High-modulus, high-elongation-at-break polyimide films, their preparation methods and applications

By adjusting the ratio of dianhydride monomer and diamine monomer and adding inorganic nanoparticle fillers, a polyimide film with high modulus and high elongation at break was prepared. This solved the problem that it is difficult to achieve both modulus and elongation at break in traditional methods, and improved the material properties and simplified the preparation process.

CN122772215BActive Publication Date: 2026-11-17DONGYING ZHAOYUAN ELECTROMECHANICAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611272478.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-17
Estimated Expiration
2046-08-21

AI Technical Summary

Technical Problem

Existing polyimide films cannot simultaneously possess both high modulus and high elongation at break, and traditional preparation methods are complex and environmentally unfriendly.

Method used

By using a specific ratio of dianhydride monomers and diamine monomers, and adding inorganic nanoparticle fillers, and by controlling the composition of the polyamic acid solution and the process flow, a polyimide film with high modulus and high elongation at break was prepared.

Benefits of technology

The modulus of polyimide film was increased to over 2.7 GPa, the elongation at break was over 25%, and the tensile strength was 115 MPa. The preparation method is simple and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_4
    Figure SMS_4
  • Figure SMS_5
    Figure SMS_5
Patent Text Reader

Abstract

This invention provides a high-modulus, high-elongation-at-break polyimide film, its preparation method, and its applications, belonging to the field of polymer material modification technology. The polyimide film is prepared from the following raw materials: dianhydride monomer, diamine monomer, and filler. The diamine monomer includes monomer I and monomer II. Monomer I is 4,4'-diaminodiphenyl ether, and monomer II is 2,2-bis[4-(4-aminophenoxy)phenyl]propane and / or 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane. The molar ratio of dianhydride monomer to diamine monomer is 0.97-1.05:1, and the molar amount of monomer II is less than 30% of the molar amount of diamine monomer. The filler is inorganic nanoparticles, and the filler amount is 0.1-10% of the mass of the polyimide film. This invention solves the problem that high modulus and high elongation at break cannot be simultaneously achieved in polyimide films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer material modification technology, specifically to a high-modulus, high-elongation-at-break polyimide film, its preparation method, and its applications. Background Technology

[0002] Polyimide (PI) refers to aromatic heterocyclic polymers containing imide structures in their main chain repeating units. It possesses excellent mechanical properties, high-temperature resistance, dimensional stability, solvent resistance, and superior electrical properties, making it widely used in aerospace, automotive manufacturing, electronics, machinery, and chemical industries. Currently, the largest application area for polyimide films is flexible printed circuit boards (FPCs). However, perfect bonding with copper-based circuitry is required to prevent curling, misalignment, or even peeling during FPC fabrication or use. This necessitates the development of high-modulus, high-elongation-at-break polyimide films to overcome the traditional bottleneck of achieving both lightweight, thin, and flexible properties with high strength and high rigidity.

[0003] In the literature (The In-plane Orientation and Thermal Mechanical Properties of the Chemically Imidized Polyimide Films, Chinese Journal of Polymer Science, 2019, 37(3): 268-278 In this study, a chemical imidization method was used. Specifically, a certain amount of dehydrating agent and catalyst were added to a polyamic acid solution containing pyromellitic dianhydride (PMDA), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), and p-phenylenediamine (PDA) in a molar ratio of 2:1:1. Data obtained after imidization film formation showed that, particularly when the molar ratio of PMDA:acetic anhydride:isoquinoline was 1:4:1, the modulus of the chemically imidized film increased by approximately 40% and the elongation at break increased by nearly 300% compared to the thermally imidized film. However, the elongation at break was still less than 20%, indicating that further improvement in elongation at break is needed. While this method can improve both the modulus and elongation at break of the polyimide film, the chemical imidization process is complex, prone to gelation, and produces a strong odor. In addition, the thermal imidized film prepared in this article has an elastic modulus of 2-3 GPa, an elongation at break of less than 10%, and a maximum tensile strength of about 80 MPa. The elastic modulus, elongation at break, and tensile strength all need to be further improved.

[0004] The polyimide film prepared according to Chinese patent document CN 111741996 A has an elastic modulus ≤2.2GPa and a tensile strength ≤81MPa, both of which need further improvement.

[0005] Therefore, there is an urgent need to develop a simple preparation method that can simultaneously improve the film modulus and elongation at break. Summary of the Invention

[0006] In view of this, the present invention provides a polyimide film with high modulus and high elongation at break, its preparation method and application, which solves the problem that high modulus and high elongation at break of polyimide film cannot be obtained at the same time.

[0007] To achieve the above objectives, the present invention provides a high-modulus, high-elongation-at-break polyimide (PI) film, comprising the following raw materials: dianhydride monomer, diamine monomer, and filler. The diamine monomer includes monomer I and monomer II. Monomer I is 4,4'-diaminodiphenyl ether, and monomer II is 2,2-bis[4-(4-aminophenoxy)phenyl]propane and / or 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane. The molar ratio of dianhydride monomer to diamine monomer is 0.97-1.05:1. The molar amount of monomer II is less than 30% of the molar amount of diamine monomer. The filler is inorganic nanoparticles, and the filler amount is 0.1-10% of the mass of the polyimide film.

[0008] By controlling the types and ratios of dianhydride and diamine monomers, and then adding fillers, the modulus and elongation at break of the film can be simultaneously improved. The molar amount of monomer II is 30% or less of the molar amount of diamine monomer; its addition within this range can effectively improve the elongation at break while having little effect on the modulus.

[0009] Monomer I is 4,4'-diaminodiphenyl ether, and its structural formula is as follows:

[0010] .

[0011] The use of monomer I, which has a certain degree of flexibility, is beneficial to improving the modulus and elongation at break of the film.

[0012] Monomer II is 2,2-bis[4-(4-aminophenoxy)phenyl]propane and / or 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, with the following structural formula: .

[0013] Polyamic acid is prepared by using dianhydrides with rigid structures and diamines with certain flexible segments. By controlling the types, ratios, and molecular order of dianhydride and diamine monomers and then adding fillers, the modulus and elongation at break of the film are simultaneously improved. The fillers are inorganic nanoparticles, which have high rigidity and dimensional stability and exhibit good compatibility with organic phases.

[0014] Due to the organic-inorganic hybrid effect of the added filler, the modulus of the polyimide film is improved, but the elongation at break decreases slightly. Adding a more flexible monomer II can improve the elongation at break; its longer chain segments and greater flexibility can improve the modulus to some extent. For example, adding 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) or 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (6FBAPP) can both improve the elongation at break of the film and enhance its mechanical properties. This is because the long and flexible structure of BAPP makes it easier for the PI chain segments to rotate.

[0015] Furthermore, the filler content is 0.5-10% of the polyimide film mass. The upper limit of filler content is 10%. Compared with adding 10% filler, adding more than 10% filler does not significantly affect the mechanical properties. However, when the filler content exceeds 10%, the material becomes more brittle, which in turn affects the mechanical properties.

[0016] Furthermore, the molar amount of monomer II is 5-30% of the molar amount of diamine monomer. Using less than 5% of monomer II has a relatively small effect on improving the elongation at break.

[0017] Furthermore, the molar ratio of dianhydride monomer to diamine monomer is 1.02:1. Because dianhydride monomer is easily hydrolyzed by air or moisture in the solvent, losing its activity and thus affecting the relative molecular mass of polyamic acid, the addition of dianhydride monomer needs to be slightly excessive in order to prepare a high molecular weight polyamic acid solution.

[0018] Furthermore, the dianhydride monomer is one or both of 1,2,4,5-pyromellitic dianhydride and 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, with the following structural formula: ; The filler is one or more of silicon dioxide, aluminum oxide, and boron nitride. Preferably, the filler is silicon dioxide with a particle size between 10-20 nm.

[0019] Furthermore, the polyimide film has an elastic modulus ≥2.7 GPa and an elongation at break ≥25%.

[0020] Furthermore, the polyimide film has an elastic modulus of 2.9-3.5 GPa and an elongation at break of 25-42%.

[0021] A method for preparing a high-modulus, high-elongation-at-break polyimide film includes the following steps: (1) In a polar organic solvent, a polyamic acid composition is prepared by mixing dianhydride monomer, diamine monomer and filler; (2) The polyamic acid composition is coated into a film and heated to imidize to obtain a polyimide film.

[0022] This method is simple to prepare, easy to operate, and easy to further process and promote.

[0023] The reaction equation for the dianhydride monomer and the diamine monomer is as follows:

[0024] Further, in step (1), the polar organic solvent is one or more of N,N'-dimethylformamide, N,N'-dimethylacetamide, N-methylpyrrolidone, m-cresol and dimethyl sulfoxide.

[0025] Further, in step (2), the heating imidization method is as follows: maintain at each temperature of 80-90℃, 95-105℃, 140-160℃, 190-220℃, 240-260℃, and 280-310℃ for 0.5-1.5h, and then maintain at 340-360℃ for 0.5-1h.

[0026] Further, in step (1), at room temperature, the diamine monomer is dispersed in a polar organic solvent, and then at 35-50°C, the dianhydride monomer is added and reacted for 1 hour. Then, the temperature is raised to 60-80°C and stirred for 6 hours to obtain a polyamic acid solution. Filler is added to the solution and mixed evenly to obtain a polyamic acid composition. Alternatively, at room temperature, the diamine monomer and filler are dispersed together in a polar organic solvent, and then the dianhydride monomer is added at 35-50°C and reacted for 1 hour. The temperature is then raised to 60-80°C and stirred for 6 hours to obtain the polyamic acid composition.

[0027] The reaction that forms polyamic acid is an exothermic reaction. Low temperature helps the reaction to proceed, resulting in polyamic acid with higher viscosity, i.e., higher molecular weight.

[0028] Furthermore, the mixing time of the filler is 1-10 hours. Preferably, the mixing time is 4-6 hours, and the mixing temperature is room temperature.

[0029] Furthermore, in step (1), the solid content of the polyamic acid solution is between 8-25%. Too low a solid content will result in a low viscosity of the prepared polyamic acid solution; too high a solid content will result in a rapid increase in the viscosity of the system, and may also lead to the formation of gel, making it difficult to process.

[0030] Furthermore, the coating method involves coating the film onto a support, which only needs to be clean, smooth, and have a certain degree of rigidity, such as a glass plate, plastic plate, or metal plate. Preferably, a clean and dry glass plate is selected as the support.

[0031] High-modulus, high-elongation-at-break polyimide films can be used in FCCL (flexible copper clad laminate) or flexible display devices.

[0032] The above-described technical solution of the present invention has at least the following beneficial effects: In this invention, polyamic acid is prepared using dianhydride with a certain rigid structure and monomer I with a certain flexible structure. By adding monomer II with a longer flexible chain segment and filler, the material can be made to have both rigidity and flexibility, and a polyimide film with both low and high modulus and high elongation at break can be obtained.

[0033] The polyimide film of the present invention has an elastic modulus of ≥2.7GPa, while also improving its elongation at break, such as reaching ≥25%, and a tensile strength of ≥115MPa.

[0034] The polyimide film preparation method of the present invention is simple, uses inexpensive raw materials, is easy to operate, and is easy to further process and promote. Detailed Implementation

[0035] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the described embodiments of the present invention are within the scope of protection of the present invention.

[0036] All raw materials used in the following specific implementation methods were purchased from the market.

[0037] Example 1 A method for preparing a polyimide film includes the following steps: Step (1): Under nitrogen protection, in a 100 mL three-necked flask equipped with a mechanical stirrer, 3.6043 g (0.018 mol) of 4,4'-diaminodiphenyl ether (ODA) and 0.821 g (0.002 mol) of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) were added to 29.8893 g of organic solvent N,N-dimethylacetamide (DMAc) and stirred at room temperature until dissolved. When ODA and BAPP were completely dissolved, the temperature was raised to 40 °C and 1.3305 g (0.0061 mol) of 1,2,4,5-pyromellitic dianhydride (PMDA) and 4.2073 g (0.0143 mol) of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride were added with stirring. After reacting for 1 hour, the temperature was raised to 60 °C. The solution was stirred at 60°C for 6 hours, and a viscous polyamic acid solution with a solid content of 25% was finally obtained, with an intrinsic viscosity of 0.64 dL / g.

[0038] Step (2): Add 0.9963g (3% of the mass of the polyimide film) of silica dispersion (commercially available, 30% solid content) to the polyimide acid reaction solution in step (1), and mechanically stir at room temperature for 4 hours to obtain a uniformly mixed polyamic acid composition.

[0039] Step (3): Immediately take 5 g of the polyamic acid composition from step (2) and pour it evenly onto a clean and dry glass plate (25cm × 15cm), then place it in a regular oven. The heating program is as follows: maintain at 80℃, 100℃, 150℃, 200℃, 250℃, and 300℃ for 1 hour each, and at 350℃ for 0.5 hours. Immerse the glass plate with the polyimide film in hot water, peel off the individual polyimide films from the glass plate, and then dry the moisture in an oven at 100℃ to obtain the final polyimide film.

[0040] Example 2 A method for preparing a polyimide film includes the following steps: Step (1): Under nitrogen protection, in a 100 mL three-necked flask equipped with a mechanical stirrer, 3.2038 g (0.016 mol) of 4,4'-diaminodiphenyl ether (ODA) and 1.642 g (0.004 mol) of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) were added to 31.1508 g of organic solvent N,N-dimethylacetamide (DMAc) and stirred at room temperature until dissolved. When ODA and BAPP were completely dissolved, the temperature was raised to 40 °C and 1.3305 g (0.0061 mol) of 1,2,4,5-pyromellitic dianhydride (PMDA) and 4.2073 g (0.0143 mol) of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride were added with stirring. After reacting for 1 hour, the temperature was raised to 60 °C. The solution was stirred at 60°C for 6 hours, and a viscous polyamic acid solution with a solid content of 25% was finally obtained, with an intrinsic viscosity of 0.61 dL / g.

[0041] Step (2): Add 1.0384 g (3% of the mass of the polyimide film) of silica dispersion (commercially available, 30% solid content) to the polyimide acid reaction solution in step (1), and mechanically stir at room temperature for 4 h to obtain a uniformly mixed polyamic acid composition.

[0042] Step (3): Immediately take 5 g of the polyamic acid composition from step (2) and pour it evenly onto a clean and dry glass plate (25cm × 15cm), then place it in a regular oven. The heating program is as follows: maintain at 80℃, 100℃, 150℃, 200℃, 250℃, and 300℃ for 1 hour each, and at 350℃ for 0.5 hours. Immerse the glass plate with the polyimide film in hot water, peel off the individual polyimide films from the glass plate, and then dry the moisture in an oven at 100℃ to obtain the final polyimide film.

[0043] Example 3 A method for preparing a polyimide film includes the following steps: Step (1): Under nitrogen protection, in a 100 mL three-necked flask equipped with a mechanical stirrer, 2.8034 g (0.014 mol) of 4,4'-diaminodiphenyl ether (ODA) and 2.463 g (0.006 mol) of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) were added to 32.3361 g of organic solvent N,N-dimethylacetamide (DMAc) and stirred at room temperature until dissolved. When ODA and BAPP were completely dissolved, the temperature was raised to 40 °C and 1.3305 g (0.0061 mol) of 1,2,4,5-pyromellitic dianhydride (PMDA) and 4.2073 g (0.0143 mol) of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride were added with stirring. After reacting for 1 hour, the temperature was raised to 60 °C. The solution was stirred at 60°C for 6 hours, and a viscous polyamic acid solution with a solid content of 25% was finally obtained, with an intrinsic viscosity of 0.59 dL / g.

[0044] Step (2): Add 1.0779 g (3% of the mass of the polyimide film) of silica dispersion (commercially available, 30% solid content) to the polyimide acid reaction solution in step (1), and mechanically stir at room temperature for 4 h to obtain a uniformly mixed polyamic acid composition.

[0045] Step (3): Immediately take 5 g of the polyamic acid composition from step (2) and pour it evenly onto a clean and dry glass plate (25 cm × 15 cm). Place it in a regular oven and heat it according to the following program: 80℃, 100℃, 150℃, 200℃, 250℃, and 300℃ for 1 h each, and 350℃ for 0.5 h. Immerse the glass plate with the polyimide film in hot water, peel off the individual polyimide film from the glass plate, and then dry it in an oven at 100℃ to obtain the final polyimide film.

[0046] Example 4 A method for preparing a polyimide film includes the following steps: Step (1): Prepare a polyamic acid solution according to the method in step (1) of Example 2.

[0047] Step (2): Add 1.7305 g (5% of the mass of the polyimide film) of silica dispersion (commercially available, 30% solid content) to the polyimide acid reaction solution in step (1), and mechanically stir at room temperature for 4 hours to obtain a uniformly mixed polyamic acid composition.

[0048] Step (3): Prepare a polyimide (PI) film according to the method in step (3) of Example 2.

[0049] Example 5 A method for preparing a polyimide film includes the following steps: Step (1): Prepare a polyamic acid solution according to the method in step (1) of Example 2.

[0050] Step (2): Add 3.4612 g (10% of the mass of the polyimide film) of silica dispersion (commercially available, 30% solid content) to the polyimide acid reaction solution in step (1), and mechanically stir at room temperature for 4 hours to obtain a uniformly mixed polyamic acid composition.

[0051] Step (3): Prepare a PI film according to the method in step (3) of Example 2.

[0052] Example 6 A method for preparing a polyimide film includes the following steps: Step (1): Under nitrogen protection, in a 100 mL three-necked flask equipped with a mechanical stirrer, 1.0384 g (3% of the mass of the polyimide film) of silica dispersion (commercially available, 30% solid content), 3.2038 g (0.016 mol) of 4,4'-diaminodiphenyl ether (ODA) and 1.642 g (0.004 mol) of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) were added to 31.1508 g of organic solvent N,N-dimethylacetamide (DMAc) and stirred at room temperature to dissolve. When ODA and BAPP were completely dissolved, 1.3305 g (0.0061 mol) of 1,2,4,5-pyromellitic dianhydride (PMDA) and 4.2073 g (0.0143 mol) of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride were added while stirring at 40°C. After reacting for 1 hour, the temperature was raised to 60°C. The solution was stirred at 60°C for 6 hours, finally yielding a polyamic acid composition with a solid content of 25% and an intrinsic viscosity of 0.68 dL / g.

[0053] Step (2): Immediately take 5 g of the polyamic acid composition from step (1) and pour it evenly onto a clean and dry glass plate (25 cm × 15 cm), then place it in a regular oven. The heating program is as follows: maintain at 80℃, 100℃, 150℃, 200℃, 250℃, and 300℃ for 1 h, and at 350℃ for 0.5 h. Immerse the glass plate with the polyimide film in hot water, peel off the individual polyimide films from the glass plate, and then dry them in an oven at 100℃ to obtain the final polyimide film.

[0054] Example 7 A method for preparing a polyimide film includes the following steps: Step (1): Under nitrogen protection, in a 100 mL three-necked flask equipped with a mechanical stirrer, 3.4612 g (10% of the mass of the polyimide film) of silica dispersion (commercially available, solid content 30%), 2.8034 g (0.014 mol) of 4,4'-diaminodiphenyl ether (ODA) and 2.463 g (0.006 mol) of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) were added to 32.3361 g of organic solvent N,N-dimethylacetamide (DMAc) and stirred at room temperature to dissolve. When ODA and BAPP were completely dissolved, the temperature was raised to 40°C, and 1.3305 g (0.0061 mol) of pyromellitic dianhydride (PMDA) and 4.2073 g (0.0143 mol) of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride were added with stirring. After reacting for 1 hour, the temperature was raised to 60°C. The solution was stirred at 60°C for 6 hours, finally yielding a polyamic acid composition with a solid content of 25% and an intrinsic viscosity of 0.60 dL / g.

[0055] Step (2): Immediately take 5 g of the polyamic acid composition from step (1) and pour it evenly onto a clean and dry glass plate (25cm × 15cm), then place it in a regular oven. The heating program is as follows: maintain at 80℃, 100℃, 150℃, 200℃, 250℃, and 300℃ for 1 hour each, and at 350℃ for 0.5 hours. Immerse the glass plate with the polyimide film in hot water, peel off the individual polyimide films from the glass plate, and then dry the moisture in an oven at 100℃ to obtain the final polyimide film.

[0056] Example 8 This embodiment is basically the same as Example 1, except that in step (1), under nitrogen protection, 2.8034 g (0.014 mol) of 4,4'-diaminodiphenyl ether (ODA), 1.2315 g (0.003 mol) of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), and 1.5553 g (0.003 mol) of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP) were added to a 100 mL three-necked flask containing a mechanical stirrer. Dissolve ODA, HFBAPP, and BAPP in the organic solvent N,N-dimethylacetamide (DMAc) at room temperature with stirring. When ODA, HFBAPP, and BAPP are completely dissolved, heat to 40°C and add 1,2,4,5-pyromellitic dianhydride (PMDA) and 3,3',4,4'-biphenyltetracarboxylic acid dianhydride while stirring. After reacting for 1 hour, heat to 60°C and stir for 6 hours.

[0057] Step (2): Add 1.1128 g (3% of the mass of the polyimide film) of silica dispersion (commercially available, 30% solid content) to step (1). In step (3), the heating imidization process is as follows: maintain at 80℃, 100℃, 160℃, 210℃, 260℃, and 310℃ for 1 hour, and then maintain at 360℃ for 1 hour.

[0058] Example 9 This embodiment is basically the same as Example 1, except that: in step (1), under nitrogen protection, 3.8046 g (0.019 mol) of 4,4'-diaminodiphenyl ether (ODA) and 0.5185 g (0.001 mol) of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP) were added to 29.5827 g of organic solvent N,N-dimethylacetamide (DMAc) and stirred at room temperature to dissolve. When ODA and HFBAPP were completely dissolved, the temperature was raised to 40°C and 1,2,4,5-pyromellitic dianhydride (PMDA) and 3,3',4,4'-biphenyltetracarboxylic acid dianhydride were added under stirring. After reacting for 1 hour, the temperature was raised to 70°C and stirred for 6 hours.

[0059] In step (2), 0.1644g of silica dispersion (commercially available, 30% solid content) is added to step (1), and the amount of silica added is 0.5% of the mass of the polyimide film; In step (3), the heating imidization process is as follows: maintain at 80℃, 100℃, 160℃, 210℃, 260℃, and 310℃ for 1.5h, and then maintain at 360℃ for 0.5h.

[0060] Comparative Example 1 A method for preparing a polyimide film includes the following steps: Step (1): Under nitrogen protection, in a 100 mL three-necked flask equipped with a mechanical stirrer, 2.4029 g (0.012 mol) of 4,4'-diaminodiphenyl ether (ODA) and 3.284 g (0.008 mol) of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) were added to 33.6742 g of organic solvent N,N-dimethylacetamide (DMAc) and stirred at room temperature until dissolved. When ODA and BAPP were completely dissolved, the temperature was raised to 40 °C and 1.3305 g (0.0061 mol) of 1,2,4,5-pyromellitic dianhydride (PMDA) and 4.2073 g (0.0143 mol) of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride were added with stirring. After reacting for 1 hour, the temperature was raised to 60 °C. The solution was stirred at 60°C for 6 hours, resulting in a viscous polyamic acid solution with a solid content of 25%. Its intrinsic viscosity was 0.55 dL / g.

[0061] Step (2): Add 1.1225g (3% of the mass of the polyimide film) of silica dispersion (commercially available, 30% solid content) to the polyimide acid reaction solution in step (1), and mechanically stir at room temperature for 4 hours to obtain a uniformly mixed polyamic acid composition.

[0062] Step (3): Immediately take 5 g of the polyamic acid composition from step (2) and pour it evenly onto a clean and dry glass plate (25cm × 15cm), then place it in a regular oven. The heating program is as follows: maintain at 80℃, 100℃, 150℃, 200℃, 250℃, and 300℃ for 1 hour each, and at 350℃ for 0.5 hours. Immerse the glass plate with the polyimide film in hot water, peel off the individual polyimide films from the glass plate, and then dry the moisture in an oven at 100℃ to obtain the final polyimide film.

[0063] Comparative Example 2 A method for preparing a polyimide film includes the following steps: Step (1): Under nitrogen protection, in a 100 mL three-necked flask equipped with a mechanical stirrer, 4.0048 g (0.02 mol) of 4,4'-diaminodiphenyl ether (ODA) was added to 28.6278 g of organic solvent N,N-dimethylacetamide (DMAc) and stirred at room temperature until dissolved. When the ODA was completely dissolved, the temperature was raised to 40°C, and 1.3305 g (0.0061 mol) of 1,2,4,5-pyromellitic dianhydride (PMDA) and 4.2073 g (0.0143 mol) of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride were added with stirring. After reacting for 1 hour, the temperature was raised to 60°C. The solution was stirred at 60°C for 6 hours, finally yielding a viscous polyamic acid solution with a solid content of 25%. Its intrinsic viscosity was 0.59 dL / g.

[0064] Step (2): Add 0.9543 g (3% of the mass of the polyimide film) of silica dispersion (commercially available, 30% solid content) to the polyimide acid reaction solution in step (1), and mechanically stir at room temperature for 4 hours to obtain a uniformly mixed polyamic acid composition.

[0065] Step (3): Immediately take 5 g of the polyamic acid composition from step (2) and pour it evenly onto a clean and dry glass plate (25 cm × 15 cm), then place it in a regular oven. The heating program is as follows: maintain at 80℃, 100℃, 150℃, 200℃, 250℃, and 300℃ for 1 h, and at 350℃ for 0.5 h. Immerse the glass plate with the polyimide film in hot water, peel off the individual polyimide films from the glass plate, and then dry the moisture in an oven at 100℃ to obtain the final polyimide film.

[0066] Comparative Example 3 A method for preparing a polyimide film includes the following steps: Step (1): Prepare a polyamic acid solution according to the method in step (1) of Example 2.

[0067] Step (2): Prepare a PI film according to the method in step (3) of Example 2.

[0068] Comparative Example 4 A method for preparing a polyimide film includes the following steps: Step (1): Prepare a polyamic acid solution according to the method in step (1) of Example 2.

[0069] Step (2): Add 5.1918 g (15% of the mass of the polyimide film) of silica dispersion (commercially available, 30% solid content) to the polyimide acid reaction solution in step (1), and mechanically stir at room temperature for 4 h to obtain a uniformly mixed polyamic acid composition.

[0070] Step (3): Prepare a PI film according to the method in step (3) of Example 2.

[0071] Comparative Example 5 A method for preparing a polyimide film includes the following steps: Step (1): Prepare a polyamic acid solution according to the method in step (1) of Example 2.

[0072] Step (2): Add 6.9224 g (20% of the mass of the polyimide film) of silica dispersion (commercially available, 30% solid content) to the polyimide acid reaction solution in step (1), and mechanically stir at room temperature for 4 hours to obtain a uniformly mixed polyamic acid composition.

[0073] Step (3): Prepare a PI film according to the method in step (3) of Example 2.

[0074] Thin film performance testing According to the testing standard ASTM D882, the elastic modulus (GPa), tensile strength (MPa), and elongation at break (%) of the films of Examples 1-7 and Comparative Examples 1-5 were tested using an Instron Model 5567 universal testing machine. The measurement mode was tensile, the test was conducted at room temperature, and the speed was controlled at 5 mm / min. The test sample films were 120 mm long, 10 mm wide, and 20-30 μm thick, and the average value of 3-5 parallel tests was taken.

[0075] The performance data of the polyimide films in the examples and comparative examples are shown in Table 1. Comparison of the data from Examples 1-3 and Comparative Examples 1 and 2 reveals that, with the same amount of silica added, the elongation at break increases with increasing BAPP content. When the BAPP content is 40%, the material modulus is <2.7 GPa (Comparative Example 1) due to increased molecular chain flexibility and weakened intermolecular forces in the PI matrix. Further increases may not achieve better overall performance. Within a certain range, the monomer II content can make the chain segments less prone to breakage, thus improving the elongation at break.

[0076] By comparing the data from Examples 2, 4, and 5 and Comparative Examples 3, 4, and 5, it was found that when the type and proportion of anhydride amine were fixed, adding more than 10% silica content resulted in an increase in modulus, but a decrease in elongation at break. Based on these results, it can be concluded that adding a small amount of silica to the polyamic acid solution is helpful in preparing polyimide films with excellent mechanical properties.

[0077] As seen in Examples 2 and 6, adding dianhydride and diamine before mixing them uniformly, followed by the addition of silica, improves the mechanical properties of the material to some extent, compared to adding them together to form a polyamic acid solution. This is because the process sequence significantly affects the microstructure of the composite film: film samples with SiO2 added after PAA (polyamic acid) polymerization exhibit uneven size and distribution; film samples prepared by uniformly dispersing SiO2 in a solvent before PAA polymerization better retain the porous structure of silica and are uniformly distributed within the PI matrix, resulting in better filler dispersion and no aggregation. SiO2 can also form hydrogen bonds with PAA chains, and this microstructure lays the foundation for good mechanical properties.

[0078] Table 1. Performance of PI films in examples and comparative examples.

Claims

1. A polyimide film with high modulus and high elongation at break, characterized in that: The preparation process includes the following raw materials: dianhydride monomer, diamine monomer, and filler. The diamine monomer includes monomer I and monomer II. Monomer I is 4,4'-diaminodiphenyl ether, and monomer II is 2,2-bis[4-(4-aminophenoxy)phenyl]propane and / or 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane. The molar ratio of dianhydride monomer to diamine monomer is 0.97-1.05:1, and the molar amount of monomer II is less than 30% of the molar amount of diamine monomer. The filler is inorganic nanoparticles, and the filler amount is 0.1-10% of the mass of the polyimide film. The dianhydride monomers are 1,2,4,5-pyromellitic dianhydride and 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, with a molar ratio of 1,2,4,5-pyromellitic dianhydride to 3,3',4,4'-biphenyltetracarboxylic acid dianhydride of 61:

143. Inorganic nanoparticles are made of silicon dioxide and have a particle size between 10 and 20 nm. The polyimide film has an elastic modulus ≥2.7 GPa and an elongation at break ≥25%; The method for preparing the polyimide film includes the following steps: (1) In a polar organic solvent, a polyamic acid composition is prepared by mixing a diamine monomer, a dianhydride monomer, and a filler; (2) The polyamic acid composition is coated into a film, and then heated to imidize to obtain a polyimide film; In step (2), the heating imidization method includes: holding at each temperature of 80-90℃, 95-105℃, 140-160℃, 190-220℃, 240-260℃, and 280-310℃ for 0.5-1.5h, and then holding at 340-360℃ for 0.5-1h; In step (1), at room temperature, the diamine monomer is dispersed in a polar organic solvent, and then at 35-50°C, the dianhydride monomer is added and reacted for 1 hour. The temperature is then raised to 60-80°C and stirred for 6 hours to obtain a polyamic acid solution. Filler is added to the solution and mixed evenly to obtain a polyamic acid composition. Alternatively, at room temperature, the diamine monomer and filler are dispersed together in a polar organic solvent, and then the dianhydride monomer is added at 35-50°C and reacted for 1 hour. The temperature is then raised to 60-80°C and stirred for 6 hours to obtain the polyamic acid composition.

2. The polyimide film according to claim 1, characterized in that: The filler dosage is 0.5-10% of the mass of the polyimide film.

3. The polyimide film according to claim 1, characterized in that, In step (1), the polar organic solvent is one or more of N,N'-dimethylformamide, N,N'-dimethylacetamide, N-methylpyrrolidone, m-cresol and dimethyl sulfoxide.

4. The polyimide film according to any one of claims 1-3 is used in FCCL or flexible display devices.

Citation Information

Patent Citations

  • Polyimide resin, polyimide varnish and polyimide film

    CN111741996A

  • Polyimide film and preparation method thereof

    CN112851982A

  • Polyimide film

    JP2008007631A