AI Technical Summary

Technical Problem

[0003]本发明提供了一种三氧化二铁的制备方法,以解决现有技术制备得到的ε-Fe2O3晶界数量多、结构杂乱的问题

Benefits of technology

1.本发明提供的三氧化二铁的制备方法,包括如下步骤:将衬底置于铁源的上方,在氧化性气氛下沉积生长8min-10min,降温后得到所述三氧化二铁;所述氧化性气氛包括氧气,所述氧气的流量为40sccm-60sccm。本发明制备得到的三氧化二铁元素分布均匀、晶相纯度高,材料具有热力学稳定的仅含单条晶界的多晶结构,单孪晶界可有效调制微观界面排布,显著提高ε-Fe2O3的晶体管的栅控能力。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122648903A_ABST
    Figure CN122648903A_ABST
Patent Text Reader

Abstract

The application relates to the technical field of nanometer materials, and discloses ferroferric oxide as well as a preparation method and application thereof. The preparation method of the ferroferric oxide provided by the application comprises the following steps: placing a substrate above an iron source, depositing and growing under an oxidizing atmosphere for 8-10 min, and obtaining the ferroferric oxide after cooling; the oxidizing atmosphere comprises oxygen, and the flow rate of the oxygen is 40-60 sccm. The ferroferric oxide prepared by the method has uniform element distribution and high crystal phase purity, the material has a thermodynamically stable polycrystalline structure containing only a single crystal boundary, the single twin boundary can effectively modulate the micro-interface arrangement, and the gate control capability of the transistor of epsilon-Fe2O3 is significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of nanomaterials technology, specifically to ferric oxide, its preparation method, and its applications. Background Technology

[0002] Nanomaterials, with their unique magnetic, electrical, and optical properties, as well as excellent magnetoelectric coupling effects and electrocatalytic properties, have shown broad application prospects in cutting-edge fields such as nanoelectronic devices, memristors, high-temperature information storage, new energy conversion, and environmental governance, and have become one of the research hotspots in the field of functional materials. Among them, ε-Fe2O3, due to its simultaneous ferromagnetic and ferroelectric properties, can effectively achieve mutual modulation of magnetoelectric signals, making it an ideal material for fabricating high-performance electronic devices. However, the ε-Fe2O3 crystals prepared by existing techniques have disordered growth directions and cannot precisely control the grain boundary structure. The large number and disordered structure of grain boundaries in polycrystalline materials significantly reduce the gate control capability of ε-Fe2O3 transistors, thus affecting the stability of transistor devices. Therefore, how to improve the preparation method of ferric oxide to prepare ferric oxide with regular crystal growth and good uniformity is a technical problem that urgently needs to be solved in this field. Summary of the Invention

[0003] This invention provides a method for preparing ferric oxide to solve the problem of the large number of grain boundaries and disordered structure of ε-Fe2O3 prepared by existing technologies.

[0004] In a first aspect, the present invention provides a method for preparing ferric oxide, comprising the following steps: The substrate was placed above the iron source, and the iron oxide was deposited and grown in an oxidizing atmosphere for 8-10 minutes. After cooling, the ferric oxide was obtained. The oxidizing atmosphere includes oxygen, and the oxygen flow rate is 40 sccm-60 sccm.

[0005] In one alternative embodiment, the deposition temperature is 690°C-700°C.

[0006] In one alternative embodiment, the iron source includes at least one of ferrous chloride, ferric carbonyl, and ferric nitrate.

[0007] In one alternative embodiment, the oxidizing atmosphere further includes the introduction of an inert gas.

[0008] In one alternative embodiment, the flow rate of the inert gas is 140 sccm-160 sccm.

[0009] In one alternative implementation, during the cooling step, the oxygen supply is stopped.

[0010] In one alternative embodiment, during the cooling step, the flow rate of the inert gas is 100 sccm-150 sccm.

[0011] In one alternative embodiment, the substrate comprises mica.

[0012] In a second aspect, the present invention provides ferric oxide prepared by the preparation method described in the first aspect.

[0013] In one alternative embodiment, the ferric oxide has an ε phase.

[0014] Thirdly, the present invention provides an application of ferric oxide prepared by the preparation method described in the first aspect or ferric oxide described in the second aspect in magnetoelectric functional devices, nanoelectronic devices, magnetic storage devices or ferroelectric storage devices.

[0015] The technical solution of this invention has the following advantages: 1. The method for preparing ferric oxide provided by this invention includes the following steps: placing a substrate above an iron source, depositing and growing it in an oxidizing atmosphere for 8-10 minutes, and then cooling it to obtain the ferric oxide; the oxidizing atmosphere includes oxygen, and the oxygen flow rate is 40 sccm-60 sccm. The ferric oxide prepared by this invention has uniform elemental distribution, high crystal phase purity, and a thermodynamically stable polycrystalline structure containing only a single grain boundary. The single twin grain boundary can effectively modulate the microscopic interface arrangement, significantly improving the gate control capability of ε-Fe2O3 transistors. Attached Figure Description

[0016] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0017] Figure 1 This is the energy dispersive X-ray spectrum of ferric oxide prepared in Example 1 of this invention; wherein, (a) is the original scanning electron microscope image; (b) is the Fe element; and (c) is the O element. Figure 2These are atomic force microscopy (AFM) and magnetic force microscopy (MFM) images of ferric oxide prepared in Examples 2-4 of this invention; wherein, (a) is an AFM image of ferric oxide in Example 2; (b) is a MFM image of ferric oxide in Example 2; (c) is an AFM image of ferric oxide in Example 3; (d) is a MFM image of ferric oxide in Example 3; (e) is an AFM image of ferric oxide in Example 4; and (f) is a MFM image of ferric oxide in Example 4. Figure 3 These are magnetic force micrographs of ferric oxide prepared in Example 1 of the present invention; wherein, (a) Example 1; (b) Example 1 after 1 year of storage; Figure 4 This is a transmission electron microscope image of ferric oxide prepared in Example 1 of this invention with spherical aberration correction. Figure 5 These are selected area electron diffraction micrographs of ferric oxide prepared in Example 1 of the present invention; wherein, (a) and (b) correspond to the diffraction signals of the grains growing on the left and right sides of the twin domains; Figure 6 These are the Raman spectra of ferric oxide (b) and mica substrate (a) prepared in Example 1 of this invention; Figure 7 These are optical microscope images of ferric oxide prepared by comparative examples 1-4 of the present invention; wherein, (a) is comparative example 1; (b) is comparative example 2; (c) is comparative example 3; and (d) is comparative example 4. Figure 8 These are the Raman spectra of ferric oxide (b) and mica substrate (a) prepared in Comparative Example 1 of this invention. Detailed Implementation

[0018] The following embodiments are provided to better understand the present invention, but the following embodiments do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the scope of protection of the present invention.

[0019] Unless otherwise specified, the experimental steps or conditions in the examples were performed in accordance with conventional experimental procedures and conditions in the art. Reagents or instruments whose manufacturers are not specified are all commercially available products.

[0020] To address the above problems, in a first aspect, the present invention provides a method for preparing ferric oxide, comprising the following steps: The substrate was placed above the iron source, and the iron oxide was deposited and grown in an oxidizing atmosphere for 8-10 minutes. After cooling, the ferric oxide was obtained. The oxidizing atmosphere includes oxygen, and the oxygen flow rate is 40 sccm-60 sccm.

[0021] For example, the deposition time can be 8 min, 8.5 min, 9 min, 9.5 min, or 10 min. The oxygen flow rate can be 40 sccm, 42 sccm, 44 sccm, 46 sccm, 48 sccm, 50 sccm, 52 sccm, 54 sccm, 56 sccm, 58 sccm, or 60 sccm.

[0022] In this invention, the oxygen flow rate is precisely controlled at 40 sccm-60 sccm. This moderate oxygen partial pressure promotes surface diffusion. Specifically, the 40 sccm-60 sccm oxygen flow rate provides a sufficiently high oxidation potential, effectively suppressing oxygen vacancy defects. This, in turn, increases the diffusion mobility of Fe and O adsorbed atoms on the growth surface, reduces the density of random secondary nucleation, and achieves precise splicing of single-crystal domains through a directional attachment mechanism, ultimately forming a polycrystalline structure containing only a single grain boundary. More importantly, this lowers the diffusion barrier of Fe and O adsorbed atoms on the growth surface, significantly increasing the diffusion length. Adsorbed atoms have sufficient time to "search" for the lowest-energy lattice position on the surface and tend to migrate to the edge of existing crystal domains rather than randomly forming new nuclei. This results in an extremely low nucleation density in the early stages of growth, forming only a few highly uniformly oriented single-crystal domain regions on the substrate. These domain regions expand laterally during subsequent growth and are precisely spliced ​​through a directional attachment mechanism, ultimately forming a polycrystalline structure containing only a single grain boundary. If the oxygen flow rate is <10 sccm, the surface is oxygen-deficient, defects increase, atomic diffusion is restricted, and fine, randomly oriented grains are easily formed. If the oxygen flow rate is too high (>60 sccm), the surface is covered with excessive oxygen, which hinders the migration of adsorbed atoms and leads to rough growth.

[0023] In this invention, the deposition time is precisely controlled to be 8-10 minutes. In the initial stage (<8 minutes): a few initial crystal nuclei with consistent orientation form on the substrate (possibly induced by substrate steps or local defects). Due to rapid surface diffusion, almost all new atoms are incorporated into the existing crystal nuclei, resulting in extremely low nucleation density. In the middle stage (8-10 minutes), the crystal nuclei grow laterally to form micron-sized single-crystal domain regions. At this time, adjacent domain regions are close but not yet in complete contact. Growth enters a critical stage – directional attachment: because each domain region has almost the same crystal orientation (with only a small angular deviation), driven by van der Waals forces or minimum interfacial energy, they will... Figure 1The samples are rotated, adjusted, and translated to converge, ultimately splicing together in a manner that shares an atomic plane to form a single, smooth, atomically merged grain boundary. This "splicing window" is typically very narrow, and the film covers the substrate in 8-10 minutes. If deposition continues, new atoms will randomly nucleate again on the existing film (secondary nucleation), thereby introducing new randomly oriented grains and more grain boundaries, disrupting the structure of the single grain boundary.

[0024] In addition, the present invention uses chemical vapor deposition, which has mild growth conditions, low raw material costs, good reproducibility, and a clean reaction process. The preparation process has no complicated steps, which is convenient for large-scale production. No toxic or harmful waste gas, waste liquid or waste residue is generated, which is environmentally friendly and in line with the development concept of green chemistry. It has broad prospects for industrial application.

[0025] In one alternative embodiment, the deposition temperature is 690°C-700°C. For example, the deposition temperature is 690°C, 692°C, 694°C, 696°C, 698°C, or 700°C.

[0026] In one alternative embodiment, the iron source includes at least one of ferrous chloride, ferric carbonyl, and ferric nitrate.

[0027] It should be noted that, in this invention, ferrous chloride is ferrous chloride tetrahydrate.

[0028] It should be noted that the iron source of this invention serves only as a supplier of iron during the deposition process. It undergoes a chemical reaction on the substrate surface and decomposes, no longer retaining its original structure. The resulting ferric oxide exhibits significant anisotropy in its crystal planes, with a specific crystal plane (e.g., the (001) plane with the lowest binding energy to the mica substrate) strongly dominating growth. Under an oxygen flow rate of 40-60 sccm and a suitable temperature, all deposited atoms preferentially stack parallel to the substrate with this low-energy plane. All initial crystal nuclei formed on the substrate possess almost identical crystal orientations, a prerequisite for their subsequent precise assembly, much like a jigsaw puzzle.

[0029] When two highly aligned single-crystal domain regions (such as two domain regions with (001) planes parallel to the substrate) approach each other during growth, if there is a small rotation angle or translational deviation between them, the system will reduce the total interface energy through atomic rearrangement, drive them to rotate and align, and finally merge with an atomically smooth interface to form a single twin boundary), the energy is much lower than that of random large-angle grain boundaries in conventional polycrystalline materials.

[0030] In one alternative embodiment, the oxidizing atmosphere further includes the introduction of an inert gas.

[0031] In one optional embodiment, the flow rate of the inert gas is 140 sccm-160 sccm. For example, the flow rate of the inert gas is 140 sccm, 142 sccm, 144 sccm, 146 sccm, 148 sccm, 150 sccm, 152 sccm, 154 sccm, 156 sccm, 158 sccm, or 160 sccm.

[0032] In one alternative implementation, during the cooling step, the oxygen supply is stopped.

[0033] In one optional embodiment, the flow rate of the inert gas during the cooling step is 100 sccm-150 sccm. For example, the flow rate of the inert gas is 100 sccm, 115 sccm, 120 sccm, 125 sccm, 130 sccm, 135 sccm, 140 sccm, 145 sccm, or 150 sccm.

[0034] In one alternative embodiment, the substrate comprises mica.

[0035] It should be noted that the substrate of the present invention has atomically flat steps or platforms, which is conducive to epitaxial nucleation. No chemical reaction occurs between the substrate and the iron source, which only provides a physical template, thus avoiding the formation of an interface reaction layer that interferes with epitaxy.

[0036] In a second aspect, the present invention provides ferric oxide prepared by the preparation method described in the first aspect.

[0037] In one alternative embodiment, the ferric oxide has an ε phase.

[0038] Thirdly, the present invention provides an application of ferric oxide prepared by the preparation method described in the first aspect or ferric oxide described in the second aspect in magnetoelectric functional devices, nanoelectronic devices, magnetic storage devices or ferroelectric storage devices.

[0039] Example 1 This embodiment provides a method for preparing ferric oxide, including the following steps: (1) Place 4 mica substrates (15×15×0.2mm) in a quartz tube with staggered stacking, and weigh 0.01g FeCl2·4H2O and place it below the substrate; (2) Before growth, rinse with 200 sccm of argon gas for 30 min, then adjust the argon gas flow rate to 160 sccm and introduce 40 sccm of oxygen. After 25 min, the temperature is raised to 690℃ and deposited for 8 min. After the reaction is completed, stop introducing oxygen and cool naturally to room temperature at a flow rate of 100 sccm to obtain ferric oxide.

[0040] Example 2 This embodiment provides a method for preparing ferric oxide, which is basically the same as the steps in Example 1, except that the deposition time is 9 minutes.

[0041] Example 3 This embodiment provides a method for preparing ferric oxide, which is basically the same as the steps in Example 1, except that the deposition time is 10 min.

[0042] Example 4 This embodiment provides a method for preparing ferric oxide, which is basically the same as the steps in Example 1, except that the oxygen flow rate is 50 sccm.

[0043] Example 5 This embodiment provides a method for preparing ferric oxide, which is basically the same as the steps in Example 1, except that the oxygen flow rate is 60 sccm.

[0044] Example 6 This embodiment provides a method for preparing ferric oxide, including the following steps: (1) Place four mica substrates (15×15×0.2mm) stacked in a quartz tube and weigh out 0.01g of carbonyl iron and place it under the substrate; (2) Before growth, rinse with 200 sccm of argon gas for 30 min, then adjust the argon gas flow rate to 150 sccm and introduce 40 sccm of oxygen. After 25 min, sinter at 695℃ for 8 min. After the reaction is completed, stop introducing oxygen and cool naturally to room temperature at 150 sccm of argon gas flow rate to obtain ferric oxide.

[0045] Example 7 This embodiment provides a method for preparing ferric oxide, including the following steps: (1) Place 4 mica substrates (15×15×0.2mm) stacked in a quartz tube and weigh 0.01g of ferric nitrate and place them below the substrate; (2) Before growth, rinse with 200 sccm of argon gas for 30 min, then adjust the argon gas flow rate to 140 sccm and introduce 40 sccm of oxygen. After 25 min, sinter at 700℃ for 8 min. After the reaction is completed, stop introducing oxygen and cool naturally to room temperature at 120 sccm of argon gas flow rate to obtain ferric oxide.

[0046] Comparative Example 1 This comparative example provides a method for preparing ferric oxide, which is basically the same as the steps in Example 1, except that the oxygen flow rate is 30 sccm.

[0047] Comparative Example 2 This comparative example provides a method for preparing ferric oxide, which is basically the same as the steps in Example 1, except that the oxygen flow rate is 70 sccm.

[0048] Comparative Example 3 This comparative example provides a method for preparing ferric oxide, which is basically the same as the steps in Example 1, except that the deposition growth time is 5 minutes.

[0049] Comparative Example 4 This comparative example provides a method for preparing ferric oxide, which is basically the same as the steps in Example 1, except that the deposition growth time is 15 min.

[0050] Experimental Example 1 The ferric oxide prepared in Example 1 was subjected to energy-dispersive X-ray spectroscopy (EDS), and the results are shown in the figure. Figure 1 As shown. From Figure 1 As can be seen, ferric oxide is in a banded form, and Fe and O elements are continuously and uniformly distributed throughout the entire region of the ferric oxide nanomaterial, without obvious elemental segregation, deficiency, or enrichment. Furthermore, the microstructure and crystal integrity of the material are clearly evident. This directly confirms that the ferric oxide nanomaterial prepared by this invention has a uniform composition, providing elemental evidence for the crystal phase purity and structural stability of the nanomaterial.

[0051] Experimental Example 2 The ferric oxide prepared in Examples 2-4 was tested using atomic force microscopy (AFM) and magnetic force microscopy (MFM). The results are shown in the figure. Figure 2 As shown. From Figure 2 As can be seen from the data, the surface of the strip-shaped ferric oxide prepared by this invention is generally flat, with only a few tiny surface protrusions (which may be residual particles or surface steps). The thickness profile shows that the thickness distribution is uniform, with no obvious undulations or structural defects, indicating that its growth uniformity is good.

[0052] Experimental Example 3 The ferric oxide prepared in Example 1 was subjected to magnetic force microscopy testing, and the results are shown below. Figure 3 As shown. From Figure 3As shown in (a), the ribbon-like ferric oxide prepared in this invention exhibits a clear bidomain structure. The magnetic domains on both sides are clearly distinguished by opposite phase signals (bright yellow and dark purple, respectively), and a distinct domain wall is formed in the middle. This indicates that the magnetic moment arrangement of the ferric oxide nanoribbons forms stable in-plane magnetic domains. The domain wall is clearly and continuously positioned, exhibiting a typical bipolar domain configuration. This further proves that the ribbon-like ferric oxide nanomaterial has a clear and stable single grain boundary configuration. After being placed under normal atmospheric conditions for one year, magnetic force microscopy tests were performed on it. Figure 3 - (b) It can be seen that the structural features of its twin boundaries do not degenerate, and the epitaxial growth orientation, geometric morphology, elemental distribution and other properties of the material can remain stable, proving that the single twin boundary structure has good environmental stability.

[0053] Experiment Example 4 The ferric oxide prepared in Example 1 was subjected to aberration-corrected transmission electron microscopy (TEM) testing, and the results are shown below. Figure 4 As shown. From Figure 4 As can be seen from the above, the banded iron oxide twin boundaries prepared by this invention are formed by the orderly splicing of single crystal domains. The single crystal domains coexist, and the orientation distribution of the crystal domains matches the symmetry of the substrate. They grow epitaxially along the

[100] direction of the crystal, and the interplanar spacing d (200) With a diameter of approximately 0.26 nm, it forms a single twin boundary with a 60° angle. There are no interfering crystal defects in the grain boundary, resulting in excellent structural stability. This provides a direct microstructural basis for the precise control of the single twin boundary structure.

[0054] Experimental Example 5 The ferric oxide prepared in Example 1 was subjected to selected area electron diffraction microscopy. The results are shown in the figure. Figure 5 As shown. From Figure 5 As can be seen from the diffraction pattern, there are two sets of regularly arranged discrete reciprocal lattice spots, which correspond to the diffraction signals of the grains growing on the left and right sides of the twin domain, respectively. The two sets of lattices are at a characteristic angle of 60° along the reciprocal vector b. The reciprocal space confirms that a single twin boundary configuration with an angle of 60° is formed during the epitaxial growth of the film along the

[100] crystal direction.

[0055] Experimental Example 6 Raman spectroscopy was performed on the ferric oxide and mica substrate prepared in Example 1. The results are shown in the figure. Figure 6 As shown. From Figure 6 As can be seen from the figure, the ferric oxide prepared by this invention has a temperature of 100 cm⁻¹. -1 Up to 200cm -1The presence of four sharp (M1, M2, M3, M4) characteristic peaks with relatively high intensity within the range, while the α and γ phases do not have any corresponding peaks within this range, proves that the ferric oxide prepared by this invention is the ε phase, and there are no scattered small protrusions or extra sharp impurity peaks, proving that the ferric oxide prepared by this invention has high purity and no impurities.

[0056] Experimental Example 7 The ferric oxide prepared in Comparative Examples 1-4 were subjected to optical microscopy testing, and the results are shown below. Figure 7 As shown. From Figure 7 As can be seen from the data, Comparative Examples 1-4 all prepared α-Fe₂O₃, which has a corundum crystal structure and belongs to the hexagonal crystal system (it can also be classified as the trigonal crystal system, space group R). c). Additionally, Raman spectroscopy was performed on the ferric oxide and mica substrate prepared in Comparative Example 1, and the results are shown in [the table below]. Figure 8 As shown. From Figure 8 As can be seen from the data, the ferric oxide obtained in Comparative Example 1 is a typical α-Fe2O3.

[0057] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A method for preparing ferric oxide, characterized in that, Includes the following steps: The substrate was placed above the iron source, and the iron oxide was deposited and grown in an oxidizing atmosphere for 8-10 minutes. After cooling, the ferric oxide was obtained. The oxidizing atmosphere includes oxygen, and the oxygen flow rate is 40 sccm-60 sccm.

2. The method for preparing ferric oxide according to claim 1, characterized in that, The deposition temperature is 690℃-700℃.

3. The method for preparing ferric oxide according to claim 1, characterized in that, The iron source includes at least one of ferrous chloride, ferric carbonyl, and ferric nitrate.

4. The method for preparing ferric oxide according to claim 1, characterized in that, The oxidizing atmosphere also includes the introduction of an inert gas; Optionally, the flow rate of the inert gas is 140 sccm-160 sccm.

5. The method for preparing ferric oxide according to claim 1, characterized in that, During the cooling step, the oxygen supply is stopped.

6. The method for preparing ferric oxide according to claim 1 or 5, characterized in that, In the cooling step, the flow rate of the inert gas is 100 sccm-150 sccm.

7. The method for preparing ferric oxide according to claim 1, characterized in that, The substrate includes mica.

8. Ferric oxide prepared by the preparation method according to any one of claims 1-7.

9. The ferric oxide according to claim 8, characterized in that, The crystalline phase of the ferric oxide is the ε phase.