A high molecular weight nylon 46 and its preparation method

By adding side reaction inhibitors during the preparation of nylon 46 and controlling the reaction conditions, the problem of 1,4-butanediamine deamination and cyclization at high temperatures was solved, achieving efficient preparation of high molecular weight nylon 46, improving product quality and stability, and making it suitable for industrial applications.

CN122772207BActive Publication Date: 2026-11-17VALIANT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202611244530.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-17
Publication Date
2026-11-17
Estimated Expiration
2046-08-17

AI Technical Summary

Technical Problem

Existing technologies for preparing high molecular weight nylon 46 suffer from severe side reactions of 1,4-butanediamine deamination and cyclization at high temperatures, resulting in low molecular weight, poor batch stability, high production costs, and difficulty in industrial production.

Method used

A salt-prepolymerization-solid-phase polymerization process was adopted, in which aliphatic tertiary amine compounds, pyridine and its derivatives, and imidazole compounds were added as side reaction inhibitors to control the reaction temperature and pressure, inhibit the cyclization reaction of 1,4-butanediamine, and improve the molecular weight and batch stability of the prepolymer.

Benefits of technology

It significantly improves the relative viscosity and number-average molecular weight of nylon 46, resulting in excellent product quality, good batch stability, mild reaction conditions, simple operation, high safety, and suitability for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention belongs to the field of polymer materials technology, specifically relating to a high molecular weight nylon 46 and its preparation method. The preparation method includes a salt-forming-prepolymerization-solid-phase polymerization process, by adding organic base-based side reaction inhibitors to the reaction system, including aliphatic tertiary amine compounds, pyridine and its derivatives, and imidazole compounds. This method can effectively inhibit the deamination and cyclization side reaction of 1,4-butanediamine at high temperatures, significantly improving the relative viscosity and molecular weight of the PA46 product. The obtained PA46 product has a relative viscosity of over 2.4 and a number-average molecular weight of over 60,000. It effectively improves the batch stability of the product. The method has mild reaction conditions, is simple and easy to control, has a high safety factor, and the side reaction inhibitors can be recycled and reused, demonstrating good feasibility for industrial production. The obtained PA46 product is whiter and lighter in color, exhibiting excellent product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention specifically relates to a high molecular weight nylon 46 and its preparation method, belonging to the field of polymer materials technology. Background Technology

[0002] Nylon 46, also known as polyamide 46 or PA46, is a high-temperature nylon material. The nylon 46 molecular chain contains four methylene groups arranged regularly between the amide groups, exhibiting a symmetrical structure. This perfectly regular arrangement can form a parallel structure in the α-type triclinic crystal system and an antiparallel structure in the β-type monoclinic crystal system. This gives Nylon 46 excellent temperature resistance, creep resistance, chemical resistance, abrasion resistance, dimensional stability, and superior processing and mechanical properties, making it widely used in the automotive, machinery, electronics, and aerospace industries.

[0003] With the continuous advancement of science and technology, the demand for PA46 products has been increasing year by year, making it of great significance to promote the research on efficient methods for preparing high molecular weight nylon 46.

[0004] The monomers for synthesizing Nylon 46 are 1,4-butanediamine and adipic acid. The preparation process generally involves salt formation, prepolymerization, and solid-state post-condensation polycondensation. However, the prepolymerization temperature typically needs to be above 180℃. Under these high-temperature conditions, 1,4-butanediamine is prone to deamination and cyclization side reactions, generating cyclic derivatives of 1,4-butanediamine, cyclic oligomers, and prepolymers with cyclic terminal groups. This results in low degrees of polymerization and molecular weight in the prepolymers, making it difficult to increase the molecular weight of the final product and causing poor batch stability during production.

[0005] US Patent No. 4408036A discloses a process that first prepares nylon 46 salt in methanol solvent, then performs a prepolymerization process in an aqueous solvent to obtain nylon 46 prepolymer. The prepolymer is then extruded and granulated using a rotary granulator, and finally undergoes solid-phase thickening under a nitrogen-water vapor mixture to obtain the final nylon 46 product. This process is complex, has high production costs, and the prepolymer contains approximately 0.2 mg / g of cyclic terminal groups, resulting in severe side reactions and a final product with a number-average molecular weight of around 30,000. Chinese Patent Application No. CN119751850A discloses a two-stage salt formation-prepolymerization-solid-phase polycondensation process to prepare nylon 46. The salt formation pressure is 5-10 MPa, which results in high equipment requirements and a high risk factor, long operation time, and low production efficiency, making it unsuitable for industrial production.

[0006] In summary, the existing technology has obvious shortcomings. Therefore, it is of great significance to propose a preparation method that has mild reaction conditions, simple operation, low risk factor, and is easy to industrialize; at the same time, it can suppress the generation of side reactions and improve the molecular weight of nylon 46. Summary of the Invention

[0007] This invention addresses the shortcomings of existing technologies by providing a high molecular weight nylon 46 and its preparation method. This method effectively suppresses the deamination and cyclization side reaction of 1,4-butanediamine at high temperatures, significantly improving the relative viscosity and molecular weight of PA46 products. The resulting PA46 product has a relative viscosity of over 2.4 and a number-average molecular weight of over 60,000. It effectively improves batch stability. The method features mild reaction conditions, simple and easy operation, high safety, and the side reaction inhibitor can be recycled and reused, demonstrating good feasibility for industrial production. The resulting PA46 product is whiter and lighter in color, exhibiting superior product quality.

[0008] The technical solution of the present invention to solve the above-mentioned technical problems is as follows: a method for preparing high molecular weight nylon 46, the preparation method comprising the following steps: S1. Add 1,4-butanediamine, adipic acid, antioxidant, side reaction inhibitor and deionized water to the reaction vessel and carry out the salt formation reaction under inert conditions; S2. After the salt formation reaction is completed, the temperature is raised to carry out the prepolymerization reaction. After the reaction is completed, the reaction system is depressurized and the by-product water is discharged to obtain the prepolymer. S3. Transfer the prepolymer to a solid-state polymerization apparatus and carry out solid-state polymerization under inert conditions to obtain Nylon 46 product; The side effect inhibitor is at least one of aliphatic tertiary amine compounds, pyridine and its derivatives, and imidazole compounds.

[0009] Furthermore, in step S1, the reaction temperature is 80~100℃ and the reaction time is 1~3h.

[0010] Furthermore, in step S2, the temperature is raised to 180~200℃, and the reaction time is 2~4h.

[0011] Furthermore, in step S2, the system pressure is 1~2MPa.

[0012] Furthermore, in step S3, the reaction temperature is 230~260℃ and the reaction time is 4~8h.

[0013] Further, in step S1, the molar ratio of 1,4-butanediamine to adipic acid is (1.005~1.05):1; the amount of deionized water used is 10%~100% of the total mass of 1,4-butanediamine and adipic acid; the amount of antioxidant used is 0.1%~1% of the total mass of 1,4-butanediamine and adipic acid; and the amount of side reaction inhibitor used is 0.5%~5% of the total mass of 1,4-butanediamine and adipic acid.

[0014] Further, the aliphatic tertiary amine compound is at least one selected from triethylamine, tripropylamine, tri-n-butylamine, tetramethylethylenediamine, N-methylmorpholine, N-ethylmorpholine, 2-morpholine ethanol, N,N-dimethylethanolamine, N,N-diethylethanolamine, and N-methyldiethanolamine.

[0015] Furthermore, the pyridine and its derivative compounds are at least one selected from pyridine, 2-methylpyridine, 3-methylpyridine, 4-methylpyridine, 2-methoxypyridine, 3-methoxypyridine, 4-dimethylaminopyridine, and isoquinoline.

[0016] Furthermore, the imidazole compound is at least one of imidazole and 1-methylimidazolium.

[0017] Further, the antioxidant is N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexamethylenediamine (also known as antioxidant 1098), pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (also known as antioxidant 1010), 3,9-bis(2,4-dicumylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosspiro[5.5]undecane (also known as antioxidant 9228), 3, At least one of 9-bis[1,1-dimethyl-2-[(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane (also known as antioxidant A080), triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate (also known as antioxidant 245), and bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite (also known as antioxidant 626).

[0018] The present invention also provides a high molecular weight nylon 46, which is prepared by the preparation method provided by the present invention.

[0019] The beneficial effects of this invention are: The PA46 preparation method of this invention includes a salt formation-prepolymerization-solid-phase polymerization process. By adding organic base side reaction inhibitors, including aliphatic tertiary amine compounds, pyridine and its derivatives, and imidazole compounds, the deamination and cyclization side reaction of 1,4-butanediamine at high temperatures can be effectively suppressed. This allows the content of pyrrolidine terminal groups in the prepolymer to be controlled below 0.01 mg / g, thereby significantly improving the relative viscosity and molecular weight of the PA46 product. The obtained PA46 product has a relative viscosity of over 2.4 and a number-average Mn molecular weight of over 60,000. Simultaneously, it effectively improves the batch stability during PA46 formation. This method features mild reaction conditions, simple and easy operation, high safety, and the side reaction inhibitors can be recycled and reused, demonstrating good feasibility for industrial production. Furthermore, thanks to the effective suppression of side reactions, the obtained PA46 product is whiter and lighter in color, exhibiting excellent product quality. Detailed Implementation

[0020] The specific embodiments of the present invention will be described in detail below. The present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed.

[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used is for describing particular embodiments only and is not intended to limit the invention.

[0022] This invention provides a method for preparing high molecular weight nylon 46, the method comprising the following steps: S1. Add 1,4-butanediamine, adipic acid, antioxidant, side reaction inhibitor and deionized water to the reactor, replace the air in the reactor with an inert gas. After the replacement is completed, seal the reactor and heat it to 80~100℃ to carry out the salt formation reaction. The reaction time is 1~3h.

[0023] S2. After the salt formation reaction is completed, the temperature is raised to 180~200℃, at which point the system pressure is 1~2MPa, and the prepolymerization reaction is carried out for 2~4 hours. After the reaction is completed, the reaction system is depressurized and the by-product water is drained to obtain the prepolymer. S3. Transfer the prepolymer to a solid-state polymerization apparatus and carry out solid-state polymerization under inert conditions at a reaction temperature of 230~260℃ for a reaction time of 4~8h to obtain Nylon 46 product. The side effect inhibitor is at least one of aliphatic tertiary amine compounds, pyridine and its derivatives, and imidazole compounds.

[0024] Nylon 46 is synthesized by the condensation polymerization of 1,4-butanediamine and adipic acid. A key challenge in its preparation lies in the severe side reactions occurring at high temperatures. Nylon 46 has a high melting point, requiring a prepolymerization temperature above 180°C. At this temperature, the 1,4-butanediamine end groups can undergo intramolecular cyclization, generating pyrrolidine end groups. Once these cyclic end groups are formed, they can no longer participate in chain growth reactions, effectively "closing" the chain and preventing further molecular weight increases. Therefore, suppressing the cyclization side reaction of butanediamine is a crucial technical bottleneck in obtaining high-molecular-weight, white nylon 46 products. This invention introduces at least one of the following side reaction inhibitors: aliphatic tertiary amine compounds, pyridine and its derivatives, and imidazole compounds. This solution is specifically designed to address this core problem.

[0025] The side reaction inhibitor provided by this invention is a nitrogen-containing basic compound, whose core role in the system is to inhibit the chemical basis of cyclization. The cyclization reaction of butanediamine (forming pyrrolidine end groups) is an acid-catalyzed process. In the reaction system, the carboxyl group (-COOH) of adipic acid provides an acidic environment, promoting the protonation of the butanediamine end groups, thereby leading to intramolecular nucleophilic substitution cyclization. The side reaction inhibitor provided by this invention, as an organic base, functions in two ways: firstly, it neutralizes the acidity by forming salts / complexes with carboxyl groups or protonated amines in the system, reducing the local acidity and slowing down the cyclization rate from the source. Secondly, it competes for protons: the lone pair electrons on the nitrogen atom can capture protons, reducing the probability of the butanediamine end groups being protonated and protecting its active end groups from being "consumed" into cyclic inert end groups.

[0026] Specifically, in step S1, the molar ratio of 1,4-butanediamine to adipic acid is (1.005~1.05):1; the amount of deionized water used is 10%~100% of the total mass of 1,4-butanediamine and adipic acid; the amount of antioxidant used is 0.1%~1% of the total mass of 1,4-butanediamine and adipic acid; and the amount of side reaction inhibitor used is 0.5%~5% of the total mass of 1,4-butanediamine and adipic acid.

[0027] Specifically, the aliphatic tertiary amine compound is at least one of triethylamine, tripropylamine, tri-n-butylamine, tetramethylethylenediamine, N-methylmorpholine, N-ethylmorpholine, 2-morpholine ethanol, N,N-dimethylethanolamine, N,N-diethylethanolamine, and N-methyldiethanolamine.

[0028] Specifically, the pyridine and its derivatives are at least one of pyridine, 2-methylpyridine, 3-methylpyridine, 4-methylpyridine, 2-methoxypyridine, 3-methoxypyridine, 4-dimethylaminopyridine, and isoquinoline.

[0029] Specifically, the imidazole compound is at least one of imidazole and 1-methylimidazolium.

[0030] Specifically, the antioxidants are N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine (also known as antioxidant 1098), pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (also known as antioxidant 1010), 3,9-bis(2,4-dicumylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane (also known as antioxidant 9228), 3,9 -At least one of bis[1,1-dimethyl-2-[(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane (also known as antioxidant A080), triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate (also known as antioxidant 245), and bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite (also known as antioxidant 626).

[0031] Preferably, the side reaction inhibitor is any two of the following: aliphatic tertiary amine compounds, pyridine and its derivatives, and imidazole compounds.

[0032] In some embodiments, the side effect inhibitors are selected from a combination of aliphatic tertiary amine compounds and pyridine and its derivatives.

[0033] In some embodiments, the side effect inhibitors are selected from a combination of aliphatic tertiary amine compounds and imidazole compounds.

[0034] In some embodiments, the side effect inhibitors are selected from a combination of pyridine and its derivatives and imidazole compounds.

[0035] More preferably, the mass ratio of aliphatic tertiary amine compounds to pyridine and its derivatives is (3~4):(1~2); the mass ratio of aliphatic tertiary amine compounds to imidazole compounds is (3~4):(1~2); and the mass ratio of pyridine and its derivatives to imidazole compounds is (1~2):(1~2).

[0036] In this invention, the combined effect of two types of side effect inhibitors, with the total dosage remaining the same or even reduced, far exceeds that of a single inhibitor.

[0037] More preferably, the side reaction inhibitors are aliphatic tertiary amine compounds, pyridine and its derivatives, and imidazole compounds present simultaneously.

[0038] The preferred mass ratio of aliphatic tertiary amine compounds, pyridine and its derivatives, and imidazole compounds is (4~5):(2.5~3):(2.5~3).

[0039] It should be noted that the side reaction inhibitor added in this invention can be recycled and reused. The side reaction inhibitor has a low boiling point and can be collected along with the by-products during the prepolymerization process and solid-phase thickening process, or in the waste liquid or waste gas, without remaining in the product, thus not affecting the subsequent performance of the product. It can be separated and recovered by means of vacuum distillation, liquid-liquid extraction, ion exchange resin adsorption or column chromatography, and the recovered product can be reused after drying or distillation purification.

[0040] The present invention also provides a high molecular weight nylon 46, which is prepared by the preparation method provided by the present invention.

[0041] The high molecular weight nylon 46 product provided by this invention has a relative viscosity of 2.4 or higher and a number average molecular weight of 60,000 or higher; after whiteness testing, it can reach more than 90%, and the product quality is excellent, reaching the superior grade.

[0042] To better illustrate the embodiments of the present invention, the present invention will be further described in detail below through specific examples.

[0043] Example 1

[0044] This embodiment prepares a high molecular weight nylon 46, including the following steps: S1. Add 8903g (101mol) of 1,4-butanediamine, 14614g (100mol) of adipic acid, 23.5g of antioxidant 1098, 47.0g of antioxidant 626, 235g of triethylamine and 4700g of deionized water to the reactor, close the feed port, and repeatedly evacuate and purge the reactor with nitrogen gas more than 10 times to ensure that the reactants are in an inert gas protective environment. Then, seal the reactor and heat it to 90°C to carry out the salt formation reaction for 2 hours.

[0045] S2. After the salt formation reaction is completed, the temperature is raised to 190℃, at which point the system pressure is 1.4MPa. The reaction is maintained at this temperature for 3 hours. After the reaction is completed, the pressure relief valve is opened to drain the byproduct water, and the prepolymer is obtained. The relative viscosity is 1.21, the molecular weight of Mn is 7287, and the content of pyrrolidine terminal groups is 0.005mg / g of the prepolymer.

[0046] S3. The prepolymer was transferred to a solid-state polymerization apparatus and solid-state polymerization was carried out at 260°C under a nitrogen atmosphere for 6 hours to obtain Nylon 46 product; the relative viscosity was tested to be 2.49 and the molecular weight of Mn was 66691.

[0047] Example 2

[0048] This embodiment prepares a high molecular weight nylon 46, including the following steps: S1. Add 8859g (100.5mol) of 1,4-butanediamine, 14614g (100mol) of adipic acid, 23.5g of antioxidant 1098, 23.5g of antioxidant 9228, 117.4g of N-methylmorpholine and 2347g of deionized water to the reactor, close the feed port, and repeatedly evacuate and purge the reactor with nitrogen gas more than 10 times to ensure that the reactants are in an inert gas protective environment. Then, seal the reactor and heat it to 80°C to carry out the salt formation reaction for 3 hours.

[0049] S2. After the salt formation reaction is completed, the temperature is raised to 180℃, at which point the system pressure is 1.0MPa. The reaction is maintained at this temperature for 3 hours. After the reaction is completed, the pressure relief valve is opened to drain the byproduct water, and the prepolymer is obtained. The relative viscosity is 1.19, the molecular weight of Mn is 6497, and the content of pyrrolidine terminal groups is 0.006mg / g of the prepolymer.

[0050] S3. The prepolymer was transferred to a solid-state polymerization apparatus and solid-state polymerization was carried out at 260°C under a nitrogen atmosphere for 8 hours to obtain Nylon 46 product; the relative viscosity was tested to be 2.69 and the molecular weight of Mn was 75456.

[0051] Example 3

[0052] This embodiment prepares a high molecular weight nylon 46, including the following steps: S1. Add 8903g (101mol) of 1,4-butanediamine, 14614g (100mol) of adipic acid, 47.0g of antioxidant 1010, 1176g of pyridine and 23517g of deionized water to the reactor, close the feed port, and repeatedly evacuate and purge the reactor with nitrogen gas more than 10 times to ensure that the reactants are in an inert gas protective environment. Then, seal the reactor and heat it to 100°C to carry out the salt formation reaction for 1 hour.

[0053] S2. After the salt formation reaction is completed, the temperature is raised to 200℃, at which point the system pressure is 2.0MPa. The reaction is maintained at this temperature for 4 hours. After the reaction is completed, the pressure relief valve is opened to drain the byproduct water, and the prepolymer is obtained. The relative viscosity is 1.18, the molecular weight of Mn is 5924, and the content of pyrrolidine terminal groups is 0.005mg / g of the prepolymer.

[0054] S3. The prepolymer was transferred to a solid-state polymerization apparatus and solid-state polymerization was carried out at 240°C under a nitrogen atmosphere for 4 hours to obtain Nylon 46 product; the relative viscosity was tested to be 2.60 and the molecular weight of Mn was 71594.

[0055] Example 4

[0056] This embodiment prepares a high molecular weight nylon 46, including the following steps: S1. Add 9256g (105mol) of 1,4-butanediamine, 14614g (100mol) of adipic acid, 238.7g of antioxidant 1098, 597g of 4-dimethylaminopyridine and 4774g of deionized water to the reactor, close the feed port, and repeatedly evacuate and purge the reactor with nitrogen gas more than 10 times to ensure that the reactants are in an inert gas protective environment. Then, seal the reactor and heat it to 90°C to carry out the salt formation reaction for 3 hours.

[0057] S2. After the salt formation reaction is completed, the temperature is raised to 190℃, at which point the system pressure is 1.4MPa. The reaction is maintained at this temperature for 2 hours. After the reaction is completed, the pressure relief valve is opened to drain the byproduct water, and the prepolymer is obtained. The relative viscosity is 1.25, the molecular weight of Mn is 8747, and the content of pyrrolidine terminal groups is 0.004mg / g of the prepolymer.

[0058] S3. The prepolymer was transferred to a solid-state polymerization apparatus and solid-state polymerization was carried out at 250°C under a nitrogen atmosphere for 6 hours to obtain Nylon 46 product; the relative viscosity was tested to be 2.73 and the molecular weight of Mn was 77398.

[0059] Example 5

[0060] This embodiment prepares a high molecular weight nylon 46, including the following steps: S1. Add 8991g (102mol) of 1,4-butanediamine, 14614g (100mol) of adipic acid, 23.6g of antioxidant A080, 47.2g of antioxidant 9228, 236g of isoquinoline and 4721g of deionized water to the reactor, close the feed port, and repeatedly evacuate and purge the reactor with nitrogen gas more than 10 times to ensure that the reactants are in an inert gas protective environment. Then, seal the reactor and heat it to 100°C to carry out the salt formation reaction for 2 hours.

[0061] S2. After the salt formation reaction is completed, the temperature is raised to 200℃, at which point the system pressure is 1.8MPa. The reaction is maintained at this temperature for 3 hours. After the reaction is completed, the pressure relief valve is opened to drain the byproduct water, and the prepolymer is obtained. The relative viscosity is 1.26, the molecular weight of Mn is 9157, and the content of pyrrolidine terminal groups is 0.005mg / g of the prepolymer.

[0062] S3. The prepolymer was transferred to a solid-state polymerization apparatus and solid-state polymerization was carried out at 230°C under a nitrogen atmosphere for 5 hours to obtain Nylon 46 product; the relative viscosity was tested to be 2.75 and the molecular weight of Mn was 78342.

[0063] Example 6

[0064] This embodiment prepares a high molecular weight nylon 46, including the following steps: S1. Add 8903g (101mol) of 1,4-butanediamine (FW=88.15), 14614g (100mol) of adipic acid, 23.5g of antioxidant 245, 47.0g of antioxidant 626, 588g of imidazole and 4700g of deionized water to the reactor. Close the feed port and repeatedly evacuate and purge the reactor with nitrogen gas more than 10 times to ensure that the reactants are in an inert gas protective environment. Then, seal the reactor and heat it to 100°C to carry out the salt formation reaction for 3 hours.

[0065] S2. After the salt formation reaction is completed, the temperature is raised to 190℃, at which point the system pressure is 1.4MPa. The reaction is maintained at this temperature for 2 hours. After the reaction is completed, the pressure relief valve is opened to drain the byproduct water, and the prepolymer is obtained. The relative viscosity is 1.19, the molecular weight of Mn is 6500, and the content of pyrrolidine terminal groups is 0.006mg / g of the prepolymer.

[0066] S3. The prepolymer was transferred to a solid-state polymerization apparatus and solid-state polymerization was carried out at 250°C under a nitrogen atmosphere for 7 hours to obtain Nylon 46 product; the relative viscosity was tested to be 2.56 and the molecular weight of Mn was 68856.

[0067] Example 7

[0068] This embodiment uses the same method as in Example 1 to prepare a high molecular weight nylon 46, except that in step S1, the side reaction inhibitors are 164.5g triethylamine and 70.5g 2-methylpyridine.

[0069] Example 8

[0070] This embodiment uses the same method as in Example 1 to prepare a high molecular weight nylon 46, except that in step S1, the side reaction inhibitors are 164.5g triethylamine and 70.5g imidazole.

[0071] Example 9

[0072] This embodiment uses the same method as in Example 1 to prepare a high molecular weight nylon 46, except that in step S1, the side reaction inhibitors are 117g of 2-methylpyridine and 118g of imidazole.

[0073] Example 10

[0074] This embodiment uses the same method as in Example 1 to prepare a high molecular weight nylon 46, except that in step S1, the side reaction inhibitors are 94g triethylamine, 70.5g 2-methylpyridine and 70.5g imidazole.

[0075] Comparative Example 1 This comparative example uses the same method as Example 1 to prepare a high molecular weight nylon 46, except that triethylamine is not added in step S1.

[0076] Specifically, the following steps are included: S1. Add 8903g (101mol) of 1,4-butanediamine, 14614g (100mol) of adipic acid, 23.5g of antioxidant 1098, 47.0g of antioxidant 626 and 4700g of deionized water to the reactor, close the feed port, and repeatedly evacuate and purge the reactor with nitrogen gas more than 10 times to ensure that the reactants are in an inert gas protective environment. Then, seal the reactor and heat it to 90°C to carry out the salt formation reaction for 2 hours.

[0077] S2. After the salt formation reaction is completed, the temperature is raised to 200℃, at which point the system pressure is 1.2MPa. The reaction is maintained at this temperature for 3 hours. After the reaction is completed, the pressure relief valve is opened to drain the byproduct water, and the prepolymer is obtained. The relative viscosity is 1.09, the molecular weight of Mn is 2642, and the content of pyrrolidine terminal groups is 0.122mg / g of the prepolymer.

[0078] S3. The prepolymer was transferred to a solid-state polymerization apparatus and solid-state polymerization was carried out at 260°C under a nitrogen atmosphere for 4 hours to obtain Nylon 46 product; the relative viscosity was tested to be 1.63 and the molecular weight of Mn was 26361.

[0079] Comparative Example 2 This comparative example uses the same method as Example 2 to prepare a high molecular weight nylon 46, except that N-methylmorpholine is not added in step S1.

[0080] Specifically, the following steps are included: S1. Add 8859g (100.5mol) of 1,4-butanediamine, 14614g (100mol) of adipic acid, 23.5g of antioxidant 1098, 23.5g of antioxidant 9228 and 2347g of deionized water to the reactor, close the feed port, and repeatedly evacuate and purge the reactor with nitrogen gas more than 10 times to ensure that the reactants are in an inert gas protective environment. Then, seal the reactor and heat it to 80°C to carry out the salt formation reaction for 3 hours.

[0081] S2. After the salt formation reaction is completed, the temperature is raised to 190℃, at which point the system pressure is 1.0MPa. The reaction is maintained at this temperature for 3 hours. After the reaction is completed, the pressure relief valve is opened to drain the byproduct water, and the prepolymer is obtained. The relative viscosity is 1.19, the molecular weight of Mn is 3117, and the content of pyrrolidine terminal groups is 0.087mg / g of the prepolymer.

[0082] S3. The prepolymer was transferred to a solid-state polymerization apparatus and solid-state polymerization was carried out at 260°C under a nitrogen atmosphere for 6 hours to obtain Nylon 46 product; the relative viscosity was tested to be 1.77 and the molecular weight of Mn was 32840.

[0083] Comparative Example 3 This comparative example uses the same method as Example 3 to prepare a high molecular weight nylon 46, except that pyridine is not added in step S1.

[0084] Specifically, the following steps are included: S1. Add 8903g (101mol) of 1,4-butanediamine, 14614g (100mol) of adipic acid, 47.0g of antioxidant 1010 and 23517g of deionized water to the reactor, close the feed port, and repeatedly evacuate and purge the reactor with nitrogen gas more than 10 times to ensure that the reactants are in an inert gas protective environment. Then, seal the reactor and heat it to 100°C to carry out the salt formation reaction for 1 hour.

[0085] S2. After the salt formation reaction is completed, the temperature is raised to 200℃, at which point the system pressure is 1.2MPa. The reaction is maintained at this temperature for 4 hours. After the reaction is completed, the pressure relief valve is opened to drain the by-product water, and the prepolymer is obtained.

[0086] S3. Transfer the prepolymer to a solid-state polymerization apparatus and carry out solid-state polymerization at 240°C under a nitrogen atmosphere for 4 hours to obtain Nylon 46 product.

[0087] Comparative Example 4 This comparative example uses the same method as Example 6 to prepare a high molecular weight nylon 46, except that imidazole is not added in step S1.

[0088] Specifically, the following steps are included: S1. Add 8903g (101mol) of 1,4-butanediamine (FW=88.15), 14614g (100mol) of adipic acid, 23.5g of antioxidant 245, 47.0g of antioxidant 626 and 4700g of deionized water to the reactor, close the feed port, and repeatedly evacuate and purge the reactor with nitrogen gas more than 10 times to ensure that the reactants are in an inert gas protective environment. Then, seal the reactor and heat it to 100°C to carry out the salt formation reaction for 3 hours.

[0089] S2. After the salt formation reaction is completed, the temperature is raised to 200℃, at which point the system pressure is 1.2MPa. The reaction is maintained at this temperature for 2 hours. After the reaction is completed, the pressure relief valve is opened to drain the byproduct water, and the prepolymer is obtained.

[0090] S3. Transfer the prepolymer to a solid-state polymerization apparatus and perform solid-state polymerization at 250°C under a nitrogen atmosphere for 4 hours to obtain Nylon 46 product.

[0091] Comparative Example 5 This comparative example uses the same method as Example 1 to prepare a high molecular weight nylon 46, except that in step S2, the reaction temperature is 210°C.

[0092] Comparative Example 6 This comparative example uses the same method as Example 1 to prepare a high molecular weight nylon 46, except that in step S3, the reaction temperature is 270°C.

[0093] The performance of the PA46 prepolymer and PA46 product prepared in the embodiments and comparative examples of the present invention was tested. The performance test data are shown in Table 1. The test methods involved are as follows: (1) Test method for relative viscosity of PA46 prepolymer and product: Weigh 0.5000g of the sample using a precision balance (accuracy 0.0001g) and add it to 100mL of 99% formic acid. Stir and dissolve the solution at 20-30℃. After complete dissolution, place the solution in an Ubbelohde viscometer and incubate it in a constant temperature bath at 25℃ for 10 minutes, then measure the rate of descent, t. Similarly, measure the rate of descent, t0, of the 99% formic acid solution. Calculate the relative viscosity from t and t0 using the following formula: Relative viscosity = t / t0.

[0094] (2) Methods for testing the molecular weight of Mn in PA46 prepolymer and products: The test was performed by gel permeation chromatography (GPC), with PMMA as the standard and trifluoroethanol + 0.05% potassium trifluoroacetate as the solvent. After complete dissolution, the solution was filtered through a PTFE membrane and injected at 40°C for analysis to obtain the molecular weight and distribution relative to PMMA.

[0095] (3) Test method for pyrrolidine terminal group content of PA46 prepolymer: Weigh 1g of prepolymer sample into a glass tube, add 2mL of 6mol / L hydrochloric acid solution, seal the tube, and heat it in an oil bath to 120℃. Maintain this temperature until the sample is completely dissolved, and continue to keep it warm for 4 hours. Then, cool the glass tube, during which adipic acid crystals precipitate. After cooling to room temperature, open the glass tube, take 0.2mL of the supernatant, and add 0.7mL of 2mol / L NaOH solution to obtain the sample for gas chromatography analysis. Calculate the pyrrolidine content in 1g of prepolymer based on the gas chromatography test results, which is the pyrrolidine terminal group content of the prepolymer.

[0096] (4) Whiteness of PA46 products: Take a sample of 50g or more and sieve it using a 100-mesh standard sieve. If the proportion of coarse particles exceeds 5%, it needs to be ground and sieved again to ensure uniform particle size. Place the sieved sample into the sample cell, with a filling depth of ≥6mm. Scrape the surface smooth, without gaps or protrusions. Test the whiteness using a whiteness meter. Take the average of three tests as the final whiteness test result. Excellent grade is generally above 90%, and ordinary grade is 80-90%.

[0097] Table 1 Performance test data of PA46 prepolymer and PA46 products

[0098] As can be seen from Table 1, PA46 was prepared using the method described in this invention in Examples 1 to 10. During the reaction, side reaction inhibitors were added, resulting in a low content of pyrrolidine terminal groups in the prepolymer (less than 0.01 mg / g prepolymer). The prepolymer had relatively high relative viscosity and Mn molecular weight, and the PA46 product after solid-state polymerization also had high relative viscosity and Mn molecular weight (above 2.4 and above, with Mn molecular weight above 60,000). The products passed the whiteness test and were all of excellent quality (above 90%).

[0099] Compared with Examples 1, 2, 3, and 6, respectively, Comparative Examples 1, 2, 3, and 4, without the addition of side reaction inhibitors, yielded prepolymers with significantly higher pyrrolidine terminal group content, lower relative viscosity and Mn molecular weight, and the PA46 product after solid-state polymerization also had lower relative viscosity and Mn molecular weight. Therefore, adding side reaction inhibitors during the reaction process can effectively suppress the deamination and cyclization side reaction of 1,4-butanediamine, thereby improving the relative viscosity and molecular weight of the PA46 prepolymer and the final product, improving batch stability during PA46 production, and the preparation method has mild reaction conditions, simple operation, easy control, low risk, and is suitable for industrial production.

[0100] Compared with Comparative Example 5 and Example 1, in step S2, the prepolymerization reaction temperature is higher than the temperature specified in this invention, which accelerates the prepolymerization reaction rate. This is reflected in the increase of the relative viscosity and Mn molecular weight of the prepolymer. However, the degree of side reactions in the prepolymerization process is also increased, which is reflected in the increase of the pyrrolidine terminal group content of the prepolymer. This leads to a decrease in the relative viscosity and Mn molecular weight of the PA46 product after solid-state polymerization, and also leads to a decrease in product whiteness, thus affecting product quality.

[0101] Compared to Comparative Example 6 and Example 1, in step S3, the solid-state polymerization reaction temperature was higher than the temperature specified in this invention, which accelerated the reaction rate of solid-state polymerization. This resulted in an increase in the relative viscosity and Mn molecular weight of the PA46 product after solid-state polymerization, but a decrease in product whiteness, affecting product quality. Therefore, the reaction temperature needs to be within the range specified in this invention.

[0102] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0103] For those skilled in the art, various modifications and improvements can be made without departing from the concept of the present invention, and these modifications and improvements are all within the scope of protection of the present invention. The scope of protection of the present invention is defined by the appended claims.

Claims

1. A method for preparing high molecular weight nylon 46, characterized in that, The preparation method includes the following steps: S1. Add 1,4-butanediamine, adipic acid, antioxidant, side reaction inhibitor and deionized water to the reaction vessel and carry out the salt formation reaction under inert conditions; S2. After the salt formation reaction is completed, the temperature is raised to carry out the prepolymerization reaction. After the reaction is completed, the reaction system is depressurized and the by-products are removed to obtain the prepolymer. S3. Transfer the prepolymer to a solid-state polymerization apparatus and carry out solid-state polymerization under inert conditions to obtain Nylon 46 product; The side effect inhibitor is at least one of aliphatic tertiary amine compounds, pyridine and its derivatives, and imidazole compounds; The aliphatic tertiary amine compound is at least one selected from triethylamine, tripropylamine, tri-n-butylamine, tetramethylethylenediamine, N-methylmorpholine, and N-ethylmorpholine; The pyridine and its derivatives are at least one of pyridine, 2-methylpyridine, 3-methylpyridine, 4-methylpyridine, 2-methoxypyridine, 3-methoxypyridine, 4-dimethylaminopyridine, and isoquinoline. The imidazole compound is at least one of imidazole and 1-methylimidazolium; In step S1, the amount of side reaction inhibitor used is 0.5% to 5% of the total mass of 1,4-butanediamine and adipic acid; In step S2, the temperature is raised to 180~200℃, and the reaction time is 2~4h; In step S3, the reaction temperature is 230~260℃ and the reaction time is 4~8h.

2. The method for preparing high molecular weight nylon 46 according to claim 1, characterized in that, In step S1, the reaction temperature is 80~100℃ and the reaction time is 1~3h.

3. The method for preparing high molecular weight nylon 46 according to claim 1, characterized in that, In step S2, the system pressure is 1~2MPa.

4. The method for preparing high molecular weight nylon 46 according to claim 1, characterized in that, In step S1, the molar ratio of 1,4-butanediamine to adipic acid is (1.005~1.05):

1.

5. The method for preparing high molecular weight nylon 46 according to claim 1, characterized in that, In step S1, the amount of deionized water used is 10% to 100% of the total mass of 1,4-butanediamine and adipic acid; The antioxidant dosage is 0.1% to 1% of the total mass of 1,4-butanediamine and adipic acid.

6. The method for preparing high molecular weight nylon 46 according to claim 1, characterized in that, The antioxidant is at least one of N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexamethylenediamine, pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 3,9-bis(2,4-dicumylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosspiro[5.5]undecane, 3,9-bis[1,1-dimethyl-2-[(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, triethylene glycol ether-bis(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, and bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite.

7. A high molecular weight nylon 46, characterized in that, It is prepared by the preparation method described in any one of claims 1-6.

Citation Information

Patent Citations

  • A kind of nylon 46 and its preparation method and application

    CN119751850A

  • Preparation of polytetramethylene adipamide

    US4408036A

  • High-temperature nylon production method based on butanediamine

    CN115819755A

  • High-viscosity nylon composition

    CN119638981A