Method for determining mineral content in coke-containing metallurgical slag for titanium extraction

CN123028862APending Publication Date: 2026-11-03PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611235625.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-03

AI Technical Summary

Technical Problem

现有技术难以准确检测含焦炭提钛冶金渣中的矿物组成,尤其是焦炭含量,导致检测结果不准确。

Method used

Coke and mineral particles were separated by density sorting using high-density zinc chloride or potassium iodide aqueous solution. The mineral composition was detected by a mineral analyzer, and the content of coke and other minerals was obtained through centrifugation, drying and rinsing steps.

Benefits of technology

It enables accurate determination of the mineral composition in coke-containing titanium extraction slag, improving the reliability and precision of the detection and meeting the needs of process parameter adjustment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123028862A_ABST
    Figure CN123028862A_ABST
Patent Text Reader

Abstract

The application discloses a method for measuring mineral content in coke-containing titanium-extracting metallurgical slag and belongs to the technical field of analysis and detection. In order to realize accurate measurement of the mineral content in the coke-containing titanium-extracting metallurgical slag, the application provides a method for measuring the mineral content in the coke-containing titanium-extracting metallurgical slag, which comprises the following steps: placing the coke-containing titanium-extracting metallurgical slag powder in a zinc chloride or potassium iodide aqueous solution, performing centrifugal drying, obtaining the proportion of coke content, filtering, rinsing and drying the solid-liquid mixture after the coke is separated, obtaining the proportion of residual solid phase content, and then using a mineral analyzer to detect the component types and content of the residual solid phase, and finally obtaining the composition and content of the minerals in the coke-containing titanium-extracting metallurgical slag after conversion. The application realizes accurate measurement of the carbon content and component conditions in the coke-containing titanium-extracting metallurgical slag, and has a positive significance for judging the progress of metallurgical reactions and improving the process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of analytical testing technology, specifically relating to a method for determining the mineral content in titanium extraction slag containing coke. Background Technology

[0002] Coke, as a key raw material in the metallurgical industry, plays an irreplaceable role in processes such as blast furnace ironmaking, titanium extraction from blast furnace slag, and high-temperature chlorination. In blast furnace ironmaking, coke serves as the main heat source and reducing agent, while also adjusting the composition of molten iron; generally, no coke residue is found in the metallurgical blast furnace slag. However, in titanium extraction processes, such as titanium extraction from blast furnace slag and high-temperature chlorination, an excessive amount of coke is usually added to ensure complete reaction. This results in varying amounts of residual coke in the metallurgical slag products after the reaction, such as carbide slag and chlorinated slag. This type of coke exists primarily in a free form, meaning it has a high degree of dissociation. For example, coke particles of varying sizes are commonly found in metallurgical slags such as molten salt chlorination slag, fluidized bed chlorination slag, SR synthetic rutile selective chlorination slag, and carbide slag, and are basically not adhered to other minerals. The raw materials for this type of metallurgical slag are generally titanium-rich materials, titanium slag, titanium concentrate, blast furnace slag, etc. The mineral composition is mainly rutile, diatomite, silicate minerals, perovskite, and ilmenite. The phases in the chlorinated slag after high-temperature chlorination are generally mainly residual diatomite, rutile, silicate minerals, and coke, while the phases in the carbide slag are generally mainly titanium nitride, pyroxene, perovskite, and coke. The coke in this type of titanium extraction metallurgical slag is not entirely crystalline; amorphous coke is also common. It is precisely because of the presence of amorphous material that accurate quantitative analysis of its mineral composition using XRD is often impossible.

[0003] Even when using existing mineral analyzers to detect its composition, complete quantification is not possible. The results generally do not include the composition and content of coke. This is because the grayscale value of the epoxy resin background of the solidified sample under electron beam electron microscopy is very close to that of coke. Therefore, mineral analysis software automatically subtracts it as background during data acquisition, resulting in the omission of coke composition in the final result. However, researchers often need to obtain information on the composition and content of all minerals in the sample to better assess the progress of the reaction and determine whether relevant process parameters need to be adjusted. But the results obtained from actual tests are often inaccurate.

[0004] Therefore, it is necessary to develop a method that can accurately detect the mineral content of titanium extraction slag containing coke. Summary of the Invention

[0005] The purpose of this invention is to provide a method for determining the mineral content in titanium extraction slag containing coke, so as to obtain the accurate mineral composition of such samples.

[0006] To achieve the above objectives, the present invention provides a method for determining the mineral content in titanium extraction slag containing coke, comprising the following steps:

[0007] A. The titanium extraction slag containing coke is crushed and ground to obtain a powder sample;

[0008] B. Prepare a zinc chloride aqueous solution with a mass fraction of 61-68% or a potassium iodide aqueous solution with a mass fraction of 58-60%.

[0009] C. Weigh an appropriate amount of powder sample, record the mass as m, place it in zinc chloride aqueous solution or potassium iodide aqueous solution, stir thoroughly, centrifuge, and after centrifugation, let it stand until no coke floats in the mixed solution.

[0010] D. Separate the coke particles, dry them and record their mass m1. The coke content in the sample is a = m1 / m × 100%.

[0011] E. Filter the solid-liquid mixture after separating the coke and rinse it with water until no white precipitate is produced after titrating the washing solution with silver nitrate solution.

[0012] F. Dry the residual solids after rinsing to obtain dried residual solids. The percentage of residual solids in the sample is b = (m - m1) / m × 100%.

[0013] G. Prepare a reflective light sheet from the dried residual solids and use a mineral analyzer to detect the types and contents of mineral components in the dried residual solids;

[0014] H. Incorporate the types and contents of mineral components in the dried residual solids into the content ratio b of the residual solids in the sample to obtain the composition and content of minerals other than coke in the coke-containing titanium extraction slag. Add the coke content ratio a to obtain the composition and content of minerals in the coke-containing titanium extraction slag.

[0015] In the above determination method, in step A, the particle size of the powder sample is 0.15~0.25mm.

[0016] In the above determination method, in steps A and C, the centrifugation time is 5-10 minutes.

[0017] In the above determination method, in steps A and C, the centrifugation speed is 2000~4000 r / min.

[0018] In the above determination method, in step A and step C, the ratio of zinc chloride aqueous solution or potassium iodide aqueous solution to powder sample is 200 mL: 15~25 g.

[0019] In the above-mentioned determination method, in steps A and D, the drying temperature is 100~120℃.

[0020] In the above-mentioned measurement method, in steps A and E, the temperature of the water used for rinsing is 50~90℃.

[0021] In the above determination method, in step A and step F, the drying temperature is 100~120℃.

[0022] In the above-mentioned determination method, step A, the titanium-extracting slag containing coke is titanium-extracting slag produced by high-temperature carbonization of blast furnace slag, high-temperature chlorination process, or selective chlorination process of SR artificial rutile.

[0023] In the above determination method, step A, the mineral components in the titanium extraction slag containing coke include coke, rutile, ilmenite, pyroxene, quartz, feldspar, and zeolite.

[0024] The beneficial effects of this invention are:

[0025] This invention provides a novel method for detecting the mineral content in coke-containing titanium extraction slag samples. This method is highly feasible and operable, and can better determine the accurate mineral composition of this type of slag sample and accurately measure the carbon content in the titanium extraction slag. This method is of positive significance for judging the extent of metallurgical chemical reactions and improving related processes. Attached Figure Description

[0026] Figure 1 This is an electron micrograph of coke in a titanium extraction slag sample containing coke.

[0027] Figure 2 This is a diagram of the apparatus used in this invention to determine the mineral content in titanium extraction slag containing coke. Detailed Implementation

[0028] Specifically, a method for determining the mineral content in coke-containing titanium extraction slag includes the following steps:

[0029] Step 1: Crush and grind the coke-containing titanium extraction slag to 0.15~0.25mm to obtain the corresponding powder sample. In this invention, the coke-containing titanium extraction slag mainly comes from titanium extraction processes, such as the high-temperature carbonization process of blast furnace slag, the high-temperature chlorination process, and the selective chlorination process of SR synthetic rutile, etc., and includes related titanium extraction slags such as carbide slag and chlorination slag. Typical electron micrographs are shown below. Figure 1 As mentioned above, since the titanium extraction slag containing coke contains carbide slag, and the carbide slag contains carbon-containing mineral titanium carbide in addition to free coke, it is impossible to obtain accurate coke content data by combustion method. Based on this, the present invention adopts density sorting method, which is more suitable for titanium extraction slag with a wider sample coverage.

[0030] Step 2: Prepare a zinc chloride aqueous solution with a mass fraction of 61-68% or a potassium iodide aqueous solution with a mass fraction of 58-60%. The basic separation principle in this invention is density separation flotation, utilizing the density difference between coke particles, mineral particles, and the zinc chloride / potassium iodide aqueous solution. The apparent density of the free coke (apparent density is used instead of true density because coke contains a large number of pores) is 0.88-1.08 g / cm³. 3 The mineral density is generally greater than 2.55 g / cm³. 3 The density of a 61-68% zinc chloride solution is 1.84-1.98 g / cm³. 3 A 58-60% potassium iodide solution has a density of 1.71-1.75 g / cm³. 3 The critical density range for sorting is 1.70~2.00 g / cm³. 3 The heavy liquid must be able to stably achieve the required density. The apparent density of coke differs significantly from that of the minerals and the zinc chloride or potassium iodide solution, and their density range meets the critical density range requirements for separation. In a selected mass fraction of zinc chloride or potassium iodide aqueous solution, coke floats while the minerals sink, thus achieving separation. Based on this, this invention selects zinc chloride or potassium iodide, which have extremely high solubility, and prepares them into a high-density, transparent aqueous solution of a specific concentration. This water-based heavy liquid does not dissolve carbonaceous coke, and the solution can be appropriately diluted with water. The density is continuously adjustable. Compared to toxic heavy liquids (such as diiodomethane), inorganic salt heavy liquids are less toxic and less expensive. Furthermore, the maximum saturated density of nickel chloride and potassium chloride is less than 1.70, which is insufficient to meet the required separation density.

[0031] Step 3: Weigh an appropriate amount of powder sample, record the mass as m, and place it in a zinc chloride solution or potassium iodide solution. The ratio of zinc chloride solution or potassium iodide solution to powder sample is 200 mL: 15~25 g. After stirring thoroughly, centrifuge for 5~10 min at a speed of 2000~4000 r / min. After centrifugation, let it stand until no coke floats to the surface in the mixed solution.

[0032] Step 4: Separate the coke particles, dry them at 100~120℃ and record their mass m1. The coke content percentage in the sample is a = m1 / m × 100%. In this invention, the floating coke can be separated from the system in the following way: Insert a 5~10ml wide-mouth Pasteur dropper (with an inner diameter of about 1.2~1.6mm at the tip) into the coke suspension layer below the liquid surface, slowly aspirate the floating coke and the upper zinc chloride or potassium iodide solution, transfer it to filter paper, and avoid touching the bottom sediment to prevent residual solids in the system from affecting the coke detection results.

[0033] Step 5: Filter the solid-liquid mixture after separating the coke, and rinse it with a large amount of 50~90℃ deionized water until no white precipitate is produced after titration with silver nitrate solution.

[0034] Step 6: Dry the residual solids after rinsing at 100~120℃ to obtain dried residual solids. The content of residual solids in the sample is b=(m-m1) / m×100%.

[0035] Step 7: Prepare a reflective light sample from the dried residual solids. Use a mineral analyzer to detect the types and contents of mineral components in the dried residual solids, and obtain data on the types and contents of each component in the dried residual solids.

[0036] Step 8: Integration and Calculation - Substitute the data on the types and contents of each component in the obtained dry residual solid into the content ratio b of the residual solid in the entire sample to obtain the components and contents of other minerals besides coke in the coke-containing titanium extraction slag in the entire sample. Add this to the coke content ratio a to obtain the component types and contents of all minerals in the coke-containing titanium extraction slag. The mineral components in the coke-containing titanium extraction slag include coke, rutile, ilmenite, pyroxene, quartz, feldspar, and zeolite.

[0037] Step seven of this invention employs a conventional method in the art for detecting mineral composition and content using a mineral analyzer. The mineral analyzer testing operation and steps are as follows: 1. The residual solid phase from step six is ​​cold-mounted and solidified into a reflective sheet using epoxy resin and a curing agent, and then ground and polished to obtain a qualified reflective sheet sample (the sheet sample diameter is 3cm and the thickness is about 1cm); 2. The sheet sample is subjected to a spray coating treatment, and then the sample is placed in the sample chamber of the mineral analyzer, and the vacuum is drawn to 3×10 -43. After vacuum preparation, apply high voltage to the electron microscope. Select 25kV for the high voltage, 40μA for the current, and 7.40 for the beam spot. Use a copper standard sample to calibrate the background brightness and contrast. Select a background subtraction threshold of approximately 120. 4. Adjust the sample focal length to approximately 10mm. Select an image resolution of 512×400, an electron microscope magnification of 500x, a frame rate of 500 frames or a minimum of 100,000 mineral particles, an energy dispersive spectroscopy (EDS) time parameter of 1.6, an EDS count rate of approximately 75,000, and a dead time of approximately 27. 5. After parameter settings are complete, the equipment will automatically acquire data until it automatically ends. 6. Combine the data obtained from the mineral analyzer's built-in mineral database and conventional metallurgical mineral databases in this field to name the minerals. Finally, the mineral analysis software on the mineral analyzer will calculate the mineral composition and content data. Note: The gray value of coke under an electron microscope is close to that of the sample background—that is, epoxy resin. When the mineral acquisition software performs sample background subtraction, it will directly treat it as the background and subtract it. Therefore, the data obtained by the mineral analyzer test does not contain coke.

[0038] This invention relates to an apparatus for determining the mineral content in titanium extraction slag containing coke. Figure 2 As shown, it is a conventional device in this field and can be built independently.

[0039] The present invention will be explained below with reference to embodiments. Those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be considered as limiting the scope of the invention. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in the art or in accordance with the product manual.

[0040] The starting compounds, raw materials and / or reagents used in the reactions described in this invention can be obtained through legitimate commercial channels or prepared by methods reported in chemical literature.

[0041] Example 1

[0042] Step 1: Crush and grind the titanium extraction slag to 0.15~0.25mm to obtain the corresponding powder sample.

[0043] Step 2: Prepare an appropriate amount of zinc chloride aqueous solution with a mass fraction of 61-68% or potassium iodide aqueous solution with a mass fraction of 59-60%.

[0044] Step 3: Weigh an appropriate amount of powder sample, record the mass as m, and place it in a zinc chloride aqueous solution or potassium iodide aqueous solution. After stirring thoroughly, centrifuge for 5-10 minutes at a speed of 2000-4000 r / min. After centrifugation, let it stand until no coke floats to the surface in the mixed solution.

[0045] Step 4: Separate the coke particles. Insert a 5-10 ml wide-mouth Pasteur dropper (with an inner diameter of about 1.2-1.6 mm at the tip) into the coke suspension layer below the liquid surface, slowly aspirate the floating coke and the upper zinc chloride solution, transfer to filter paper for filtration, dry at 100-120℃ and record its mass m1. The coke content percentage in the sample is a = m1 / m × 100%.

[0046] Step 5: After filtering and separating the coke, the solid-liquid mixture is rinsed with a large amount of deionized water at 50~90℃ until no white precipitate is produced after titration with silver nitrate solution.

[0047] Step Six: Dry the residual solids after rinsing (100~120℃) to obtain dried residual solids. The percentage of residual solids in the sample is b = (m-m1) / m × 100%.

[0048] Step 7: Prepare a reflective light sample from the residual solids and analyze its mineral types and contents using a mineral analyzer to obtain the types and contents of each component in the residual solids.

[0049] Step 8: Integration Calculation—Incorporate the types and contents of each component of the residual solids into the content percentage b of the residual solids in the entire sample to obtain the actual content percentage of other mineral components besides coke in the entire sample. Add this to the coke content percentage a to obtain the composition types and contents of all minerals in the entire sample.

[0050] Application Example 1:

[0051] Adopting such Figure 2 The apparatus diagram shows the process of weighing 20g of a titanium metallurgical slag sample, grinding and mixing it, and then adding 200ml of a 65% zinc chloride solution (density calibrated to 1.90g / cm³ at 20℃). 3 The mixture was stirred thoroughly, centrifuged at 3000 r / min for 8 min, and allowed to stand until no coke floated to the surface. The coke particles were separated, dried at 110℃, and weighed to 1.07 g, indicating a coke content of 5.35% in the sample (a). The residual solid-liquid mixture was rinsed with deionized water at 85℃, and titration with silver nitrate solution confirmed the absence of white precipitate in the washing solution. The residual solid content after drying at 110℃ was 94.65% in the sample (b). The residual solid was prepared into a reflective sheet sample and tested using a mineral analyzer (model: MLA650, manufacturer: FEI Corporation, USA) to obtain coke-free mineral composition data (Table 1). All data were integrated and processed to obtain the final mineral composition of the titanium extraction slag sample (Table 1).

[0052] Table 1. Mineral composition and content (%) of titanium extraction slag

[0053]

[0054] Based on the sample coke content of 5.35% measured in Table 1, this was recorded as the background coke content. Using this as a blank control, three spiking gradients were set up from low to high, with added coke mass fractions of 1.5%, 3.0%, and 4.5%, respectively, so that the theoretical total coke mass fractions after spiking were 6.85%, 8.35%, and 9.85%, respectively. Three parallel experiments were set up for each spiking group.

[0055] Experimental Procedure: 1. Take an appropriate amount of the original sample, grind it to 0.15~0.25mm and mix thoroughly for later use. 2. Accurately weigh 20g of the original sample prepared in step 1 into nine groups, and mix it with coke standard samples (0.3221g, 0.6547g, 0.9983g) according to the set spiking gradient. Grind to 0.15~0.25mm and mix thoroughly to ensure homogeneity and no segregation. Prepare three gradient spiking samples. 3. Conduct the test on the spiked samples according to the above operation method, and measure the total coke content in each spiked sample. 4. Perform three parallel tests for each spiking gradient, and take the average value as the measured value of each group. 5. Coke recovery rate calculation formula: Coke recovery rate (%) = [(20g + spiking amount) × measured total coke content after spiking - 1.07g)] / spiking amount × 100%. 6. Criteria for acceptance: Referring to the industry standard for spiked recovery rate of solid mineral samples (DZ / T 0130.3-2006 "Quality Management Specifications for Geological and Mineral Laboratory Testing Part 3: Chemical Composition Analysis of Rock and Mineral Samples"): Major components (mass fraction 1~10%): 90%~110%. If the result is within this range, it indicates that the test method used in this invention is accurate in quantifying coke, has no systematic bias, and is reliable.

[0056] Experimental Results: 1. With a spiked amount of 0.3221g, the measured total coke content after spiked addition was 6.81%. Therefore, the coke recovery rate = [(20g + 0.3221g) × 6.81% - 1.07g)] / 0.3221g × 100% = 97.5%. 2. With a spiked amount of 0.6547g, the measured total coke content after spiked addition was 8.33%. Therefore, the coke recovery rate = [(20g + 0.6547g) × 8.33% - 1.07g)] / 0.6547g × 100% = 99.4%. 3. With a spiked amount of 0.9983g, the measured total coke content after spiked addition is 9.79%. Therefore, the coke recovery rate = [(20g + 0.9983g) × 9.79% - 1.07g)] / 0.9983g × 100% = 98.7%. 4. The average coke recovery rate = (97.5% + 99.4% + 98.7%) / 3 = 98.5%. All results fall within the acceptable range of 90-110%, indicating that the results of this invention are accurate and reliable.

[0057] Coke content precision test: 1. Divide the same homogeneous original sample into 6 independent parallel tests. Determine the coke content in each sample independently according to the above procedure, and calculate the average value, standard deviation, and relative deviation. Acceptance criteria: According to DZ / T 0130.3-2006 and GB / T 20899.9-2025, for constant component content of 1~10%, an acceptable RSD ≤ 3.0% is considered acceptable. For high-precision quantitative analysis, an RSD ≤ 2.0% is generally required.

[0058] The measured results of coke content are shown in Table 2.

[0059] Table 2. Results of Coke Content Detection / %

[0060]

[0061] Calculate the average value =5.34%, standard deviation S=0.0498, RSD=0.93%. The results show that the relative standard deviation of the parallel test of the whole process of the present invention is 0.93%, which is less than the industry allowable error threshold of 3.0% and also less than the error threshold of 2.0% required for high-precision quantification. This indicates that the present invention has good repeatability, small random error and reliable precision for coke content detection.

Claims

1. A method for determining the mineral content in titanium extraction slag containing coke, characterized in that: Includes the following steps: A. The titanium extraction slag containing coke is crushed and ground to obtain a powder sample; B. Prepare a zinc chloride aqueous solution with a mass fraction of 61-68% or a potassium iodide aqueous solution with a mass fraction of 58-60%. C. Weigh an appropriate amount of powder sample, record the mass as m, place it in zinc chloride aqueous solution or potassium iodide aqueous solution, stir thoroughly, centrifuge, and after centrifugation, let it stand until no coke floats in the mixed solution. D. Separate the coke particles, dry them and record their mass m1. The coke content in the sample is a = m1 / m × 100%. E. Filter the solid-liquid mixture after separating the coke and rinse it with water until no white precipitate is produced after titrating the washing solution with silver nitrate solution. F. Dry the residual solids after rinsing to obtain dried residual solids. The percentage of residual solids in the sample is b = (m-m1) / m × 100%. G. Prepare a reflective light sample from the dried residual solids and use a mineral analyzer to detect the types and contents of mineral components in the dried residual solids; H. Incorporate the types and contents of mineral components in the dried residual solids into the content ratio b of the residual solids in the sample to obtain the composition and content of minerals other than coke in the coke-containing titanium extraction slag. Add the coke content ratio a to obtain the composition and content of minerals in the coke-containing titanium extraction slag.

2. The method for determining the mineral content in coke-containing titanium extraction slag according to claim 1, characterized in that: In step A, the particle size of the powder sample is 0.15~0.25mm.

3. The method for determining the mineral content in coke-containing titanium extraction slag according to claim 1, characterized in that: In step C, the centrifugation time is 5-10 minutes.

4. The method for determining the mineral content in coke-containing titanium extraction slag according to claim 1, characterized in that: In step C, the centrifugation speed is 2000~4000 r / min.

5. The method for determining the mineral content in coke-containing titanium extraction slag according to claim 1, characterized in that: In step C, the ratio of zinc chloride aqueous solution or potassium iodide aqueous solution to powder sample is 200 mL: 15~25 g.

6. The method for determining the mineral content in coke-containing titanium extraction slag according to claim 1, characterized in that: In step D, the drying temperature is 100~120℃.

7. The method for determining the mineral content in coke-containing titanium extraction slag according to claim 1, characterized in that: In step E, the temperature of the water used for rinsing is 50~90℃.

8. The method for determining the mineral content in coke-containing titanium extraction slag according to claim 1, characterized in that: In step F, the drying temperature is 100~120℃.

9. The method for determining the mineral content in coke-containing titanium extraction slag according to claim 1, characterized in that: The titanium-extraction slag containing coke is a titanium-extraction slag produced by high-temperature carbonization, high-temperature chlorination, and selective chlorination of SR artificial rutile.

10. The method for determining the mineral content in coke-containing titanium extraction slag according to claim 1, characterized in that: The mineral components of titanium extraction slag containing coke include coke, rutile, ilmenite, pyroxene, quartz, feldspar, and zeolite.