An epoxy resin-silica sol interpenetrating network material, its preparation method, and its application in liquid-like coatings.

By utilizing the physical interpenetration and chemical cross-linking of epoxy resin-silica sol interpenetrating network materials, the adhesion and stability issues of liquid-like coatings on non-silica substrates have been resolved, achieving coating performance with high strength, wide applicability, and excellent functionality.

CN122772494BActive Publication Date: 2026-11-17SHANDONG UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611241201.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-08-17
Publication Date
2026-11-17
Estimated Expiration
2046-08-17

AI Technical Summary

Technical Problem

Existing liquid-like coatings are difficult to build on non-silicon substrates, lack mechanical strength, and have poor stability in humid environments, which limits their practical applications.

Method used

By using epoxy resin-silica sol interpenetrating network material, an intermediate layer is constructed through physical interpenetration and chemical cross-linking, achieving a bonding strength ≥15 MPa and a pencil hardness ≥6 H, thus enabling firm adhesion to substrates of different materials.

Benefits of technology

It significantly improves the versatility, mechanical properties, and environmental stability of liquid-like coatings, and possesses excellent liquid-repellent, anti-corrosion, anti-icing, and easy-to-clean properties, making it suitable for complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122772494B_ABST
    Figure CN122772494B_ABST
Patent Text Reader

Abstract

This invention discloses an epoxy resin-silica sol interpenetrating network material, its preparation method, and its application in liquid-like coatings, belonging to the field of epoxy resin / silica sol interpenetrating network construction technology. The material comprises the following raw materials in parts by weight: 1 part by weight of silica sol, 0.1-0.8 parts by weight of epoxy resin, and 0.025-0.2 parts by weight of amine curing agent; the silica sol is polymerized from tetraethoxysilane, γ-aminopropyltriethoxysilane, and hydroxyl-terminated silicone oil; in the epoxy resin-silica sol interpenetrating network material, the epoxy resin network and the silica sol network interpenetrate and crosslink, synergistically improving its overall mechanical properties and stability. Furthermore, through the covalent bonding of silanes and the non-covalent interaction of polymer chains, it can firmly adhere to the surface of substrates of different materials and shapes, significantly expanding the application versatility of liquid-like coatings, ultimately achieving long-term durability and excellent functional performance of the coating in complex environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of epoxy resin / silica sol interpenetrating network construction technology, specifically relating to an epoxy resin-silica sol interpenetrating network material, its preparation method, and its application in liquid-like coatings. Background Technology

[0002] The information disclosed in this background section is intended only to enhance understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.

[0003] Liquid-like surface technology, by constructing covalently anchored dynamic molecular layers, exhibits excellent liquid repulsion and low adhesion properties, showing promise in fields such as antifouling, anti-icing, droplet transport, and membrane separation. However, the practical application of liquid-like coatings is limited by two major bottlenecks: first, their preparation heavily relies on smooth substrates with specific chemical activity (such as glass and silicon wafers), making it difficult to directly construct them on the surfaces of common materials such as metals and plastics; second, they themselves are nanoscale molecular brushes, only a few nanometers thick, lacking sufficient mechanical strength and durability, and are easily damaged by moisture or friction.

[0004] To broaden the substrate adaptability, existing technologies employ the sol-gel method to introduce a silicon-based transition layer onto non-silicon substrates. However, such silicon sol interlayers exhibit intrinsic brittleness, with a critical thickness threshold (300-400 nm). Excessive thickness leads to cracking, resulting in limited improvement in overall mechanical properties. More significantly, this interlayer exhibits poor stability in humid environments, easily swelling, cracking, and peeling after prolonged immersion in water, making it difficult to guarantee the long-term reliability of the coating system. Therefore, developing a novel interlayer that combines broad substrate adaptability, excellent mechanical properties, and good environmental stability is crucial for driving the practical application of liquid-like coatings. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide an epoxy resin-silica sol interpenetrating network material, its preparation method, and its application in liquid-like coatings. The material provided by the present invention is synergistically constructed from a silica sol network and an epoxy resin network through physical interpenetration and chemical cross-linking. It provides sufficient active sites for liquid-like coatings, possesses excellent mechanical properties, and can bond with substrate surfaces of any material and shape through covalent and non-covalent bonds, significantly improving the versatility of liquid-like coatings.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows: In a first aspect, the present invention provides an epoxy resin-silica sol interpenetrating network material comprising the following raw materials in parts by weight: 1 part by weight of silica sol, 0.1-0.8 parts by weight of epoxy resin, and 0.025-0.2 parts by weight of amine curing agent; The silica sol is polymerized from tetraethoxysilane, γ-aminopropyltriethoxysilane and hydroxyl-terminated silicone oil; the volume ratio of tetraethoxysilane, γ-aminopropyltriethoxysilane and hydroxyl-terminated silicone oil is (1~5):(1~5):(0.1~0.2); In the epoxy resin-silica sol interpenetrating network material, the epoxy resin network and the silica sol network interpenetrate and crosslink.

[0007] In some embodiments of the present invention, the epoxy resin includes any one of epoxy resin E-51 and epoxy resin E-44.

[0008] In some embodiments of the present invention, the amine curing agent includes any one of polyetheramine and polyimide.

[0009] In some embodiments of the present invention, after the epoxy resin-silica sol interpenetrating network material is bonded to the substrate, the bonding strength is ≥15 MPa and the pencil hardness is ≥6 H.

[0010] A second aspect of the present invention provides a method for preparing the epoxy resin-silica sol interpenetrating network material described in the first aspect, comprising: Tetraethoxysilane, γ-aminopropyltriethoxysilane and double-hydroxyl-terminated silicone oil were added to the solvent, stirred well, and then a catalyst was added. The reaction was stirred at a certain temperature to obtain a silica sol network solution. Epoxy resin and amine curing agent are added to a silica sol network solution and stirred at a certain temperature to obtain a prepolymer solution; The prepolymer solution is applied to the substrate and cured to obtain an epoxy resin-silica sol interpenetrating network material.

[0011] In some embodiments of the present invention, the solvent is an alcohol solvent.

[0012] In some embodiments of the present invention, the catalyst is water and acid.

[0013] In some embodiments of the present invention, tetraethoxysilane, γ-aminopropyltriethoxysilane and bi-hydroxyl-terminated silicone oil are added to a solvent, stirred until homogeneous, and then a catalyst is added. The mixture is stirred at 50-70°C for 8-12 h and then allowed to stand for aging for 2-4 h to obtain a silica sol network solution.

[0014] In some embodiments of the present invention, the acid includes any one or more of concentrated sulfuric acid, nitric acid, and acetic acid.

[0015] A third aspect of the present invention provides the application of the epoxy resin-silica sol interpenetrating network material described in the first aspect or the epoxy resin-silica sol interpenetrating network material prepared by the preparation method described in the second aspect in the construction of liquid-like coatings.

[0016] A fourth aspect of the present invention provides a method for constructing a liquid-like coating, comprising: An intermediate layer is constructed on the surface of the substrate, wherein the intermediate layer is the epoxy resin-silica sol interpenetrating network material described in the first aspect or the epoxy resin-silica sol interpenetrating network material prepared by the preparation method described in the second aspect. The intermediate layer surface is activated, and then a liquid-like coating slurry is coated on its surface and cured to obtain the liquid-like coating.

[0017] The beneficial effects of this invention are as follows: This invention constructs an epoxy resin-silica sol interpenetrating network material, which solves existing problems through the synergistic effect of the silica sol network and the epoxy resin network. The silica sol network uses tetraethoxysilane and γ-aminopropyltriethoxysilane as a framework, and introduces bihydroxyl-terminated silicone oil as a flexible component to reduce brittleness, improve film formation and mechanical properties, and can produce a thicker intermediate layer, thus providing better wear resistance. During heating, the bihydroxyl-terminated silicone oil migrates to the surface, further increasing the silicon content of the coating surface and providing sufficient grafting sites for the upper liquid-like coating; the epoxy resin network contributes core mechanical strength and toughness. The two have a physically interpenetrating structure, achieving mutual reinforcement, and the amino groups in the silica sol network chemically crosslink with the epoxy groups in the epoxy resin network, forming a stable covalent bond, thereby synergistically improving the overall mechanical properties and stability of the interpenetrating material. Furthermore, this interpenetrating material can firmly adhere to the surface of substrates of different materials and shapes through the covalent bonding of silanes and the non-covalent interaction of polymer chains, significantly expanding the versatility of liquid-like coatings and ultimately achieving long-term durability and excellent performance of the coating in complex environments.

[0018] This invention combines epoxy resin networks and silica sol networks through a dual mechanism of physical interpenetrating network and chemical crosslinking to prepare a liquid-like coating interlayer with high mechanical properties and stability, namely, an epoxy resin-silica sol interpenetrating network material. Compared with silica sol coatings prepared by the traditional sol-gel method, the interlayer obtained by this invention has higher bonding strength (≥15 MPa) and pencil hardness (≥6 H). The resulting liquid-like coating exhibits better hydrophobic properties (20 μL water sliding angle ≤5°, 10 μL n-hexadecane sliding angle ≤3°) and corrosion resistance (corrosion current density ≤10). -6 A / cm 2 It exhibits excellent anti-icing properties (ice adhesion reduction ≥92.5%) and easy-to-clean properties. Furthermore, compared to traditional silica sol coatings, the epoxy resin / silica sol interlayer prepared in this invention does not crack after prolonged immersion in water, making it suitable for high humidity or underwater environments. Attached Figure Description

[0019] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.

[0020] Figure 1 This demonstrates the hydrophobic effect of the liquid-like coatings constructed with the assistance of epoxy resin-silica sol interpenetrating network materials on different substrate surfaces in Example 4.

[0021] Figure 2 This demonstrates the ink-resistant effect of the liquid-like coating constructed with the aid of epoxy resin-silica sol interpenetrating network material on the surface of the iron sheet obtained in Example 1.

[0022] Figure 3 This describes the anti-corrosion effect of the liquid-like coating constructed with the epoxy resin-silica sol interpenetrating network material on the surface of the iron sheet obtained in Example 1. In the figure, (a1) represents the initial state of the uncoated iron sheet, (a2) represents the state of the uncoated iron sheet on the first day, (a3) ​​represents the state of the uncoated iron sheet on the third day, (a4) represents the state of the uncoated iron sheet on the fifth day, (a5) represents the state of the uncoated iron sheet on the seventh day, (b1) represents the initial state of the coated iron sheet, (b2) represents the state of the coated iron sheet on the first day, (b3) represents the state of the coated iron sheet on the third day, (b4) represents the state of the coated iron sheet on the fifth day, and (b5) represents the state of the coated iron sheet on the seventh day.

[0023] Figure 4 The electrochemical corrosion test results are for the liquid-like coating constructed with the help of epoxy resin-silica sol interpenetrating network material on the surface of the iron sheet obtained in Example 1.

[0024] Figure 5 This describes the dynamic hydrophobic effect of the liquid-like coating constructed with the aid of epoxy resin-silica sol interpenetrating network material on the surface of the iron sheet obtained in Example 1.

[0025] Figure 6 This demonstrates the anti-icing effect of the liquid-like coating constructed with the aid of epoxy resin-silica sol interpenetrating network material on the surface of the iron sheet obtained in Example 1.

[0026] Figure 7 The optical properties of the liquid-like coating constructed with the help of epoxy resin-silica sol interpenetrating network material on the surface of the iron sheet obtained in Example 1 are shown. Among them, (a) is the transparency test result, (b) is the light transmittance curve, and (c) is the haze curve.

[0027] Figure 8 SEM images of the surface (a) and cross-section (b) of the epoxy resin-silica sol interpenetrating network material obtained in Example 1, and the silicon element distribution (c).

[0028] Figure 9This is a comparison of the water resistance of the epoxy resin-silica sol interpenetrating network material obtained in Example 1 and the liquid-like coating constructed with the help of a conventional silica sol intermediate layer obtained in Comparative Example 4.

[0029] Figure 10 The mechanical properties of the epoxy resin-silica sol interpenetrating network material obtained in Example 1 are compared with those of the conventional silica sol intermediate layers obtained in Comparative Examples 1, 2, and 3. Among them, (a) is a comparison of the adhesion strength between Example 1 and Comparative Example 1, (b) is a comparison of the pencil hardness between Example 1 and Comparative Example 2, and (c) is a comparison of the elongation at break between Example 1 and Comparative Example 3. Detailed Implementation

[0030] Given the lack of an intermediate layer in existing technologies that can be widely adapted to different substrate materials while possessing excellent mechanical strength, sufficient thickness, and long-term environmental stability, which severely limits the practical application scope and reliability of liquid-like coating technology, this invention proposes an epoxy resin-silica sol interpenetrating network material, its preparation method, and its application in liquid-like coatings.

[0031] A first typical embodiment of the present invention provides an epoxy resin-silica sol interpenetrating network material comprising the following raw materials in parts by weight: 1 part by weight of silica sol, 0.1-0.8 parts by weight of epoxy resin, and 0.025-0.2 parts by weight of amine curing agent; The silica sol is polymerized from tetraethoxysilane, γ-aminopropyltriethoxysilane and hydroxyl-terminated silicone oil; the volume ratio of tetraethoxysilane, γ-aminopropyltriethoxysilane and hydroxyl-terminated silicone oil is (1~5):(1~5):(0.1~0.2); In the epoxy resin-silica sol interpenetrating network material, the epoxy resin network and the silica sol network interpenetrate and crosslink.

[0032] This invention constructs an epoxy resin / silica sol interpenetrating network (IPN) intermediate layer, which fundamentally solves the problems of poor universality, weak mechanical properties, and insufficient durability of existing liquid-like coating substrates through the synergistic effect of physical interpenetration and chemical crosslinking. Its core working principle is as follows: 1. Dual-network collaborative construction and functional division of labor Silica sol network: As a functional carrier network, its main function is to provide abundant active silanol sites for grafting onto the upper liquid-like coating. This network is formed with tetraethoxysilane and γ-aminopropyltriethoxysilane as its backbone. Among them, the double-terminated hydroxyl silicone oil acts as a key flexibility regulating component; its long-chain structure functions as a "molecular spring" within the network, buffering internal stress through movement, effectively reducing the brittleness of traditional silica sol, improving film formation, and migrating to the surface during heat treatment to further enrich surface silicon elements and increase the density of active sites.

[0033] Epoxy resin network: As a reinforcing support network, it primarily contributes to excellent mechanical strength, toughness, and crack resistance. It is formed by the polymerization of epoxy resin and amine curing agent to create a dense cross-linked structure, providing skeletal support for the entire intermediate layer.

[0034] 2. Synergistic enhancement mechanism of "interpenetration" and "cross-linking" Physical interpenetration: A stepwise polymerization process is used to first form a silica sol network, and then epoxy resin monomers are introduced into its pores for polymerization and curing. This allows the two networks to interpenetrate and entangle at the nanoscale, restricting the movement of molecular chains and achieving a physical reinforcement effect similar to "woven fabrics," significantly improving the mechanical properties and dimensional stability of the material.

[0035] Chemical crosslinking: The γ-aminopropyltriethoxysilane in the silica sol network provides amino groups, which can undergo ring-opening reactions with the epoxy groups in the epoxy resin network to form strong covalent bonds. This chemical bridging tightly connects two independent networks into a whole, greatly enhancing interfacial bonding and structural integrity, and preventing delamination.

[0036] 3. The working principle of achieving universal adhesion This intermediate layer forms a strong bond with various substrates through two bonding methods: Covalent bonding: The silane component of the intermediate layer (especially the silica sol part) can undergo condensation reactions with active groups such as hydroxyl groups on the surface of various substrates such as metals, glass, and plastics to form covalent bonds.

[0037] Non-covalent bonding: The polar groups and long-chain polymers in the intermediate layer can be widely adsorbed onto substrates of different materials and shapes (including complex curved surfaces) through van der Waals forces, hydrogen bonds and other forces.

[0038] 4. Overall performance improvement path This intermediate layer achieves the following performance leaps through the aforementioned principles: the flexible silicone oil-toughened silica sol network provides high surface activity and resistance to brittleness; the interpenetrating cross-linked epoxy network imparts high strength and toughness; and the strong substrate adhesion mechanism overcomes the limitations of the substrate material. These three elements work synergistically, enabling it not only to stably support liquid-like functional layers but also to withstand mechanical and chemical effects in complex environments, thereby comprehensively improving the coating's durability and application range.

[0039] In this invention, the epoxy resin network mainly serves to improve the mechanical properties of the intermediate layer and prevent cracking, and is polymerized from epoxy resin and curing agent.

[0040] In some typical embodiments of the present invention, the epoxy resin includes, but is not limited to, any one of epoxy resin E-51 and epoxy resin E-44.

[0041] In some typical embodiments of the present invention, the amine curing agent includes, but is not limited to, any one of polyetheramine and polyimide.

[0042] Amine curing agents not only cure with epoxy resin to form a high-strength network, but more importantly, their active amino groups synergistically react with the amino groups provided by γ-aminopropyltriethoxysilane in the silica sol network, jointly reacting with epoxy groups to build a strong covalent bond between the silica sol network and the epoxy resin network. This chemical crosslinking tightly "stitches" the two physically interpenetrating networks into a whole, greatly enhancing the structural stability, mechanical properties, and crack resistance of the intermediate layer, achieving a synergistic reinforcement effect. Simultaneously, amine curing agents typically cure at medium to low temperatures, facilitating the smooth penetration and reaction of epoxy resin within the formed silica sol network framework, thus forming a uniform and stable interpenetrating network structure.

[0043] The amine curing agent of this invention is not only a curing agent for epoxy resin, but also a "chemical bridge" connecting the epoxy resin network and the amino-containing silica sol network. Through the unique reaction between its amino and epoxy groups, it drives and completes the covalent cross-linking between the two networks, achieving a synergistic reinforcement effect of "1+1>2", resulting in a high-strength, high-toughness, and high-stability intermediate layer. If it is replaced with other types of curing agents, it is impossible to obtain a high-strength, high-toughness, and high-stability intermediate layer. For example, anhydride curing agents usually require high-temperature curing, which may damage the pre-formed silica sol network structure or cause excessive migration of flexible silicone oil, and cannot effectively cross-link with the amino groups of the silica sol network, thus failing to form chemical interpenetration. Phenolic resin curing requires strong acid catalysts and high temperatures, which are harsh conditions that adversely affect the silica sol network and the substrate, and also lack the ability to directly cross-link with silane amino groups.

[0044] In this invention, the silica sol network primarily serves to provide silicon and active sites for grafting liquid-like coatings. It is polymerized from tetraethoxysilane, γ-aminopropyltriethoxysilane, and bihydroxyl-terminated silicone oil. Tetraethoxysilane and γ-aminopropyltriethoxysilane form the main framework of the silica sol network, while the bihydroxyl-terminated silicone oil, with its high flexibility and extensibility, acts as a "spring," buffering stress within the silica sol network, reducing its brittleness, and improving its film-forming properties and mechanical properties. Simultaneously, the bihydroxyl-terminated silicone oil migrates to the coating surface during heating, further increasing the silicon content on the coating surface and providing more active sites for the construction of the liquid-like coating.

[0045] By controlling the copolymerization of tetraethoxysilane (the framework builder) and γ-aminopropyltriethoxysilane (providing amino crosslinking sites) in similar proportions, sufficient structural strength and chemically reactive sites are ensured in the network. Simultaneously, the addition of a small but crucial amount of double-terminated hydroxyl silicone oil (a flexibility modifier) ​​is limited, allowing it to effectively function as a "molecular spring" for toughening and stress buffering without compromising the network's integrity, and promoting silicon enrichment on the surface during curing. This synergistic volume ratio achieves a precise balance between the "rigid framework," "flexible segments," and "reactive sites" in the silica sol network, fundamentally overcoming the brittleness and cracking defects of traditional silica sols, and laying an ideal foundation for the subsequent construction of a high-strength and tough interpenetrating network intermediate layer.

[0046] In some typical embodiments of the present invention, after the epoxy resin-silica sol interpenetrating network material is bonded to the substrate, the bonding strength is ≥15 MPa and the pencil hardness is ≥6 H.

[0047] A second typical embodiment of the present invention provides a method for preparing the epoxy resin-silica sol interpenetrating network material, comprising: Tetraethoxysilane, γ-aminopropyltriethoxysilane and double-hydroxyl-terminated silicone oil were added to the solvent, stirred well, and then a catalyst was added. The reaction was stirred at a certain temperature to obtain a silica sol network solution. Epoxy resin and curing agent are added to a silica sol network solution and stirred at a certain temperature to obtain a prepolymer solution; The prepolymer solution is applied to the substrate and cured to obtain an epoxy resin-silica sol interpenetrating network material.

[0048] The silica sol network and epoxy resin network are formed stepwise. First, the silica sol network is formed, and then the epoxy resin and amine curing agent are added to the silica sol network for polymerization, thereby achieving the effect of a physical interpenetrating network. At the same time, the amino groups on the silica sol network can chemically crosslink with the epoxy bonds in the epoxy resin network, further improving the mechanical properties and stability of the interpenetrating network intermediate layer.

[0049] In some typical embodiments of the present invention, the solvent is an alcohol solvent, including but not limited to any one or more of anhydrous ethanol, methanol, n-propanol, and isopropanol.

[0050] In some typical embodiments of the present invention, the catalyst is water and acid, which promotes the hydrolysis of silanes and the polymerization of silica sol networks. The volume ratio of water to acid can be 8-12:1, preferably 10:1.

[0051] The acid mentioned includes, but is not limited to, any one or more of concentrated sulfuric acid, nitric acid, and acetic acid.

[0052] In some typical embodiments of the present invention, tetraethoxysilane, γ-aminopropyltriethoxysilane and bi-hydroxyl-terminated silicone oil are added to a solvent, stirred until homogeneous, and then a catalyst is added. The mixture is stirred at 50-70°C for 8-12 h and then allowed to stand for aging for 2-4 h to obtain a silica sol network solution.

[0053] In some typical embodiments of the present invention, the epoxy resin-silica sol interpenetrating network material, as an intermediate layer, can be prepared on any substrate by methods such as spraying, spin coating, and dip coating. This material possesses excellent mechanical properties and stability, effectively improving the hydrophobic and antifouling properties of liquid-like coatings, and can meet the application requirements in complex environments.

[0054] In some typical embodiments of the present invention, the substrate is pretreated using methods such as plasma treatment, ultraviolet light irradiation, piranha solution treatment, and alkali treatment to introduce active hydroxyl groups. The appropriate treatment method is selected based on the substrate material. After substrate pretreatment, the prepolymerization solution is then coated onto the substrate.

[0055] In some typical embodiments of the present invention, a prepolymer solution is applied to a substrate, then heated and cured at 80~120°C for 1~3 hours, and washed with water multiple times to obtain an epoxy resin-silica sol interpenetrating network material.

[0056] A third typical embodiment of the present invention provides an application of the epoxy resin-silica sol interpenetrating network material described above or the epoxy resin-silica sol interpenetrating network material prepared by the preparation method described above in the construction of liquid-like coatings.

[0057] A fourth typical embodiment of the present invention provides a method for constructing a liquid-like coating, comprising: An intermediate layer is constructed on the surface of the substrate, wherein the intermediate layer is the epoxy resin-silica sol interpenetrating network material described above or the epoxy resin-silica sol interpenetrating network material prepared by the preparation method described above. The intermediate layer surface is activated, and then a liquid-like coating slurry is coated on its surface and cured to obtain the liquid-like coating.

[0058] In some typical embodiments of the present invention, the surface of the intermediate layer is first activated using methods such as plasma treatment. Then, dimethyldimethoxysilane and perfluorosilane are mixed at a certain mass ratio and diluted to a mass fraction of 5% to 20% with organic solvents such as ethanol and isopropanol. An appropriate amount of acid or alkali is then added as a catalyst to prepare a mixed solution. The mixed solution is uniformly coated onto the surface of the intermediate layer using methods such as spraying, spin coating, or dip coating. Subsequently, the coated sample is dried in an environment of 10 to 50°C. After drying, the sample is washed sequentially with deionized water and ethanol, and finally dried to obtain a liquid-like coating constructed with the assistance of epoxy resin-silica sol interpenetrating network material.

[0059] The epoxy resin-silica sol interpenetrating network material developed in this invention can bond with any substrate surface, providing active sites for the grafting of liquid-like coatings, and greatly increasing the application range of liquid-like coatings.

[0060] This invention combines an epoxy resin network and a silica sol network through a dual mechanism of physical interpenetrating network and chemical crosslinking to prepare a liquid-like coating intermediate layer with high mechanical properties and stability. Compared with silica sol coatings prepared by the traditional sol-gel method, the intermediate layer prepared by this invention has higher bonding strength (≥15 MPa) and pencil hardness (≥6H). Simultaneously, this invention innovatively adds bi-hydroxyl-terminated silicone oil to the silica sol network, allowing it to act as a "spring," buffering stress within the silica sol network, reducing its brittleness, and improving its film-forming properties and mechanical properties. This allows for the preparation of a thicker intermediate layer, thus providing better wear resistance. During heating, the bi-hydroxyl-terminated silicone oil migrates to the coating surface, further increasing the silicon content on the coating surface and providing more active sites for the construction of the liquid-like coating. The resulting liquid-like coating exhibits better hydrophobic properties (20 μL water sliding angle ≤5°, 10 μL n-hexadecane sliding angle ≤3°) and corrosion resistance (corrosion current density ≤10). -6 A / cm 2 It exhibits excellent anti-icing properties (ice adhesion reduction ≥92.5%) and easy-to-clean properties. Furthermore, compared to traditional silica sol coatings, the epoxy resin-silica sol interpenetrating network material prepared in this invention does not crack after prolonged immersion in water, making it suitable for high humidity or underwater environments.

[0061] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below with reference to specific embodiments.

[0062] Example 1 This embodiment provides an epoxy resin-silica sol interpenetrating network material, using an iron sheet as the matrix material, on which an epoxy resin-silica sol interpenetrating network material is prepared and a liquid-like coating is constructed. Specifically: After polishing, the iron sheet was placed in deionized water and anhydrous ethanol respectively, and ultrasonically treated for 10 minutes each time. It was then removed and dried. The dried iron sheet was then subjected to plasma treatment for 15 minutes to activate its surface.

[0063] Mix 1 mL of water and 10 mL of anhydrous ethanol evenly, then add 1 mL of tetraethoxysilane, 1 mL of γ-aminopropyltriethoxysilane and 0.1 mL of hydroxyl-terminated silicone oil, stir evenly, then add 0.1 mL of concentrated sulfuric acid, stir the mixture at 60 °C for 10 h, and then let it stand for 3 days to obtain a silica sol network solution.

[0064] Add 10% of epoxy resin E-51 by mass of silane to the silica sol network solution. After the epoxy resin dissolves, add 25% of polyetheramine D300 by mass of epoxy resin. After stirring evenly, a silica sol / epoxy resin interpenetrating network solution is obtained.

[0065] The above interpenetrating network solution was dropped onto the surface of the plasma-activated iron sheet, and the solution was homogenized at 2000 rpm for 8 seconds using a spin coater. After heating at 120°C for 2 hours, an epoxy resin / silica sol interpenetrating network intermediate layer was obtained, namely epoxy resin-silica sol interpenetrating network material.

[0066] An iron sheet with an epoxy resin / silica sol interpenetrating network intermediate layer was plasma-treated for 15 min and then immersed in a liquid-like coating prepolymer solution (obtained by uniformly mixing 10 mL isopropanol, 1 mL dimethyldimethoxysilane, and 0.1 mL concentrated sulfuric acid). After removal, it was cured at 30°C for 20 min and then washed sequentially with deionized water and isopropanol. After cleaning, it was removed and dried at room temperature to obtain a liquid-like coating constructed with the assistance of epoxy resin-silica sol interpenetrating network material.

[0067] Example 2 This embodiment provides an epoxy resin-silica sol interpenetrating network material, using an iron sheet as the matrix material, on which an epoxy resin-silica sol interpenetrating network material is prepared and a liquid-like coating is constructed. Specifically: After polishing, the iron sheet was placed in deionized water and anhydrous ethanol respectively, and ultrasonically treated for 10 minutes each time. It was then removed and dried. The dried iron sheet was then subjected to plasma treatment for 15 minutes to activate its surface.

[0068] Mix 10 mL of water and 10 mL of anhydrous ethanol evenly, then add 5 mL of tetraethoxysilane, 5 mL of γ-aminopropyltriethoxysilane and 0.2 mL of hydroxyl-terminated silicone oil. After stirring evenly, add 0.5 mL of concentrated sulfuric acid. Stir the mixture at 60 °C for 10 h, and then let it stand for 3 days to obtain a silica sol network solution.

[0069] Add epoxy resin E-51, accounting for 80% of the silane mass, to the silica sol network solution. After the epoxy resin dissolves, add polyetheramine D300, accounting for 25% of the epoxy resin mass. After stirring evenly, a silica sol / epoxy resin interpenetrating network solution is obtained.

[0070] The above interpenetrating network solution was dropped onto the surface of the plasma-activated iron sheet, and the solution was homogenized at 2000 rpm for 8 seconds using a spin coater. Then, it was heated at 120°C for 2 hours to obtain the epoxy resin / silica sol interpenetrating network intermediate layer, i.e., epoxy resin-silica sol interpenetrating network material.

[0071] After plasma treatment for 15 minutes, an iron sheet with an epoxy resin / silica sol interpenetrating network intermediate layer was immersed in a liquid-like coating prepolymer solution (obtained by uniformly mixing 10 mL isopropanol, 1 mL dimethyldimethoxysilane, and 0.1 mL concentrated sulfuric acid). After removal, it was cured at 30°C for 20 minutes. Then, it was washed sequentially with deionized water and isopropanol. After cleaning, it was removed and dried at room temperature to obtain a liquid-like coating constructed with the assistance of epoxy resin-silica sol interpenetrating network material.

[0072] Example 3 This embodiment provides an epoxy resin-silica sol interpenetrating network material, using an iron sheet as the matrix material, on which an epoxy resin-silica sol interpenetrating network material is prepared and a liquid-like coating is constructed. Specifically: After polishing, the iron sheet was placed in deionized water and anhydrous ethanol respectively, and ultrasonically treated for 10 minutes each time. It was then removed and dried. The dried iron sheet was then subjected to plasma treatment for 15 minutes to activate its surface.

[0073] Mix 5 mL of water and 10 mL of anhydrous ethanol evenly, then add 2.5 mL of tetraethoxysilane, 2.5 mL of γ-aminopropyltriethoxysilane and 0.15 mL of hydroxyl-terminated silicone oil. After stirring evenly, add 0.25 mL of concentrated sulfuric acid. Stir the mixture at 60 °C for 10 h, and then let it stand for 3 days to obtain a silica sol network solution.

[0074] Add 40% of the silane mass of epoxy resin E-51 to the silica sol network solution. After the epoxy resin dissolves, add 25% of the epoxy resin mass of polyetheramine D300. Stir evenly to obtain a silica sol / epoxy resin interpenetrating network solution.

[0075] The above interpenetrating network solution was dropped onto the surface of the plasma-activated iron sheet, and the solution was homogenized at 2000 rpm for 8 seconds using a spin coater. After heating at 120°C for 2 hours, an epoxy resin / silica sol interpenetrating network intermediate layer was obtained, namely epoxy resin-silica sol interpenetrating network material.

[0076] An iron sheet with an epoxy resin / silica sol interpenetrating network intermediate layer was plasma-treated for 15 min and then immersed in a liquid-like coating prepolymer solution (obtained by uniformly mixing 10 mL isopropanol, 1 mL dimethyldimethoxysilane, and 0.1 mL concentrated sulfuric acid). After removal, it was cured at 30°C for 20 min and then washed sequentially with deionized water and isopropanol. After cleaning, it was removed and dried at room temperature to obtain a liquid-like coating constructed with the assistance of epoxy resin-silica sol interpenetrating network material.

[0077] Example 4 This embodiment provides an epoxy resin-silica sol interpenetrating network material, using sandpaper, wood chips, copper alloy, aluminum alloy, ABS plastic, acrylic, Teflon, and PET plastic as matrix materials. An epoxy resin-silica sol interpenetrating network material is prepared on the surface of these materials to assist in constructing a liquid-like coating. The preparation method is completely consistent with that of Example 1.

[0078] Comparative Example 1 This comparative example provides an epoxy resin-silica sol interpenetrating network material, using an iron sheet as the matrix material. An epoxy resin-silica sol interpenetrating network material is prepared on its surface to assist in the construction of a liquid-like coating. The preparation method differs from Example 1 in that: 1 mL of water and 10 mL of anhydrous ethanol are mixed uniformly, then 2 mL of tetraethoxysilane and 0.1 mL of hydroxyl-terminated silicone oil are added. After stirring evenly, 0.1 mL of concentrated sulfuric acid is added. The mixture is stirred at 60°C for 10 h, and then allowed to stand for 3 days to obtain a silica sol network solution. The remaining steps are completely consistent with Example 1.

[0079] Comparative Example 2 This comparative example provides an epoxy resin-silica sol interpenetrating network material, using an iron sheet as the matrix material. An epoxy resin-silica sol interpenetrating network material is prepared on its surface to assist in the construction of a liquid-like coating. The preparation method differs from Example 1 in that: 1 mL of water and 10 mL of anhydrous ethanol are mixed uniformly, then 2 mL of γ-aminopropyltriethoxysilane and 0.1 mL of hydroxyl-terminated silicone oil are added. After stirring evenly, 0.1 mL of concentrated sulfuric acid is added, and the mixture is stirred at 60°C for 10 h, then allowed to stand for 3 days to obtain a silica sol network solution. The remaining steps are completely consistent with Example 1.

[0080] Comparative Example 3 This comparative example provides an epoxy resin / silica sol interpenetrating network material, using an iron sheet as the matrix material. An epoxy resin-silica sol interpenetrating network material is prepared on its surface to assist in constructing a liquid-like coating. The preparation method differs from Example 1 in that: 1 mL of water and 10 mL of anhydrous ethanol are mixed uniformly, then 1.05 mL of tetraethoxysilane and 1.05 mL of γ-aminopropyltriethoxysilane are added, and after stirring evenly, 0.1 mL of concentrated sulfuric acid is added. The mixture is stirred at 60°C for 10 h, and then allowed to stand for 3 days to obtain a silica sol network solution. The remaining steps are completely consistent with Example 1.

[0081] Comparative Example 4 This comparative example provides a conventional silica sol interlayer material using an iron sheet as the substrate. A conventional silica sol material is prepared on the surface of the iron sheet to assist in constructing a liquid-like coating. The preparation method differs from Example 1 in that: 1 mL of water and 10 mL of anhydrous ethanol are uniformly mixed, then 1 mL of tetraethoxysilane is added, and after stirring until homogeneous, 0.1 mL of concentrated sulfuric acid is added. The mixture is stirred at 60°C for 10 h, and then allowed to stand for 3 days to obtain a silica sol network solution. The silica sol is directly coated onto the plasma-activated iron sheet surface and cured by heating. The remaining steps are completely consistent with Example 1.

[0082] Performance verification The performance of the materials and coatings obtained in the examples and comparative examples was verified.

[0083] 1. Hydrophobic effect The static contact angle of the sample was quantitatively analyzed using a contact angle analyzer (CAM101, KSV Instruments, Finland) with a droplet volume of 5 μL. The sliding angle was evaluated using the tilt stage method, which involved systematically increasing the tilt angle of the substrate until the droplet began to move, with a droplet volume of 20 μL.

[0084] 2. Anti-inking effect Stamp the sample surface with the logo, observe the coverage of the oil film on the sample surface, and then wipe the sample surface with a non-woven cloth to evaluate the ink residue on the sample surface.

[0085] 3. Anti-corrosion effect Salt spray tests were conducted on the samples using a salt spray chamber. The salt spray solution was a 3.5% (w / w) NaCl aqueous solution, and the test temperature was 50℃ for 7 days. The corrosion voltage (E) of different samples was measured using an electrochemical workstation in a 3.5 wt% NaCl aqueous solution. corr ) and corrosion current density (I corr The experiment used a standard three-electrode system: a platinum sheet as the counter electrode, a saturated Ag / AgCl electrode as the reference electrode, and the sample as the working electrode, with an exposure area of ​​1 cm² for each electrode. 2 .

[0086] 4. Optical performance The light transmittance and haze of the sample were tested using a spectrophotometer to evaluate its optical performance.

[0087] 5. Morphological Analysis The microstructure of the coating was obtained using a scanning electron microscope, and the silicon element distribution in the coating cross section was obtained using an energy dispersive spectrometer.

[0088] 6. Water resistance test The water resistance of the coating was evaluated by comparing the changes in the contact angle before and after immersion in water for seven days.

[0089] 7. Anti-icing performance test A copper alloy ring (2 cm high, 2 cm inner diameter) was placed on the surface of a 5 cm diameter sample. Then, 5 mL of deionized water was added to the copper ring, and the sample was cooled to -18°C until the deionized water was completely frozen. After freezing, the sample was moved to room temperature for adhesion testing.

[0090] 8. Mechanical property testing The tensile strength and elongation at break of the coating were tested using a universal electronic testing machine. Tensile specimens were prepared using a polytetrafluoroethylene template with a gauge length of 20 mm and a width of 5 mm. The clamping speed was 15 mm / min. Adhesion strength was tested according to ISO 4624 standard.

[0091] like Figure 1 As shown, the liquid-like coatings constructed with the help of epoxy resin-silica sol interpenetrating network materials on different substrate surfaces obtained in Example 4 have the same hydrophobic effect. The material surface with the liquid-like coating has basically no solution residue, which proves that the liquid-like coating has a good hydrophobic effect.

[0092] Figure 2 This study demonstrates the ink-resistant effect of the liquid-like coating constructed with the epoxy resin-silica sol interpenetrating network material on the iron sheet surface obtained in Example 1. The results show that the uncoated iron sheet has a large ink coverage area, and ink residue remains after wiping, while the coated iron sheet has a small ink coverage area, and no ink residue remains after wiping.

[0093] Figure 3 This study examines the anti-corrosion effect of the liquid-like coating constructed with the epoxy resin-silica sol interpenetrating network material on the iron sheet surface obtained in Example 1. The results show that, after salt spray testing, severe corrosion appeared on the uncoated iron sheet surface on the first day, while the coated surface only showed minor pitting corrosion on the seventh day, demonstrating the coating's superior anti-corrosion effect.

[0094] Figure 4 The electrochemical corrosion test results show the liquid-like coating constructed with the help of epoxy resin-silica sol interpenetrating network material on the iron sheet surface obtained in Example 1. The results show that the corrosion voltage and corrosion current of the coated sample are significantly lower than those of the uncoated sample, proving that the coating has excellent anti-corrosion effect.

[0095] Figure 5 The sliding angles of hexadecane and water droplets on the liquid-like coating assisted by the epoxy resin-silica sol interpenetrating network material on the iron sheet surface obtained in Example 1 are shown. The results indicate that the sliding angle of 10 μL hexadecane on the coated sample is ≤3° and the sliding angle of 20 μL water is ≤5°, demonstrating that the coating has excellent dynamic hydrophobic properties.

[0096] Figure 6 This study demonstrates the anti-icing effect of the liquid-like coating constructed with the epoxy resin-silica sol interpenetrating network material on the iron sheet surface obtained in Example 1. The results show that, compared to the uncoated sample, the ice shear force on the surface of the coated sample is reduced by 92.5%, proving that the coating has excellent anti-icing properties.

[0097] Figure 7 The optical properties of the liquid-like coating constructed with the assistance of the epoxy resin-silica sol interpenetrating network material on the PET plastic surface obtained in Example 1 are shown. The results indicate that both the uncoated and coated PET plastics have high transparency, and the coated PET plastic has higher transmittance in the visible light range than the uncoated PET plastic, with a haze of less than 0.01%, demonstrating that the epoxy resin-silica sol interpenetrating network material developed in this invention has excellent optical properties.

[0098] Figure 8 SEM images of the surface (a) and cross-section (b) of the epoxy resin-silica sol interpenetrating network material obtained in Example 1, and the silicon element distribution (c). The results show that the epoxy resin-silica sol interpenetrating network material has a high degree of smoothness and good uniformity, and the coating thickness is about 3 μm. At the same time, the addition of double-terminated hydroxyl silicone oil can also effectively increase the silicon element content on the surface of the intermediate layer.

[0099] Figure 9 This study compares the water resistance of the conventional silica sol intermediate layer obtained in Comparative Example 4 with the liquid-like coating constructed with the epoxy resin-silica sol interpenetrating network material obtained in Example 1 of this invention. The results show that the conventional silica sol coating rapidly decreased in contact angle and failed after one day of immersion, while the liquid-like coating constructed with the epoxy resin-silica sol interpenetrating network material of this invention maintained a high water contact angle even after seven days of immersion, demonstrating better water resistance.

[0100] Figure 10 This study compares the mechanical properties of the conventional silica sol interlayers obtained in Comparative Examples 1, 2, and 3 with the epoxy resin-silica sol interpenetrating network material obtained in Example 1 of this invention. The results show that, compared to Comparative Example 1, the epoxy resin-silica sol interpenetrating network material of this invention exhibits higher adhesion strength; compared to Comparative Example 2, the epoxy resin-silica sol interpenetrating network material of this invention exhibits higher hardness; and compared to Comparative Example 3, the epoxy resin-silica sol interpenetrating network material of this invention exhibits higher flexibility, demonstrating better mechanical properties.

[0101] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method of constructing a quasi-liquid coating, characterized by, include: An intermediate layer is constructed on the surface of the substrate, wherein the intermediate layer is an epoxy resin-silica sol interpenetrating network material; The intermediate layer surface is activated, and then a liquid-like coating slurry is coated on its surface and cured to obtain a liquid-like coating. The epoxy resin-silica sol interpenetrating network material comprises the following raw materials in parts by weight: 1 part silica sol, 0.1-0.8 parts epoxy resin, and 0.025-0.2 parts amine curing agent. The silica sol is polymerized from tetraethoxysilane, γ-aminopropyltriethoxysilane and hydroxyl-terminated silicone oil; the volume ratio of tetraethoxysilane, γ-aminopropyltriethoxysilane and hydroxyl-terminated silicone oil is (1~5):(1~5):(0.1~0.2); In the epoxy resin-silica sol interpenetrating network material, the epoxy resin network and the silica sol network interpenetrate and crosslink, and the amino groups in the silica sol network chemically crosslink with the epoxy groups in the epoxy resin network to form a stable covalent bond. After the epoxy resin-silica sol interpenetrating network material is bonded to the substrate, the bonding strength is ≥15 MPa and the pencil hardness is ≥6 H. The preparation method of the epoxy resin-silica sol interpenetrating network material includes: Tetraethoxysilane, γ-aminopropyltriethoxysilane and double-terminated hydroxyl silicone oil were added to the solvent, stirred well, and then the catalyst was added. The mixture was stirred at 50-70°C for 8-12 h, and then allowed to stand and age for 2-4 days to obtain a silica sol network solution. Epoxy resin and amine curing agent are added to a silica sol network solution and stirred at a certain temperature to obtain a prepolymer solution; The prepolymer solution is applied to the substrate and cured to obtain an epoxy resin-silica sol interpenetrating network material.

2. The method of constructing a quasi-liquid coating of claim 1, wherein, The epoxy resin includes any one of epoxy resin E-51 and epoxy resin E-44.

3. The method of constructing a quasi-liquid coating of claim 1, wherein, The amine curing agent is polyetheramine.

4. The method of constructing a quasi-liquid coating of claim 1, wherein, The solvent is an alcohol-based solvent; The catalyst is water and acid.

5. The method of constructing a quasi-liquid coating of claim 4, wherein, The acid includes any one or more of concentrated sulfuric acid, nitric acid, and acetic acid.

6. The application of epoxy resin-silica sol interpenetrating network material in the construction of liquid-like coating in the method for constructing liquid-like coating according to claim 1.

Citation Information

Patent Citations

  • Preparation method of silicon dioxide / epoxy resin inorganic-organic hybrid adhesive

    CN115181524A