A method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes
By purifying and performing high-temperature carbothermal reduction on the negative electrode sheets of waste batteries, the problems of low recycling rate of waste graphite and high cost of lithium sulfide preparation have been solved, achieving efficient and low-cost lithium sulfide preparation, which is suitable as a key raw material for all-solid-state batteries.
Patent Information
- Application Number
- CN202611310466.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-10
AI Technical Summary
In existing technologies, the recycling rate of graphite anodes from waste lithium-ion batteries is low, leading to resource waste and environmental pollution. At the same time, the traditional carbothermal reduction method for preparing lithium sulfide relies on expensive commercial high-purity carbon powder, which is costly.
Lithium sulfide is prepared by purifying the negative electrode sheets of waste batteries to remove binders and metal impurities, and then using high-purity recycled graphite and lithium sulfate to carry out a high-temperature carbothermic reduction reaction under an inert atmosphere, controlling the reaction conditions.
This technology enables high-value-added resource utilization of waste negative electrode graphite, significantly reduces the preparation cost of lithium sulfide, improves recycling efficiency, and yields high-purity lithium sulfide products, which are suitable as key raw materials for all-solid-state batteries.
Smart Images

Figure CN123061918A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid waste recycling technology, and in particular relates to a method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes. Background Technology
[0002] With the explosive growth of the new energy vehicle and energy storage industries, the number of retired lithium-ion batteries has been increasing year by year. These waste batteries contain a large amount of negative electrode graphite. Currently, recycling of waste batteries mainly focuses on the valuable metals of the positive electrode (such as lithium, cobalt, and nickel), while the negative electrode graphite is often downgraded or directly discarded, causing serious resource waste and environmental pressure. On the other hand, lithium sulfide, as a core raw material for the solid electrolyte of sulfide-based all-solid-state batteries, has huge market demand. Traditional carbothermal reduction methods for preparing lithium sulfide typically use high-purity commercial carbon powder (such as carbon black and high-purity graphite) as a reducing agent, resulting in high production costs. How to achieve high-value reuse of waste negative electrode graphite while reducing the production cost of lithium sulfide is a pressing technical challenge for the industry.
[0003] It is worth noting that during long-term charge-discharge cycles, the interlayer structure of graphite from waste lithium-ion batteries undergoes a certain degree of expansion and defect formation. This defect-rich carbon structure exhibits higher reactivity in carbothermic reduction reactions than conventional graphite, which helps to lower the reduction temperature or shorten the reaction time. Introducing this naturally reactive waste anode graphite as a carbon source into the lithium sulfide preparation process can not only replace expensive commercial high-purity carbon sources, significantly reducing the production cost of core raw materials for all-solid-state batteries, but also provide a high-value-added, green, closed-loop recycling path for waste battery anode materials. Based on this, this invention proposes a method for preparing lithium sulfide from waste battery anode graphite via carbothermic reduction. The method involves purifying the waste anode sheets to obtain the recycled graphite carbon source, mixing it with lithium sulfate, and then conducting a high-temperature carbothermic reduction reaction under an inert atmosphere. After cooling, lithium sulfide is obtained. This method combines the advantages of resource recycling and low-cost preparation, aligning with the development concepts of circular economy and green chemistry, and has significant prospects for industrial application. Summary of the Invention
[0004] Based on the technical problems existing in the prior art, the present invention provides a method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrode.
[0005] According to the technical solution of the present invention, a method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes is provided, which includes the following steps: Step S1: Obtain the negative electrode sheet of the waste battery, and purify the graphite in the negative electrode sheet to obtain a recycled graphite carbon source. Step S2: Mix the recycled graphite carbon source with lithium sulfate to obtain precursor powder; Step S3: The precursor powder is subjected to a high-temperature carbothermic reduction reaction under an inert atmosphere to obtain the reduction product; Step S4: Cool the reduction product to obtain crude lithium sulfide.
[0006] A further improvement of the present invention is that step S1 specifically includes the following steps: Step S11: Discharge and physically disassemble the waste batteries to obtain the negative electrode sheet; Step S12: Immerse the negative electrode sheet in an organic solution to remove the graphite powder inside the negative electrode sheet, filter the organic solution to obtain graphite powder; Step S13: Add the graphite powder to an inorganic acid solution for acid washing; Step S14: The acid-washed graphite powder is washed with water until neutral and then dried to obtain the recovered graphite carbon source.
[0007] A further improvement of the present invention is that the organic solution is one or a mixture of several of N-methylpyrrolidone, N,N-dimethylformamide, or dimethyl carbonate.
[0008] A further improvement of the present invention is that the molar ratio of the recovered graphite carbon source to the lithium sulfate is 1:2 to 1:3.
[0009] A further improvement of the present invention is that the temperature of the high-temperature carbothermal reduction reaction is 750℃~950℃, and the holding time of the high-temperature carbothermal reduction reaction is 2h~8h.
[0010] A further improvement of the present invention is that the inert atmosphere is nitrogen or argon.
[0011] A further improvement of the present invention is that: in step S2, the recovered graphite carbon source is mixed with lithium sulfate using dry ball milling or wet ball milling.
[0012] A further improvement of the present invention is that: the wet ball milling uses anhydrous ethanol or isopropanol as the ball milling medium, the ball-to-material mass ratio is 10:1 to 30:1, the ball milling speed is 200 rpm to 500 rpm, and the ball milling time is 60°C to 90°C.
[0013] A further improvement of the present invention is that step S3 specifically includes the following steps: Step S31: Load the precursor into a high-temperature resistant reaction vessel and place the high-temperature resistant reaction vessel in a heating furnace; Step S32: Inert gas is introduced into the heating furnace until all the air in the heating furnace is exhausted; Step S33: Heat to the target temperature for high-temperature carbothermic reduction reaction at a heating rate of 2℃ / min to 10℃ / min, and maintain the target temperature for a preset time.
[0014] A further improvement of the present invention is that it also includes step S5: adding the crude lithium sulfide to anhydrous ethanol and stirring, filtering the stirred anhydrous ethanol solution to obtain a filtrate, heating the filtrate under vacuum until the anhydrous ethanol evaporates, and obtaining lithium sulfide powder with a purity of greater than or equal to 99%.
[0015] Compared with the prior art, the above-mentioned technical solution of the present invention has the following beneficial technical effects: 1. This invention solves the problem of high production costs caused by the reliance on expensive commercial high-purity carbon powder in the traditional carbothermal reduction method for lithium sulfide preparation. It involves purifying graphite from waste battery negative electrode sheets and using it as a carbon source, mixing it with lithium sulfate, and then conducting a high-temperature carbothermal reduction reaction under an inert atmosphere. Simultaneously, it addresses the resource waste and environmental pollution problems caused by the low recycling rate of waste battery negative electrode graphite, which is often downgraded or directly discarded. This achieves high-value-added resource utilization of waste negative electrode graphite and significantly reduces the preparation cost of lithium sulfide, a core raw material for all-solid-state batteries.
[0016] 2. This invention, through steps S11 to S14, employs a combined purification process involving discharge disassembly, organic solvent immersion and removal, inorganic acid washing, and water washing to neutrality followed by drying. This solves the problem of effectively removing residual binders, metallic impurities, and solid electrolyte interfacial film components from waste battery negative electrode graphite. It achieves highly efficient purification of waste negative electrode graphite, obtaining a high-purity recycled graphite carbon source. This provides clean and highly reactive carbon raw materials for subsequent carbothermic reduction reactions, ensuring the purity and quality of lithium sulfide products.
[0017] 3. This invention solves the process problem of ineffective dissolution and peeling of binders such as PVDF or SBR in the negative electrode sheet, which prevents graphite powder from completely detaching from the copper foil current collector, by using N-methylpyrrolidone, N,N-dimethylformamide, or dimethyl carbonate as organic solvents to soak the negative electrode sheet. This achieves efficient and complete detachment and separation of graphite powder, and the aforementioned organic solvents can be recycled and reused, reducing environmental pollution and improving the recovery efficiency of negative electrode graphite and the yield of recovered graphite powder.
[0018] 4. This invention solves the technical problem of incomplete reduction of lithium sulfate in the carbothermic reduction reaction due to insufficient carbon source, which leads to residual lithium sulfate impurities in the product and affects the purity of lithium sulfide. This is achieved by controlling the molar ratio of recycled graphite carbon source to lithium sulfate within the range of 1:2 to 1:3, with a moderate excess of graphite. This ensures complete reduction of lithium sulfate, guarantees a high conversion rate, and avoids excessive carbon source causing excessive carbon impurities in subsequent products, thus increasing purification difficulty.
[0019] 5. This invention solves the dilemma of balancing incomplete carbothermic reduction reaction and low product conversion rate at excessively low temperatures, while excessively high temperatures lead to increased energy consumption and equipment burden, by controlling the carbothermic reduction reaction temperature to 750℃ to 950℃ and holding it at that temperature for 2 to 8 hours. It achieves efficient conversion of lithium sulfate to lithium sulfide within a relatively mild and energy-controllable temperature window, ensuring high crystallinity and purity of the product, while balancing production efficiency and energy costs.
[0020] 6. This invention solves the problem that the presence of oxygen or water vapor in the reaction system easily leads to the oxidation of the carbon source or the generated lithium sulfide at high temperatures, resulting in impurities and a decrease in product purity. By using high-purity nitrogen or argon as the inert protective atmosphere in the carbothermic reduction reaction process, this invention addresses the issue of decreased product purity due to the easy oxidation of the carbon source or generated lithium sulfide at high temperatures when oxygen or water vapor is present in the reaction system. The complete isolation of oxygen and water vapor throughout the reaction process ensures the smooth progress of the carbothermic reduction reaction and the chemical stability and high purity of the lithium sulfide product. Furthermore, nitrogen or argon is widely available and its cost is controllable.
[0021] 7. This invention solves the problem of uneven local reactions caused by the difficulty in achieving uniform molecular-level mixing due to the large differences in density and particle size between the two raw material powders, which are difficult to achieve with simple stirring. It utilizes dry or wet ball milling to mix the recovered graphite carbon source and lithium sulfate. This achieves close contact and high homogenization of the carbon and lithium sources at the microscale, ensuring that the carbothermic reduction reaction proceeds uniformly and fully in the solid state, significantly improving product consistency and conversion efficiency.
[0022] 8. This invention optimizes the specific parameters of the wet ball milling process to use anhydrous ethanol or isopropanol as the medium, a ball-to-material ratio of 10:1 to 30:1, a rotation speed of 200 to 500 rpm, and a temperature of 60°C to 90°C. This solves the process stability problems caused by improper parameters during wet ball milling, such as uneven material mixing, impurities introduced by grinding ball wear, or solvent residue. It achieves efficient and precise mixing of recovered graphite carbon source and lithium sulfate, and the medium is easily removed by subsequent vacuum drying, ensuring the purity and uniformity of the precursor powder.
[0023] 9. This invention, through steps S31 to S33, employs a process of charging, purging air with inert gas, and programmed heating to the target temperature at a rate of 2 to 10°C / min followed by holding. This solves the problems of uneven heating of the precursor, oxidation products from residual air in the furnace, and uncontrolled reaction or material splashing caused by excessively rapid heating. It achieves precise control and stable, uniform heating of the reaction process, ensuring high reproducibility of the carbothermic reduction reaction and batch stability of lithium sulfide products.
[0024] 10. This invention solves the key problem of unreacted carbon powder remaining in the crude lithium sulfide after carbothermic reduction due to excessive carbon source, which prevents the product purity from meeting battery-grade requirements. This is achieved by purifying the crude lithium sulfide by dissolving it in anhydrous ethanol, filtering to remove insoluble carbon impurities, and then evaporating the ethanol from the filtrate under vacuum. Utilizing the selective solubility difference between lithium sulfide and carbon (which is soluble in ethanol), the invention achieves efficient separation and removal of unreacted carbon, ultimately yielding battery-grade high-purity lithium sulfide powder with a purity of over 99%, meeting the stringent purity requirements of solid-state electrolytes. Attached Figure Description
[0025] The accompanying drawings are provided to better understand the invention and are not intended to unduly limit the scope of the invention. Wherein: Figure 1 This is the X-ray diffraction pattern of lithium sulfide prepared in Example 3; Figure 2 This is a scanning electron microscope image of the lithium sulfide prepared in Example 3; Figure 3 This is a physical image of the recycled graphite carbon source prepared in Example 1. Detailed Implementation
[0026] The following description, in conjunction with the accompanying drawings, illustrates exemplary embodiments of the present invention, including various details to aid understanding. These details should be considered merely exemplary. Therefore, those skilled in the art will recognize that various changes and modifications can be made to the embodiments described herein without departing from the scope and spirit of the invention. Similarly, for clarity and brevity, descriptions of well-known functions and structures are omitted in the following description.
[0027] This invention discloses a method for preparing lithium sulfide from recycled graphite in waste battery negative electrodes via carbothermic reduction, belonging to the field of solid waste recycling technology. The method includes the following steps: Step S1: Obtain the negative electrode sheet from the waste battery, purify the graphite within the negative electrode sheet to obtain a recycled graphite carbon source; Step S2: Mix the recycled graphite carbon source with lithium sulfate to obtain a precursor powder; Step S3: Perform a high-temperature carbothermic reduction reaction on the precursor powder under an inert atmosphere to obtain a reduction product; Step S4: Cool the reduction product to obtain crude lithium sulfide. This invention solves the problem of high production costs caused by the reliance on expensive commercial high-purity carbon powder in traditional carbothermic reduction methods for lithium sulfide preparation, by using purified graphite from waste battery negative electrode sheets as a carbon source, mixing it with lithium sulfate, and performing a high-temperature carbothermic reduction reaction under an inert atmosphere. It also addresses the low recycling rate of graphite from waste battery negative electrodes and the environmental pollution problem.
[0028] The technical solution of the present invention will be further described below with reference to the embodiments.
[0029] Example 1 This embodiment provides a method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes, which includes the following steps: Step S1: Obtain the negative electrode sheet of the waste battery, and purify the graphite in the negative electrode sheet to obtain a recycled graphite carbon source. Step S2: Mix the recycled graphite carbon source with lithium sulfate to obtain precursor powder; Step S3: The precursor powder is subjected to a high-temperature carbothermic reduction reaction under an inert atmosphere to obtain the reduction product; Step S4: Cool the reduction product to obtain crude lithium sulfide.
[0030] Specifically, the overall technical concept of the preparation method in this embodiment lies in constructing a complete, green, and low-cost conversion path from waste lithium-ion battery anode graphite to high-value-added lithium sulfide products. The preparation method first purifies the graphite in the waste anode sheet through step S1, effectively removing binders, residual metal impurities, and SEI film components, thereby obtaining a high-purity recycled graphite carbon source rich in structural defects. This solves the resource waste and environmental pollution problems caused by traditional downgrading or disposal of waste anode graphite, and utilizes the unique advantages of recycled graphite's numerous defects and high reactivity, providing a low-cost carbon source with superior performance to commercial graphite for the subsequent carbothermic reduction reaction. Step S2 uses mechanical mixing to thoroughly and uniformly mix the recycled graphite carbon source with lithium sulfate, ensuring close contact between the two reactants at the microscale, creating favorable kinetic conditions for the high-temperature solid-phase reaction. Step S3 involves a high-temperature carbothermal reduction reaction under an inert atmosphere. Utilizing the strong reducing properties of recycled graphite, the sulfate ions in lithium sulfate are gradually reduced to sulfide ions, while the graphite itself is oxidized to CO or CO2 gas and escapes, thus achieving the chemical conversion from lithium salt to lithium sulfide. Step S4, the cooling process, is carried out under inert gas protection, effectively preventing the high-temperature reduction products from being oxidized or hydrolyzed during cooling, ensuring the yield and purity of the crude lithium sulfide. This method is the first to use waste battery negative electrode graphite as the carbon source for carbothermal reduction to prepare lithium sulfide. It not only significantly reduces the production cost of lithium sulfide (by approximately 30%–50% compared to using commercial high-purity carbon sources), but also provides a high-value-added closed-loop recycling path for waste lithium battery negative electrode materials. Furthermore, the prepared lithium sulfide can serve as a key raw material for the sulfide solid electrolyte of all-solid-state lithium batteries, which is of great significance for promoting the sustainable development of the new energy materials industry.
[0031] Specifically, step S1 includes the following steps: Step S11: Discharge and physically disassemble the waste batteries to obtain the negative electrode sheet; Step S12: Immerse the negative electrode sheet in an organic solution, then remove the graphite powder from the negative electrode sheet, filter the organic solution, and obtain graphite powder; Step S13: Add the graphite powder to an inorganic acid solution for acid washing; Step S14: The acid-washed graphite powder is washed with water until neutral and then dried to obtain the recovered graphite carbon source.
[0032] Specifically, in step S12, the negative electrode sheet is immersed in an organic solvent and ultrasonically treated at 25°C to 80°C for 0.5 to 3 hours to completely detach the graphite powder from the current collector (copper foil). The organic solvent is one or a mixture of N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), or dimethyl carbonate (DMC). The purpose of this step is to utilize the good dissolving power of the organic solvent for the binder (such as polyvinylidene fluoride PVDF or styrene-butadiene rubber SBR), combined with the cavitation effect and mechanical vibration of the ultrasonic treatment, to effectively destroy the cross-linked network structure of the binder, thereby completely peeling off the graphite powder from the surface of the copper foil current collector. Compared with simple heat treatment or mechanical peeling, the ultrasonic-assisted solvent peeling method has significant advantages such as mild operating conditions, minimal damage to the graphite layered structure, and high peeling efficiency, and can preserve the original morphology and structural characteristics of the recovered graphite to the greatest extent.
[0033] Specifically, in step S13, the filtered and collected graphite powder is added to an inorganic acid solution and mechanically stirred and leached at 25℃~60℃ for 1h~6h to dissolve and remove residual copper, iron, aluminum, and other metallic impurities, as well as solid electrolyte interphase (SEI) membrane components. The inorganic acid is hydrochloric acid, sulfuric acid, or nitric acid, with a concentration of 0.5mol / L~3.0 mol / L. The solid-liquid ratio of the graphite powder to the inorganic acid solution is controlled at 10g / L~50 g / L. The core purpose of this acid leaching step is to dissolve and remove copper (mainly from residual copper foil in the current collector), iron, aluminum, nickel, cobalt (possibly from cross-contamination of the cathode material), and lithium salts (such as Li2CO3, LiF, etc.) from the waste graphite through the chemical reaction between the inorganic acid and the metallic impurities. Mechanical stirring enhances the mass transfer process between the solid and liquid phases, increases the kinetic rate of the acid leaching reaction, and ensures that the metallic impurities are fully leached out. This step significantly improves the purity of the recovered graphite, laying the foundation for the smooth progress of the subsequent carbothermic reduction reaction.
[0034] Specifically, in step S14: the acid-washed graphite powder is filtered, washed multiple times with deionized water until the pH of the filtrate is 6.5–7.5, and then dried in a vacuum drying oven at 80°C–120°C for 10–24 hours to obtain a high-purity recovered graphite carbon source, such as… Figure 3As shown. Washing to neutrality with water thoroughly removes residual acid and soluble metal salts from the graphite powder surface, preventing adverse effects of residual acid on subsequent mixing and high-temperature reaction processes. Vacuum drying effectively removes adsorbed moisture from the graphite powder at lower temperatures, avoiding oxidation of the graphite surface caused by high-temperature drying. The recovered graphite carbon source obtained through the above purification process meets the purity requirements of the carbothermic reduction reaction. Furthermore, due to the expansion and defect formation of the interlayer structure during long-term charge-discharge cycles, the waste graphite exhibits higher reactivity than conventional commercial graphite.
[0035] Specifically, the molar ratio of the recovered graphite carbon source to the lithium sulfate is 1:2 to 1:3.
[0036] Specifically, the temperature during the high-temperature carbothermic reduction reaction is 750℃~950℃, and the holding time during the high-temperature carbothermic reduction reaction is 2h~8h.
[0037] Specifically, the inert atmosphere is nitrogen or argon, and the purity of the inert gas is greater than or equal to 99.99%.
[0038] Specifically, in step S2 of 1, the recovered graphite carbon source is mixed with lithium sulfate using dry ball milling or wet ball milling.
[0039] Specifically, the wet ball milling uses anhydrous ethanol or isopropanol as the milling medium, the ball-to-material mass ratio is 10:1 to 30:1, the milling speed is 200 rpm to 500 rpm, and the milling time is 60°C to 90°C.
[0040] Specifically, step S3 includes the following steps: Step S31: Load the precursor into a high-temperature resistant reaction vessel and place the high-temperature resistant reaction vessel in a heating furnace; Step S32: Inert gas is introduced into the heating furnace until all the air in the heating furnace is exhausted; Step S33: Heat to the target temperature for high-temperature carbothermic reduction reaction at a heating rate of 2℃ / min to 10℃ / min, and maintain the target temperature for a preset time.
[0041] Specifically, in step S31, the high-temperature resistant reaction vessel is either a corundum boat or a graphite boat, and the heating furnace is any one of a tube furnace, a rotary kiln, or a pusher kiln. Corundum boats possess excellent high-temperature resistance and chemical stability, maintaining structural integrity under a high-temperature reducing atmosphere and not reacting chemically with reactants or products. Graphite boats, on the other hand, have good thermal conductivity and thermal shock resistance, and being a carbon material themselves, they do not introduce additional impurities into the reaction system. Tube furnaces are suitable for small-batch preparation at the laboratory scale, while rotary kilns and pusher kilns are suitable for continuous industrial production, and can be flexibly selected according to the actual production scale.
[0042] Specifically, in step S32, when the inert gas is introduced, the gas flow rate is controlled at 100 mL / min to 500 mL / min, and the purging time is 30 min to 60 min. The purpose of this step is to completely remove the air (especially oxygen and water vapor) from the heating furnace through continuous purging with high-purity inert gas, thereby creating a strictly oxygen-free atmosphere for the carbothermic reduction reaction. The presence of oxygen and water vapor not only oxidizes and recycles the graphite carbon source, causing additional loss of the carbon source, but may also oxidize the lithium sulfide generated in the reaction into byproducts such as lithium sulfate or sulfite, seriously affecting the purity and yield of the product. Therefore, sufficient atmosphere replacement is a key prerequisite for ensuring the smooth progress of the carbothermic reduction reaction.
[0043] Specifically, in step S33, under continuous protection of an inert gas, the temperature is increased to a reaction temperature of 750℃~950℃ (preferably 800℃~850℃) at a heating rate of 2℃ / min~10℃ / min, and then held at this temperature for 2~8 hours (preferably 4~6 hours). During this process, the carbon recovered from the graphite undergoes a carbothermic reduction reaction with lithium sulfate to generate lithium sulfide and carbon dioxide / carbon monoxide gas. This step is the core of the entire preparation method, and its working principle is as follows: under high temperature conditions, lithium sulfate (Li2SO4) first undergoes thermal decomposition to generate intermediate products such as sulfur dioxide (SO2) and lithium oxide (Li2O); subsequently, the carbon recovered from the graphite is used as a reducing agent to gradually reduce the sulfate ions in the intermediate products to sulfide ions (S²). - Simultaneously, carbon itself is oxidized into CO or CO2 gas and escapes. Controlling the appropriate heating rate is beneficial for the reactants to fully contact and react during the heating process, avoiding uneven reaction or localized overheating due to excessively rapid heating. The isothermal holding stage is the critical period for the full progress of the carbothermal reduction reaction; a sufficiently long holding time ensures that lithium sulfate is completely reduced to lithium sulfide. Furthermore, the abundant defect structures in waste negative electrode graphite provide more active reaction sites, helping to lower the activation energy of the carbothermal reduction reaction, allowing the reaction to proceed efficiently at relatively low temperatures.
[0044] Specifically, in step S4, after the reaction is complete, heating is stopped, and the furnace is allowed to cool naturally to room temperature (≤30°C) under the protection of continuous inert gas circulation. The reaction vessel is then transferred to a glove box filled with high-purity argon (water and oxygen content <1 ppm) for product collection, yielding crude lithium sulfide. The purpose of continuously circulating inert gas during natural cooling is to prevent the high-temperature product from oxidizing or hydrolyzing due to contact with oxygen and water vapor in the air during the cooling stage. Lithium sulfide is highly sensitive to water and oxygen, readily reacting with water to form hydrogen sulfide (H2S) and lithium hydroxide, and reacting with oxygen to form lithium sulfate or sulfite. Therefore, the entire cooling and collection process must be carried out under strictly anhydrous and oxygen-free conditions. The environment in the glove box, where water and oxygen content are both below 1 ppm, ensures that the crude lithium sulfide does not deteriorate during collection, guaranteeing the purity and quality of the product.
[0045] Specifically, step S5 includes: in a glove box, the crude lithium sulfide is added to anhydrous ethanol and stirred. After stirring at room temperature for 1-3 hours, the mixture is filtered. The filtered anhydrous ethanol solution yields a filtrate. Under vacuum conditions, the filtrate is heated to 80°C-150°C to evaporate the anhydrous ethanol, yielding lithium sulfide powder with a purity of ≥99%. The basic principle of this purification step is based on the difference in solubility between lithium sulfide, which is soluble in anhydrous ethanol, and unreacted carbon (graphite), which is insoluble in ethanol. By stirring, the crude lithium sulfide is fully dissolved in anhydrous ethanol to form a homogeneous lithium sulfide-ethanol solution, while the excess unreduced carbon powder remains suspended in the solution in solid form. Subsequently, filtration effectively separates the solid carbon powder from the lithium sulfide solution. During the process of heating and evaporating the solvent under vacuum conditions, the vacuum environment significantly lowers the boiling point of ethanol, allowing the solvent to evaporate rapidly at a lower temperature, avoiding side reactions or decomposition of lithium sulfide caused by high-temperature heating. After this purification step, battery-grade high-purity lithium sulfide powder with a purity of not less than 99% can be obtained, which meets the purity requirements of key raw materials for the preparation of sulfide solid electrolytes for all-solid-state lithium batteries.
[0046] Example 2 This embodiment provides a process for recycling and processing graphite from battery negative electrodes, which includes the following steps: Battery physical dismantling: The collected waste lithium-ion batteries are immersed in a 3%–10% sodium chloride (NaCl) or sodium sulfate (Na2SO4) aqueous solution for 12–24 hours to completely discharge them and eliminate the risk of short circuits and fire. After discharge, the batteries are mechanically cut or manually dismantled to separate the casing, separator, positive electrode, and negative electrode. The negative electrode is collected for later use.
[0047] Anode material stripping: The collected anode sheets are cut to appropriate sizes and immersed in an organic solvent. The organic solvent is preferably N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), or dimethyl carbonate (DMC). The solution is treated with an ultrasonic cleaner for 0.5–3 hours at a water bath temperature of 25°C–80°C (preferably 60°C). The ultrasonic cavitation combined with the solvent's dissolving power effectively breaks down the cross-linking network of binders such as polyvinylidene fluoride (PVDF) or styrene-butadiene rubber (SBR), allowing the anode graphite powder to completely detach from the copper foil current collector. The detached mixture is then filtered through a sieve (e.g., 100 mesh) to remove copper foil fragments. The suspension is then centrifuged or filtered to obtain preliminary coarse graphite powder.
[0048] Acid washing (removal of metal ions) and drying: The graphite powder directly stripped after heat treatment is added to an inorganic acid solution. The inorganic acid is hydrochloric acid (HCl), sulfuric acid (H2SO4), or nitric acid (HNO3), with a concentration controlled at 0.5–3.0 mol / L. The solid-liquid ratio is controlled at 10–50 g / L, and mechanical stirring is performed at 25℃–60℃ for 1–6 hours. This process can effectively dissolve and remove copper (from the current collector), iron, aluminum, nickel, cobalt (from cross-contamination at the positive electrode), and lithium salts (such as Li2CO3, LiF, etc.) impurities trapped in the graphite. The acid-washed graphite powder is then filtered, and the filter cake is repeatedly washed with a large amount of deionized water until the pH of the washing filtrate reaches 6.5–7.5, and no precipitate is formed upon the addition of silver nitrate (if acid washing with hydrochloric acid) or barium chloride (if acid washing with sulfuric acid), ensuring no residual acid or metal salts. The washed graphite powder was placed in a vacuum drying oven and dried at 80℃~120℃ for 10~24 hours to completely remove moisture. The dried block material was then lightly ground and passed through a 200~400 mesh sieve to obtain recycled graphite powder with uniform particle size, high purity, and rich surface defects, which was used as the carbon source for the subsequent carbothermic reduction reaction.
[0049] Example 3 This embodiment provides a carbothermal reduction method for preparing lithium sulfide. The X-ray diffraction pattern of the lithium sulfide prepared in this embodiment is shown below. Figure 1 As shown, all peak positions are completely consistent with the characteristic peak positions of lithium sulfide, and no other impurity peak positions appear. The scanning electron microscope image of the lithium sulfide prepared in this embodiment is shown below. Figure 2 As shown, the high-purity lithium sulfide particles obtained are at the micron level and vary in size. The process includes the following steps: Precursor mixing: Weigh the lithium sulfate and recycled graphite according to a molar ratio of 1:2.05 to 1:3.5 (with a slight excess of carbon source to ensure complete reduction). Place both into a pulverizer, pulverize for 10-30 minutes, and dry to obtain precursor powder.
[0050] Carbothermic reduction: The precursor powder is loaded into an alumina boat and pushed into a tube furnace. High-purity argon / nitrogen gas (flow rate 200 mL / min) is introduced, and the temperature is increased to 750-900℃ at a heating rate of 2-10℃ / min, and held at that temperature for 2-4 hours.
[0051] Cooling and product collection: The product was cooled to room temperature under the protection of high-purity argon / nitrogen, and then transferred to a glove box for collection. XRD analysis showed that the product was pure phase lithium sulfide (Li2S) with no obvious impurity peaks.
[0052] Product purification: In a glove box, add crude lithium sulfide to anhydrous ethanol (lithium sulfide is soluble in ethanol, while the residual graphite carbon is insoluble). Stir magnetically at room temperature for 1–3 hours to ensure complete dissolution.
[0053] Filtration and drying: A microporous membrane is used for vacuum filtration to remove unreacted black carbon powder. The clear filtrate is collected and heated to 200℃~600℃ under vacuum or argon protection to evaporate and remove the ethanol solvent. After complete solvent evaporation, battery-grade high-purity white lithium sulfide (Li2S) powder with a purity of approximately 99.95% is obtained.
[0054] Those skilled in the art will clearly understand that, for the sake of convenience and brevity, the above-described division of functional units and modules is merely an example. In practical applications, the above functions can be assigned to different functional units and modules as needed, that is, the internal structure of the device can be divided into different functional units or modules to complete all or part of the functions described above. The functional units and modules in the embodiments can be integrated into one processing unit, or each unit can exist physically separately, or two or more units can be integrated into one unit. The integrated unit can be implemented in hardware or as a software functional unit. Furthermore, the specific names of the functional units and modules are only for easy differentiation and are not intended to limit the scope of protection of this application. The specific working process of the units and modules in the above system can be referred to the corresponding process in the foregoing method embodiments, and will not be repeated here.
[0055] The specific embodiments described above do not constitute a limitation on the scope of protection of this invention. Those skilled in the art should understand that various modifications, combinations, sub-combinations, and substitutions can occur depending on design requirements and other factors. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this invention should be included within the scope of protection of this invention.
Claims
1. A method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes, characterized in that, Includes the following steps: Step S1: Obtain the negative electrode sheet of the waste battery, and purify the graphite in the negative electrode sheet to obtain a recycled graphite carbon source. Step S2: Mix the recycled graphite carbon source with lithium sulfate to obtain precursor powder; Step S3: The precursor powder is subjected to a high-temperature carbothermic reduction reaction under an inert atmosphere to obtain the reduction product; Step S4: Cool the reduction product to obtain crude lithium sulfide.
2. The method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes according to claim 1, characterized in that, Step S1 specifically includes the following steps: Step S11: Discharge and physically disassemble the waste batteries to obtain the negative electrode sheet; Step S12: Immerse the negative electrode sheet in an organic solution to remove the graphite powder inside the negative electrode sheet, filter the organic solution to obtain graphite powder; Step S13: Add the graphite powder to an inorganic acid solution for acid washing; Step S14: The acid-washed graphite powder is washed with water until neutral and then dried to obtain the recovered graphite carbon source.
3. The method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes according to claim 2, characterized in that, The organic solution is one or a mixture of several of N-methylpyrrolidone, N,N-dimethylformamide, or dimethyl carbonate.
4. The method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes according to claim 1, characterized in that, The molar ratio of the recovered graphite carbon source to the lithium sulfate is 1:2 to 1:
3.
5. The method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes according to claim 1, characterized in that, The temperature during the high-temperature carbothermic reduction reaction is 750℃~950℃, and the holding time during the high-temperature carbothermic reduction reaction is 2h~8h.
6. The method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes according to claim 1, characterized in that, The inert atmosphere is nitrogen or argon.
7. The method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes according to claim 1, characterized in that, In step S2, the recovered graphite carbon source is mixed with lithium sulfate using dry ball milling or wet ball milling.
8. The method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes according to claim 7, characterized in that, The wet ball milling uses anhydrous ethanol or isopropanol as the milling medium, with a ball-to-material mass ratio of 10:1 to 30:1, a milling speed of 200 rpm to 500 rpm, and a milling time of 60°C to 90°C.
9. The method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes according to claim 1, characterized in that, Step S3 specifically includes the following steps: Step S31: Load the precursor into a high-temperature resistant reaction vessel and place the high-temperature resistant reaction vessel in a heating furnace; Step S32: Inert gas is introduced into the heating furnace until all the air in the heating furnace is exhausted; Step S33: Heat to the target temperature for high-temperature carbothermic reduction reaction at a heating rate of 2℃ / min to 10℃ / min, and maintain the target temperature for a preset time.
10. The method for preparing lithium sulfide by carbothermic reduction of graphite recovered from waste battery negative electrodes according to claim 1, characterized in that, The method also includes step S5: adding the crude lithium sulfide to anhydrous ethanol and stirring, filtering the stirred anhydrous ethanol solution to obtain a filtrate, heating the filtrate under vacuum until the anhydrous ethanol evaporates, and obtaining lithium sulfide powder with a purity of greater than or equal to 99%.