of the early-strength component and 0.1~5 parts by weight of the pH-adjusting component to the third solution, and then stir to obtain a completely dissolved fourth solution. Step S5: After the temperature of the fourth solution drops to 50~60℃, add 0.1~5 parts by weight of emulsion suspension stabilizer and 0.1~3 parts by weight of organic alcohol amino ester polymer to the fourth solution, and then stir to obtain a completely dissolved fifth solution. Step S6: After the temperature of the fifth solution drops to 35~40℃, add 0.1~10 parts by weight of the amine stabilizing component and 0.001~3 parts by weight of the nanomaterial component to the fifth solution, and then stir to obtain a completely dissolved sixth solution. Step S7: Add 0.01 to 3 parts by weight of thickening agent, 0.0001 to 0.06 parts by weight of surfactant agent and 0.005 to 0.5 parts by weight of water-reducing and defoaming agent to the sixth solution, and then perform a seventh stirring treatment to obtain a completely dissolved seventh solution; Step S8: Adjust the pH of the seventh solution to 2-4.5 using an alkaline solution, and then perform an eighth stirring process to obtain the eighth solution, which is cooled to room temperature; this is the concrete quick-setting agent. The main coagulating component includes high aluminum-to-sulfur ratio polyaluminum sulfate; The preparation method of the high alumina-to-sulfur ratio type polyaluminum sulfate includes: Step A1: Add 10-40 parts by weight of aluminum sulfate to 60-120 parts by weight of water, heat to 25-35°C, and control the stirring speed to 200-300 r / min, stirring until the aluminum sulfate is completely dissolved to obtain the first aluminum sulfate aqueous solution. Step A2: In the first aluminum sulfate aqueous solution, the stirring rate is controlled at 200~500 r / min, and 10~30 parts by weight of catalyst ammonia aqueous solution are added dropwise over a time of 20~30 min. The volume concentration of the ammonia aqueous solution is 10%~35%. Subsequently, the pH of the first aluminum sulfate aqueous solution is adjusted to 5.5~6.5, and hydrolysis is carried out at a temperature of 30~50℃ for 4~6 h to prepare an aluminum hydroxide colloidal solution. Step A3: After filtering and washing the aluminum hydroxide colloidal solution, place it under vacuum drying at 50~80℃ for more than 24 hours to obtain aluminum hydroxide colloid. Step A4: Grind the aluminum hydroxide colloid into a fine powder and pass it through a 200-mesh square-hole sieve to obtain aluminum hydroxide amorphous powder; add 10-40 parts by weight of aluminum sulfate to 60-120 parts by weight of water, control the stirring speed at 100-300 r / min and the temperature at 30-40℃, and stir until the aluminum sulfate is completely dissolved to obtain a second aluminum sulfate aqueous solution; then, add 10-25 parts by weight of the aluminum hydroxide amorphous powder to the second aluminum sulfate aqueous solution, heat to 60-90℃, stir at a stirring speed of 100-300 r / min for 1-3 hours until completely dissolved, and cool to room temperature to obtain a high aluminum-sulfur ratio polyaluminum sulfate solution; Step A5: The high aluminum-sulfur ratio polyaluminum sulfate solution is dried by vacuum suction drying for 24-72 hours to obtain high aluminum-sulfur ratio polyaluminum sulfate solid; then, the high aluminum-sulfur ratio polyaluminum sulfate solid is ground and passed through a 200-mesh square hole sieve to obtain powdered high aluminum-sulfur ratio polyaluminum sulfate. The preparation method of the organic alcohol amino ester polymer includes: Step C1: Heat 60-120 parts by weight of ethanol to 30-40°C at a stirring rate of 50-200 r / min. Step C2: Add 30-60 parts by weight of gallic acid to the ethanol, control the stirring speed at 100-200 r / min, and continue stirring for 30-60 min to ensure complete dissolution, so as to obtain a gallic acid alcohol solution. Step C3: Add 80-120 parts by weight of an alcohol amine and 4-10 parts by weight of an acidic catalyst to the gallic acid alcohol solution, heat to 80-85°C, and keep at this temperature for 2-3 hours to remove ethanol; then heat to 130°C, control the stirring rate at 100-300 r / min, and continue stirring for at least 4 hours; after the reaction is complete, allow it to cool naturally to room temperature to obtain a viscous liquid, which is the organic alcohol amine ester polymer.

2. The method for preparing the concrete quick-setting agent as described in claim 1, characterized in that, In step A5, the vacuum suction drying process uses a suction negative pressure of -0.08 to -0.1 MPa and a drying temperature of 60 to 90°C.

3. The method for preparing the concrete quick-setting agent as described in claim 1, characterized in that, The preparation method of the emulsion suspension stabilizer includes: Step B1: Mix 10-25 parts by weight of acrylamide and 60-120 parts by weight of water, purge with nitrogen for protection, and control the stirring speed at 100-200 r / min. Heat to 70-95℃ until the mixture is completely dissolved to obtain an aqueous solution of acrylamide. Step B2: Mix 5-15 parts by weight of acrylic acid, 3-5 parts by weight of methacrylic acid, 2-5 parts by weight of acrylamide, 2-10 parts by weight of ammonium persulfate solution, 4-10 parts by weight of mercaptoacetic acid, and 2-10 parts by weight of potassium hydrogen tartrate, and then add the acrylamide aqueous solution dropwise at a constant rate to obtain a reaction system; control the pH of the reaction system to be 5-6, the dropwise rate to be 1-3 mL / min, the dropwise time to be no more than 3 h, and after the dropwise addition, keep the reaction at a constant temperature of 40-60℃ for 2-6 h to obtain an emulsion; Step B3: Adjust the pH of the emulsion to 7-8, and cool it to room temperature to obtain an emulsion suspension stabilizer.

4. The method for preparing the concrete quick-setting agent as described in claim 1, characterized in that, The alkanolamines include at least one of diethanolamine, triethanolamine, and triisopropanolamine; The gallic acid compounds include at least one of gallic acid, octyl gallate, and octadecyl gallate; The acidic catalyst includes at least one of p-toluenesulfonic acid ethanol solution and methanesulfonic acid.

5. The method for preparing the concrete quick-setting agent as described in claim 1, characterized in that, The coagulant component includes at least one of calcium sulfate, calcium nitrite, and calcium nitrate. The solubilizing agent includes at least one of aluminum formate, aluminum nitrate, and methacrylic acid. The complexing component includes at least one of ethylenediaminetetraacetic acid and sodium ethylenediaminetetraacetic acid; The early strength component includes at least one of calcium formate, lithium carbonate, urea, lithium oxalate, lithium hydroxide, magnesium sulfate, and magnesium sulfate heptahydrate. The pH adjusting ingredients include at least one of phosphoric acid, oxalic acid, sulfuric acid, citric acid, salicylic acid, tartaric acid, maleic acid, formic acid, ascorbic acid, and lactic acid. The amine stabilizing component includes at least one of diethanolamine, triethanolamine, triisopropanolamine, and diethanol monoisopropanolamine; The nanomaterial composition includes at least one of nano-silica, graphene, nano-titanium dioxide, and nano-alumina; The thickening component is one or more of polyacrylamide and hydroxycellulose; The surfactant component includes at least one of sodium dodecylbenzenesulfonate and sodium dodecyl sulfate; The water-reducing and defoaming components include at least one of the following: tributyl phosphate, tributyl citrate, butyl acetate, polyether-modified silicone oil, polycarboxylate water-reducing agent, naphthalene-based water-reducing agent, and sulfonate water-reducing agent.

6. The method for preparing the concrete quick-setting agent as described in claim 1, characterized in that, The stirring rate used in the first stirring treatment is 100~200 r / min, and the stirring time is 0.5~1 h; The second stirring treatment uses a stirring rate of 150~300 r / min and a stirring time of 0.5~2 h; The third stirring process uses a stirring rate of 150~300 r / min and a stirring time of 10~45 min; The fourth stirring process uses a stirring rate of 200-300 r / min and a stirring time of 10-50 min. The fifth stirring process uses a stirring rate of 100~200 r / min and a stirring time of not less than 3 hours. The sixth stirring process uses a stirring rate of 300-400 r / min and a stirring time of 5-30 min. The seventh stirring process uses a stirring rate of 100~200 r / min and a stirring time of not less than 1 hour. The eighth stirring process uses a stirring rate of 100~200 r / min and a stirring time of not less than 3 h.

7. The method for preparing the concrete quick-setting agent as described in claim 1, characterized in that, It also includes sealing and storing the prepared concrete quick-setting agent.

8. A concrete quick-setting agent, characterized in that, It is prepared by the method for preparing concrete quick-setting agent as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Low-resilience liquid accelerator for shotcrete and preparation method thereof

    CN106082750A

  • Super-early-strength fluoride-free alkali-free liquid accelerator and preparation method thereof