A method for preparing a binary solid solution and its application as a photothermal catalyst in a reverse water-gas shift reaction.
By using a binary solid solution Ga2-xInxO3 photothermal catalyst with specific composition and morphology, combined with photothermal synergistic process parameters, the problem of insufficient catalytic activity was solved, achieving efficient CO2 conversion and high CO yield, with good long-term stability.
Patent Information
- Application Number
- CN202610734227.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-26
- Publication Date
- 2026-11-10
AI Technical Summary
Existing catalysts have insufficient catalytic activity in the reverse water-gas shift reaction, resulting in low CO yield. Furthermore, traditional thermocatalysis requires high temperature and pressure, leading to high energy consumption. Electrocatalysis and photocatalysis exhibit poor stability and low light energy conversion efficiency, making them difficult to apply industrially.
By using a binary solid solution Ga2-xInxO3 with a specific composition and morphology as a photothermal catalyst, and combining it with specific process parameters, CO2 conversion and CO yield can be improved through photothermal synergy.
It significantly improves the CO2 conversion rate and CO yield in the reverse water-gas shift reaction, while also exhibiting good long-term stability in photothermal catalysis and avoiding catalyst carbon deposition.
Smart Images

Figure CN123059636A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a binary solid solution Ga 2-x In x The preparation method of O3 also involves the binary solid solution Ga obtained by the above method. 2-x In x Application of O3 as a photothermal catalyst in reverse water-gas shift reaction. Background Technology
[0002] With the acceleration of global industrialization, the excessive consumption of fossil fuels has led to a continuous rise in the concentration of carbon dioxide (CO2) in the atmosphere, triggering severe greenhouse effect and climate change problems. Therefore, realizing the resource conversion and emission reduction of CO2 has become a core issue in the global energy and environment field.
[0003] In CO2 hydrogenation technology, traditional thermocatalysis requires high temperature and pressure, resulting in high energy consumption and easy catalyst deactivation. While electrocatalysis and photocatalysis offer milder conditions, they suffer from poor stability and low light energy conversion efficiency, hindering industrial application. Photothermal catalytic CO2 hydrogenation technology, through the synergistic effect of light and heat energy, can reduce energy consumption, regulate reaction pathways, and improve conversion efficiency and stability. Its core advantage lies in achieving light energy capture and conversion using photothermal materials, while simultaneously optimizing reaction kinetics through photogenerated carriers to lower the activation energy barrier.
[0004] Although photothermal catalytic CO2 hydrogenation technology has made some progress, many bottlenecks still exist before its industrial application. Reverse water-gas shift reaction (RWGS) is a core elementary reaction in the CO2 hydrogenation process, laying the foundation for the subsequent synthesis of high-value-added chemicals. Currently, catalysts used in RWGS suffer from insufficient catalytic activity and low CO yield. Summary of the Invention
[0005] Purpose of the invention: The purpose of this invention is to provide a binary solid solution Ga 2-x In x A method for preparing O3; another objective of this invention is to provide a binary solid solution Ga obtained by the above method. 2-x In x The application of O3 as a photothermal catalyst in the reverse water-gas shift reaction: This invention utilizes Ga with a specific composition and morphology. 2-x In x O3, as a photothermal catalyst, works in conjunction with specific process parameters in the photothermal catalysis process to significantly improve the conversion rate of CO2 and the yield of CO in the reverse water-gas shift reaction.
[0006] Technical solution: The binary solid solution Ga of the present invention 2-x In xThe application of O3 as a photothermal catalyst in the reverse water-gas shift reaction is as follows: the binary solid solution Ga... 2-x In x The O3 catalyst is placed in the reaction apparatus, nitrogen gas is introduced into the apparatus, and the apparatus is heated to 400-600°C. At this time, the nitrogen atmosphere is switched to CO2 hydrogenation reduction feed gas, and the xenon lamp is turned on to carry out the RWGS reaction. In the CO2 hydrogenation reduction feed gas, the molar ratio of H2 to CO2 is not less than 4:1; the flow rate of the CO2 hydrogenation reduction feed gas is not less than 60 mL / min; the xenon lamp output current is 10-20 mA, and the reaction is carried out under full-spectrum illumination with a condenser lens; the condenser lens is a φ63mm convex lens with a focal length of 120mm.
[0007] Wherein, the binary solid solution Ga 2-x In x In O3, X takes values from 1.36 to 1.76.
[0008] The binary solid solution Ga 2-x In x O3 was prepared using the following method, with the specific steps as follows:
[0009] (1) Weigh gallium nitrate and indium nitrate according to the stoichiometric ratio. Combine gallium nitrate, indium nitrate and urea (CO(NH2)2, urea decomposes gradually upon heating to release OH-). - This increases the pH of the solution, allowing Ga and In to decompose synchronously and uniformly to form Ga-In hydroxide precursors. The appropriate amount allows urea to decompose at a uniform rate, resulting in a moderate nucleation rate that is more suitable for forming a solid solution. This mixture is added to a mixed solution of diethylene glycol and deionized water and stirred thoroughly to obtain the mixture.
[0010] (2) The mixture from step (1) is subjected to a hydrothermal reaction at high temperature. After the reaction is completed, the resulting solid is centrifuged, washed, and vacuum dried.
[0011] (3) The solid material dried in step (2) is heated in air at 400~450℃ for 2~2.5h to obtain the binary solid solution Ga. 2-x In x O3.
[0012] In step (1), the volume ratio of diethylene glycol to water in the mixed solution is 70~75:4 (adding a trace amount of water to the system is more conducive to the dissolution of urea), and the stirring time is not less than 0.5h.
[0013] In step (2), the hydrothermal reaction temperature is 200~250℃, and the heating time is 22~24h. The number of centrifugal washing cycles is 3~5, the vacuum drying temperature is 60~70℃, and the drying is carried out overnight.
[0014] The method of this invention can obtain binary solid solution catalysts Ga 2-x In x O3, in which Ga and In elements are evenly distributed and remain stable after thermal and photothermal reactions, indicates that its solid solution state is maintained. Under the action of light, dynamic vacancies can be induced to form reaction sites. The accumulation of dynamic defect sites and photogenerated electrons promotes CO2 activation, which is beneficial to the RWGS reaction. At the same time, photoactivation excites reactant molecules, reducing the activation energy required for the reaction process, thus enabling the catalyst in the photothermal system to exhibit superior catalytic performance.
[0015] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: The present invention uses Ga with a specific composition and specific morphology 2-x In x O3, as a photothermal catalyst, works synergistically with specific process parameters in the photothermal catalysis process to significantly improve the conversion rate of CO2 and the yield of CO in the reverse water-gas shift reaction. Meanwhile, long-term stability experiments show that there is no obvious carbon deposition on the catalyst surface during the reaction process, thus it also has good long-term stability in photothermal catalysis. Attached Figure Description
[0016] Figure 1 The binary solid solutions Ga prepared in Examples 1-3 and Comparative Examples 1 and 2 1.76 In 0.24 O3, Ga 1.6 In 0.4 O3, Ga 1.36 In 0.64 The CO yield and CO selectivity of O3 and oxides Ga2O3 and In2O3 under thermal and photothermal reaction systems, respectively; the photothermal reaction conditions were: 500℃, 10h, WHSV = 24000mL / g / h, H2 / CO2 = 4, P = 0.1MPa, and light intensity of 2.38W / cm². 2 ;
[0017] Figure 2 The binary solid solution Ga prepared in Example 2 1.6 In 0.4 The long-term stability of O3 in a photothermal reaction system was tested. The photothermal reaction conditions were: 500℃, 50h, WHSV = 24000mL / g / h, H2 / CO2 = 4, P = 0.1MPa, and light intensity of 2.38W / cm². 2 ;
[0018] Figure 3 The binary solid solutions Ga prepared in Examples 1, 3 and Comparative Examples 1 and 2 1.76 In 0.24O3, Ga 1.36 In 0.64 XRD patterns of O3 and oxides Ga2O3 and In2O3 before the reaction;
[0019] Figure 4 The binary solid solution Ga prepared in Example 2 1.6 In 0.4 XRD patterns of O3 before and after the thermal and photothermal reactions, respectively; the conditions for the photothermal reaction were: 500℃, 10h, WHSV = 24000mL / g / h, H2 / CO2 = 4, P = 0.1MPa, and light intensity of 2.38W / cm². 2 ;
[0020] Figure 5 The binary solid solution Ga prepared in Examples 1-3 1.76 In 0.24 O3, Ga 1.6 In 0.4 O3 and Ga 1.36 In 0.64 UV-Vis diffuse reflectance spectrum of O3;
[0021] Figure 6 The binary solid solution Ga prepared in Example 2 1.6 In 0.4 X-ray photoelectron spectra (XPS) of O3 in thermal and photothermal reaction systems; a represents Ga 2p, b represents In 3d; the photothermal reaction conditions were: 500℃, 10h, WHSV = 24000mL / g / h, H2 / CO2 = 4, P = 0.1MPa, and light intensity of 2.38W / cm². 2 ;
[0022] Figure 7 The binary solid solution Ga prepared in Example 2 1.6 In 0.4 X-ray photoelectron spectra (XPS) of O3 in thermal and photothermal reaction systems at 1s; the photothermal reaction conditions were: 500℃, 10h, WHSV = 24000mL / g / h, H2 / CO2 = 4, P = 0.1MPa, and light intensity of 2.38W / cm². 2 ;
[0023] Figure 8 The binary solid solutions Ga prepared in Examples 1-3 and Comparative Examples 1 and 2 1.76 In 0.24 O3, Ga 1.6 In 0.4 O3, Ga 1.36 In 0.64N2 adsorption-desorption and pore size distribution of O3 and oxides Ga2O3 and In2O3;
[0024] Figure 9 The binary solid solutions Ga prepared in Examples 1-3 and Comparative Examples 1 and 2 1.76 In 0.24 O3, Ga 1.6 In 0.4 O3, Ga 1.36 In 0.64 Hydrogen temperature programmed reduction (H2-TPR) diagram of O3 and oxides Ga2O3 and In2O3;
[0025] Figure 10 The binary solid solutions Ga from Examples 1-3 1.76 In 0.24 O3, Ga 1.6 In 0.4 O3, Ga 1.36 In 0.64 O3 CO2 temperature-programmed adsorption-desorption (CO2-TPD) diagram;
[0026] Figure 11 The binary solid solution Ga prepared in Example 2 1.6 In 0.4 High-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM), energy-dispersive X-ray (EDX) spectral mapping images, and high-resolution transmission electron microscopy (HRTEM) images of O3;
[0027] Figure 12 The binary solid solution Ga prepared in Example 2 1.6 In 0.4 Images of O3 after the thermocatalytic reaction: high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM), energy-dispersive X-ray (EDX) spectral mapping, and high-resolution transmission electron microscopy (HRTEM); the conditions for the thermocatalytic reaction were: 500℃, 10h, WHSV = 24000mL / g / h, H2 / CO2 = 4, P = 0.1MPa.
[0028] Figure 13 The binary solid solution Ga prepared in Example 2 1.6 In 0.4 Images of O3 after the photothermal catalytic reaction: high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM), energy-dispersive X-ray (EDX) spectral mapping, and high-resolution transmission electron microscopy (HRTEM). The photothermal reaction conditions were: 500℃, 10 h, WHSV = 24000 mL / g / h, H2 / CO2 = 4, P = 0.1 MPa, and light intensity of 2.38 W / cm².2 ;
[0029] Figure 14 The ternary solid solution 2.5Cu-Ga prepared in Comparative Examples 3 and 4 1.6 In 0.4 O3, Ce 0.25 Ga 0.6 In 0.4 O x CO2 conversion rate and CO selectivity in a photothermal reaction system; the photothermal reaction conditions were: 500℃, 10h, WHSV = 24000mL / g / h, H2 / CO2 = 4, P = 0.1MPa, and light intensity of 2.38W / cm². 2 ;
[0030] Figure 15 The binary solid solution Ga prepared in Example 2 1.6 In 0.4 The binary solid solution Ga was prepared by calcining O3 and Comparative Example 5 at 1000℃. 1.6 In 0.4 CO2 conversion rate and CO selectivity of O3 in a photothermal system; the photothermal reaction conditions were: 500℃, 10h, WHSV = 24000mL / g / h, H2 / CO2 = 4, P = 0.1MPa, and light intensity of 2.38W / cm². 2 . Detailed Implementation
[0031] Example 1
[0032] The present invention provides a binary solid solution Ga 1.76 In 0.24 The method for preparing O3 includes the following steps:
[0033] (1) Weigh 2.7016 g of gallium nitrate hydrate and 0.4297 g of indium nitrate hydrate, and disperse these two substances together with 4 g of CO(NH2)2 in 70 mL of diethylene glycol (C4H2O). 10 In a mixed solution consisting of O3 and 4 mL of deionized water, stir thoroughly at room temperature for 0.5 h to ensure uniform dispersion;
[0034] (2) The mixture from step (1) was transferred to a stainless steel high-pressure hydrothermal reactor lined with polytetrafluoroethylene and reacted at 200°C for 24 h. After the reaction was completed, the product was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. The product was then vacuum dried at 60°C for 4 h.
[0035] (3) The sample dried in step (2) was heated to 400°C in air at a heating rate of 2°C / min and calcined at this temperature for 2 hours to obtain the binary solid solution Ga.1.76 In 0.24 O3.
[0036] Binary solid solution Ga 1.76 In 0.24 In O3, the loading of Ga is 61.9% of the mass of the binary solid solution; the loading of In is 13.9% of the mass of the binary solid solution.
[0037] Example 2
[0038] The present invention provides a binary solid solution Ga 1.6 In 0.4 The method for preparing O3 includes the following steps:
[0039] (1) Weigh 2.0783 g of gallium nitrate hydrate and 0.6139 g of indium nitrate hydrate, and disperse these two substances together with 4 g of CO(NH2)2 in 70 mL of diethylene glycol (C4H2O). 10 In a mixed solution consisting of O3 and 4 mL of deionized water, stir thoroughly at room temperature for 0.5 h to ensure uniform dispersion;
[0040] (2) The mixture from step (1) was transferred to a stainless steel high-pressure hydrothermal reactor lined with polytetrafluoroethylene and reacted at 200°C for 24 h. After the reaction was completed, the product was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. The product was then vacuum dried at 60°C for 4 h.
[0041] (3) The sample dried in step (2) was heated to 400°C in air at a heating rate of 2°C / min and calcined at this temperature for 2 hours to obtain the binary solid solution Ga. 1.6 In 0.4 O3.
[0042] Binary solid solution Ga 1.6 In 0.4 In O3, the loading of Ga is 54.3% of the mass of the binary solid solution; the loading of In is 22.4% of the mass of the binary solid solution.
[0043] Example 3
[0044] The present invention provides a binary solid solution Ga 1.36 In 0.64 The method for preparing O3 includes the following steps:
[0045] (1) Weigh 1.4548 g of gallium nitrate hydrate and 0.7982 g of indium nitrate hydrate, and disperse these two substances together with 4 g of CO(NH2)2 in 70 mL of diethylene glycol (C4H2O). 10In a mixed solution consisting of O3 and 4 mL of deionized water, stir thoroughly at room temperature for 0.5 h to ensure uniform dispersion;
[0046] (2) The mixture from step (1) was transferred to a stainless steel high-pressure hydrothermal reactor lined with polytetrafluoroethylene and reacted at 200°C for 24 h. After the reaction was completed, the product was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. The product was then vacuum dried at 60°C for 4 h.
[0047] (3) The sample dried in step (2) was heated to 400°C in air at a heating rate of 2°C / min and calcined at this temperature for 2 hours to obtain the binary solid solution Ga. 1.36 In 0.64 O3.
[0048] Binary solid solution Ga 1.36 In 0.64 In O3, the loading of Ga is 50.4% of the mass of the binary solid solution; the loading of In is 35.9% of the mass of the binary solid solution.
[0049] This invention demonstrates the effectiveness of Ga through XRD and TEM characterization results. 2-x In x The formation of the O3 solid solution, combined with the UV-Vis diffuse reflectance spectroscopy, demonstrated that the binary solid solution altered the band gap structure of the catalyst, resulting in better light absorption performance at a specific ratio. XPS characterization results showed an increase in oxygen vacancies, further illustrating the role of Ga... 2-x In x O3 exhibits excellent photothermal catalytic activity in the reverse water-gas shift reaction.
[0050] Comparative Example 1
[0051] A method for preparing a Ga2O3 catalyst includes the following steps:
[0052] (1) Weigh 1.5458 g of gallium nitrate hydrate and disperse it together with 4 g of CO(NH2)2 in 70 mL of diethylene glycol (C4H2O). 10 In a mixed solution consisting of O3 and 4 mL of deionized water, stir thoroughly at room temperature for 0.5 h to ensure uniform dispersion;
[0053] (2) The mixture from step (1) was transferred to a stainless steel high-pressure hydrothermal reactor lined with polytetrafluoroethylene and reacted at 200°C for 24 h. After the reaction was completed, the product was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. The product was then vacuum dried at 60°C for 4 h.
[0054] (3) The sample dried in step (2) was heated to 400°C in air at a heating rate of 2°C / min and calcined at this temperature for 2 hours to obtain white catalyst Ga2O3.
[0055] Comparative Example 2
[0056] A method for preparing an In2O3 nanocubic catalyst includes the following steps:
[0057] (1) Weigh 1.2033 g of indium nitrate hydrate and disperse it together with 4 g of CO(NH2)2 in 70 mL of diethylene glycol (C4H2O). 10 In a mixed solution consisting of O3 and 4 mL of deionized water, stir thoroughly at room temperature for 0.5 h to ensure uniform dispersion;
[0058] (2) The mixture from step (1) was transferred to a stainless steel high-pressure hydrothermal reactor lined with polytetrafluoroethylene and reacted at 200°C for 24 h. After the reaction was completed, the product was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. The product was then vacuum dried at 60°C for 4 h.
[0059] (3) The sample dried in step (2) was heated to 400°C in air at a heating rate of 2°C / min and calcined at this temperature for 2 hours to obtain a pale yellow In2O3 catalyst.
[0060] Comparative Example 3
[0061] A ternary solid solution 2.5Cu-Ga 1.6 In 0.4 The preparation method of O3 includes the following steps:
[0062] (1) Weigh 2.0783 g of gallium nitrate hydrate, 0.6139 g of indium nitrate hydrate and 0.1048 g of copper nitrate hydrate, and disperse these three substances together with 4 g of CO(NH2)2 in 70 mL of diethylene glycol (C4H2O). 10 In a mixed solution consisting of O3 and 4 mL of deionized water, stir thoroughly at room temperature for 0.5 h to ensure uniform dispersion;
[0063] (2) The mixture from step (1) was transferred to a stainless steel high-pressure hydrothermal reactor lined with polytetrafluoroethylene and reacted at 200°C for 24 h. After the reaction was completed, the product was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. The product was then vacuum dried at 60°C for 4 h.
[0064] (3) The sample dried in step (2) was heated to 400°C in air at a heating rate of 2°C / min and calcined at this temperature for 2 hours to obtain the ternary solid solution 2.5Cu-Ga. 1.6 In0.4 O3.
[0065] ternary solid solution 2.5Cu-Ga 1.6 In 0.4 In O3, the loading of Cu is 2.5% of the mass of the ternary solid solution; the loading of Ga is 54.3% of the mass of the binary solid solution; and the loading of In is 22.4% of the mass of the binary solid solution.
[0066] Comparative Example 4
[0067] A ternary solid solution Ce 0.25 Ga 0.6 In 0.15 O x The preparation method includes the following steps:
[0068] (1) Weigh 2.0783 g of gallium nitrate hydrate, 0.6139 g of indium nitrate hydrate and 1.4716 g of cerium nitrate hydrate, and disperse these three substances together with 4 g of CO(NH2)2 in 70 mL of diethylene glycol (C4H2O). 10 In a mixed solution consisting of O3 and 4 mL of deionized water, stir thoroughly at room temperature for 0.5 h to ensure uniform dispersion;
[0069] (2) The mixture from step (1) was transferred to a stainless steel high-pressure hydrothermal reactor lined with polytetrafluoroethylene and reacted at 200°C for 24 h. After the reaction was completed, the product was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. The product was then vacuum dried at 60°C for 4 h.
[0070] (3) The sample dried in step (2) was heated to 400°C in air at a heating rate of 2°C / min and calcined at this temperature for 2 hours to obtain the ternary solid solution Ce. 0.25 Ga 0.6 In 0.15 O x The atomic ratio of Ce, Ga, and In is 5:12:3.
[0071] Comparative Example 5
[0072] The preparation method of Comparative Example 5 is the same as that of Example 2, except that the calcination temperature in step (3) is 1000℃ and the heating rate is 2℃ / min. Specifically:
[0073] (1) Weigh 2.0783 g of gallium nitrate hydrate and 0.6139 g of indium nitrate hydrate, and disperse these two substances together with 4 g of CO(NH2)2 in 70 mL of diethylene glycol (C4H2O). 10In a mixed solution consisting of O3 and 4 mL of deionized water, stir thoroughly at room temperature for 0.5 h to ensure uniform dispersion;
[0074] (2) The mixture from step (1) was transferred to a stainless steel high-pressure hydrothermal reactor lined with polytetrafluoroethylene and reacted at 200°C for 24 h. After the reaction was completed, the product was collected by centrifugation and washed several times with anhydrous ethanol and deionized water. The product was then vacuum dried at 60°C for 4 h.
[0075] (3) The sample dried in step (2) is heated to 1000℃ in air at a heating rate of 2℃ / min, and calcined at this temperature for 2h to obtain Ga. 1.6 In 0.4 O3-1000 cannot form a continuous binary solid solution at this temperature of 1000℃; it mainly consists of the β-Ga2O3 phase and the In2O3 phase.
[0076] The samples prepared in Examples 1-3 and Comparative Examples 1-5 were used as catalysts in the reverse water-gas shift reaction. The apparatus used was as follows: the catalyst was packed into an inner flat quartz reaction tube (RT-100, with a central void height of 13 mm, width of 13 mm, thickness of 4 mm, and length of 400 mm), and external heating was used. A xenon lamp PLS-SXE300+ / UV was installed 18 cm directly in front of the light window of the reaction tube; a condenser lens, a φ63 mm convex lens with a focal length of 120 mm, was installed at the light outlet of the xenon lamp.
[0077] To further improve light energy utilization, a condenser lens is installed at the xenon lamp's output port. Introducing the condenser lens enhances the light power density, effectively improving light energy utilization and thus promoting the photothermal effect. The light power output is controlled by the xenon lamp's output current.
[0078] The samples prepared in Examples 1-3 and Comparative Examples 1-5 were used as photothermal catalysts in the reverse water-gas shift reaction. The specific application process was as follows: 0.15 g of catalyst was loaded into a quartz reaction tube, and the temperature was raised to 500 °C under a nitrogen atmosphere with a flow rate of 50 mL / min. Then, the nitrogen atmosphere was switched to CO2 hydrogenation reduction feed gas for RWGS reaction, and the xenon lamp was turned on at the same time. The reaction was carried out for 10 h. The flow rate of CO2 hydrogenation reduction feed gas was 60 mL / min, the molar ratio of gas CO2:H2 was 1:4, the xenon lamp current density was 20 mA, and the reaction was carried out under full-spectrum illumination with a condenser lens.
[0079] Comparative Example 6: Ga prepared in Example 2 1.6 In 0.4The application of O3 as a thermal catalyst in the reverse water-gas shift reaction is as follows: 0.15g of catalyst is loaded into a quartz reaction tube, and the temperature is raised to 500℃ under a nitrogen atmosphere with a flow rate of 50mL / min. Then, the nitrogen atmosphere is switched to CO2 hydrogenation reduction feed gas for RWGS reaction, and the reaction is carried out for 10h. The flow rate of CO2 hydrogenation reduction feed gas is 60mL / min, and the molar ratio of CO2 to H2 is 1:4.
[0080] Comparative Example 7: Ga prepared in Example 2 1.6 In 0.4 The application of O3 as a photothermal catalyst in the reverse water-gas shift reaction is as follows: 0.15g of the catalyst Ga... 1.6 In 0.4 O3 was heated to 500℃ under a nitrogen atmosphere with a flow rate of 50 mL / min. The nitrogen atmosphere was then switched to CO2 hydrogenation reduction feed gas for RWGS reaction, and the xenon lamp was turned on at the same time. The reaction was carried out for 10 h. The flow rate of CO2 hydrogenation reduction feed gas was 60 mL / min, the molar ratio of gas CO2:H2 was 1:4, the xenon lamp current density was 16 mA, and the reaction was carried out under full-spectrum illumination with a condenser lens.
[0081] Table 1. CO2 conversion and CO yield of various catalysts in photothermal catalytic CO2 hydrogenation reduction reaction
[0082]
[0083] a As a thermal catalyst
[0084] Depend on Figure 1 It can be seen that as the In content increases, Ga 2-x In x The photothermal catalytic performance of O3 first increases and then decreases, with Ga... 1.6 In 0.4 O3 exhibited the highest CO yield under photothermal catalytic conditions. After 10 h of CO2 hydrogenation reduction reaction, Ga under photothermal conditions... 1.6 In 0.4 The CO yield of the O3 catalyst can reach 4.86*10 -2 mol h -1 g cat -1 The CO yield under thermal conditions is 1.76 * 10⁻⁶. -2 molh -1 g cat -1 2.76 times that of ).
[0085] Depend on Figure 2 It can be seen that the binary solid solution Ga 1.6In 0.4 O3 exhibits good long-term stability in photothermal catalysis; after 50 hours of RWGS reaction, its photothermal catalytic activity decreased by only 2% compared to the initial reaction activity.
[0086] Depend on Figure 3 It can be seen that, compared to Ga2O3, Ga 1.76 In 0.24 O3 and Ga 1.36 In 0.64 The characteristic diffraction peaks of the O3 sample at 36° and 64° both showed a significant shift towards lower angles (i.e., to the left). This shift increased with increasing In content, indicating the formation of a solid solution. Simultaneously, with increasing In content, Ga... 2-x In x O3 exhibits distinct characteristic peaks at 21° and 43°. These phenomena indicate that the introduction of In into Ga2O3 leads to a change in the crystal structure.
[0087] Depend on Figure 4 It can be seen that, compared with thermocatalytic reactions, Ga after photothermal catalytic reactions... 1.6 In 0.4 The presence of a distinct characteristic peak at 21° and a sharp peak indicates higher crystallinity, suggesting that the catalyst crystal structure changes under different reaction conditions.
[0088] Depend on Figure 5 (a) It can be seen that, compared to Ga 1.76 In 0.24 O3 and Ga 1.36 In 0.64 O3 sample, Ga 1.6 In 0.4 The O3 sample exhibits stronger light absorption in the ultraviolet region, indicating that Ga 1.6 In 0.4 The optical properties of O3 are more conducive to photothermal catalysis. Furthermore, Ga... 1.6 In 0.4 The absorption wavelength of O3 samples exhibits a red shift, which can improve the effective utilization rate of sunlight. Figure 7 It can be seen that Ga 1.76 In 0.24 O3, Ga 1.6 In 0.4 O3 and Ga 1.36 In 0.64 The band gaps of the O3 samples were 3.11 eV, 2.97 eV, and 3.78 eV, respectively. Therefore, controlling the incorporation of In can effectively modulate the electronic band structure of the solid solution; Ga 1.6 In 0.4O3 has a smaller band gap, which is beneficial for improving the light absorption range of materials and enhancing their utilization of photons. Under illumination, it is easy to generate photogenerated electrons / holes or hot carriers.
[0089] Depend on Figure 6 (a) It can be seen that Ga 1.6 In 0.4 The Ga 2p orbital of O3 has two peaks at 1118.1 eV and 1145.0 eV, which are attributed to Ga, respectively. 3+ 2p 3 / 2 and 2p 1 / 2 Ga can be observed 1.6 In 0.4 O3 did not show a significant peak shift after undergoing both thermocatalytic and photothermal catalytic reactions, indicating that Ga... 1.6 In 0.4 No significant changes were observed in the surface chemical state of Ga in O3. 1.6 In 0.4 The In 3d binding energy of O3 is as follows Figure 8 As shown in (b), the peaks at 444.7 eV and 452.3 eV are attributed to In, respectively. 3+ 3D 5 / 2 and 3D 3 / 2 Similarly, after thermocatalytic and photothermal catalytic reactions, In 3d 5 / 2 and 3D 3 / 2 The peak position did not shift significantly, indicating that Ga... 1.6 In 0.4 The surface compound state of In in O3 did not change significantly.
[0090] Depend on Figure 7 As can be seen, the XPS fitting results show asymmetric characteristic peaks, indicating that Ga before and after the reaction... 1.6 In 0.4 O3 contains different types of O. The main peak at 529.5–531.0 eV is attributed to lattice oxygen (O). L The main peak at 531.0~532.0 eV belongs to oxygen vacancies (O). v The main peak at 532.5~533.0 eV belongs to chemisorbed oxygen (O). C Ga 1.6 In 0.4 O3 O v The content was 19.10%, and after 10 hours of thermocatalytic CO2 reduction reaction, O v The content decreased to 17.08%. However, Ga undergoing photothermal catalytic reaction... 1.6 In 0.4 O3 O vThe content remained at 19.10%. This may be because light can induce the formation of dynamic defects that become reaction sites. v The presence of [something] is beneficial for CO2 adsorption and increases the activity of reaction sites; therefore, photothermal conditions are more favorable for Ga. 1.6 In 0.4 The hydrogenation reduction reaction of O3 with CO2.
[0091] Depend on Figure 8 It can be seen that Ga2O3 and Ga 1.76 In 0.24 O3, Ga 1.6 In 0.4 O3, Ga 1.36 In 0.64 Both O3 and In2O3 catalysts exhibit mesoporous structure characteristics. The specific surface area of the Ga2O3 sample is 166.70 m². 2 g -1 Ga doped with In 1.76 In 0.24 O3 exhibits a larger specific surface area (189.10 m²). 2 g -1 This can be attributed to the fact that the incorporation of In alters the microstructure of Ga2O3. However, with further increases in the amount of In species doped, Ga... 2-x In x The specific surface area of the O3 sample showed a decreasing trend, which can be attributed to the smaller specific surface area (28.40 m²) exhibited by the In₂O₃ sample. 2 g -1 The increase in doping concentration causes the microstructure of the sample to transform into that of In2O3 crystal.
[0092] Depend on Figure 9 It is known that, within the low-temperature range of 200-400°C, the surface reduction of Ga₂O₃ is more difficult than that of In₂O₃. Furthermore, within the 200-400°C range, Ga… 1.76 In 0.24 O3, Ga 1.6 In 0.4 O3 and Ga 1.36 In 0.64 The reduction peak temperature of O3 falls between that of Ga2O3 and In2O3. This can be attributed to the fact that the incorporation of In alters the electronic properties of the material, indicating that Ga... 2-x In x Formation of O3 solid solution.
[0093] Depend on Figure 10 It can be seen that Ga 1.76 In 0.24 O3, Ga 1.6 In 0.4 O3, Ga1.36 In 0.64 O3 exhibits a broad peak in the range of 200–500 °C, among which Ga 1.6 In 0.4 The low-temperature characteristics of O3 show a significant leftward shift. Higher desorption peak temperatures correspond to a greater number of CO2 adsorption centers and a higher CO2 adsorption capacity. However, in photothermal catalysis, Ga... 1.6 In 0.4 O3 exhibits significant advantages in CO2 reduction, therefore, Ga is used in photothermal catalysis. 1.6 In 0.4 The crystal structure of O3 has changed, which is related to Figure 5 The analysis results are consistent.
[0094] Depend on Figure 11 It can be seen that Ga 1.6 In 0.4 O3 exhibits distinct lattice fringes with a spacing of 0.263 nm, corresponding to a (311) interplanar spacing of 0.248 nm in the Ga2O3 crystal. The increase in interplanar spacing indicates that In... 3+ It is incorporated into Ga2O3 crystals. 1.6 In 0.4 The distribution sites of Ga and In in O3 highly overlap, indicating that In 3+ Completely integrated into the Ga2O3 crystal, forming Ga 1.6 In 0.4 O3 solid solution.
[0095] Depend on Figure 12 It can be seen that Ga after the thermocatalytic reaction 1.6 In 0.4 O3 was observed to contain lattice fringes with a spacing of 0.305 nm. Further increases in lattice spacing indicate that Ga... 1.6 In 0.4 O3 undergoes structural changes. Ga follows a thermocatalytic reaction. 1.6 In 0.4 The Ga and In distributions in the O3 sample remained overlapping, indicating that Ga... 1.6 In 0.4 The O3 sample remains in a solid solution state.
[0096] Depend on Figure 13 It can be seen that Ga after the photothermal catalytic reaction 1.6 In 0.4 O3 showed lattice fringes of 0.287 nm and 0.266 nm, which differed significantly from the characterization results after the thermocatalytic reaction, indicating that Ga under different conditions... 1.6 In 0.4 O3 exhibits different structural changes during catalysis. Ga after photothermal catalysis... 1.6 In0.4 The distribution of O3 elements did not change significantly compared to the sample before the reaction, indicating that it still remained in a solid solution state.
[0097] Depend on Figure 14 It can be seen that the ternary solid solution 2.5Cu-Ga doped with Cu and Ce is... 1.6 In 0.4 O3, Ce 0.25 Ga 0.6 In 0.15 O x Their catalytic performance is lower than that of Ga. 1.6 In 0.4 O3. The above results indicate that although the doping of the new element regulates the catalyst structure, it does not optimize the catalytic performance; in fact, it reduces it.
[0098] Depend on Figure 15 It can be seen that the calcination temperature has a significant impact on this catalytic system. The binary solid solution Ga prepared by calcination at 400℃... 1.6 In 0.4 O3 exhibits significantly better catalytic performance than Ga prepared by calcination at 1000℃. 1.6 In 0.4 O3-1000. Although Ga 1.6 In 0.4 The CO2 conversion rate of O3-1000 increases over time during the catalytic reaction, but its initial performance and 10-hour catalytic performance are significantly inferior to those of Ga. 1.6 In 0.4 O3. This is mainly due to the fact that under the high-temperature calcination conditions of 1000℃, a binary solid solution cannot be formed, and instead, β-Ga2O3 and In2O3 phases are mainly formed.
Claims
1. A method for preparing a binary solid solution, characterized in that, Includes the following steps: (1) Weigh gallium nitrate and indium nitrate according to the stoichiometric ratio, add gallium nitrate, indium nitrate and urea to a mixed solution of diethylene glycol and deionized water, and stir thoroughly to obtain a mixture; (2) The mixture from step (1) is subjected to a hydrothermal reaction at high temperature. After the reaction is completed, the resulting solid is centrifuged, washed, and vacuum dried. (3) The solid material dried in step (2) is heated in air at 400~450℃ for 2~2.5h to obtain the binary solid solution Ga. 2-x In x O3.
2. The method for preparing a binary solid solution according to claim 1, characterized in that: In step (1), the volume ratio of diethylene glycol to water in the mixed solution is 70~75:4, and the stirring time is not less than 0.5h.
3. The method for preparing a binary solid solution according to claim 1, characterized in that: In step (2), the temperature of the hydrothermal reaction is 200~250℃ and the heating time is 22~24h.
4. The method for preparing a binary solid solution according to claim 1, characterized in that: In step (2), the number of centrifugal washing cycles is 3 to 5, the vacuum drying temperature is 60 to 70°C, and the drying is carried out overnight.
5. The method for preparing a binary solid solution according to claim 1, characterized in that: In step (3), the binary solid solution Ga 2-x In x In O3, X takes values from 1.36 to 1.
76.
6. The application of the binary solid solution prepared by the method of claim 1 as a photothermal catalyst in the reverse water-gas shift reaction.
7. The application of the binary solid solution according to claim 6 as a photothermal catalyst in the reverse water-gas shift reaction, characterized in that, The specific application process is as follows: The binary solid solution Ga... 2-x In x The O3 catalyst is placed in the reaction apparatus, nitrogen gas is introduced into the apparatus, and the apparatus is heated to 400-600°C. At this time, the nitrogen atmosphere is switched to CO2 hydrogenation reduction feed gas, and the xenon lamp is turned on to carry out the RWGS reaction. In the CO2 hydrogenation reduction feed gas, the molar ratio of H2 to CO2 is not less than 4:1; the flow rate of CO2 hydrogenation reduction feed gas is not less than 60 mL / min; the xenon lamp output current is 10-20 mA, and the reaction is carried out under full-spectrum illumination with a condenser lens.
8. The application of the binary solid solution according to claim 7 as a photothermal catalyst in the reverse water-gas shift reaction, characterized in that: The condenser lens is a φ63mm convex lens with a focal length of 120mm.