A surface-enriched aluminum-supported yttrium-doped cerium-zirconium composite oxide iron-cobalt bimetallic catalyst, its preparation method and application
By using a surface-enriched aluminum-supported yttrium-doped cerium-zirconium composite oxide to support an iron-cobalt bimetallic catalyst, the problems of active metal agglomeration and lack of defect control in electric field-assisted low-temperature ammonia synthesis catalysts were solved, achieving high catalytic performance and stability.
Patent Information
- Application Number
- CN202611087671.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-22
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-07-22
AI Technical Summary
Existing electric field-assisted low-temperature ammonia synthesis catalysts suffer from problems such as easy aggregation of active metals, lack of synergistic effect, and lack of defect control capability of the support.
A bimetallic catalyst for iron and cobalt was supported by a surface aluminum enrichment-bulk yttrium-doped cerium-zirconium composite oxide. By constructing a structure with bulk Y doping, surface aluminum enrichment, and Fe-Co bimetallic support, the synergistic control of support defects, active metal dispersion state, and metal-support interface was achieved.
Under electric field-assisted conditions, the defect structure of the support, the dispersion of active metals, and the interfacial stability are improved, thereby enhancing the low-temperature reaction efficiency and the stability of the catalyst.
Smart Images

Figure CN122582974B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of ammonia synthesis catalytic materials and electric field enhanced catalysis technology, and particularly to an iron-cobalt bimetallic catalyst supported on a surface aluminum-enriched bulk yttrium-doped cerium-zirconium composite oxide, its preparation method, and its application. Background Technology
[0002] Ammonia is not only an important basic chemical raw material, but also a potential hydrogen storage and carrier medium. The traditional Haber-Bosch ammonia synthesis process typically requires high temperatures and pressures, resulting in high energy consumption, which is not conducive to matching with small-scale, distributed ammonia production scenarios driven by renewable energy sources. Recent studies on electric field-assisted catalysis have shown that, in the presence of semiconductor or reducible oxide supports, applying a weak direct current can promote the ammonia synthesis reaction at lower temperatures, exhibiting reaction characteristics distinct from traditional thermocatalytic processes.
[0003] Existing research has disclosed Co / Ce 0.5 Zr 0.5 The O2 system can be used for electric field-assisted ammonia synthesis, in which Ce 0.5 Zr 0.5 O2 supports can be prepared using a composite polymerization method, while Co is supported using an impregnation method, and the pre-reduction conditions have a significant impact on the activity. Other studies have shown that iron-based catalysts also have application potential in electric field-assisted systems, but usually require additional structural stabilization strategies and interface modulation techniques. However, existing technologies still have shortcomings. First, single-active-metal systems may suffer from insufficient active sites and limited electronic structure modulation range under low-temperature electric field conditions. Second, active metals are prone to aggregation during reduction and reaction, leading to a decrease in the metal-support interface length. Third, existing schemes lack the ability to simultaneously address support defect modulation, metal anchoring, and bimetallic synergistic effects.
[0004] Therefore, it is of great significance to develop a novel supported catalyst that combines defect control capability, interface stability capability, and bimetallic synergistic potential. Summary of the Invention
[0005] The purpose of this invention is to provide a surface aluminum-enriched bulk yttrium-doped cerium-zirconium composite oxide supported iron-cobalt bimetallic catalyst to solve the problems of active metal agglomeration, lack of synergistic effect, and lack of defect control ability of the support in existing electric field-assisted low-temperature ammonia synthesis catalysts.
[0006] The present invention also aims to provide a preparation method for preparing a novel supported catalyst that combines defect control capability, interface stability capability and bimetallic synergistic potential.
[0007] Another objective of this invention is to provide an application of a catalyst in electric field-assisted low-temperature ammonia synthesis.
[0008] In a first aspect, the present invention discloses a surface aluminum-enriched bulk yttrium-doped cerium-zirconium composite oxide supported iron-cobalt bimetallic catalyst, the catalyst comprising a support and an active component supported on the surface of the support; The carrier is a cerium-zirconium composite oxide with aluminum enriched on the surface and yttrium doped in the bulk phase; The active components include Fe and Co; The chemical formula of cerium-zirconium composite oxide is Ce. 0.45 Zr 0.50 Y 0.05 O2 δ , where 0 < δ ≤ 0.30.
[0009] Preferably, the loading of Fe is 5 to 25 wt% and the loading of Co is 0.5 to 5 wt% relative to the mass of the carrier.
[0010] Preferably, aluminum, calculated as Al2O3, accounts for 0.3 to 3.0 wt% of the carrier mass.
[0011] More preferably, aluminum, calculated as Al2O3, accounts for 0.8 to 2.0 wt% of the carrier mass.
[0012] Secondly, the present invention also discloses a preparation method, comprising the following steps: S1. Preparation of bulk yttrium-doped cerium-zirconium composite oxide support; S2. Perform surface aluminum enrichment modification on the carrier; S3. Introduce Fe and Co precursors onto the modified support; S4. The precursor catalyst is obtained by drying and heat treatment.
[0013] Preferably, the bulk yttrium-doped cerium-zirconium composite oxide support is prepared by complexation polymerization, sol-gel method or co-precipitation method; Complexation polymerization includes the following steps: Ce source, Y source and Zr source are added to deionized water according to the molar ratio in the chemical formula of cerium-zirconium composite oxide to form a mixed metal salt solution; citric acid, EDTA and polymerization aid are added according to the total metal ion molar ratio, and the mixture is stirred and slowly evaporated to form a gel; after drying and crushing, it is calcined at a temperature of 450-600℃ for 3-6 hours to obtain the final product.
[0014] Preferably, the Ce source includes Ce(NO3)3·6H2O and (NH4)2Ce(NO3)6.
[0015] Preferably, the Y source includes Y(NO3)3·6H2O and Y(CH3COO)3·xH2O.
[0016] Preferably, the Zr source includes ZrO(NO3)2·2H2O and ZrOCl2·8H2O.
[0017] Preferably, the polymerization aids include ethylene glycol and polyacrylamide.
[0018] Preferably, the molar ratio of citric acid to total metal ions is 1.5 to 2.0.
[0019] Preferably, the molar ratio of EDTA to total metal ions is 0.5 to 1.0.
[0020] Preferably, the surface aluminum enrichment modification is achieved by deposition-precipitation method, surface complexation method or surface impregnation method; The sedimentation-precipitation method includes the following steps: A bulk yttrium-doped cerium-zirconium composite oxide support was dispersed in deionized water to obtain a support dispersion. An Al source and urea were dissolved in deionized water, and the resulting solution was added dropwise to the support dispersion at 80–90 °C with stirring, and allowed to settle for 2–6 h. The solution was filtered and washed until it was neutral, dried, and then calcined at 400–600 °C for 1–4 h to obtain the final product.
[0021] Preferably, the Al source includes Al(NO3)3·9H2O and Al(C5H7O2)3.
[0022] Preferably, the Fe and Co precursors are introduced through the following steps: Fe and Co sources are dissolved in a solvent, and Fe and Co are introduced by a two-step equal-volume co-impregnation method. After impregnation, the mixture is aged for 4-6 hours, dried, and then pre-decomposed at 300-400℃ for 1-3 hours under an inert gas atmosphere to obtain the final product.
[0023] Preferably, the solvent is a mixture of ethanol and water.
[0024] More preferably, the volume ratio of ethanol to water is 1:1.
[0025] Preferably, the precursor catalyst further includes a reduction activation treatment in a hydrogen-containing atmosphere.
[0026] Preferably, the hydrogen-containing atmosphere for the reduction and activation treatment is a 10 vol% H2 / N2 mixture, with a total flow rate of 60 sccm or 240 sccm, a reduction temperature of 700–1000 K, and a reduction time of 0.5–4 h.
[0027] Thirdly, the present invention also discloses the application of the catalyst in electric field-assisted low-temperature ammonia synthesis, wherein the reaction is carried out in a fixed-bed reactor and an electric field is applied by a DC power supply; the reaction feed gas includes N2 and H2.
[0028] The beneficial effects of this invention are: The catalyst of this invention achieves synergistic regulation of support defects, active metal dispersion, and metal-support interface by constructing a structure of bulk yttrium doping, surface aluminum enrichment, and iron-cobalt bimetallic support, thereby providing a new catalytic material system for electric field-assisted low-temperature ammonia synthesis. Specifically, bulk yttrium doping is beneficial for regulating the structure of support defects, increasing oxygen vacancy concentration, and improving ion migration characteristics; surface Al enrichment is beneficial for enhancing active metal anchoring and inhibiting the aggregation of Fe and Co during reduction and reaction processes; the co-introduction of Fe and Co bimetals is beneficial for forming a Fe-Co / oxide peripheral interface, where Fe is mainly responsible for N2 adsorption and hydrogenation-related steps, while a small amount of Co is beneficial for promoting H2 activation, regulating the electronic structure of Fe, and stabilizing small-sized metal species, thus demonstrating a synergistic effect; under electric field-assisted conditions, support defects, surface aluminum enrichment, and the Fe-Co bimetallic interface can jointly improve interface stability, local electric field response, and low-temperature reaction efficiency. Attached Figure Description
[0029] Figure 1 The X-ray diffraction (XRD) pattern of the catalyst in Example 1 of this invention; Figure 2 Here is a SEM image of the catalyst in Example 1 of this invention; Figure 3 The following is a mapping diagram of the catalyst in Example 1 of the present invention: (a) is a superimposed distribution diagram of each element, and (b) to (h) are surface distribution diagrams of elements O, Fe, Zr, Y, Co, Al and Ce, respectively, showing the distribution of different elements in the catalyst; Figure 4 This is a schematic diagram of the performance testing device for the catalyst of the present invention under electric field-assisted ammonia synthesis conditions; Figure 5 This is a comparison chart of the ammonia synthesis rates of the catalysts in Examples 1 to 5 and Comparative Examples 1 to 5 of the present invention; Figure 6 The graph shows the stability test results of the catalysts in Examples 1 to 5 and Comparative Examples 1 to 5 of the present invention.
[0030] Figure label: 1-Raw material gas cylinder; 2-Mass flow meter; 3-Tube furnace; 4-High-pressure reaction tube; 5-Catalyst; 6-Wire; 7-External DC power supply; 8-Gas chromatograph. Detailed Implementation
[0031] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of the embodiments of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0032] A surface aluminum-enriched bulk yttrium-doped cerium-zirconium composite oxide supported iron-cobalt bimetallic catalyst, the catalyst comprising a support and an active component supported on the surface of the support; The carrier is a cerium-zirconium composite oxide with aluminum enriched on the surface and yttrium doped in the bulk phase; The active components include Fe and Co; The chemical formula of cerium-zirconium composite oxide is Ce. 0.45 Zr 0.50 Y 0.05 O2 δ , where 0 < δ ≤ 0.30.
[0033] By adopting the above technical solutions, this invention solves the problems of insufficient number of active sites and limited range of electronic structure regulation in existing electric field-assisted low-temperature ammonia synthesis catalysts, as well as the tendency of active metals to agglomerate and the sharp reduction in the number of active sites during reduction and reaction.
[0034] This invention simultaneously addresses three aspects: carrier defect structure, metal anchoring interface, and bimetallic synergistic activity, constructing a triple synergistic structure of bulk Y doping, surface Al enrichment, and Fe / Co bimetallic loading. Bulk Y 3+ Replace Ce 4+ Introducing oxygen vacancy defects improves the oxygen ion mobility and electric field response of the support, providing ample electron conduction channels and charge transfer centers for electric field-assisted catalysis. Surface Al is selectively enriched on the support surface in the form of Al2O3, forming strong metal-support interactions with Fe and Co through Lewis acid sites. This effectively anchors metal particles and inhibits their sintering and agglomeration during reduction and reaction, maintaining the high dispersion and small size effect of the metal. The Fe-Co bimetallic synergy undertakes the functional division of N2 adsorption activation (Fe-dominant) and H2 activation and Fe electronic structure regulation (Co-assisted), respectively, forming an active interface around the Fe-Co / oxide, achieving efficient synergistic activation of N2 and H2 at low temperatures.
[0035] This invention organically integrates three strategies into the same catalyst system. These three strategies are not simply superimposed, but rather mutually promote and synergistically enhance each other. The oxygen vacancies generated by Y doping enhance the electronic conductivity of the support, which is beneficial for electron transfer between the metal and the support under an electric field. While the surface Al is enriched to anchor the metal, its Lewis acid sites interact with the lattice oxygen on the support surface, optimizing the interfacial electronic environment. The Fe-Co bimetallic material maintains high dispersion under the stabilizing effect of the surface Al, while the small-sized metal particles and the oxygen-vacancy-rich support form more metal-support peripheral active interfaces. Under the action of an electric field, local electric field enhancement and interfacial polarization effects are generated, further amplifying the overall efficiency of electric field-assisted catalysis.
[0036] In some embodiments, the loading of Fe is 5 to 25 wt% and the loading of Co is 0.5 to 5 wt% relative to the carrier mass meter.
[0037] By adopting the above technical solutions, this invention achieves an optimal balance between the number of active sites and the metal dispersion within a loading range of Fe 5–25 wt% and Co 0.5–5 wt%. When the loading is too low, there are insufficient active sites on the catalyst surface, limiting the reaction rate; when the loading is too high, it exceeds the stabilizing ability of the surface Al anchoring sites, making the metal prone to agglomeration and sintering, resulting in a decrease in dispersion.
[0038] In some embodiments, aluminum, calculated as Al2O3, accounts for 0.3 to 3.0 wt% of the carrier mass.
[0039] Aluminum, calculated as Al2O3, accounts for 0.8 to 2.0 wt% of the carrier mass.
[0040] By adopting the above technical solutions, the present invention achieves the optimal balance between metal anchoring and carrier activity within the surface Al2O3 content range of 0.3–3.0 wt% (preferably 0.8–2.0 wt%). Appropriate surface Al enrichment can form strong metal-carrier interactions with Fe and Co through Lewis acidic sites, effectively inhibiting metal aggregation; however, excessive Al will mask carrier defect sites, block pores, and weaken the electric field enhancement effect and electron transport efficiency.
[0041] A preparation method, comprising the following steps: S1. Preparation of bulk yttrium-doped cerium-zirconium composite oxide support; S2. Perform surface aluminum enrichment modification on the carrier; S3. Introduce Fe and Co precursors onto the modified support; S4. The precursor catalyst is obtained by drying and heat treatment.
[0042] By employing the above technical solutions, this invention adopts a stepwise preparation strategy. First, a cerium-zirconium composite oxide support with bulk Y doping and abundant oxygen vacancy defects is prepared through complexation polymerization, sol-gel method, or co-precipitation method. Then, selective enrichment and modification of surface Al is achieved through deposition-precipitation method, surface complexation method, or surface impregnation method. Finally, Fe and Co precursors are introduced through a two-step equal-volume co-impregnation method and pre-decomposed. This stepwise strategy ensures uniform bulk Y doping, precise surface enrichment of Al, and synergistic loading of Fe-Co, avoiding mutual interference between components during the preparation process. This results in a catalyst exhibiting high activity, high stability, and excellent metal dispersion in electric field-assisted low-temperature ammonia synthesis.
[0043] In some embodiments, the bulk yttrium-doped cerium-zirconium composite oxide support is prepared by complexation polymerization, sol-gel method or co-precipitation method; Complexation polymerization includes the following steps: Ce source, Y source and Zr source are added to deionized water according to the molar ratio in the chemical formula of cerium-zirconium composite oxide to form a mixed metal salt solution; citric acid, EDTA and polymerization aid are added according to the total metal ion molar ratio, and the mixture is stirred and slowly evaporated to form a gel; after drying and crushing, it is calcined at a temperature of 450-600℃ for 3-6 hours to obtain the final product.
[0044] Ce sources include Ce(NO3)3·6H2O and (NH4)2Ce(NO3)6.
[0045] Y sources include Y(NO3)3·6H2O and Y(CH3COO)3·xH2O.
[0046] Zr sources include ZrO(NO3)2·2H2O and ZrOCl2·8H2O.
[0047] Polymerization aids include ethylene glycol and polyacrylamide.
[0048] The molar ratio of citric acid to total metal ions is 1.5 to 2.0.
[0049] The molar ratio of EDTA to total metal ions is 0.5–1.0.
[0050] By employing the above technical solutions, this invention utilizes a citric acid-EDTA dual complexing system in conjunction with polymerization aids to achieve uniform mixing and stable complexation of Ce, Y, and Zr metal ions at the molecular level through complexation polymerization. Citric acid, as the primary complexing agent, forms stable five- or six-membered ring complexes with the metal ions through its carboxyl and hydroxyl groups. EDTA, as an auxiliary complexing agent, further enhances the complexation stability and the uniformity of metal ion dispersion. Polymerization aids such as ethylene glycol promote the formation of a gel network through esterification reactions, inhibiting the segregation and aggregation of metal ions. Under calcination conditions of 450–600℃ for 3–6 hours, the organic components completely decompose, forming a carrier with a high specific surface area, abundant oxygen vacancies, and a stable crystal phase structure, providing an ideal structural basis for subsequent surface Al modification and metal loading.
[0051] In some embodiments, the surface aluminum enrichment modification is achieved by deposition-precipitation, surface complexation, or surface impregnation. The sedimentation-precipitation method includes the following steps: A bulk yttrium-doped cerium-zirconium composite oxide support was dispersed in deionized water to obtain a support dispersion. An Al source and urea were dissolved in deionized water, and the resulting solution was added dropwise to the support dispersion at 80–90 °C with stirring, and allowed to settle for 2–6 h. The solution was filtered and washed until it was neutral, dried, and then calcined at 400–600 °C for 1–4 h to obtain the final product.
[0052] Al sources include Al(NO3)3·9H2O and Al(C5H7O2)3.
[0053] By adopting the above technical solutions, this invention utilizes urea as a homogeneous precipitant, and slowly releases OH- through the hydrolysis reaction of urea at 80-90℃. - and CO3 2- , making Al 3+ Uniform and controllable deposition-precipitation occurs on the carrier surface, rather than homogeneous nucleation in the bulk solution.
[0054] In some embodiments, Fe and Co precursors are introduced via the following steps: Fe and Co sources are dissolved in a solvent, and Fe and Co are introduced by a two-step equal-volume co-impregnation method. After impregnation, the mixture is aged for 4-6 hours, dried, and then pre-decomposed at 300-400℃ for 1-3 hours under an inert gas atmosphere to obtain the final product.
[0055] The solvent is a mixture of ethanol and water.
[0056] The volume ratio of ethanol to water is 1:1.
[0057] By adopting the above technical solutions, this invention employs a two-step equal-volume co-impregnation method, using ethanol / water (volume ratio 1:1) as a mixed solvent, to achieve uniform and quantitative loading of Fe and Co precursors on the support surface. The equal-volume impregnation method ensures complete absorption of the impregnation solution by the support, avoiding uneven distribution of the metal precursors within the pores caused by excess solution. The two-step impregnation strategy facilitates the formation of a synergistic interface with tight Fe-Co contact rather than individual metal particles. The aging process of 4–6 hours after impregnation allows the metal ions to fully interact with the support surface, forming stable surface complexes. Pre-decomposition at 300–400℃ for 1–3 hours under N2 atmosphere decomposes the nitrate precursor into oxides, while avoiding excessive oxidation and sintering of the metal under high-temperature oxidizing atmosphere, laying the foundation for subsequent reduction activation to obtain highly dispersed metal active sites.
[0058] In some embodiments, the precursor catalyst further includes a reduction activation treatment in a hydrogen-containing atmosphere.
[0059] The hydrogen-containing atmosphere for the reduction and activation treatment is a 10 vol% H2 / N2 mixture, with a total flow rate of 60 sccm or 240 sccm, a reduction temperature of 700–1000 K, and a reduction time of 0.5–4 h.
[0060] By employing the above technical solutions, this invention enables the controlled reduction and activation of precursor catalysts in a hydrogen-containing atmosphere, reducing Fe and Co oxide precursors to catalytically active metallic or partially reduced species. Using an H2 / N2 mixture instead of pure hydrogen ensures reduction efficiency while avoiding over-reduction that could lead to metal sintering and damage to the support structure. The reduction temperature window of 700–1000 K balances reduction kinetics and metal dispersion; too low a temperature results in incomplete reduction, with residual oxides reducing the number of active sites; too high a temperature intensifies metal migration, leading to particle growth and sintering. A reduction time of 0.5–4 h ensures the complete progress of the reduction reaction.
[0061] Example Example 1: A surface aluminum-enriched, bulk yttrium-doped cerium-zirconium composite oxide supported iron-cobalt bimetallic catalyst was prepared by the following method: S1. Preparation of bulk yttrium-doped cerium-zirconium composite oxide supports Taking the preparation of 5g of carrier as an example, 5.86g of Ce(NO3)3·6H2O, 0.57g of Y(NO3)3·6H2O, and 4.01g of ZrO(NO3)2·2H2O were weighed according to the molar ratio of Ce:Y:Zr = 0.45:0.05:0.50, and added to 80mL of deionized water to form a mixed metal salt solution. Based on the total molar number of metal ions, 9.46g of citric acid monohydrate (citric acid / total metal ion molar ratio of 1.5) and 4.38g of EDTA (EDTA / total metal ion molar ratio of 0.5) were added, along with 6.0mL of ethylene glycol as a polymerization aid. After stirring at 80℃ and 500rpm for 4h, the mixture was slowly evaporated at 90℃ to form a gel. The resulting gel was dried at 120℃ for 12 hours, then ground and heated to 500℃ at 5℃ / min in air and held for 5 hours to obtain a bulk yttrium-doped cerium-zirconium composite oxide support.
[0062] S2, Surface aluminum enrichment modification Taking the 5.00 g support obtained from S1 as an example, it was dispersed in 100 mL of deionized water and sonicated for 30 min. Separately, 0.44 g of Al(NO3)3·9H2O and 0.70 g of urea were dissolved in 20 mL of deionized water. The resulting solution was added dropwise to the support suspension at 85 °C and 600 rpm and deposition continued for 4 h. After filtration, the solution was washed with deionized water until the filtrate was nearly neutral, dried at 110 °C for 12 h, and then heated to 500 °C at 2 °C / min and held at that temperature for 2.5 h in air atmosphere to obtain a bulk yttrium-doped cerium-zirconium composite oxide support with aluminum enrichment on the surface.
[0063] Preparation of S3, iron-cobalt bimetallic supported catalyst Taking the 5.00g surface aluminum enrichment support obtained from S2 as an example, 7.24g of Fe(NO3)3·9H2O and 0.49g of Co(NO3)2·6H2O were dissolved in 15mL of a mixed solvent of ethanol / deionized water (volume ratio 1:1). The Fe and Co precursors were introduced using a two-step equal-volume co-impregnation method, with 7.5mL of impregnation solution added each time and thoroughly mixed until the support completely absorbed the impregnation solution. After impregnation, the mixture was aged at room temperature for 6h, dried at 110℃ for 12h, and then pre-decomposed at 320℃ under N2 atmosphere for 2h to obtain the precursor catalyst.
[0064] The loading amounts of Fe and Co are 20wt% and 2wt% respectively.
[0065] S4, Catalyst Activation The precursor catalyst obtained from S3 was reduced in a hydrogen-containing atmosphere. Preferably, the reducing atmosphere was a 10 vol% H2 / N2 mixture with a total flow rate of 60 sccm; the reduction temperature was 973 K, and the reduction time was 0.5 h, thus obtaining a surface aluminum-enriched, bulk yttrium-doped cerium-zirconium composite oxide supported iron-cobalt bimetallic catalyst 20Fe-2Co / Al-surface-Ce 0.45 Zr 0.50 Y 0.05 O2 δ (Al2O3=1.2wt%).
[0066] To verify the successful synthesis of the catalyst in Example 1, the following was performed: Figure 1 X-ray diffraction, Figure 2 Morphological analysis and Figure 3 Elemental distribution map representation. (From...) Figure 1 and Figure 3 It can be seen that Fe, Co, and Al were successfully loaded onto the bulk yttrium-doped cerium-zirconium composite oxide support. Its overall morphology is as follows: Figure 2 The catalyst in Example 1 exhibits an irregular polyhedral or near-spherical particle morphology with a relatively uniform particle size distribution. Fine particulate matter is visible dispersed on the catalyst surface; these are the Fe-Co metallic active components formed after reduction.
[0067] Example 2, a surface aluminum-enriched bulk yttrium-doped cerium-zirconium composite oxide supported iron-cobalt bimetallic catalyst, differs from Example 1 in the amount of surface aluminum modification in step S2, as detailed below: S2, Surface aluminum enrichment modification Taking 5.00 g of the carrier obtained from S1 as an example, it was dispersed in 100 mL of deionized water and sonicated for 30 min. Separately, 0.11 g of Al(NO3)3·9H2O and 0.18 g of urea were dissolved in 20 mL of deionized water. The resulting solution was added dropwise to the carrier suspension at 85 °C and 600 rpm and deposition continued for 4 h. After filtration, the solution was washed with deionized water until the filtrate was nearly neutral, dried at 110 °C for 12 h, and then heated to 500 °C at 2 °C / min and held at that temperature for 2.5 h in air atmosphere to obtain a carrier with a surface aluminum modification amount of approximately 0.3 wt% (based on Al2O3).
[0068] The catalyst composition is 20Fe-2Co / Al-surface–Ce 0.45 Zr 0.50 Y 0.05 O2 δ (Al2O3=0.3wt%).
[0069] Example 3: A surface aluminum-enriched bulk yttrium-doped cerium-zirconium composite oxide supported iron-cobalt bimetallic catalyst, differing from Example 1 in the amount of surface aluminum modification in step S2, as detailed below: S2, Surface aluminum enrichment modification Taking 5.00 g of the carrier obtained from S1 as an example, it was dispersed in 100 mL of deionized water and sonicated for 30 min. Separately, 1.10 g of Al(NO3)3·9H2O and 1.75 g of urea were dissolved in 25 mL of deionized water. The resulting solution was added dropwise to the carrier suspension at 85 °C and 600 rpm and deposition continued for 4 h. After filtration, the solution was washed with deionized water until the filtrate was nearly neutral, dried at 110 °C for 12 h, and then heated to 500 °C at 2 °C / min and held at that temperature for 2.5 h in air atmosphere to obtain a carrier with a surface aluminum modification amount of approximately 3.0 wt% (based on Al2O3).
[0070] The catalyst composition is 20Fe-2Co / Al-surface–Ce 0.45 Zr 0.50 Y 0.05 O2 δ (Al2O3=3.0wt%).
[0071] Example 4: A surface aluminum-enriched bulk yttrium-doped cerium-zirconium composite oxide supported iron-cobalt bimetallic catalyst, differing from Example 1 in that the Fe loading is 5 wt% and the Co loading is 0.5 wt% in step S3, as detailed below: Taking the 5.00g surface aluminum enrichment support obtained from S2 as an example, 1.81g of Fe(NO3)3·9H2O and 0.12g of Co(NO3)2·6H2O were dissolved in 12mL of ethanol / deionized water (volume ratio 1:1). The Fe and Co precursors were introduced using a two-step equal-volume co-impregnation method, with 6mL of impregnation solution added each time and thoroughly mixed. After impregnation, the mixture was aged at room temperature for 4h, dried at 110℃ for 12h, and then pre-decomposed at 300℃ for 2h under N2 atmosphere to obtain the precursor catalyst.
[0072] The loading amounts of Fe and Co are 5wt% and 0.5wt% respectively.
[0073] The catalyst composition is 5Fe-0.5Co / Al-surface–Ce 0.45 Zr 0.50 Y 0.05 O2 δ .
[0074] Example 5: A surface-enriched aluminum-bulk yttrium-doped cerium-zirconium composite oxide supported iron-cobalt bimetallic catalyst, differing from Example 1 in that the Fe loading in step S3 is 25 wt% and the Co loading is 5 wt%, as detailed below: Taking the 5.00g surface aluminum enrichment support obtained from S2 as an example, 9.05g of Fe(NO3)3·9H2O and 1.23g of Co(NO3)2·6H2O were dissolved in 20mL of ethanol / deionized water (volume ratio 1:1). The Fe and Co precursors were introduced using a two-step equal-volume co-impregnation method, with 10mL of impregnation solution added each time and thoroughly mixed. After impregnation, the mixture was aged at room temperature for 6h, dried at 110℃ for 12h, and then pre-decomposed at 320℃ for 2h under N2 atmosphere to obtain the precursor catalyst.
[0075] The loading amounts of Fe and Co are 25wt% and 5wt% respectively.
[0076] The catalyst composition is 25Fe-5Co / Al-surface–Ce 0.45 Zr 0.50 Y 0.05 O2 δ .
[0077] Comparative Example Comparative Example 1 is an iron-cobalt bimetallic catalyst supported on a surface aluminum-enriched bulk yttrium-doped cerium-zirconium composite oxide, which differs from Example 1 only in that it does not introduce Co.
[0078] The catalyst composition is 20Fe / Al-surface–Ce 0.45 Zr 0.50 Y 0.05 O2 δ .
[0079] Comparative Example 2 is an iron-cobalt bimetallic catalyst supported on a surface aluminum-enriched bulk yttrium-doped cerium-zirconium composite oxide, which differs from Example 1 only in that Fe is not introduced.
[0080] The catalyst composition is 2Co / Al-surface–Ce 0.45 Zr 0.50 Y 0.05 O2 δ .
[0081] Comparative Example 3 is an iron-cobalt bimetallic catalyst supported on a surface aluminum-enriched bulk yttrium-doped cerium-zirconium composite oxide, which differs from Example 1 only in that Y is not introduced.
[0082] The catalyst composition is 20Fe-2Co / Al-surface–Ce0.50 Zr 0.50 O2 δ .
[0083] Comparative Example 4 is a surface aluminum enrichment-bulk yttrium-doped cerium-zirconium composite oxide supported iron-cobalt bimetallic catalyst, which differs from Example 1 only in that the surface aluminum enrichment modification in step S2 is not performed.
[0084] The catalyst composition is 20Fe-2Co / Ce 0.45 Zr 0.50 Y 0.05 O2 δ .
[0085] Comparative Example 5: The catalyst prepared in this invention was replaced with A301 commercial iron-based ammonia synthesis catalyst.
[0086] Performance testing: 1. The activated catalyst is loaded into a fixed-bed reactor, and an N2 / H2 mixture is introduced. Ammonia synthesis is tested under a DC electric field. The apparatus is as follows: Figure 4 As shown, the electric field-assisted ammonia synthesis performance testing device includes a raw material gas cylinder 1, a mass flow meter 2, a tubular furnace 3, a high-pressure reaction tube 4, a catalyst 5, an external DC power supply 7, and a gas chromatograph 8. The raw material gas cylinder 1 stores a mixture of 75% H2 and 25% N2 by volume. After being precisely metered by the mass flow meter 2, the raw material gas is introduced into the high-pressure reaction tube 4, which is placed inside the tubular furnace 3. The catalyst 5 is packed in the middle of the high-pressure reaction tube 4 to form a catalyst bed. The tubular furnace 3 provides the reaction temperature required for the catalyst bed. The external DC power supply 7 is electrically connected to both sides of the catalyst bed in the high-pressure reaction tube 4 via wires 6, applying a DC electric field to the catalyst 5, allowing the ammonia synthesis reaction to proceed under electric field-assisted conditions. The tail gas after the reaction is introduced into the gas chromatograph 8 through a pipeline to detect the ammonia content in the product online, thereby calculating the ammonia production rate and evaluating the activity and stability of the catalyst.
[0087] The specific parameters are shown in Table 1: Table 1
[0088] The test results are shown in Table 2 and Figure 5 As shown: Table 2
[0089] 2. Stability testing: The activated catalyst was loaded into a fixed-bed reactor, and a N2 / H2 mixture was introduced. A long-term ammonia synthesis test was conducted for 2400 hours under a DC electric field. The apparatus is as follows: Figure 4As shown in Table 3. The stability test results are also shown in Table 3. Figure 6 As shown: Table 3
[0090] Based on Tables 2 and 3, and considering Examples 1 and Comparative Example 1, it can be seen that the ammonia production rate and stability retention rate of Comparative Example 1 are significantly lower than those of Example 1, indicating that the introduction of Co plays a crucial role in improving catalytic activity and stability. This is because the introduction of Co forms a Fe-Co bimetallic synergistic system. Fe acts as the main N2 adsorption and activation center, while the presence of Co promotes the activation and dissociation of H2. Simultaneously, Co modulates the electronic structure of Fe through electronic effects, placing Fe in a more suitable electronic state to facilitate N2 adsorption. Furthermore, the alloy or close-contact interface structure formed by Co and Fe effectively stabilizes small-sized metal species, inhibiting sintering and agglomeration of Fe during reduction and long-term reaction processes, thereby significantly improving the stability of the catalyst.
[0091] Combining Example 1 and Comparative Example 2, it can be seen that the ammonia production rate and stability retention rate of Comparative Example 2 are significantly lower than those of Example 1. This indicates that Fe is the key active component responsible for the main catalytic activity in this catalyst system. This is because Fe has excellent N2 adsorption and activation capabilities, effectively dissociating stable N≡N; while Co, when present alone, although it can promote H2 activation, has weak N2 adsorption capabilities and cannot effectively drive the ammonia synthesis reaction. Simultaneously, lacking the anchoring effect of Fe, Co metal particles are more prone to migration and aggregation under electric fields and reducing atmospheres, leading to a sharp decrease in the number of active sites and a significant decline in stability.
[0092] Combining Example 1 and Comparative Example 3, it can be seen that the ammonia production rate and stability retention rate of Comparative Example 3 are lower than those of Example 1. This indicates that bulk Y doping plays an important role in improving catalytic activity. The reason for this is that Y... 3+ Replace Ce 4+ Entering the lattice of cerium-zirconium composite oxides, oxygen vacancy defects are introduced into the support due to differences in valence state and ionic radius. These oxygen vacancy defects not only improve the oxygen ion mobility and surface oxygen activity of the support, but more importantly, under electric field-assisted conditions, oxygen vacancies can act as electron trapping centers, promoting electron conduction and interfacial charge transfer in the support, and enhancing the electronic interaction between the metal and the support. Furthermore, Y doping improves the thermal and structural stability of the support, enabling it to maintain a stable defect structure under electric fields and reducing atmospheres, providing a stable anchoring environment for the Fe-Co bimetallic compound, thereby synergistically enhancing catalytic activity and long-term stability.
[0093] Combining Example 1 and Comparative Example 4, it can be seen that the ammonia production rate and stability retention rate of Comparative Example 4 are lower than those of Example 1. This indicates that surface Al enrichment modification is crucial for maintaining high activity. The reason is that the surface-enriched Al exists on the support surface in the form of Al₂O₃. Al₂O₃ has strong Lewis acidic sites, which can form strong metal-support interactions with Fe and Co precursors. This strong interaction effectively anchors Fe and Co metal particles during reduction, inhibiting the sintering and agglomeration of metal species under high-temperature reduction and long-term reaction conditions, thus maintaining the high dispersion and small size effect of the metals.
[0094] Combining Example 1 and Comparative Example 5, it can be seen that the ammonia production rate and stability retention rate of Comparative Example 5 are significantly lower than those of Example 1. This indicates that the catalyst of the present invention has performance advantages far exceeding those of traditional commercial catalysts under electric field-assisted low-temperature ammonia synthesis conditions.
[0095] The above-disclosed embodiments are merely a few specific examples of the present invention. However, the embodiments of the present invention are not limited thereto, and any variations that can be conceived by those skilled in the art should fall within the protection scope of the present invention.
Claims
1. A surface-enriched aluminum-bulk yttrium-doped cerium-zirconium composite oxide supported iron-cobalt bimetallic catalyst, characterized in that, The catalyst includes a support and an active component supported on the surface of the support; The carrier is a cerium-zirconium composite oxide with aluminum enriched on the surface and yttrium doped in the bulk phase; The active components include Fe and Co; The chemical formula of the cerium-zirconium composite oxide is Ce. 0.45 Zr 0.50 Y 0.05 O2 δ , where 0 < δ ≤ 0.30; Relative to the mass of the carrier, the loading of Fe is 5–25 wt%, and the loading of Co is 0.5–5 wt%. The aluminum, calculated as Al2O3, accounts for 0.3 to 3 wt% of the carrier mass.
2. A preparation method for preparing the catalyst of claim 1, characterized in that, Includes the following steps: S1. Preparation of bulk yttrium-doped cerium-zirconium composite oxide support; S2. Perform surface aluminum enrichment modification on the carrier; S3. Introduce Fe and Co precursors onto the modified support; S4. The precursor catalyst is obtained by drying and heat treatment; The Fe and Co precursors are introduced through the following steps: Fe and Co sources are dissolved in a solvent, and Fe and Co are introduced by a two-step equal-volume co-impregnation method. After impregnation, the mixture is aged for 4-6 hours, dried, and then pre-decomposed at 300-400℃ under an inert gas for 1-3 hours to obtain the product. The precursor catalyst also includes a reduction and activation treatment in a hydrogen-containing atmosphere; The hydrogen-containing atmosphere for the reduction and activation treatment is a 5-20 vol% H2 / N2 mixture, the reduction temperature is 700-1000 K, and the reduction time is 0.5-4 h.
3. The preparation method according to claim 2, characterized in that, The bulk yttrium-doped cerium-zirconium composite oxide support was prepared by complexation polymerization, sol-gel method or co-precipitation method; The complexation polymerization method includes the following steps: Ce source, Y source and Zr source are added to deionized water according to the molar ratio in the chemical formula of cerium-zirconium composite oxide to form a mixed metal salt solution; citric acid, EDTA and polymerization aid are added according to the total metal ion molar ratio, and the mixture is stirred and slowly evaporated to form a gel; after drying and crushing, it is calcined at a temperature of 450-600℃ for 3-6 hours to obtain the final product.
4. The preparation method according to claim 2, characterized in that, The surface aluminum enrichment modification is achieved by deposition-precipitation method, surface complexation method or surface impregnation method; The deposition-precipitation method includes the following steps: A bulk yttrium-doped cerium-zirconium composite oxide support was dispersed in deionized water to obtain a support dispersion. An Al source and urea were dissolved in deionized water, and the resulting solution was added dropwise to the support dispersion at 80–90 °C with stirring, and allowed to settle for 2–6 h. The solution was filtered and washed until it was neutral, dried, and then calcined at 400–600 °C for 1–4 h to obtain the final product.
5. The application of the catalyst according to claim 1 in electric field-assisted low-temperature ammonia synthesis, characterized in that, The reaction takes place in a fixed-bed reactor, with an electric field applied by a DC power supply; the reactant gases include N2 and H2.