A primer for photocurable diamond Martian coating and its preparation method

By combining functional polyurethane acrylates and epoxy acrylates with multifunctional acrylate monomers, the storage stability and adhesion problems of the primer for UV-cured diamond Mars coatings were solved, achieving a balance between high hardness and wear resistance on wood substrates.

CN122772485BActive Publication Date: 2026-11-17HUARONG COUNTY HENGXING BUILDING MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611231782.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17
Estimated Expiration
2046-08-14

AI Technical Summary

Technical Problem

Existing UV-cured diamond Mars coating primers suffer from poor storage stability and adhesion deviations, making it difficult to achieve a balance between high hardness and wear resistance on wood substrates.

Method used

Functional polyurethane acrylate is used as the main film-forming resin, combined with epoxy acrylate and multifunctional acrylate monomers. The sulfonic acid groups generate strong polar interactions with the surface of the superhard wear-resistant powder. Organosiloxane segments are used to prevent powder sedimentation, and polyether segments provide flexibility and stress release capabilities, thereby achieving comprehensive performance optimization of the coating.

Benefits of technology

It improves the storage stability and adhesion of the primer, while also possessing excellent abrasion resistance and toughness, ensuring high hardness and good adhesion of the coating on wood substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122772485B_ABST
    Figure CN122772485B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of polymer composite materials technology, specifically a primer for photocurable diamond Mars coating and its preparation method. The primer for photocurable diamond Mars coating provided by this invention uses a functional polyurethane acrylate as the main film-forming resin, with bis(trimethylol)propane-isophorone diisocyanate as the crosslinking core and containing sulfonic acid groups, organosiloxane side chains, and polyether side chains in its molecular structure. The sulfonic acid groups can generate strong polar interactions with the surface of ultra-hard wear-resistant powder, enhancing filler anchoring; the organosiloxane segments, due to their low surface energy and excellent wettability, can preferentially migrate to the inorganic powder interface to form a dense coating layer, effectively preventing powder agglomeration and sedimentation, and effectively improving storage stability; the polyether segments provide flexibility and stress release capabilities, giving the coating good wear resistance and toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer composite materials technology, specifically a primer for photocurable diamond Mars coating and its preparation method. Background Technology

[0002] With the increasing demands for both the decorative and durable properties of wood-based panels from modern home decoration, high-end wood product processing, and commercial space renovation industries, traditional coating systems are struggling to meet the performance requirements of high-frequency use and high-wear environments. In the field of wood-based panel surface coating technology, hardness and abrasion resistance remain core indicators for evaluating coating performance. While UV curing technology has brought about rapid drying and environmental benefits, existing UV coatings still face bottlenecks such as increased brittleness due to high cross-linking and insufficient adhesion of highly abrasion-resistant fillers to wood substrates.

[0003] Against this technological backdrop, the industry has proposed the concept of "Diamond Spark Coating." This coating uses diamond micropowder as the core wear-resistant reinforcing phase, producing a spark (spark) phenomenon during high-speed polishing, which is a direct representation of its ultra-high hardness and wear resistance. However, the primer plays a crucial role in the successful application of Diamond Spark Coating to wood-based panels. The primer needs to connect the loose and porous wood substrate (such as solid wood, plywood, and high-density fiberboard, HDF) with the extremely hard topcoat, providing interfacial adhesion and stress transition. To match the high hardness of the topcoat and achieve a gradient transition in coating hardness, the primer also needs to incorporate ultra-hard powders such as diamond and silicon carbide. However, these powders have a much higher density than conventional resins, and are prone to gravity settling in low-viscosity UV primers, resulting in hard sedimentation (dead settling) at the bottom within a short time, affecting construction and coating quality.

[0004] Furthermore, the porous and loose surface of wood-based substrates contains polar functional groups, resulting in poor compatibility with highly cross-linked resins. To stabilize the powder and improve adhesion, existing technologies often introduce epoxy acrylates or conventional polyurethanes. However, if only epoxy acrylates are used, the cured product becomes extremely brittle and cannot release the internal stress caused by the high load of inorganic powders, making it prone to cracking and peeling when the wood is subjected to impact or deformation. If only conventional flexible polyurethanes are used, although stress can be relieved, the coating has low cohesive strength and cannot provide a solid supporting substrate for the topcoat. Summary of the Invention

[0005] To address the above problems, this invention provides a primer for photocurable diamond Mars coating and its preparation method, which solves the problems of poor storage stability and adhesion deviation in current photocurable diamond Mars coating primers.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A primer for a light-cured diamond Martian coating comprises the following components in parts by weight: 30-40 parts of functional polyurethane acrylate, 9-12 parts of epoxy acrylate, 25-36 parts of multifunctional acrylate monomers, 18-25 parts of superhard abrasion-resistant powder, and 4-5 parts of photoinitiator; wherein the superhard abrasion-resistant powder is composed of diamond particles, zirconium oxide particles, and silicon carbide particles; and the multifunctional acrylate monomers are composed of trifunctional and difunctional acrylate monomers; the total mass of the multifunctional acrylate monomers is used as the basis. The trifunctional acrylate monomer accounts for 30%~40%, and the difunctional acrylate monomer accounts for 60%~71%; the trifunctional acrylate monomer is composed of pentaerythritol ethoxylated triacrylate and trimethylolpropane propoxylated triacrylate in a mass ratio of (3~9):(1~5); the difunctional acrylate monomer is composed of tripropylene glycol diacrylate and ethoxylated bisphenol A diacrylate in a mass ratio of (5~7):(2~4); the chemical structure of the functional polyurethane acrylate is as follows: .

[0007] Preferably, the pentaerythritol ethoxylated triacrylate is pentaerythritol ethoxy(5) triacrylate.

[0008] Preferably, the ethoxylated bisphenol A diacrylate is 10(ethoxy)bisphenol A diacrylate.

[0009] In this invention, pentaerythritol ethoxy(5) triacrylate is pentaerythritol ethoxylated triacrylate with an average ethoxy addition number of 5, and 10(ethoxy)bisphenol A diacrylate is ethoxylated bisphenol A diacrylate with an average ethoxy addition number of 10.

[0010] Preferably, the mass ratio of the diamond particles, zirconium oxide particles and silicon carbide particles is (3~5):(4~9):(10~12).

[0011] Preferably, the average particle sizes of the diamond particles, zirconium oxide particles, and silicon carbide particles are 10~20μm, 20~40μm, and 20~40μm, respectively.

[0012] Preferably, the functional polyurethane acrylate is prepared by a method comprising the following steps: (1) After reacting 3-hydroxypropanesulfonic acid with phosphorus oxychloride, it is then reacted with hydroxyethyl methacrylate to obtain phosphoryl chloride intermediate of methacrylate; the molar ratio of 3-hydroxypropanesulfonic acid, phosphorus oxychloride and hydroxyethyl methacrylate is 1:1:1; (2) The methacrylate phosphoryl chloride intermediate with a molar ratio of 1:1 was reacted with 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane to obtain a siloxane monohydroxy intermediate; the methacrylate phosphoryl chloride intermediate with a molar ratio of 1:1 was reacted with tetraethylene glycol triethylene glycol to obtain a polyether monohydroxy intermediate. (3) Reaction of isophorone diisocyanate with bis(trimethylolpropane) to obtain a terminal isocyanate compound; then reaction of the terminal isocyanate compound with the siloxane monohydroxy intermediate and the polyether monohydroxy intermediate to obtain a functional polyurethane acrylate; the molar ratio of isophorone diisocyanate, bis(trimethylolpropane), siloxane monohydroxy intermediate and polyether monohydroxy intermediate is 1.2:0.3:0.6:0.65.

[0013] Preferably, the epoxy acrylate is a bisphenol A type epoxy acrylate.

[0014] Preferably, the photoinitiator is composed of 1-hydroxycyclohexylphenyl ketone and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a mass ratio of 2:1 to 1.5.

[0015] A method for preparing a primer for a photocurable diamond Mars coating as described above includes the following steps: mixing functional polyurethane acrylate, epoxy acrylate, multifunctional acrylate monomer, superhard wear-resistant powder and photoinitiator to obtain a primer for a photocurable diamond Mars coating.

[0016] Compared to existing technologies, the beneficial effects of the photocurable diamond Martian coating primer of the present invention are as follows: 1) The photocurable diamond Mars coating primer provided by this invention uses a functional polyurethane acrylate as the main film-forming resin, with bis(trimethylol)propane-isophorone diisocyanate as the crosslinking core and containing sulfonic acid groups, organosiloxane side chains, and polyether side chains in its molecular structure. The sulfonic acid groups can generate strong polar interactions with the surface of the superhard wear-resistant powder, enhancing filler anchoring; the organosiloxane segments, due to their low surface energy and excellent wettability, can preferentially migrate to the inorganic powder interface to form a dense coating layer, effectively preventing powder agglomeration and sedimentation, and effectively improving storage stability; the polyether segments provide flexibility and stress release capabilities, giving the coating good wear resistance and toughness.

[0017] (2) This invention optimizes the overall performance of the primer by compounding functional polyurethane acrylate with epoxy acrylate. Epoxy acrylate contains benzene ring structure and polar groups, which endow the coating with high hardness, high cohesive strength and polar adhesion to wood substrates, while its dense cross-linked network can effectively resist solvent penetration; functional polyurethane acrylate provides powder dispersion stability and coating flexibility. The synergistic effect of the two makes the primer have excellent storage stability, adhesion and abrasion resistance.

[0018] (3) The multifunctional acrylate monomers in this invention are obtained by compounding trifunctional and difunctional monomers. They serve as reactive diluents to adjust the viscosity of the system to facilitate construction, and as key regulators of the crosslinking network. The trifunctional monomer (a compound of pentaerythritol ethoxytriacrylate and trimethylolpropane propoxytriacrylate) provides high reactivity and crosslinking points; the difunctional monomer (a compound of tripropylene glycol diacrylate and a monomer containing bisphenol A structure) provides low viscosity to wet the powder, and imparts excellent cohesive strength and solvent resistance to the coating through the rigid structure of bisphenol A, effectively balancing the curing speed, volume shrinkage and mechanical properties of the coating film. Attached Figure Description

[0019] Figure 1 The above is the 1H NMR spectrum of the methacrylate phosphoryl chloride intermediate prepared in Example 1 of this invention; Figure 2 The above is the 1H NMR spectrum of the siloxane monohydroxy intermediate prepared in Example 1 of this invention; Figure 3 The above is the 1H NMR spectrum of the polyether monohydroxy intermediate prepared in Example 1 of this invention; Figure 4 The image shows the 1H NMR spectrum of the functional polyurethane acrylate prepared in Example 1. Detailed Implementation

[0020] To enable those skilled in the art to better understand the technical solution, the present invention will be described in detail below with reference to embodiments. The description in this part is only exemplary and explanatory, and should not be used to limit the scope of protection of the present invention in any way. Example

[0021] The primer for the photocurable diamond Mars coating of this embodiment is composed of the following components in parts by weight: 30 parts functional polyurethane acrylate, 9 parts epoxy acrylate, 8 parts trifunctional acrylate monomer, 17 parts difunctional acrylate monomer, 18 parts superhard wear-resistant powder, and 4 parts photoinitiator; the trifunctional acrylate monomer is composed of pentaerythritol ethoxy (5) triacrylate and trimethylolpropane propoxy (3) triacrylate in a mass ratio of 3:1; the difunctional acrylate monomer is composed of pentaerythritol ethoxy (5) triacrylate and trimethylolpropane propoxy (3) triacrylate in a mass ratio of 5:2. The product is composed of propylene glycol diacrylate and 10(ethoxy)bisphenol A diacrylate; the superhard wear-resistant powder consists of diamond particles, zirconium oxide particles, and silicon carbide particles in a mass ratio of 3:5:10, with average particle sizes of 10 μm, 20 μm, and 20 μm for the diamond particles, zirconium oxide particles, and silicon carbide particles, respectively; the photoinitiator is a mixture of 1-hydroxycyclohexylphenyl ketone and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a mass ratio of 2:1; the epoxy acrylate is EBECRYL600. The preparation method of the functional polyurethane acrylate is as follows: (1) Under nitrogen protection, add 1.2 mol of phosphorus oxychloride and 600 mL of dichloromethane to a dry reaction flask equipped with a mechanical stirrer, thermometer and constant pressure dropping funnel. Turn on the stirrer and cool down to 0℃. Dissolve 1.0 mol of 3-hydroxypropanesulfonic acid in 300 mL of anhydrous tetrahydrofuran and add it dropwise to the reaction flask. Control the dropping rate so that the temperature of the reaction solution does not exceed 5℃. After the addition is complete, continue stirring the reaction at 0℃ for 3 h. After the reaction is complete, remove the solvent and unreacted phosphorus oxychloride under reduced pressure at 45℃ to obtain the intermediate 3-sulfonic acid propyl phosphate diacyl chloride. The intermediate 3-sulfonyl propyl phosphate diacyl chloride, 400 mL of anhydrous dichloromethane, and 100 mL of anhydrous tetrahydrofuran were added to a reaction flask. After stirring until homogeneous, the mixture was cooled to 0°C. 1.0 mol of hydroxyethyl methacrylate and 2.2 mol of the acid-binding agent triethylamine were dissolved in 180 mL of anhydrous dichloromethane and then added dropwise to the reaction solution. The dropping rate was controlled, and the reaction temperature was maintained between 0 and 5°C. After the addition was complete, the mixture was stirred at 0°C for 6 hours. After the reaction was completed, the mixture was filtered under nitrogen protection while cold. The filtrate was then concentrated by vacuum distillation at 35°C to a volume equal to [amount missing] of the filtrate. 1 / 3 of the solution was added to obtain a concentrated solution. Under stirring, the concentrated solution was added dropwise to 500 mL of anhydrous petroleum ether. After the addition was complete, the solution was cooled to 0°C in an ice-water bath, stirred for 15 min, and allowed to stand for 2 h. The lower viscous phase was separated, and the upper petroleum ether supernatant was discarded. 20 mL of dichloromethane was added to the lower viscous phase, and after thorough stirring, 100 mL of anhydrous petroleum ether was added. After stirring and standing, the lower viscous phase was separated. The lower viscous phase was concentrated under reduced pressure to constant weight under nitrogen protection, at 35°C and a vacuum degree ≤-0.095 MPa to obtain the methacrylate phosphoryl chloride intermediate. The 1H NMR spectrum of the methacrylate phosphoryl chloride intermediate is shown below. Figure 1As shown, the chemical structure is as follows: .

[0022] (2) Under nitrogen protection, 0.06 mol of 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane, 80 mL of anhydrous tetrahydrofuran, and 0.1 mol of triethylamine were added to a dry reaction flask. The temperature was lowered to 0°C. 0.06 mol of methacrylate phosphoryl chloride intermediate was dissolved in 35 mL of anhydrous tetrahydrofuran and then added dropwise to the reaction flask. The dropping rate was controlled to maintain the material temperature at 0~5°C. After the addition was complete, the temperature was naturally raised to room temperature, and the reaction was stirred for 6 h. After the reaction was completed, the mixture was filtered to remove the generated triethylamine hydrochloride. The filtrate was concentrated under reduced pressure to constant weight at 40°C and a vacuum degree ≤-0.095 MPa to obtain the siloxane monohydroxy intermediate. The chemical structure of 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane is as follows: ; The 1H NMR spectrum of the siloxane monohydroxy intermediate is shown below. Figure 2 As shown, the chemical structure is as follows: .

[0023] Under nitrogen protection, 0.06 mol of tetraethylene glycol, 80 mL of anhydrous tetrahydrofuran, and 0.1 mol of triethylamine were added to a dry reaction flask. The mixture was cooled to 0°C. 0.06 mol of methacrylate phosphoryl chloride intermediate was dissolved in 35 mL of anhydrous tetrahydrofuran and added dropwise to the reaction flask. The dropping rate was controlled to maintain the material temperature between 0 and 5°C. After the addition was complete, the mixture was allowed to naturally warm to room temperature, and the reaction was continued with stirring for 6 hours. After the reaction was complete, the mixture was filtered to remove the generated triethylamine hydrochloride. The filtrate was concentrated under reduced pressure to constant weight at 40°C and a vacuum degree ≤ -0.095 MPa to obtain the polyether monohydroxy intermediate. The chemical structure of tetraethylene glycol is as follows: ; The 1H NMR spectrum of the polyether monohydroxy intermediate is shown below. Figure 3 As shown, the chemical structure is as follows: .

[0024] (3) Under nitrogen protection, 0.12 mol of isophorone diisocyanate and 100 mL of anhydrous tetrahydrofuran were added to a dry four-necked flask equipped with a mechanical stirrer, thermometer, and constant-pressure dropping funnel. Stirring was started, and the mixture was cooled to 0°C in an ice-water bath. 0.03 mol of bis(trimethylol)propane was dissolved in 120 mL of anhydrous tetrahydrofuran and then added dropwise to the reaction flask. The dropping rate was controlled so that the temperature of the reaction solution did not exceed 10°C. After the addition was complete, 0.24 mmol of dibutyltin dilaurate was added as a catalyst. After stirring evenly, the mixture was heated to 45°C and stirred for 6 hours. After the reaction was completed, the mixture was cooled to room temperature to obtain a tetrahydrofuran solution of the isocyanate-terminated compound. The chemical structure of bis(trimethylol)propane is as follows: .

[0025] A tetrahydrofuran solution of the isocyanate-terminated compound was added to the reaction flask, followed by 0.16 mmol of dibutyltin dilaurate. The temperature of the reaction mixture was adjusted to 30°C. 0.06 mol of a siloxane monohydroxy intermediate was dissolved in 80 mL of anhydrous tetrahydrofuran and added dropwise to the reaction flask, maintaining the temperature at 30–35°C. After the addition was complete, the mixture was stirred and kept at 30°C for 5 hours. Then, 0.065 mol of a polyether monohydroxy intermediate was dissolved in 70 mL of anhydrous tetrahydrofuran and added dropwise to the reaction flask. The temperature was then increased. The mixture was heated to 55℃ and stirred for 6 hours. After the reaction, it was cooled to room temperature, and the insoluble matter was removed by filtration. The filtrate was concentrated under reduced pressure at 40℃ to 1 / 5 of its original volume to obtain a concentrate. 50 mL of anhydrous tetrahydrofuran was added to the concentrate, and after stirring evenly, it was added dropwise to 500 mL of anhydrous petroleum ether. After the addition was complete, the mixture was cooled to 0℃ in an ice-water bath and allowed to stand for 1 hour. The lower viscous phase was separated, and the upper clear liquid was discarded. The lower viscous phase was washed twice with anhydrous petroleum ether (50 mL × 2). Finally, it was dried under vacuum at 50℃ to constant weight to obtain the functional polyurethane acrylate. The 1H NMR spectrum of the functional polyurethane acrylate is shown below. Figure 4 As shown, the chemical structure is as follows: . Example

[0026] The primer for the photocurable diamond Mars coating of this embodiment is composed of the following components in parts by weight: 35 parts functional polyurethane acrylate, 11 parts epoxy acrylate, 9 parts trifunctional acrylate monomer, 22 parts difunctional acrylate monomer, 22 parts superhard wear-resistant powder, and 4.5 parts photoinitiator; the trifunctional acrylate monomer is composed of pentaerythritol ethoxy (5) triacrylate and trimethylolpropane propoxy (3) triacrylate in a mass ratio of 5:3; the difunctional acrylate monomer is composed of pentaerythritol ethoxy (5) triacrylate and trimethylolpropane propoxy (3) triacrylate in a mass ratio of 2: The mixture consists of 1% tripropylene glycol diacrylate and 10% (ethoxy)bisphenol A diacrylate; the superhard wear-resistant powder is composed of diamond particles, zirconium oxide particles, and silicon carbide particles in a mass ratio of 4:5:10, with average particle sizes of 16 μm, 30 μm, and 30 μm, respectively; the photoinitiator is a mixture of 1-hydroxycyclohexylphenyl ketone and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a mass ratio of 2:1; the epoxy acrylate is EBECRYL 600. The functional polyurethane acrylate is the same as that in Example 1. Example

[0027] The primer for the photocurable diamond Mars coating of this embodiment is composed of the following components in parts by weight: 40 parts functional polyurethane acrylate, 12 parts epoxy acrylate, 11 parts trifunctional acrylate monomer, 25 parts difunctional acrylate monomer, 25 parts superhard wear-resistant powder, and 5 parts photoinitiator; the trifunctional acrylate monomer is composed of pentaerythritol ethoxy (5) triacrylate and trimethylolpropane propoxy (3) triacrylate in a mass ratio of 9:5; the difunctional acrylate monomer is composed of pentaerythritol ethoxy (5) triacrylate and trimethylolpropane propoxy (3) triacrylate in a mass ratio of 7:4. The composition is tripropylene glycol diacrylate and 10(ethoxy)bisphenol A diacrylate; the superhard wear-resistant powder is composed of diamond particles, zirconium oxide particles and silicon carbide particles in a mass ratio of 4:4:12, with average particle sizes of 20 μm, 40 μm and 40 μm for the diamond particles, zirconium oxide particles and silicon carbide particles, respectively; the photoinitiator is a mixture of 1-hydroxycyclohexylphenyl ketone and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a mass ratio of 2:1.5; the epoxy acrylate is EBECRYL 600. The functional polyurethane acrylate is the same as the functional polyurethane acrylate in Example 1.

[0028] The preparation method of the primer for the photocurable diamond Mars coating in Examples 1-3 includes the following steps: adding trifunctional acrylate monomers and difunctional acrylate monomers to a dispersion tank and stirring to mix evenly; then adding superhard wear-resistant powder and stirring to disperse evenly; then adding functional polyurethane acrylate and epoxy acrylate and stirring to mix evenly; finally adding a photoinitiator and stirring until the initiator is completely dissolved to obtain the primer for the photocurable diamond Mars coating.

[0029] Comparative Example 1 The only difference between the UV-curable diamond Mars coating primer of this comparative example and the UV-curable diamond Mars coating primer of Example 1 is that the UV-curable diamond Mars coating primer of this comparative example contains 39 parts by mass of functional polyurethane acrylate and 0 parts by mass of epoxy acrylate.

[0030] Comparative Example 2 The only difference between the UV-curable diamond Mars coating primer of this comparative example and the UV-curable diamond Mars coating primer of Example 1 is that the UV-curable diamond Mars coating primer of this comparative example contains 39 parts by mass of epoxy acrylate and 0 parts by mass of functional polyurethane acrylate.

[0031] Comparative Example 3 The only difference between the UV-curable diamond Mars coating primer of this comparative example and the UV-curable diamond Mars coating primer of Example 1 is that the trifunctional acrylate monomer in the UV-curable diamond Mars coating primer of this comparative example is pentaerythritol ethoxy(5) triacrylate.

[0032] Comparative Example 4 The only difference between the UV-curable diamond Mars coating primer of this comparative example and the UV-curable diamond Mars coating primer of Example 1 is that the trifunctional acrylate monomer in the UV-curable diamond Mars coating primer of this comparative example is trimethylolpropanepropoxy(3)triacrylate.

[0033] Comparative Example 5 The only difference between the UV-curable diamond Mars coating primer of this comparative example and the UV-curable diamond Mars coating primer of Example 1 is that the two functional group acrylate monomers in the UV-curable diamond Mars coating primer of this comparative example are 10(ethoxy)bisphenol A diacrylate.

[0034] Comparative Example 6 The only difference between the UV-curable diamond Mars coating primer of this comparative example and the UV-curable diamond Mars coating primer of Example 1 is that the two functional group acrylate monomers in the UV-curable diamond Mars coating primer of this comparative example are tripropylene glycol diacrylate.

[0035] Comparative Example 7 The only difference between the UV-curable diamond Mars coating primer of this comparative example and the UV-curable diamond Mars coating primer of Example 1 is that the preparation method of the functional polyurethane acrylate in the UV-curable diamond Mars coating primer of this comparative example is as follows: (1) This step is the same as step (1) of the preparation method of functional polyurethane acrylate in Example 1.

[0036] (2) This step is the same as step (2) of the preparation method of functional polyurethane acrylate in Example 1.

[0037] (3) Under nitrogen protection, add 0.12 mol of isophorone diisocyanate and 100 mL of anhydrous tetrahydrofuran to a dry four-necked flask equipped with a mechanical stirrer, thermometer and constant pressure dropping funnel. Start stirring and cool to 0°C in an ice-water bath. Dissolve 0.03 mol of bis(trimethylol)propane in 120 mL of anhydrous tetrahydrofuran and add it dropwise to the reaction flask. Control the dropping rate so that the temperature of the reaction solution does not exceed 10°C. After the addition is complete, add 0.24 mmol of dibutyltin dilaurate as a catalyst. Stir evenly and heat to 45°C. Keep the temperature and stir for 6 h. After the reaction is completed, cool to room temperature to obtain a tetrahydrofuran solution of the isocyanate-terminated compound.

[0038] A tetrahydrofuran solution of the isocyanate-terminated compound was added to the reaction flask, followed by 0.16 mmol of dibutyltin dilaurate. The temperature of the mixture in the reaction flask was adjusted to 30°C. 0.125 mol of a siloxane monohydroxy intermediate was dissolved in 150 mL of anhydrous tetrahydrofuran and then added dropwise to the reaction flask, maintaining the temperature at 30–35°C. After the addition was complete, the mixture was kept at 30°C with stirring for 5 hours, then the temperature was increased to 55°C and the mixture was kept at this temperature with stirring for 6 hours. After the reaction was completed... The solution was cooled to room temperature, filtered to remove insoluble matter, and concentrated under reduced pressure at 40°C to 1 / 5 of its original volume to obtain a concentrate. 50 mL of anhydrous tetrahydrofuran was added to the concentrate, and after stirring thoroughly, it was added dropwise to 500 mL of anhydrous petroleum ether. After the addition was complete, the solution was cooled to 0°C in an ice-water bath and allowed to stand for 1 hour. The lower viscous phase was separated, and the upper supernatant was discarded. The lower viscous phase was washed twice with anhydrous petroleum ether (50 mL × 2). Finally, it was dried under vacuum at 50°C to constant weight to obtain the functionalized polyurethane acrylate. The chemical structure of the functionalized polyurethane acrylate is as follows: .

[0039] Comparative Example 8 The only difference between the UV-curable diamond Mars coating primer of this comparative example and the UV-curable diamond Mars coating primer of Example 1 is that the preparation method of the functional polyurethane acrylate in the UV-curable diamond Mars coating primer of this comparative example is as follows: (1) This step is the same as step (1) of the preparation method of functional polyurethane acrylate in Example 1.

[0040] (2) This step is the same as step (2) of the preparation method of functional polyurethane acrylate in Example 1.

[0041] (3) Under nitrogen protection, add 0.12 mol of isophorone diisocyanate and 100 mL of anhydrous tetrahydrofuran to a dry four-necked flask equipped with a mechanical stirrer, thermometer and constant pressure dropping funnel. Start stirring and cool to 0°C in an ice-water bath. Dissolve 0.03 mol of bis(trimethylol)propane in 120 mL of anhydrous tetrahydrofuran and add it dropwise to the reaction flask. Control the dropping rate so that the temperature of the reaction solution does not exceed 10°C. After the addition is complete, add 0.24 mmol of dibutyltin dilaurate as a catalyst. Stir evenly and heat to 45°C. Keep the temperature and stir for 6 h. After the reaction is completed, cool to room temperature to obtain a tetrahydrofuran solution of the isocyanate-terminated compound.

[0042] A tetrahydrofuran solution of the isocyanate-terminated compound was added to the reaction flask, followed by 0.16 mmol of dibutyltin dilaurate. The temperature of the mixture in the reaction flask was adjusted to 30°C. 0.125 mol of the polyether monohydroxy intermediate was dissolved in 150 mL of anhydrous tetrahydrofuran and then added dropwise to the reaction flask, maintaining the temperature at 30–35°C. After the addition was complete, the mixture was kept at 30°C with stirring for 5 hours, then the temperature was increased to 55°C and the mixture was kept at this temperature with stirring for 6 hours. After the reaction was completed, the temperature was lowered... The solution was cooled to room temperature, filtered to remove insoluble matter, and the filtrate was concentrated under reduced pressure at 40°C to 1 / 5 of its original volume to obtain a concentrate. 50 mL of anhydrous tetrahydrofuran was added to the concentrate, and after stirring thoroughly, it was added dropwise to 500 mL of anhydrous petroleum ether. After the addition was complete, the solution was cooled to 0°C in an ice-water bath and allowed to stand for 1 hour. The lower viscous phase was separated, and the upper supernatant was discarded. The lower viscous phase was washed twice with anhydrous petroleum ether (50 mL × 2). Finally, it was dried under vacuum at 50°C to constant weight to obtain the functionalized polyurethane acrylate. The chemical structure of the functionalized polyurethane acrylate is as follows: .

[0043] Comparative Example 9 The only difference between the UV-curable diamond Mars coating primer of this comparative example and the UV-curable diamond Mars coating primer of Example 1 is that the preparation method of the functional polyurethane acrylate in the UV-curable diamond Mars coating primer of this comparative example is as follows: the functional polyurethane acrylate prepared in Comparative Example 7 and the functional polyurethane acrylate prepared in Comparative Example 8 are mixed evenly at a mass ratio of 17.5:15.9.

[0044] Comparative Example 10 The only difference between the UV-curable diamond Mars coating primer of this comparative example and the UV-curable diamond Mars coating primer of Example 1 is that the preparation method of the functional polyurethane acrylate in the UV-curable diamond Mars coating primer of this comparative example is as follows: (1) This step is the same as step (1) of the preparation method of functional polyurethane acrylate in Example 1.

[0045] (2) This step is the same as step (2) of the preparation method of functional polyurethane acrylate in Example 1.

[0046] (3) Under nitrogen protection, add 0.12 mol of isophorone diisocyanate and 100 mL of anhydrous tetrahydrofuran to a dry four-necked flask equipped with a mechanical stirrer, thermometer and constant pressure dropping funnel. Start stirring and cool to 0°C in an ice-water bath. Dissolve 0.03 mol of bis(trimethylol)propane in 120 mL of anhydrous tetrahydrofuran and add it dropwise to the reaction flask. Control the dropping rate so that the temperature of the reaction solution does not exceed 10°C. After the addition is complete, add 0.24 mmol of dibutyltin dilaurate as a catalyst. Stir evenly and heat to 45°C. Keep the temperature and stir for 6 h. After the reaction is completed, cool to room temperature to obtain a tetrahydrofuran solution of the isocyanate-terminated compound.

[0047] A tetrahydrofuran solution of the isocyanate-terminated compound was added to the reaction flask, followed by 0.16 mmol of dibutyltin dilaurate. The temperature of the mixture in the reaction flask was adjusted to 30°C. 0.03 mol of a siloxane monohydroxy intermediate was dissolved in 40 mL of anhydrous tetrahydrofuran and added dropwise to the reaction flask, maintaining the temperature at 30–35°C. After the addition was complete, the mixture was stirred and kept at 30°C for 4 hours. Then, 0.095 mol of a polyether monohydroxy intermediate was dissolved in 110 mL of anhydrous tetrahydrofuran and added dropwise to the reaction flask. The temperature was then increased. The mixture was heated to 55℃ and stirred for 8 hours. After the reaction, it was cooled to room temperature, and the insoluble matter was removed by filtration. The filtrate was concentrated under reduced pressure at 40℃ to 1 / 5 of its original volume to obtain a concentrate. 50 mL of anhydrous tetrahydrofuran was added to the concentrate, and after stirring evenly, it was added dropwise to 500 mL of anhydrous petroleum ether. After the addition was complete, the mixture was cooled to 0℃ in an ice-water bath and allowed to stand for 1 hour. The lower viscous phase was separated, and the upper clear liquid was discarded. The lower viscous phase was washed twice with anhydrous petroleum ether (50 mL × 2). Finally, it was dried under vacuum at 50℃ to constant weight to obtain the functional polyurethane acrylate. The chemical structure of the functional polyurethane acrylate is as follows: .

[0048] Comparative Example 11 The only difference between the UV-curable diamond Mars coating primer of this comparative example and the UV-curable diamond Mars coating primer of Example 1 is that the preparation method of the functional polyurethane acrylate in the UV-curable diamond Mars coating primer of this comparative example is as follows: (1) This step is the same as step (1) of the preparation method of functional polyurethane acrylate in Example 1.

[0049] (2) This step is the same as step (2) of the preparation method of functional polyurethane acrylate in Example 1.

[0050] (3) Under nitrogen protection, add 0.12 mol of isophorone diisocyanate and 100 mL of anhydrous tetrahydrofuran to a dry four-necked flask equipped with a mechanical stirrer, thermometer and constant pressure dropping funnel. Start stirring and cool to 0°C in an ice-water bath. Dissolve 0.03 mol of bis(trimethylol)propane in 120 mL of anhydrous tetrahydrofuran and add it dropwise to the reaction flask. Control the dropping rate so that the temperature of the reaction solution does not exceed 10°C. After the addition is complete, add 0.24 mmol of dibutyltin dilaurate as a catalyst. Stir evenly and heat to 45°C. Keep the temperature and stir for 6 h. After the reaction is completed, cool to room temperature to obtain a tetrahydrofuran solution of the isocyanate-terminated compound.

[0051] A tetrahydrofuran solution of the isocyanate-terminated compound was added to the reaction flask, followed by 0.16 mmol of dibutyltin dilaurate. The temperature of the reaction mixture was adjusted to 30°C. 0.09 mol of a siloxane monohydroxy intermediate was dissolved in 110 mL of anhydrous tetrahydrofuran and added dropwise to the reaction flask, maintaining the temperature at 30–35°C. After the addition was complete, the mixture was stirred and kept at 30°C for 7 hours. Then, 0.035 mol of a polyether monohydroxy intermediate was dissolved in 40 mL of anhydrous tetrahydrofuran and added dropwise to the reaction flask. The temperature was then increased. The mixture was heated to 55℃ and stirred for 4 hours. After the reaction was complete, it was cooled to room temperature, and the insoluble matter was removed by filtration. The filtrate was concentrated under reduced pressure at 40℃ to 1 / 5 of its original volume to obtain a concentrate. 50 mL of anhydrous tetrahydrofuran was added to the concentrate, and after stirring until homogeneous, it was added dropwise to 500 mL of anhydrous petroleum ether. After the addition was complete, the mixture was cooled to 0℃ in an ice-water bath and allowed to stand for 1 hour. The lower viscous phase was separated, and the upper clear liquid was discarded. The lower viscous phase was washed twice with anhydrous petroleum ether (50 mL × 2). Finally, it was dried under vacuum at 50℃ to constant weight to obtain the functional polyurethane acrylate. The chemical structure of the functional polyurethane acrylate is as follows: .

[0052] Experimental Example To investigate the stability and mechanical properties of the UV-cured diamond Mars coating primers in the various embodiments and comparative examples, the storage stability, adhesion, solvent wiping resistance, and abrasion resistance of the UV-cured diamond Mars coating primers in the various embodiments and comparative examples were tested. The storage stability test method was as follows: the prepared primer sample was poured into a 50mL stoppered graduated cylinder to full volume, sealed, and placed in a 30℃ constant temperature incubator. Observations were made every 24 hours, and the number of days until the first visible sediment appeared at the bottom of the graduated cylinder was recorded. For the adhesion, solvent wiping resistance, and abrasion resistance tests, the primer was first prepared into a coating, as follows: [The text abruptly ends here, likely due to an incomplete sentence or missing information.] 3The surface of the high-density fiberboard is sanded with a 240-grit finish, and then a UV-cured diamond Mars coating primer is applied to the sanded surface at a coverage of 65 g / m². 2 After coating, the product is dried using a UV curing lamp with a UV energy of 150 mJ / cm². 2 After UV curing, the primer layer is formed and then cured at 25°C for 12 hours before being tested for adhesion, solvent wiping resistance and abrasion resistance.

[0053] Adhesion was tested according to GB / T 5210-2006 "Paints and Varnishes - Pull-off Adhesion Test". A 20mm diameter test column was used, and a two-component epoxy adhesive was used to bond the test column to the coating surface. The test was conducted on a universal testing machine at a tensile speed of 1mm / min. The maximum tensile force at which the coating failed was recorded, and the pull-off adhesion was calculated. MEK wiping resistance was tested according to GB / T 23989-2009 "Coatings - Solvent Resistance Wiping Test". A degreased cotton ball soaked in methyl ethyl ketone (MEK) solvent was used to wipe the coating surface bidirectionally at a frequency of 1 swipe / second. The number of unidirectional wipings when the coating surface exposed the substrate was recorded. Abrasion resistance was tested according to GB / T 1768-2006 "Determination of Abrasion Resistance of Paints and Varnishes - Rotary Rubber Grinding Wheel Method". A Taber 5135 abrasion tester was used, with a CS-10 rubber grinding wheel and a 500g weight loaded. The mass loss of the coating after 1000 revolutions was measured, and the unit was mg. Before each test, the grinding wheel was pre-polished with S-11 sandpaper for 50 revolutions. The average value of three parallel samples was taken. The stability and mechanical properties of the primers for the UV-cured diamond Martian coatings in each example and comparative example are shown in Table 1.

[0054] Table 1. Test results of stability and mechanical properties of primer for UV-cured diamond Martian coating. primer Storage stability (d) <![CDATA[Adhesion force (N / mm 2 )]]> MEK wipe resistance (number of wipes) Abrasion resistance (mg) Example 1 15 7.1 350 11 Example 2 14 6.9 342 14 Example 3 12 7.3 356 12 Comparative Example 1 8 3.4 171 45 Comparative Example 2 2 2.2 195 71 Comparative Example 3 10 4.3 253 35 Comparative Example 4 8 3.8 187 48 Comparative Example 5 9 4.7 159 52 Comparative Example 6 7 3.9 224 41 Comparative Example 7 3 1.4 51 93 Comparative Example 8 2 2.6 74 52 Comparative Example 9 3 1.8 62 78 Comparative Example 10 6 4.1 155 47 Comparative Example 11 5 3.5 162 50 As can be seen from the test results in Table 1, the primer for the light-cured diamond Mars coating provided by the present invention has good storage stability, adhesion, solvent resistance and abrasion resistance, and exhibits good overall performance in terms of bottom anchoring and load bearing.

[0055] As shown in Example 1 and Comparative Examples 1-2, when the primer lacks epoxy acrylate and contains only functional polyurethane acrylate, the coating's adhesion and solvent resistance decrease, and its abrasion resistance deteriorates. When the primer lacks functional polyurethane acrylate and contains only epoxy acrylate, the coating's storage stability is poor, and its adhesion and abrasion resistance also deteriorate to varying degrees. Epoxy acrylate contains a large number of benzene rings and polar groups, giving the coating high hardness and polar adhesion to the substrate. At the same time, its dense cross-linked network can effectively resist solvent penetration. Functional polyurethane acrylate, through its sulfonic acid groups anchoring inorganic powders and the steric hindrance and solvation layer formed on the powder surface by siloxane and polyether side chains, can improve the suspension stability of superhard abrasion-resistant powder in the system and provide the necessary flexibility to absorb wear stress.

[0056] As shown in Example 1 and Comparative Examples 3-6, when only a single component of the trifunctional or difunctional acrylate monomer is used, the storage stability, adhesion, and abrasion resistance of the coating all decrease to varying degrees. When pentaerythritol ethoxytriacrylate and trimethylolpropane propoxytriacrylate are used in combination, the hardness resulting from the high crosslinking density is balanced with the internal stress release capability provided by the long-chain alkoxy groups. When tripropylene glycol diacrylate and long-chain ethoxylated bisphenol A diacrylate are used in combination, both good wetting and penetration into the substrate are provided, and the rigid structure of bisphenol A enhances the cohesive strength and solvent resistance of the coating.

[0057] As shown in Example 1 and Comparative Examples 7-9, when only siloxane side chains are introduced into the functional polyurethane acrylate without polyether side chains, the coating exhibits poor storage stability and adhesion, and decreased abrasion resistance. When only polyether side chains are introduced without siloxane side chains, the coating also shows poor storage stability, and its solvent resistance and abrasion resistance deteriorate. Siloxane segments have low surface energy and excellent wettability, enabling them to migrate well to the inorganic powder interface to form a dense coating layer, effectively preventing powder agglomeration and sedimentation, while enhancing the coating's interfacial spreading and adhesion to the substrate. Polyether segments, on the other hand, possess high flexibility and polar ether bonds, which can regulate the microstructure of the resin network, providing good stress release capabilities and endowing the coating with toughness against dynamic friction and solvent swelling. Comparative Example 9 physically blends resins containing only siloxane segments and resins containing only polyether segments. Due to their poor thermodynamic compatibility, microphase separation easily occurs after curing, making it difficult to construct a continuous and uniform dispersion and stress transfer network.

[0058] As shown in Example 1 and Comparative Examples 10-11, when the ratio of siloxane side chains to polyether side chains in the functional polyurethane acrylate is changed, the storage stability of the coating deteriorates, and the adhesion and abrasion resistance also deteriorate to varying degrees. This result demonstrates that the ratio of siloxane side chains to polyether side chains around the rigid crosslinked core constructed from isophorone diisocyanate and bis(trimethylol)propane is crucial for balancing the powder dispersion stability of the resin system, the substrate wetting and anchoring force, and the abrasion toughness of the coating itself.

[0059] In summary, the primer for the light-cured diamond Mars coating provided by this invention is made by mixing a functional polyurethane acrylate with bis(trimethylol)propane as the core skeleton and containing triethylamine sulfonate, siloxane side chains and polyether side chains in its molecular structure, with epoxy acrylate, a trifunctional monomer compounded with pentaerythritol ethoxytriacrylate and trimethylolpropane propoxytriacrylate, a bifunctional monomer compounded with tripropylene glycol diacrylate and ethoxylated bisphenol A diacrylate, and superhard abrasion-resistant powder. It has good storage stability, adhesion, solvent resistance and abrasion resistance, providing a solid and stable underlying support for the topcoat.

[0060] It should be noted that, in this document, the terms "comprising," "including," and any other variations are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Specific examples have been used in this document to illustrate the principles and implementation methods of the present invention. These examples are merely for the purpose of helping to understand the method and core ideas of the present invention. The above descriptions are only preferred embodiments of the present invention. It should be pointed out that, due to the limitations of written expression and the objective existence of infinite specific structures, those skilled in the art can make several improvements, modifications, or variations without departing from the principles of the present invention, and can also combine the above technical features in an appropriate manner. These improvements, modifications, variations, or combinations, or the direct application of the concept and technical solution of the present invention to other situations without modification, should all be considered within the scope of protection of the present invention.

Claims

1. A primer for a light-cured diamond Martian coating, characterized in that, It is composed of the following components in parts by weight: 30-40 parts functional polyurethane acrylate, 9-12 parts epoxy acrylate, 25-36 parts multifunctional acrylate monomer, 18-25 parts superhard wear-resistant powder, and 4-5 parts photoinitiator; the superhard wear-resistant powder is composed of diamond particles, zirconium oxide particles, and silicon carbide particles; the multifunctional acrylate monomer is composed of trifunctional acrylate monomer and difunctional acrylate monomer; based on the total mass of the multifunctional acrylate monomer, the trifunctional... The acrylate monomers comprise 30%–40%, and the difunctional acrylate monomers comprise 60%–71%; the trifunctional acrylate monomers are composed of pentaerythritol ethoxylated triacrylate and trimethylolpropane propoxylated triacrylate in a mass ratio of (3–9):(1–5); the difunctional acrylate monomers are composed of tripropylene glycol diacrylate and ethoxylated bisphenol A diacrylate in a mass ratio of (5–7):(2–4); the chemical structure of the functional polyurethane acrylate is as follows: 。 2. The primer for photocurable diamond Martian coating according to claim 1, characterized in that, The pentaerythritol ethoxylated triacrylate is pentaerythritol ethoxy(5) triacrylate.

3. The primer for photocurable diamond Martian coating according to claim 1, characterized in that, The ethoxylated bisphenol A diacrylate is 10(ethoxy)bisphenol A diacrylate.

4. The primer for photocurable diamond Martian coating according to claim 1, characterized in that, The mass ratio of the diamond particles, zirconium oxide particles and silicon carbide particles is (3~5):(4~9):(10~12).

5. The primer for photocurable diamond Martian coating according to claim 1, characterized in that, The average particle sizes of the diamond particles, zirconium oxide particles, and silicon carbide particles are 10~20μm, 20~40μm, and 20~40μm, respectively.

6. The primer for photocurable diamond Martian coating according to any one of claims 1-5, characterized in that, The functional polyurethane acrylate is prepared by a method comprising the following steps: (1) After reacting 3-hydroxypropanesulfonic acid with phosphorus oxychloride, it is then reacted with hydroxyethyl methacrylate to obtain phosphoryl chloride intermediate of methacrylate; the molar ratio of 3-hydroxypropanesulfonic acid, phosphorus oxychloride and hydroxyethyl methacrylate is 1:1:1; (2) The methacrylate phosphoryl chloride intermediate with a molar ratio of 1:1 was reacted with 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane to obtain a siloxane monohydroxy intermediate; the methacrylate phosphoryl chloride intermediate with a molar ratio of 1:1 was reacted with tetraethylene glycol triethylene glycol to obtain a polyether monohydroxy intermediate. (3) Reaction of isophorone diisocyanate with bis(trimethylolpropane) to obtain a terminal isocyanate compound; then reaction of the terminal isocyanate compound with the siloxane monohydroxy intermediate and the polyether monohydroxy intermediate to obtain functional polyurethane acrylate.

7. The primer for photocurable diamond Martian coating according to claim 6, characterized in that, The molar ratio of isophorone diisocyanate, bis(trimethylolpropane), siloxane monohydroxy intermediate and polyether monohydroxy intermediate is 1.2:0.3:0.6:0.

65.

8. The primer for photocurable diamond Martian coating according to claim 1, characterized in that, The epoxy acrylate is a bisphenol A type epoxy acrylate.

9. The primer for photocurable diamond Martian coating according to claim 1, characterized in that, The photoinitiator is composed of 1-hydroxycyclohexylphenyl ketone and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a mass ratio of 2:1 to 1.

5.

10. A method for preparing a primer for a photocurable diamond Martian coating as described in any one of claims 1-9, characterized in that, Includes the following steps: Functional polyurethane acrylate, epoxy acrylate, multifunctional acrylate monomer, superhard wear-resistant powder and photoinitiator are mixed to obtain a primer for photocurable diamond Martian coating.

Citation Information

Patent Citations

  • UV-light (ultraviolet light) solidified stereoscopic diamond plating lacquer

    CN103242743A

  • Diamond spark coating for wood board as well as preparation method and coating process of diamond spark coating

    CN119186967A