An antibacterial sponge for furniture and its preparation method

By combining a layered soft and hard sponge structure, multi-layered nylon woven mesh reinforcement, and transparent superhydrophobic resin, the problems of insufficient antibacterial properties, easy collapse, and easy contamination of furniture sponges are solved, achieving efficient photothermal sterilization and self-cleaning effects, and improving the durability and comfort of the sponge.

CN123060993APending Publication Date: 2026-11-10FOSHAN JINGHUI FURNITURE ACCESSORIES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611508621.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing furniture foam has problems such as insufficient antibacterial properties, easy compression and collapse, susceptibility to moisture and pollution, and unreasonable distribution of structural strength, making it difficult to balance comfort and durability.

Method used

It adopts a soft and hard layered sponge structure, with multiple layers of nylon woven mesh reinforcement at the corners and stress concentration areas. Combined with transparent superhydrophobic elastic reinforcing resin and loaded photothermal antibacterial material, Ag-MnO2 nanoparticles are grown in situ with the assistance of polydopamine to form a multiple antibacterial mechanism, and the interface adhesion is enhanced by silane treatment.

Benefits of technology

While maintaining softness and comfort, it significantly improves the sponge's tear resistance and resistance to repeated compression fatigue, extends its antibacterial lifespan, achieves transparent self-cleaning and efficient photothermal sterilization, and solves multiple problems in the use of furniture sponges.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060993A_ABST
    Figure CN123060993A_ABST
Patent Text Reader

Abstract

This invention discloses an antibacterial sponge for furniture and its preparation method, belonging to the technical field of functional sponge materials. The antibacterial sponge comprises an upper soft sponge layer, a lower hard sponge layer, and a nylon woven mesh reinforcement layer sandwiched between the two. The upper sponge layer has a lower density than the lower sponge layer. The nylon woven mesh reinforcement layer has multiple layers of nylon mesh in the corners / stress concentration areas and a single layer of nylon mesh in the central area. The sponge also contains photothermal antibacterial materials, and the layers are bonded together with a transparent superhydrophobic elastic reinforcing resin to prevent loss of the photothermal antibacterial materials. The preparation method includes sponge cleaning, nylon mesh pretreatment, photothermal material loading, resin formulation, layered impregnation, differentiated layer assembly, and curing. The sponge of this invention combines the comfortable support of a soft upper layer and a hard lower layer, gradient-enhanced anti-collapse properties, photothermal synergistic active antibacterial properties, and superhydrophobic self-cleaning properties, making it suitable for furniture applications such as sofas and mattresses.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of functional sponge materials technology, and in particular to an antibacterial sponge for furniture and its preparation method. Background Technology

[0002] Sponge materials are widely used in furniture making due to their excellent softness, cushioning, and plasticity, such as sofa cushions, mattresses, chair backs, and armrest fillings. However, traditional polyurethane foam has the following prominent problems in furniture use: First, the antibacterial properties are insufficient. The porous structure of sponges easily absorbs human sweat, dander, and moisture from the environment, providing an ideal growth environment for bacteria, fungi, and mites. With prolonged use, microorganisms proliferate inside the sponge, not only producing odors but also potentially causing health problems such as skin allergies and respiratory infections. While some antibacterial sponge products exist, such as those made by adding tourmaline powder and silver phosphate powder, and antibacterial polyurethane sponges that pre-disperde antibacterial agents in polyurethane prepolymers, these solutions often suffer from uneven distribution of antibacterial agents, poor antibacterial durability, or complex processes. In recent years, photothermal antibacterial technology has received widespread attention as an emerging physical antibacterial method. It converts light energy into heat energy through photothermal materials under illumination, using localized high temperatures to kill bacteria. Zhu et al. prepared a superhydrophobic sponge with a water contact angle of 156.5° by in-situ growth of Ag-MnO2 nanoparticles on a sponge with polydopamine assistance and hydrophobic modification. The sponge exhibited a surface temperature of 64.1℃ under simulated light irradiation and demonstrated excellent antibacterial properties against Escherichia coli and Staphylococcus aureus. However, this technology is currently mainly used in oil-water separation and has not yet been effectively integrated into furniture sponge materials.

[0003] Secondly, it is prone to compression and collapse. After prolonged sitting or lying down, the polymer molecular chains in the pore walls of soft foam used in furniture are prone to irreversible displacement or breakage, causing the foam to lose its resilience and exhibit noticeable indentations and deformation, severely affecting the lifespan and comfort of the furniture. While existing technologies have attempted to improve elasticity by adding reinforcing fibers or using high-resilience polyurethane, these often come at the cost of softness, making it difficult to balance comfort and durability. Existing research indicates that a gradient structure with a soft upper layer and a firm lower layer can provide gentle cushioning during initial contact while ensuring sufficient support. However, simply stacking foams of different densities still cannot effectively solve the structural fatigue problem after long-term use.

[0004] Third, sponges are susceptible to moisture and contamination and lack self-cleaning capabilities. Their hydrophilic nature makes them prone to absorbing liquid contaminants such as spilled beverages and sweat, which are not only difficult to clean but also accelerate bacterial growth and material aging. While there are existing technologies that modify sponges with low surface energy materials to impart superhydrophobic properties, these solutions are mostly geared towards industrial applications such as oil-water separation and have not yet been effectively applied to the furniture industry. Furthermore, existing superhydrophobic sponges often use opaque coatings. When the sponge contains photothermal antibacterial materials, the opaque coating hinders light penetration, severely impacting photothermal conversion efficiency. Therefore, developing sponge materials with both transparent and superhydrophobic properties, allowing light to penetrate the surface coating and activate the internal photothermal antibacterial materials, is a pressing technical challenge.

[0005] Fourth, the structural strength distribution is unreasonable. Single-layer sponge structures lack an effective stress dispersion mechanism under repeated stress, leading to excessive pressure on localized pores and eventual collapse. While existing technologies include embedding woven mesh layers into the sponge or attempting to place nylon mesh layers between sponges of different densities, these solutions typically employ uniform reinforcement, failing to consider the stress differences in different areas of the sponge. In reality, furniture sponges, such as sofa cushions and mattresses, experience significantly greater pressure at the edges and corners, as well as in areas of concentrated stress, such as the hip support area of ​​a cushion, compared to the central area. Uniform reinforcement not only wastes material but may also affect the breathability and softness of the central area. Currently, there is no technical solution for differentiated reinforcement of different areas of the sponge.

[0006] Therefore, developing a composite sponge for furniture that combines long-lasting active antibacterial properties, transparent superhydrophobic self-cleaning properties, high elasticity and anti-collapse properties, and a gradient reinforcement structure, along with its simple and efficient preparation method, has significant practical importance and market value. Summary of the Invention

[0007] The purpose of this invention is to address the shortcomings of existing technologies by proposing an antibacterial sponge for furniture and its preparation method.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: The present invention first proposes an antibacterial sponge for furniture, comprising an upper soft sponge layer, a lower hard sponge layer, and a nylon woven mesh reinforcement layer sandwiched between the two; The density of the upper soft sponge layer is lower than the density of the lower hard sponge layer; The upper soft sponge layer is in direct contact with the human body. It has a low density and a rebound of ≥50%, providing a soft sitting feel and ensuring the surface comfort and rebound of the sofa and mattress. The lower hard sponge layer serves as a support base. It has a high modulus and small compression deformation, bearing most of the load, preventing collapse after long-term use, and providing overall support. The sponge, which consists of a cut upper soft sponge layer and a lower hard sponge layer, is reinforced with two or more layers of nylon woven mesh symmetrically arranged in the corner areas and / or stress concentration areas of the sponge through a nylon woven mesh reinforcement layer; a whole layer of nylon woven mesh is arranged between the upper soft sponge layer and the lower hard sponge layer. Two or more layers of nylon 6 / nylon 66 woven mesh are installed at the corners and stress-concentrated areas. The corners, edges, and frequently compressed areas of furniture sponge are high-risk locations for tearing and fatigue damage. Multiple layers of woven mesh can disperse stress, inhibit crack propagation, and improve tear resistance and resistance to repeated compression fatigue. A single layer of woven mesh is installed in the central area. The central area mainly takes into account flexibility. If multiple layers of mesh are used, it will result in an overall stiffness and a rigid sitting feel. A single layer of mesh only serves to bind the interface and does not compromise the softness of the sponge.

[0009] The upper soft sponge layer, the nylon woven mesh reinforcement layer, and the lower hard sponge layer are bonded together by a transparent superhydrophobic elastic reinforcing resin. The bonding resin is not just glue; it also plays multiple roles, including interface bonding, elastic buffering, superhydrophobic antifouling, and light transmission to ensure photothermal function.

[0010] The sponge also contains photothermal antibacterial materials. The visible light transmittance of the transparent superhydrophobic elastic reinforced resin is ≥80%.

[0011] Preferably, the upper soft sponge layer has a density of 25–45 kg / m³. 3 The lower layer is a low-density polyurethane soft sponge with a resilience of ≥50%; the lower rigid sponge layer has a density of 60-120 kg / m³. 3 High-density polyurethane foam.

[0012] Preferably, the nylon woven mesh is a woven mesh fabric made of nylon 66 or nylon 6, with a mesh count of 10-50 mesh and a weight of 50-200 g / m². 2 .

[0013] Preferably, the transparent superhydrophobic elastic reinforcing resin comprises the following components in parts by weight: Bisphenol F type epoxy resin: 50-70 parts; Hydroxyl-terminated polydimethylsiloxane: 10-20 parts; Hydrophobic vapor-phase nano-silica: 5-15 parts; Fluorine-modified cage-like silsesquioxane: 2-8 parts; Long-chain silane coupling agent: 2-5 parts; Polyamide curing agent: 10-25 parts.

[0014] Preferably, the photothermal antibacterial material is an Ag-MnO2 nanocomposite or reduced graphene oxide; the Ag-MnO2 nanocomposite is obtained by in-situ growth on a sponge skeleton with the assistance of polydopamine.

[0015] Dopamine undergoes oxidative polymerization under Tris-HCl conditions, resulting in a polydopamine coating encapsulating a polyurethane sponge skeleton. The polydopamine contains numerous phenolic hydroxyl and amino groups, which strongly adhere to the sponge skeleton and simultaneously act as active sites for Ag adsorption. + MnO4 - This enables in-situ nucleation and growth of nanoparticles, preventing them from falling off later; polydopamine itself also has a certain adhesion and antibacterial effect.

[0016] After subsequent resin impregnation, a thin, continuous elastic resin film forms on the surface of the sponge skeleton and nanoparticles. However, due to repeated compression and friction over long periods, the in-situ grown Ag-MnO2 and rGO nanoparticles are at risk of being mechanically peeled off and turned into dust. The cured resin film coats the photothermal nanomaterials, forming a physical barrier that confines the nanoparticles within the sponge matrix, preventing the nanoparticles from detaching or volatilizing, and avoiding the release of silver nanoparticles, manganese dioxide, and graphene particles into the environment, thus preventing human contact and dust leakage. Salt, oil, and dust from the furniture environment, if deposited directly on the surface of the photothermal nanomaterials, can cover the active sites and reduce photothermal conversion efficiency. The superhydrophobic resin layer on the surface repels most water, sweat, and oil, reducing direct contact between contaminants and photothermal particles, indirectly protecting the photothermal antibacterial sites.

[0017] Preferably, the water contact angle of the sponge surface is ≥150°.

[0018] The present invention also proposes a method for preparing the aforementioned antibacterial sponge for furniture, characterized by comprising the following steps: S1: Clean and dry the upper soft sponge layer and the lower hard sponge layer; It removes residual mold release agents and small molecule additives from sponge production, improving the wetting and adhesion of subsequent materials.

[0019] S2: Pre-treat the nylon woven mesh by immersing it in an ethanol solution containing γ-aminopropyltriethoxysilane, and then dry it; The silane coupling agent hydrolyzes, with one end of the silanol group attaching to the nylon surface and the other end of the amino group reacting with the epoxy resin, greatly improving the bonding strength between the nylon mesh and the resin and preventing delamination between the woven mesh and the sponge.

[0020] S3: Load the photothermal antibacterial material onto the upper and lower layers of sponge; In-situ growth / vacuum impregnation anchors antibacterial photothermal materials to the sponge cell skeleton, rather than filling the cells, thus not severely damaging the sponge's pores and softness.

[0021] S4: Prepare a transparent superhydrophobic elastic reinforced resin solution; Solvent dilution reduces viscosity, facilitating impregnation and allowing the sponge to penetrate the pores and gaps in the woven mesh; excessive concentration will clog the pores and harden the sponge; insufficient concentration will result in insufficient bonding strength.

[0022] S5: Immerse the nylon woven mesh and the upper and lower sponges loaded with photothermal material into the resin solution respectively, and remove them to remove excess resin solution; Impregnation allows the resin to soak into the interface between the sponge and the woven mesh; squeezing / centrifugation removes a large amount of excess resin from inside the cells, preventing the resin from filling the cells and causing the sponge to harden and lose its elasticity; resin is left only at the cell skeleton and interface, taking into account both adhesion and hydrophobic functions, while preserving the porous elastic structure of the sponge.

[0023] S6: Place two or more layers of nylon woven mesh in the corner areas and / or areas of concentrated stress of the sponge, and place one layer of nylon woven mesh in the central area. Stack the layers in the order of "lower layer of rigid sponge - nylon woven mesh reinforcement layer - upper layer of soft sponge" and apply pressure. Low pressure prevents the sponge cells from collapsing; ensures tight adhesion between layers, resin impregnation at the interface, elimination of interlayer air bubbles, and gap-free interface after curing; multi-layer mesh in the corner stress area and single-layer mesh in the center achieve zoned reinforcement.

[0024] S7: Place the composite sponge assembled in S6 at 40-80℃ for 8-24 hours to cure, and the antibacterial sponge for furniture is obtained.

[0025] Low-temperature pre-curing: The solvent evaporates slowly, the resin undergoes initial cross-linking, and the solvent is prevented from boiling and foaming rapidly, thus avoiding bubble defects in the adhesive layer; High-temperature post-curing: The epoxy resin is fully cross-linked to obtain high bonding strength, elasticity, and superhydrophobic properties; the curing temperature is 40-80℃. If the temperature is too high, the polyurethane foam will undergo thermal aging, shrinkage, and deformation.

[0026] Preferably, the photothermal antibacterial material in S3 is an Ag-MnO2 nanocomposite, and its loading method is as follows: the sponge is immersed in a Tris-HCl buffer solution containing dopamine to react and form a polydopamine coating, and then immersed in a mixed solution containing AgNO3 and KMnO4 to react, so that Ag-MnO2 nanoparticles grow in situ on the sponge skeleton.

[0027] Preferably, the photothermal antibacterial material in S3 is reduced graphene oxide, and its loading method is as follows: the sponge is immersed in a graphene oxide aqueous dispersion under vacuum-assisted impregnation, then taken out and dried, and then immersed in a reducing agent solution for reduction to obtain a sponge loaded with reduced graphene oxide.

[0028] Preferably, the solid content of the transparent superhydrophobic elastic reinforcing resin solution in S4 is 15-30 wt%; the method for removing excess resin solution in S5 is by extrusion by a squeeze roller or centrifugal separation, so that the weight gain of the sponge is controlled within 10-30%; the pressure in S6 is 0.01-0.08 MPa; the curing in S7 is divided into two stages: first curing at 40-50℃ for 4-12 hours, and then heating to 60-80℃ for 4-12 hours.

[0029] Layered soft and hard sponge with partitioned nylon woven mesh solves the contradiction of furniture sponges being "soft and comfortable but prone to tearing and collapsing at the edges." Resin serves as the bonding medium, achieving elastic bonding, superhydrophobicity, stain resistance, and high light transmittance. Superhydrophobicity reduces liquid retention, thus reducing bacterial survival in the environment. High light transmittance ensures that photothermal antibacterial materials receive light. Superhydrophobicity physically blocks liquid contaminants, while the photothermal material provides multiple antibacterial effects. Silane pretreatment of the nylon mesh and polydopamine anchoring of nano-antibacterial particles, along with modification of each interface, solve the problem of interlayer delamination and functional filler detachment caused by long-term pressure on composite sponges.

[0030] Compared with the prior art, the beneficial effects of the present invention are: 1. Existing antibacterial furniture sponges either simply increase sponge density to improve tear and collapse resistance, resulting in overly hard sponges and a stiff seating experience; or they only lay a single reinforcing mesh in the overall interlayer, leaving stress concentration at corners and areas of high stress, leading to corner tearing and interlayer delamination failure after repeated compression. This invention uses a layered sponge matrix with differentiated zoning of the middle nylon woven mesh reinforcing layer. Multiple layers of nylon woven mesh are used at corners and areas of high stress to disperse stress and inhibit crack initiation and propagation, while a single layer of woven mesh is used in the central area to retain the sponge's inherent flexibility. Simultaneously, the silane-pretreated nylon woven mesh forms a strong interface bond with the transparent superhydrophobic elastic reinforcing resin, preventing interlayer delamination. Without sacrificing the sponge's softness and resilience, this significantly improves the sponge's tear resistance and resistance to repeated compression fatigue, resolving the technical contradiction of balancing comfort and mechanical durability.

[0031] 2. In existing technologies, the adhesive resins used in composite sponges mostly only serve a bonding and fixing function, with limited functionality. If the sponge is loaded with silver-based photothermal antibacterial fillers, long-term friction and compression can easily cause nanoparticles to detach and become dusty. When exposed to water, silver ions are rapidly released, leading to a rapid decline in antibacterial performance and posing a safety hazard of nanoparticle leakage. The transparent superhydrophobic elastic reinforcing resin of this invention, on the one hand, acts as an adhesive phase to composite the layers into an elastic whole. After curing, it constructs a micro-nano rough-low surface energy surface to achieve superhydrophobicity, blocking sweat and liquid dirt from penetrating into the sponge and reducing the environment for bacterial growth from the source. On the other hand, the resin forms a thin coating barrier layer on the outside of the photothermal antibacterial material, physically restricting the detachment of nanofillers and simultaneously regulating the diffusion rate of silver ions to achieve slow release, extending the antibacterial service life. Furthermore, the resin has a visible light transmittance of ≥80%, allowing light to penetrate the resin layer to reach the photothermal active sites without weakening the photothermal sterilization effect, achieving an integration of structural bonding, antifouling protection, filler barrier slow release, and light transmission.

[0032] 3. Traditional antibacterial sponges often directly blend antibacterial agents into the sponge's pore matrix. These agents are easily lost through sweat and rinsing, resulting in short-lasting antibacterial effects and a single antibacterial mechanism. This invention utilizes Ag-MnO2 nanocomposites, grown in situ with polydopamine assistance or through vacuum impregnation to obtain reduced graphene oxide, anchoring the photothermal antibacterial material onto the sponge's pore framework. This combines the physical sterilization of localized high temperatures generated by photothermal conversion with the chemical antibacterial effect of silver ions in the Ag-MnO2 system, forming a photothermal-ion synergistic sterilization. Furthermore, the superhydrophobic surface of the resin prevents liquid contamination, creating a multi-layered antibacterial mechanism. Simultaneously, the resin barrier layer inhibits the loss of active components, preventing rapid depletion of antibacterial components. Compared to simply blended antibacterial sponges, this significantly improves antibacterial stability and service life, making it suitable for long-term, repeated use of furniture such as sofas and mattresses. Attached Figure Description

[0033] Figure 1 This is a schematic diagram of the structure of the antibacterial sponge proposed in this invention; In the diagram: 1 is the upper soft sponge layer, 2 is the nylon woven mesh reinforcement layer between the upper soft sponge layer and the lower hard sponge layer, 3 is the lower hard sponge layer, 4 is the upper / lower sponge cut-out, 5 is the upper sponge at the cut-out, 6 is the lower sponge at the cut-out, and 7 is the nylon woven mesh symmetrically arranged in the corner area and / or stress concentration area. Detailed Implementation

[0034] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with existing known technologies. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0035] Example 1:

[0036] This embodiment provides an antibacterial sponge for furniture and its preparation method.

[0037] (1) Raw material preparation: Upper soft sponge layer: 30 kg / m³ 3 A 15mm thick polyurethane soft sponge with a resilience of 55%.

[0038] Lower rigid sponge layer: 80 kg / m³ density selected 3 The polyurethane rigid foam has a thickness of 15mm.

[0039] Nylon woven mesh: Made of nylon 66 woven mesh fabric with a mesh count of 20 meshes and a weight of 100g / m². 2 .

[0040] Photothermal antibacterial material: using Ag-MnO2 nanocomposite.

[0041] Transparent superhydrophobic elastic reinforced resin formulation: Bisphenol F type epoxy resin (epoxy equivalent 180g / eq): 60 parts; Hydroxyl-terminated polydimethylsiloxane (HO-PDMS, Mn≈500): 15 parts; Hydrophobic vapor-phase nano-silica (particle size 15nm): 10 parts; Fluorine-modified cage-like silsesquioxane (F-POSS): 5 parts; Hexadecyltrimethoxysilane: 4 parts; Polyamide curing agent: 18 parts; Propylene glycol methyl ether acetate: appropriate amount (adjust solid content to 25wt%).

[0042] (2) Preparation steps: S1: Clean the upper and lower layers of sponge sequentially with distilled water and anhydrous ethanol using ultrasonic cleaning for 30 minutes each, and dry at 60°C until constant weight.

[0043] S2: Immerse the nylon woven mesh in an ethanol solution containing 2% KH550 (pH 4.5) for 30 minutes, then remove and dry at 60°C.

[0044] S3: Immerse the pretreated sponge in Tris-HCl buffer (pH 8.5) containing 2 g / L dopamine and stir at room temperature for 5 hours; remove and wash with deionized water, then immerse in a mixed solution containing 0.02 mol / L AgNO3 and 0.01 mol / L KMnO4 and react in a water bath at 60°C for 3 hours; remove and wash with deionized water and dry at 60°C.

[0045] S4: Bisphenol F type epoxy resin, HO-PDMS, hydrophobic nano silica, F-POSS, and hexadecyltrimethoxysilane were added to propylene glycol methyl ether acetate and stirred at 1000 rpm for 30 minutes, followed by ultrasonic dispersion for 15 minutes; polyamide curing agent was added and stirring was continued for 15 minutes; the mixture was allowed to stand for degassing for 30 minutes to obtain a transparent superhydrophobic elastic reinforced resin solution with a solid content of 25 wt%.

[0046] S5: Immerse the nylon woven mesh completely in the resin solution for 30 minutes, then remove and drain off the excess resin solution; immerse the upper and lower sponge layers separately in the resin solution for 15 minutes, then remove and use a squeeze roller to remove the excess resin solution, so that the weight gain of the sponge is controlled within 20%.

[0047] S6: Place two layers of nylon woven mesh on each of the four corner areas of the sponge, and place one layer of nylon woven mesh in the central area; stack them in the order of "lower layer of rigid sponge - nylon woven mesh reinforcement layer - upper layer of soft sponge", and apply a uniform pressure of 0.04MPa.

[0048] S7: Place the assembled composite sponge in an oven, first cure it at 50℃ for 6 hours, then raise the temperature to 70℃ and cure it for another 6 hours to obtain an antibacterial sponge for furniture.

[0049] Example 2:

[0050] The difference between this embodiment and Embodiment 1 is that the photothermal antibacterial material uses reduced graphene oxide (rGO); the density of the upper sponge is 35 kg / m³. 3 The density of the lower layer of sponge is 100 kg / m³. 3 The transparent superhydrophobic elastic reinforced resin formula was adjusted to: 55 parts of bisphenol F type epoxy resin, 18 parts of HO-PDMS, 12 parts of hydrophobic nano silica, 6 parts of F-POSS, 5 parts of dodecyltrimethoxysilane, and 20 parts of polyamide curing agent; the curing conditions were 45℃ for 8 hours, followed by heating to 75℃ for 4 hours.

[0051] rGO loading steps: Prepare a 3 mg / mL graphene oxide aqueous dispersion and sonicate for 30 minutes; immerse a sponge in the dispersion and vacuum-assisted impregnation for 40 minutes (-0.09 MPa); remove and dry at 60°C, immerse in a 10 mg / mL ascorbic acid solution and reduce at 80°C for 4 hours; wash with deionized water and dry at 60°C.

[0052] The remaining preparation steps are the same as in Example 1.

[0053] Example 3:

[0054] The difference between this embodiment and Embodiment 1 is that the thickness of both the upper and lower sponge layers is 20mm; the nylon woven mesh has a mesh count of 30 and a weight of 150g / m².2 Three layers of nylon woven mesh are set in the corner area; the solid content of the transparent superhydrophobic elastic reinforcing resin is 20wt%; the curing conditions are 40℃ for 10 hours, and then heated to 65℃ for 8 hours.

[0055] The remaining preparation steps are the same as in Example 1.

[0056] Comparative Example 1: The difference between this comparative example and Example 1 is that no nylon braided mesh reinforcement layer is provided. All other raw materials and preparation steps are the same as in Example 1.

[0057] Comparative Example 2: The difference between this comparative example and Example 1 is that the nylon woven mesh is uniformly arranged in a single layer across the entire surface, without multiple layers of reinforcement in the corner areas. The remaining raw materials and preparation steps are the same as in Example 1.

[0058] Comparative Example 3: The difference between this comparative example and Example 1 is that the upper and lower layers of sponge use the same density (both 55 kg / m³). 3 The remaining raw materials and preparation steps are the same as in Example 1.

[0059] Comparative Example 4: The difference between this comparative example and Example 1 is that F-POSS and hydrophobic nano-silica are not added to the transparent superhydrophobic elastic reinforcing resin. The remaining raw materials and preparation steps are the same as in Example 1.

[0060] Comparative Example 5: The difference between this comparative example and Example 1 is that the particle size of the hydrophobic nano-silica is 80 nm (greater than 20 nm). The remaining raw materials and preparation steps are the same as in Example 1.

[0061] Comparative Example 6: The difference between this comparative example and Example 1 is that it does not contain photothermal antibacterial material (Ag-MnO2). The remaining raw materials and preparation steps are the same as in Example 1.

[0062] Performance testing: Water contact angle: The contact angle of a water droplet on the sample surface, measured using a contact angle meter.

[0063] Visible light transmittance: The transmittance at a wavelength of 550nm was measured using a UV-Vis spectrophotometer.

[0064] Photothermal heating performance: Under simulated sunlight irradiation (1kW / m²) 2 The temperature rise of the sponge surface was measured within 10 minutes.

[0065] Compression permanent deformation: tested according to GB / T6669-2008 standard.

[0066] Antibacterial properties: Tested according to GB / T20944.3-2008 standard, the test strain is Staphylococcus aureus.

[0067] Interlayer peel strength: tested according to GB / T2790-1995 standard.

[0068] Table 1. Summary of performance tests for each experimental group

[0069] Data Analysis: Examples 1-3 represent the complete solution of this invention. The water contact angle is ≥150°, achieving superhydrophobicity; visible light transmittance is ≥80%; photothermal heating ΔT >21℃; low compression set and excellent compression resilience; antibacterial rate against Staphylococcus aureus is >98.5%; high interlayer peel strength and strong composite interface bonding. Example 3 uses a three-layer nylon woven mesh at the corners, exhibiting optimal interlayer peel strength, lowest compression set, and best mechanical durability. Example 2 uses an rGO photothermal system, whose overall performance is slightly lower than the Ag-MnO2 system, but still meets the usage requirements.

[0070] Comparative Example 1 (without nylon braided mesh reinforcement): The hydrophobicity, light transmittance, photothermal properties, and antibacterial properties are similar to those of Example 1; however, the compression set is significantly larger, and the interlayer peel strength is greatly reduced. Without the braided mesh reinforcement, the composite sponge is prone to delamination under pressure, exhibiting poor fatigue resistance and tear resistance.

[0071] Comparative Example 2 (single-layer woven mesh with multi-layer partitioned reinforcement without corners): other indicators are similar to Example 1; the compression set is higher than that of Example 1. The single-layer mesh cannot strengthen the stress concentration areas at the corners, and fatigue cracking is prone to occur at the corners, demonstrating the advantage of partitioned multi-layer reinforcement.

[0072] Comparative Example 3 (with identical density of upper and lower sponges and no soft-hard layering): Hydrophobicity, light transmittance, photothermal properties, antibacterial properties, and peel strength showed little change; however, compression set increased. Without a soft-hard density gradient structure, the soft feel of the upper layer could not match the support of the lower layer, resulting in decreased resistance to collapse under long-term pressure.

[0073] Comparative Example 4 (removal of F-POSS + hydrophobic fumed silica): transmittance, photothermal properties, compression deformation, and peel strength remained basically unchanged; the water contact angle plummeted to 102°, essentially losing its superhydrophobic effect.

[0074] Comparative Example 5 (silica particle size 80nm): The filler particle size is too large, which causes enhanced light scattering inside the resin and a decrease in visible light transmittance; the water contact angle decreases, making it impossible to achieve superhydrophobicity; large filler particles are prone to causing local defects, and photothermal heating, antibacterial rate and peel strength all show a slight decrease.

[0075] Comparative Example 6 (without photothermal antibacterial material): hydrophobicity, light transmission, compression deformation, and peel strength are basically the same as in Example 1; there is almost no photothermal heating, the antibacterial rate is only 42.6%, and it relies only on the hydrophobicity of the resin surface to bring weak physical antibacterial effect, with almost no antibacterial function.

[0076] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. An antibacterial sponge for furniture, characterized in that, It includes an upper soft sponge layer, a lower hard sponge layer, and a nylon woven mesh reinforcement layer; The density of the upper soft sponge layer is lower than the density of the lower hard sponge layer; The sponge, which consists of a cut upper soft sponge layer and a lower hard sponge layer, is reinforced with two or more layers of nylon woven mesh symmetrically arranged in the corner areas and / or stress concentration areas of the sponge through a nylon woven mesh reinforcement layer; a whole layer of nylon woven mesh is arranged between the upper soft sponge layer and the lower hard sponge layer. The upper soft sponge layer, the lower hard sponge layer, and the nylon woven mesh reinforcement layer are bonded together by a transparent superhydrophobic elastic reinforcing resin. The sponge also contains photothermal antibacterial materials. The visible light transmittance of the transparent superhydrophobic elastic reinforced resin is ≥80%.

2. The antibacterial sponge for furniture according to claim 1, characterized in that, The upper soft sponge layer has a density of 25-45 kg / m³. 3 The lower layer is a low-density polyurethane soft sponge with a resilience of ≥50%; the lower rigid sponge layer has a density of 60-120 kg / m³. 3 High-density polyurethane foam.

3. The antibacterial sponge for furniture according to claim 1, characterized in that, The nylon woven mesh is made of nylon 66 or nylon 6 woven mesh fabric with a mesh count of 10-50 mesh and a weight of 50-200 g / m². 2 .

4. The antibacterial sponge for furniture according to claim 1, characterized in that, The transparent superhydrophobic elastic reinforcing resin comprises the following components in parts by weight: Bisphenol F type epoxy resin: 50-70 parts; Hydroxyl-terminated polydimethylsiloxane: 10-20 parts; Hydrophobic vapor-phase nano-silica: 5-15 parts; Fluorine-modified cage-like silsesquioxane: 2-8 parts; Long-chain silane coupling agent: 2-5 parts; Polyamide curing agent: 10-25 parts.

5. The antibacterial sponge for furniture according to claim 1, characterized in that, The photothermal antibacterial material is an Ag-MnO2 nanocomposite or reduced graphene oxide; the Ag-MnO2 nanocomposite is obtained by in-situ growth on a sponge skeleton with the assistance of polydopamine.

6. The antibacterial sponge for furniture according to claim 1, characterized in that, The water contact angle of the sponge surface is ≥150°.

7. A method for preparing an antibacterial sponge for furniture as described in any one of claims 1 to 6, characterized in that, Includes the following steps: S1: Clean and dry the upper soft sponge layer and the lower hard sponge layer; S2: Pre-treat the nylon woven mesh by immersing it in an ethanol solution containing γ-aminopropyltriethoxysilane, and then dry it; S3: Load the photothermal antibacterial material onto the upper and lower layers of sponge; S4: Prepare a transparent superhydrophobic elastic reinforced resin solution; S5: Immerse the nylon woven mesh and the upper and lower sponges loaded with photothermal material into the resin solution respectively, and remove them to remove excess resin solution; S6: Place two or more layers of nylon woven mesh in the corner areas and / or areas of concentrated stress of the sponge, and place one layer of nylon woven mesh in the central area. Stack the layers in the order of lower hard sponge, nylon woven mesh reinforcement layer, and upper soft sponge and apply pressure. S7: Place the composite sponge assembled in S6 at 40-80℃ for 8-24 hours to cure, and the antibacterial sponge for furniture is obtained.

8. The preparation method according to claim 7, characterized in that, The photothermal antibacterial material described in S3 is an Ag-MnO2 nanocomposite. Its loading method is as follows: the sponge is immersed in a Tris-HCl buffer solution containing dopamine to form a polydopamine coating, and then immersed in a mixed solution containing AgNO3 and KMnO4 to react, so that Ag-MnO2 nanoparticles grow in situ on the sponge skeleton.

9. The preparation method according to claim 7, characterized in that, The photothermal antibacterial material described in S3 is reduced graphene oxide, and its loading method is as follows: the sponge is immersed in a graphene oxide aqueous dispersion under vacuum-assisted impregnation, then taken out, dried, and immersed in a reducing agent solution for reduction, to obtain a sponge loaded with reduced graphene oxide.

10. The preparation method according to claim 7, characterized in that, The solid content of the transparent superhydrophobic elastic reinforcing resin solution in S4 is 15-30 wt%; the method for removing excess resin solution in S5 is extrusion by extrusion rollers or centrifugal separation, so that the weight gain of the sponge is controlled within 10-30%; the pressure in S6 is 0.01-0.08 MPa; the curing in S7 is divided into two stages: first curing at 40-50℃ for 4-12 hours, and then heating to 60-80℃ for 4-12 hours.