A method for producing high-strength titanium fibers using a bundle drawing method

By introducing an electroplating solution containing hydroxylated hexagonal boron nitride and lanthanum chloride into the bundle drawing process, the problem of grain coarsening in the copper isolation layer under high-temperature annealing was solved, achieving high strength and surface smoothness of titanium fibers and improving product reliability.

CN122517403BActive Publication Date: 2026-11-10HEBEI SWIIT METALLIC FIBER CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202610831841.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-06-10
Publication Date
2026-11-10
Estimated Expiration
2046-06-10

AI Technical Summary

Technical Problem

In the traditional bundle drawing method, the copper separator layer coarsens and its microstructure uniformity decreases under high-temperature annealing, resulting in reduced tensile strength and rough surface of the titanium fiber, which affects product reliability.

Method used

Hydroxylated hexagonal boron nitride and lanthanum chloride are introduced into the electroplating solution to provide solid lubrication using their layered structure, thereby improving the deposition uniformity and structural continuity of the copper isolation layer. The lubrication channels and isolation protection functions of the copper isolation layer are maintained through six-pass drawing and high-temperature annealing.

Benefits of technology

This improves the protective stability of the copper isolation layer, ensuring that the titanium fiber maintains its isolation effect during large deformation drawing, and enhances the mechanical properties and surface quality of the titanium fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a method for producing high-strength titanium fibers using a bundled drawing method, belonging to the field of titanium fiber material manufacturing technology. First, metallic titanium precursor wires are degreased, acid-washed, and activated. Then, they are electroplated in a modified electroplating solution containing hydroxylated hexagonal boron nitride and lanthanum chloride to form a copper isolation layer. The copper-plated titanium wires are then bundled and rolled into shape. The diameter is reduced to the target size through a six-pass drawing and intermediate annealing process. Finally, the isolation layer is removed by chemical dissolution of copper, yielding high-strength titanium fibers. By synergistically introducing hydroxylated hexagonal boron nitride and lanthanum chloride into the electroplating solution, and combining this with the six-pass drawing and intermediate annealing process, the copper isolation layer maintains good structural continuity and lubrication stability during drawing deformation and high-temperature annealing, helping to reduce inter-fiber adhesion and surface damage, resulting in titanium fibers with better mechanical properties and surface quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of titanium fiber material manufacturing technology, specifically a method for producing high-strength titanium fibers using a bundle drawing method. Background Technology

[0002] In the titanium manufacturing industry, high-strength titanium fibers, represented by titanium fibers, are widely used in many cutting-edge industries. To meet the stringent requirements for micron-sized, ultrafine, continuous titanium fibers, drawing has become the core preparation method. However, traditional monofilament drawing processes suffer from low production efficiency and high costs. To overcome this bottleneck, the industry has widely adopted the bundled drawing method, which involves simultaneously drawing and changing the diameter of metal filaments together. Compared with the traditional monofilament drawing process, the bundled drawing method allows a large number of microfilaments to undergo coordinated plastic deformation simultaneously, greatly improving production efficiency and significantly reducing manufacturing costs.

[0003] During the bundle drawing process, extremely high frictional forces are generated between the metal microfilaments, making them highly susceptible to cold welding and adhesion. Therefore, a copper layer is typically plated onto the surface of the titanium precursor wire as an insulating layer before drawing to isolate the individual filaments and provide basic lubrication. In actual production, titanium fibers undergo severe work hardening after large-deformation drawing. To eliminate internal stress and restore material plasticity to ensure smooth subsequent drawing, the wire must undergo repeated cycles of drawing and high-temperature annealing. However, under repeated high-temperature annealing, the copper layer gradually coarsens, its microstructure uniformity decreases, and its ductility and insulating durability deteriorate, making it prone to thinning failure or localized cracking. Internal tensile stress cannot be effectively dispersed through the smooth deformation of the insulating layer, thus severely aggravating material wear. This results in a significant reduction in the tensile strength of the titanium fibers, a rough fiber surface after copper removal, and a serious impact on product reliability.

[0004] Therefore, how to effectively improve the protective stability of the copper isolation layer and ensure that the wire can maintain a reliable isolation effect when subjected to large deformation drawing, thereby guaranteeing the mechanical properties and surface finish of titanium fiber products, has become a key technical problem that urgently needs to be solved in the current field of ultrafine titanium fiber bundle drawing manufacturing. Summary of the Invention

[0005] The purpose of this invention is to provide a method for producing high-strength titanium fibers using a bundle drawing method. By synergistically introducing hydroxylated hexagonal boron nitride and lanthanum chloride into the copper isolation layer electroplating system of the bundle drawing method, the layered structure of hydroxylated hexagonal boron nitride provides solid lubrication during the drawing process, and lanthanum chloride improves the deposition uniformity and structural continuity of the copper isolation layer. This allows the copper isolation layer to maintain relatively complete lubrication channels and isolation protection functions during the six-pass drawing and high-temperature intermediate annealing process, thus meeting the requirements for mechanical properties and surface quality in the manufacture of titanium fiber materials.

[0006] The objective of this invention can be achieved through the following technical solutions: This invention provides a method for producing high-strength titanium fibers using a bundle drawing method, comprising the following steps: Step 1: The titanium precursor wire is continuously fed into an alkaline hot degreasing bath at a temperature of 60-65℃ and soaked for 5-10 minutes. Then, it is passed through an acid washing and activation bath for 2-4 minutes to obtain activated titanium precursor wire. Using the activated titanium precursor wire as the cathode and a pure copper plate as the anode, it is fed into an electroplating bath containing modified electroplating solution and electroplated until a copper isolation layer with a thickness of 15μm is formed on the surface of the single wire. After washing with deionized water and drying with hot air, copper-plated titanium wire is obtained.

[0007] Furthermore, the temperature of the electroplating bath is 45-55℃, and the current density is 2-4 A / dm³. 2 .

[0008] The specific preparation process of the modified electroplating solution is as follows: Copper sulfate pentahydrate, concentrated sulfuric acid (98 wt%), and deionized water were placed in a reaction vessel and stirred at 40-50°C for 20-30 minutes. Sodium chloride and lanthanum chloride were added, and stirring was continued at 25-35°C for 20-40 minutes until completely dissolved. A hydroxylated hexagonal boron nitride dispersion was added, and stirring was continued at the same temperature for 1-2 hours to obtain the modified electroplating solution.

[0009] The hydroxylated hexagonal boron nitride dispersion was prepared by mixing hydroxylated hexagonal boron nitride and deionized water at a solid-liquid ratio of 1:10.

[0010] The concentrations of copper sulfate pentahydrate are 180-220 g / L, sulfuric acid is 60-80 g / L, sodium chloride is 0.04-0.06 g / L, lanthanum chloride is 0.1-0.15 g / L, and hydroxylated hexagonal boron nitride is 0.5-1 g / L.

[0011] Step 2: After arranging the copper-plated titanium wires in parallel, wrap the arranged copper-plated titanium wires with copper strip, and then close them after multi-roll rolling to obtain a copper strip-wrapped bundle.

[0012] Furthermore, the rolling speed of the multi-roll mill is 1-2 m / min.

[0013] Step 3: The copper strip-coated bundle is fed into the wire drawing equipment for six drawing passes. After each six drawing passes, an intermediate annealing treatment is performed. The six drawing passes and intermediate annealing treatment are repeated. Finally, the bundled composite microfilaments are drawn to a sizing degree.

[0014] Furthermore, the cross-sectional area reduction rate of each drawing pass is 15-22% of the cross-sectional area after the previous drawing pass; the intermediate annealing temperature is 680-690℃; and the outer diameter of the bundled composite microfilaments is 0.2mm.

[0015] Step 4: Immerse the bundled composite microfilaments in a chemical dissolution bath containing etching solution, and dissolve and remove the copper strip coating and the copper plating between the single filaments at 30-40℃. The dissolved titanium fibers are then ultrasonically rinsed with deionized water and dried to obtain high-strength titanium fibers.

[0016] Furthermore, the etching solution is prepared by mixing 10wt% ammonia water and 3wt% hydrogen peroxide in a volume ratio of 1:1.

[0017] Furthermore, hydroxylated hexagonal boron nitride is obtained by hydroxylating and modifying hexagonal boron nitride using an alkaline hydrothermal method.

[0018] The specific preparation process of hydroxylated hexagonal boron nitride is as follows: Hexagonal boron nitride and a 5 mol / L sodium hydroxide solution were placed in a reaction vessel, ultrasonically dispersed at 25 °C for 40 min, reacted at 120 °C for 24 h, centrifuged, washed, and vacuum dried to constant weight to obtain hydroxylated hexagonal boron nitride.

[0019] The solid-liquid ratio of the hexagonal boron nitride and sodium hydroxide solution is 1:20.

[0020] The beneficial effects of this invention are: 1. In the method for producing high-strength titanium fibers using the bundle drawing method of this invention, hydroxylated hexagonal boron nitride and lanthanum chloride are introduced simultaneously into the electroplating solution. Utilizing the layered structure of hydroxylated hexagonal boron nitride, a certain solid lubrication effect is provided to the titanium fibers during the bundle drawing process, which helps to reduce interfacial friction. At the same time, lanthanum chloride helps to improve the deposition uniformity of the copper isolation layer, enabling the copper isolation layer to maintain dense structural stability and continuous lubrication under six-pass drawing and repeated high-temperature annealing conditions. This provides more stable isolation protection for the titanium fibers, reduces the risk of adhesion, and allows the titanium fibers after copper removal to obtain better surface quality and mechanical properties.

[0021] 2. In the method for producing high-strength titanium fibers using the bundle drawing method, this invention combines a modified electroplating solution synergistically introduced with hydroxylated hexagonal boron nitride and lanthanum chloride with the overall process of bundle drawing and intermediate annealing. Under the process route of six-pass drawing combined with intermediate annealing, the titanium fibers can undergo structural recovery and recrystallization after work hardening. The modified copper isolation layer can maintain structural integrity well within the corresponding temperature range, allowing the annealing softening effect to be more effectively transferred to the interior of the titanium fibers. This helps to coordinate the synchronous deformation of the monofilaments in the bundle, reduce uneven deformation and stress concentration caused by local lubrication failure, maintain the high performance of the titanium fibers, and ensure the reliability of the product. Detailed Implementation

[0022] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0023] Example 1: This example provides a method for producing high-strength titanium fibers using a bundle drawing method, comprising the following steps: S1: Copper sulfate pentahydrate, concentrated sulfuric acid with a concentration of 98wt%, and deionized water are placed in a reaction vessel and stirred at 400 r / min for 20 min at 40℃. Sodium chloride and lanthanum chloride are added, and stirring is continued at the same stirring rate at 25℃ for 20 min until completely dissolved. Hydroxylated hexagonal boron nitride dispersion (prepared by mixing hydroxylated hexagonal boron nitride and deionized water at a solid-liquid ratio of 1:10) is added, and the mixture is stirred at 600 r / min for 1 h at the same temperature to obtain the modified electroplating solution.

[0024] Based on the total volume of the final modified electroplating solution, the concentrations of each component are: copper sulfate pentahydrate 180 g / L, sulfuric acid 60 g / L, sodium chloride 0.04 g / L, lanthanum chloride 0.1 g / L, and hydroxylated hexagonal boron nitride (based on solid content) 0.5 g / L.

[0025] S2: Titanium precursor wire is immersed in an alkaline hot degreasing bath at 60℃ for 5 minutes, followed by acid pickling and activation in an acid pickling and activation bath for 2 minutes to obtain activated titanium precursor wire. (The alkaline pickling solution in the alkaline hot degreasing bath consists of 5wt% sodium hydroxide and 1.5wt% sodium carbonate; the acid pickling solution in the acid pickling and activation bath is prepared by a volume ratio of 3:1 to 20wt% nitric acid and 3wt% hydrofluoric acid). Using the activated titanium precursor wire as the cathode and a pure copper plate as the anode, the wire is placed in an electroplating bath containing a modified electroplating solution at 45℃ and a current density of 2 A / dm³. 2 Under certain conditions, a copper isolation layer with a thickness of 15μm is formed on the surface of the monofilament by electroplating. The electroplated monofilament is then washed with deionized water to remove residual plating solution, dried with hot air, and wound up for later use to obtain copper-plated titanium wire.

[0026] S3: After arranging the copper-plated titanium wires in parallel, a copper strip with a thickness of 0.2 mm and a width of 30 mm is used to cover the arranged copper-plated titanium wires. After multi-roll rolling, the rolls are closed at a rolling speed of 1 m / min to obtain a copper strip-covered bundle.

[0027] S4: The copper strip-coated bundle is fed into the wire drawing equipment for six drawing passes. After each six drawing passes, the bundle is sent into a continuous annealing furnace at a temperature of 680℃ for 5 minutes of intermediate annealing. Through the alternating process of six drawing passes and intermediate annealing, the cross-sectional area of ​​the bundle after the previous drawing pass is used as a reference, and the cross-sectional area reduction rate of each pass is controlled at 15%. Finally, the sizing drawing is performed to reduce the outer diameter of the copper strip-coated bundle to 0.2mm, thus obtaining the bundled composite microfilament.

[0028] S5: The bundled composite microfilaments are immersed in a chemical dissolution bath containing etching solution (prepared by mixing 10wt% ammonia and 3wt% hydrogen peroxide in a volume ratio of 1:1). At 30°C, the copper strip coating and the copper plating between the monofilaments are dissolved and removed. The dissolved titanium fibers are then ultrasonically rinsed with deionized water for 10 minutes and dried in a hot air circulating oven at 80°C to obtain high-strength titanium fibers.

[0029] Example 2: This example provides a method for producing high-strength titanium fibers using a bundle drawing method, comprising the following steps: S1: Copper sulfate pentahydrate, concentrated sulfuric acid with a concentration of 98wt%, and deionized water are placed in a reaction vessel and stirred at 500r / min for 25min at 45℃. Sodium chloride and lanthanum chloride are added, and stirring is continued at the same stirring rate at 30℃ for 30min until completely dissolved. Hydroxylated hexagonal boron nitride dispersion (prepared by hydroxylated hexagonal boron nitride and deionized water at a solid-liquid ratio of 1:10) is added, and stirring is carried out at 700r / min for 1.5h at the same temperature to obtain the modified electroplating solution.

[0030] Based on the total volume of the final modified electroplating solution, the concentrations of each component are: copper sulfate pentahydrate 200 g / L, sulfuric acid 70 g / L, sodium chloride 0.05 g / L, lanthanum chloride 0.12 g / L, and hydroxylated hexagonal boron nitride (based on solid content) 0.8 g / L.

[0031] S2: Titanium precursor wire is continuously fed into an alkaline hot degreasing bath at 62℃ for 8 minutes, followed by acid pickling and activation in an acid pickling and activation bath for 3 minutes to obtain activated titanium precursor wire. (The alkaline pickling solution in the alkaline hot degreasing bath consists of 5wt% sodium hydroxide and 1.5wt% sodium carbonate; the acid pickling solution in the acid pickling and activation bath is prepared by a volume ratio of 3:1 to 20wt% nitric acid and 3wt% hydrofluoric acid). Using the activated titanium precursor wire as the cathode and a pure copper plate as the anode, the wire is fed into an electroplating bath containing a modified electroplating solution at 50℃ and a current density of 3 A / dm³. 2 Under certain conditions, a copper isolation layer with a thickness of 15μm is formed on the surface of the monofilament by electroplating. The electroplated monofilament is then washed with deionized water to remove residual plating solution, dried with hot air, and wound up for later use to obtain copper-plated titanium wire.

[0032] S3: After arranging the copper-plated titanium wires in parallel, a copper strip with a thickness of 0.2 mm and a width of 30 mm is used to cover the arranged copper-plated titanium wires. After multi-roll rolling, the rolls are closed at a rolling speed of 1.5 m / min to obtain a copper strip-covered bundle.

[0033] S4: The copper strip-coated bundle is fed into the wire drawing equipment for six drawing passes. After each six drawing passes, the bundle is sent into a continuous annealing furnace at a temperature of 685℃ for 5 minutes of intermediate annealing. Through the alternating process of six drawing passes and intermediate annealing, the cross-sectional area of ​​the bundle after the previous drawing pass is used as a reference, and the cross-sectional area reduction rate of each pass is controlled at 18%. Finally, the sizing drawing is performed to reduce the outer diameter of the copper strip-coated bundle to 0.2mm, thus obtaining the bundled composite microfilament.

[0034] S5: The bundled composite microfilaments are immersed in a chemical dissolution bath containing etching solution (prepared by mixing 10wt% ammonia and 3wt% hydrogen peroxide in a volume ratio of 1:1). At 35°C, the copper strip coating and the copper plating between the monofilaments are dissolved and removed. The dissolved titanium fibers are then ultrasonically rinsed with deionized water for 12 minutes and dried in a hot air circulating oven at 100°C to obtain high-strength titanium fibers.

[0035] Example 3: This example provides a method for producing high-strength titanium fibers using a bundle drawing method, comprising the following steps: S1: Copper sulfate pentahydrate, concentrated sulfuric acid with a concentration of 98wt%, and deionized water are placed in a reaction vessel and stirred at 600r / min for 30min at 50℃. Sodium chloride and lanthanum chloride are added, and stirring is continued at the same stirring rate at 35℃ for 40min until completely dissolved. Hydroxylated hexagonal boron nitride dispersion (prepared by hydroxylated hexagonal boron nitride and deionized water at a solid-liquid ratio of 1:10) is added, and stirring is carried out at 800r / min for 2h at the same temperature to obtain the modified electroplating solution.

[0036] Based on the total volume of the final modified electroplating solution, the concentrations of each component are: copper sulfate pentahydrate 220 g / L, sulfuric acid 80 g / L, sodium chloride 0.06 g / L, lanthanum chloride 0.15 g / L, and hydroxylated hexagonal boron nitride (based on solid content) 1 g / L.

[0037] S2: Titanium precursor wire is continuously fed into an alkaline hot degreasing bath at 65℃ for 10 minutes, followed by acid pickling and activation in an acid pickling and activation bath for 4 minutes to obtain activated titanium precursor wire. (The alkaline pickling solution in the alkaline hot degreasing bath consists of 5wt% sodium hydroxide and 1.5wt% sodium carbonate; the acid pickling solution in the acid pickling and activation bath is prepared by a volume ratio of 3:1 to 20wt% nitric acid and 3wt% hydrofluoric acid). Using the activated titanium precursor wire as the cathode and a pure copper plate as the anode, the wire is fed into an electroplating bath containing modified electroplating solution at 55℃ and a current density of 4 A / dm³. 2 Under certain conditions, a copper isolation layer with a thickness of 15μm is formed on the surface of the monofilament by electroplating. The electroplated monofilament is then washed with deionized water to remove residual plating solution, dried with hot air, and wound up for later use to obtain copper-plated titanium wire.

[0038] S3: After arranging the copper-plated titanium wires in parallel, the copper-plated titanium wires are wrapped with copper strip with a thickness of 0.2 mm and a width of 30 mm. After being rolled by multiple rollers, the rolls are closed at a rolling speed of 2 m / min to obtain a copper strip-wrapped bundle.

[0039] S4: The copper strip-coated bundle is fed into the wire drawing equipment for six drawing passes. After each six drawing passes, the bundle is sent into a continuous annealing furnace at a temperature of 690℃ for 5 minutes of intermediate annealing. Through the alternating process of six drawing passes and intermediate annealing, the cross-sectional area of ​​the bundle after the previous drawing pass is used as a reference, and the cross-sectional area reduction rate of each pass is controlled at 22%. Finally, the sizing drawing is performed to reduce the outer diameter of the copper strip-coated bundle to 0.2mm, thus obtaining the bundled composite microfilament.

[0040] S5: The bundled composite microfilaments are immersed in a chemical dissolution bath containing etching solution (prepared by mixing 10wt% ammonia and 3wt% hydrogen peroxide in a volume ratio of 1:1). At 40°C, the copper strip coating and the copper plating between the monofilaments are dissolved and removed. The dissolved titanium fibers are then ultrasonically rinsed with deionized water for 15 minutes and dried in a hot air circulating oven at 120°C to obtain high-strength titanium fibers.

[0041] The high-strength titanium fibers prepared in Examples 1-3 above have an average diameter of 20 μm.

[0042] Comparative Example 1: The difference from Example 2 is that commercially available hexagonal boron nitride was used instead of hydroxylated hexagonal boron nitride in step S1 to prepare the electroplating solution, while the other steps remained unchanged to prepare high-strength titanium fibers.

[0043] Comparative Example 2: The difference from Example 2 is that the hydroxylated hexagonal boron nitride is removed in step S1 to prepare an electroplating solution, while the remaining steps remain unchanged to prepare high-strength titanium fibers.

[0044] Comparative Example 3: The difference from Example 2 is that lanthanum chloride is removed in step S1 to prepare an electroplating solution, while the remaining steps remain unchanged to prepare high-strength titanium fibers.

[0045] The titanium precursor wires in the above embodiments and comparative examples were produced by Baoji Titanium Industry Co., Ltd., and were TA1 grade industrial pure titanium wires with an initial diameter of 1.0 mm. The hydroxylated hexagonal boron nitride was obtained by hydroxylating boron nitride (produced by Jiangsu Xianfeng Nanomaterials Technology Co., Ltd., with an average particle size of 100 nm) using an alkaline hydrothermal method. The edges and defect sites of the hexagonal boron nitride layered structure were etched using sodium hydroxide solution under high temperature conditions to introduce hydroxyl functional groups onto its surface.

[0046] The specific preparation process of hydroxylated hexagonal boron nitride is as follows: Hexagonal boron nitride and a 5 mol / L sodium hydroxide solution were placed in a reaction vessel at a solid-liquid ratio of 1:20. The mixture was ultrasonically dispersed at 25 °C for 40 min and stirred at 120 °C at 800 r / min for 24 h. After the reaction was completed, the mixture was cooled to room temperature, the supernatant was removed by centrifugation, deionized water was added and the mixture was washed four times by centrifugation. The mixture was then vacuum dried at 80 °C to constant weight to obtain hydroxylated hexagonal boron nitride.

[0047] The high-strength titanium fibers prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to performance tests, and the test results are shown in Table 1. Sample preparation: In the above examples and comparative examples, 20 titanium fibers of the same diameter were selected as samples for performance testing.

[0048] Mechanical properties: Referring to the standard GB / T 228.1-2021 "Metallic materials, tensile testing - Part 1: Test at room temperature", 20 specimens in each group were tested in parallel using an electronic universal testing machine. The average tensile strength and elongation at break of the specimens were recorded and calculated.

[0049] Friction coefficient: The average friction coefficient of the sample was determined and calculated using the cylindrical friction method and a fiber dynamic friction coefficient tester. The smaller the friction coefficient, the smaller the surface roughness of the titanium fiber.

[0050] Table 1 Performance Test Table of High-Strength Titanium Fiber

[0051] As shown in Table 1, the high-strength titanium fibers prepared in Examples 1–3 all outperformed those in Comparative Examples 1–3. This indicates that the present invention, by introducing hydroxylated hexagonal boron nitride into the electroplating solution and cooperating with lanthanum chloride for synergistic modification, constructed a good copper isolation layer system and a steady-state deformation mechanism of alternating six-pass drawing-intermediate annealing, thus maintaining the stability and consistency of titanium fiber product quality.

[0052] The mechanical properties and surface quality of the titanium fibers in Comparative Example 1 showed a certain degree of decline. This may be because commercially available hexagonal boron nitride lacks active hydroxyl sites, resulting in insufficient dispersion stability in the electroplating solution and difficulty in uniform embedding in the copper plating layer. This leads to local peeling or uneven thinning of the copper isolation layer during the bundle drawing process, which reduces the isolation effect between titanium wires and thus reduces the quality and mechanical properties of the finished product.

[0053] The titanium fiber in Comparative Example 2 had the worst mechanical properties and surface quality because the hydroxylated hexagonal boron nitride was completely removed from the electroplating solution. Under these conditions, the copper isolation layer lost the reinforcing support of the solid lubricating phase, which made it easy for the copper isolation layer to peel off and break during the drawing process. This caused adhesion or scratches between the titanium fibers, resulting in a significant decrease in the performance of the titanium fiber.

[0054] The quality indicators of the titanium fibers in Comparative Example 3 also decreased because of the lack of lanthanum chloride in the electroplating solution. Although hydroxylated hexagonal boron nitride has active hydroxyl groups, the uniformity of copper separator deposition may decrease in the absence of lanthanum chloride, making the coating more prone to localized damage during drawing, thus hindering the sustained function of the layered solid lubricating phase. Simultaneously, the structural stability of the copper separator under high-temperature annealing may also be weakened. This prevents the separator from fully exerting its lubricating and protective effects during drawing, resulting in a decline in the surface quality and mechanical properties of the titanium fibers.

[0055] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention.

Claims

1. A method for producing high-strength titanium fibers using a bundle drawing method, characterized in that, Includes the following steps: Step 1: The titanium precursor is continuously fed into an alkaline hot degreasing bath at a temperature of 60-65℃ for 5-10 minutes, followed by acid washing and activation in an acid washing and activation bath for 2-4 minutes to obtain activated titanium precursor. Using activated titanium precursor wire as cathode and pure copper plate as anode, the wire is fed into an electroplating bath containing modified electroplating solution and electroplated until a copper isolation layer with a thickness of 15μm is formed on the surface of the single wire. After washing with deionized water and drying with hot air, copper-plated titanium wire is obtained. The specific preparation process of the modified electroplating solution is as follows: copper sulfate pentahydrate, concentrated sulfuric acid with a concentration of 98wt% and deionized water are placed in a reaction vessel and stirred at 40-50℃ for 20-30 min. Sodium chloride and lanthanum chloride are added, and stirring is continued at 25-35℃ for 20-40 min until completely dissolved. A hydroxylated hexagonal boron nitride dispersion is added, and stirring is continued at the same temperature for 1-2 h to obtain the modified electroplating solution. The hydroxylated hexagonal boron nitride dispersion is prepared by mixing hydroxylated hexagonal boron nitride and deionized water at a solid-liquid ratio of 1:

10. The concentrations of copper sulfate pentahydrate, sulfuric acid, sodium chloride, lanthanum chloride, and boron nitride hydroxylated are 180-220 g / L, 60-80 g / L, 0.04-0.06 g / L, 0.1-0.15 g / L, and 0.5-1 g / L, respectively. Step 2: After arranging the copper-plated titanium wires in parallel, wrap the arranged copper-plated titanium wires with copper strip, and close them after multi-roll rolling to obtain a copper strip-wrapped bundle. Step 3: The copper strip-coated bundle is fed into the wire drawing equipment for six drawing passes. After the six drawing passes, intermediate annealing is performed. The six drawing passes and intermediate annealing are repeated. Finally, the bundled composite microfilaments are drawn to obtain the final size. Step 4: Immerse the bundled composite microfilaments in a chemical dissolution bath containing etching solution, and dissolve and remove the copper strip coating and the copper plating between the single filaments at 30-40℃. The dissolved titanium fibers are then ultrasonically rinsed with deionized water and dried to obtain high-strength titanium fibers.

2. The method for producing high-strength titanium fibers using a bundle drawing method according to claim 1, characterized in that, The specific preparation process of the hydroxylated hexagonal boron nitride is as follows: Hexagonal boron nitride and a 5 mol / L sodium hydroxide solution were placed in a reaction vessel, ultrasonically dispersed at 25 °C for 40 min, reacted at 120 °C for 24 h, centrifuged, washed, and vacuum dried to constant weight to obtain hydroxylated hexagonal boron nitride. The solid-liquid ratio of the hexagonal boron nitride and sodium hydroxide solution is 1:

20.

3. The method for producing high-strength titanium fibers using a bundle drawing method according to claim 1, characterized in that, The temperature of the electroplating bath in step one is 45-55℃, and the current density is 2-4 A / dm³. 2 .

4. The method for producing high-strength titanium fibers using a bundle drawing method according to claim 1, characterized in that, The speed of the multi-roll rolling process in step two is 1-2 m / min.

5. The method for producing high-strength titanium fibers using a bundle drawing method according to claim 1, characterized in that, In step three, the reduction rate of the cross-sectional area for each drawing pass is 15-22% of the cross-sectional area after the previous drawing pass.

6. The method for producing high-strength titanium fibers using a bundle drawing method according to claim 1, characterized in that, The intermediate annealing temperature in step three is 680-690℃.

7. The method for producing high-strength titanium fibers using a bundle drawing method according to claim 1, characterized in that, The outer diameter of the bundled composite microfilaments mentioned in step three is 0.2 mm.

8. A method for producing high-strength titanium fibers using a bundle drawing method according to claim 1, characterized in that, The etching solution described in step four is prepared by mixing 10wt% ammonia water and 3wt% hydrogen peroxide in a volume ratio of 1:1.

Citation Information

Patent Citations

  • Preparation method of micrometer order super-strength continuous aluminum alloy fiber

    CN108515086A

  • Titanium fiber production process

    CN112246894A

  • Manufacturing method of titanium fiber

    CN114713658A