Anatase associated silicon extraction and nano-silicon oxide photochemical synthesis process

By combining ball milling with dilute hydrochloric acid, reflux with concentrated sulfuric acid, and alkali dissolution with photothermal spraying via a fluidized bed, selective separation and high-value utilization of titanium, iron, aluminum, and silicon components in low-grade ilmenite were achieved, solving the problem of unutilized silicon components and producing high-performance nano-silica powder.

CN123061968APending Publication Date: 2026-11-10TECHNICAL INST OF PHYSICS & CHEMISTRY - CHINESE ACAD OF SCI +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611556904.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies struggle to selectively separate titanium, iron, aluminum, and silicon components in low-grade symbiotic ilmenite without relying on complex physical beneficiation pretreatment. This results in the silicon component not being utilized at high value, and traditional processes pose environmental risks and waste resources.

Method used

Selective stepwise separation of titanium, iron, aluminum, and silicon components was achieved by ball milling with dilute hydrochloric acid for pre-removal of impurities, deep extraction of titanium and iron by reflux with concentrated sulfuric acid, preparation of silicate solution by alkali dissolution, and photofluidized bed photothermal spraying. Monodisperse nano-silica powder was then prepared via a peroxidation-photochemical route.

Benefits of technology

This approach achieves source reduction of silicon slag solid waste, improves the overall utilization rate of mineral resources, produces high-value-added nano-silica products, and avoids environmental risks and resource waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123061968A_ABST
    Figure CN123061968A_ABST
Patent Text Reader

Abstract

The application discloses a kind of anatase associated silicon extraction and nano-silica photochemical synthesis process, comprising the following steps: (1) dilute hydrochloric acid ball milling pre-impurity removal;(2) concentrated sulfuric acid reflux depth titanium removal iron;(3) preparation of silicate solution by alkali solution;(4) preparation of peroxysilicate precursor solution;(5) nano-silica is photochemically synthesized by photo-fluidized bed photo-thermal spray.The process is selective step-by-step separation of titanium, iron, aluminum, silicon components in low-grade symbiotic ilmenite, which makes silicon component directional enrichment and selective dissolution, and the obtained mineral source sodium silicate solution containing a small amount of sodium metaaluminate impurities is directly used as silicon source, and monodisperse, high specific surface area nano-silica powder is prepared by peroxide-photochemical route, so as to realize the resource high-value utilization of silicon component in low-grade ilmenite, and reduce the discharge of silicon slag solid waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of ilmenite solid waste resource utilization and nano-inorganic silicon material preparation technology, specifically to a stepwise separation and extraction method for silicon components in low-grade anatase ilmenite, and a method for preparing monodisperse nano-silicon oxide using mineral-derived sodium silicate solution as raw material under alkaline conditions through alkaline leaching-peroxidation-photofluidized bed photothermal spray decomposition. Background Technology

[0002] my country possesses vast titanium ore reserves, but the ore grade is generally low, with titanium, iron, aluminum, and silicon closely intergrown and symbiotic. Low-grade anatase-type ilmenite, exemplified by the Yanxigou mining area in Ya'an, Sichuan, has high silica content and a poor compatibility with conventional beneficiation processes due to its titanium-to-iron ratio. Conventional physical beneficiation methods such as gravity separation, magnetic separation, and electrostatic separation are insufficient for effectively separating and enriching the titanium components.

[0003] The industry commonly uses acid leaching to process this type of ore: first, titanium and iron components are dissolved by acid leaching, and then the leachate is hydrolyzed or extracted to recover titanium. This process generates a large amount of silica-containing leaching slag (silicon slag) while extracting titanium and iron components. The stockpiling of silicon slag not only occupies a large amount of land but also poses environmental risks such as dust diffusion and salt rainwater leaching and leakage. Furthermore, the resource value of the silicon components is not utilized, resulting in low overall ore utilization, which has become a prominent issue restricting the economic benefits and environmental compliance of low-grade ilmenite processing projects.

[0004] Therefore, the key to improving the comprehensive utilization rate of this type of mineral resource and reducing solid waste emissions lies in how to directionally separate the silicon component from low-grade symbiotic ilmenite and further transform it into high-value-added nano-silica products without relying on complex physical mineral beneficiation pretreatment.

[0005] Various reaction processes have been explored in existing technologies. For example, the technical solution in CN122850338A involves feeding iron ore tailings into a spiral sluice for gravity separation to obtain gravity concentrate and gravity tailings. The gravity concentrate is then screened into coarse and fine concentrates. The fine concentrate is then subjected to dry high-intensity magnetic upgrading, and the resulting dry magnetic titanium middlings are returned to the upgrading process. The coarse concentrate and dry magnetic titanium concentrate are combined to obtain titanium concentrate. This solution mainly addresses the problems of poor enrichment effect, long process, and low titanium recovery rate in iron ore tailings with low TiO2 grade. This solution belongs to a purely physical beneficiation route, which only achieves the enrichment and recovery of titanium components. The silicon components in the ore still all enter the tailings. For low-grade ores with densely embedded multi-element components and low individual liberation, the enrichment effect and recovery rate of physical beneficiation are limited, and it is also impossible to achieve high-value utilization of silicon components.

[0006] The technical solution in CN122853846A first involves acid washing to extract iron from iron tailings and alkali dissolution to extract silicon, separating the silicon-containing alkali leachate and tailings residue. After purification, the pH of the leachate is adjusted to obtain amorphous nano-silica sol. The residue is then activated by alkali and modified with a silane coupling agent to obtain functionalized products. The end product of this solution is the preparation of building insulation materials by combining nano-silica sol with fibers, not the preparation of monodisperse nano-silica powder. Furthermore, the acid washing target is iron tailings, which does not involve the selective and stepwise separation of the four components (titanium, aluminum, iron, and silicon) in ilmenite, making it difficult to directly use in powder form as a rubber reinforcing filler or a coating matting filler.

[0007] However, the above-mentioned existing technologies have the following common problems: (1) Physical beneficiation routes have no solution for silicon components. (2) Fluorine / strong acid desiliconization routes have high environmental costs and silicon is not valued. (3) The "acid washing-alkali dissolution for silicon extraction" route stops at sol and does not solve the problem of mineral impurities. (4) Existing nano-silica preparation routes have poor adaptability to mineral sodium silicate and are prone to hard agglomeration. (5) There is a "last mile" gap in the high-value utilization of mineral sodium silicate. In the existing technologies, the sodium silicate solution obtained by alkali dissolution of silicon-containing solid waste is either used to make low-value-added products such as water glass and white carbon black, or it needs to be deeply purified by resin / flocculation before it can be used for nano-silica preparation; there is a lack of an integrated process that can directly use mineral sodium silicate solution containing a small amount of sodium aluminate impurities as raw material and the product is a monodisperse high specific surface area powder. Summary of the Invention

[0008] To address the shortcomings of the existing technologies, the technical problem to be solved by this invention is: how to selectively and stepwise separate the titanium, iron, aluminum, and silicon components of low-grade symbiotic ilmenite without relying on complex physical beneficiation pretreatment, so that the silicon component is directionally enriched and selectively dissolved, and the resulting mineral-source sodium silicate solution containing a small amount of sodium aluminate impurities is directly used as the silicon source to prepare monodisperse, high specific surface area nano-silica powder through a peroxidation-photochemical route, thereby realizing the high-value resource utilization of silicon components in low-grade ilmenite and reducing the emission of silicon slag solid waste.

[0009] To address the aforementioned technical problems, this invention provides a process for the extraction of anatase-associated silica and the photochemical synthesis of nano-silica, comprising the following steps: (1) Pre-removal of impurities by ball milling with dilute hydrochloric acid 1.1 Ore pretreatment: The low-grade anatase-type ilmenite ore is coarsely crushed to obtain ilmenite particles.

[0010] 1.2 Pre-removal of impurities by ball milling with hydrochloric acid: The ilmenite particles obtained in step 1.1 are simultaneously added to a planetary ball mill with dilute hydrochloric acid and ball milling is carried out at room temperature. During the leaching process, aluminum and iron impurities in the ore are leached out by dilute hydrochloric acid and enter the liquid phase, while silicon and titanium components are resistant to dilute acid and remain in the solid residue. After ball milling, solid-liquid separation is carried out, and the acidic leaching solution containing iron and aluminum is discarded to obtain silicon-titanium enriched solid material.

[0011] (2) Deep titanium extraction and iron removal by concentrated sulfuric acid reflux The silicon-titanium enriched solid material obtained in step (1) is mixed with a concentrated sulfuric acid system and refluxed. During the reaction, the iron and titanium components in the material are leached out by concentrated sulfuric acid and enter the liquid phase, while the silicon component remains in the solid phase. After the reaction is completed, the mixture is cooled and the solid and liquid are separated to remove the titanium-iron sulfuric acid leaching solution and obtain silicon-rich residue.

[0012] (3) Preparation of silicate solution by alkaline dissolution The silicon-rich residue obtained in step (2) is added to sodium hydroxide solution for atmospheric pressure reflux reaction. During the reaction, the silicon dioxide in the silicon-rich residue reacts with sodium hydroxide to generate sodium silicate and enters the liquid phase. The titanium component is retained in the solid phase. The small amount of aluminum impurities remaining in the ore generates sodium aluminate and enters the liquid phase together. After the reaction is completed, the insoluble titanium-containing solid phase residue is removed by filtration to obtain an aqueous solution of sodium silicate containing a small amount of sodium aluminate impurities.

[0013] (4) Preparation of peroxide silicate precursor solution The sodium silicate aqueous solution obtained in step (3) is thoroughly mixed with hydrogen peroxide at a mass percentage concentration of 30% to obtain a peroxide silicate aqueous solution, i.e., peroxide silicate precursor solution.

[0014] (5) Photothermal spray photochemical synthesis of nano-silica in a fluidized bed The peroxide silicate precursor liquid obtained in step (4) is fed into the photofluidized bed device and sprayed out through the atomizing nozzle. Under photothermal conditions, hydrogen peroxide decomposes rapidly, and peroxide species undergo controllable nucleation and agglomeration precipitation. The gas-solid mixture after the reaction is collected by gas-solid separation to obtain monodisperse nano silica powder.

[0015] Preferably, the iron-aluminum acidic leachate generated in step (1) and the titanium-iron sulfuric acid leachate generated in step (2) can be used to recover valuable metal components of iron, aluminum and titanium, respectively; the titanium-containing solid residue obtained by filtration in step (3) can be returned to the titanium recovery process, so as to realize the full utilization of low-grade ilmenite mineral resources.

[0016] Preferably, in step 1.1, the ilmenite ore is coarsely crushed to particles with a diameter of less than 3 mm. If the particle size is too large (>3 mm), the specific surface area of ​​the mineral is insufficient during ball milling, the aluminum-iron minerals are not fully liberated, and the acid solution has difficulty penetrating into the interior of the particles.

[0017] Preferably, in step 1.2, the solid-liquid weight ratio of ilmenite particles to dilute hydrochloric acid is 1:5 to 1:20, more preferably 1:5 to 1:10, and even more preferably 1:5 to 1:6.

[0018] Preferably, in step 1.2, the concentration of hydrochloric acid is 1.0~6.5 mol / L, more preferably 3.0~6.0 mol / L.

[0019] Preferably, in step 1.2, the ball mill speed is 120~800 r / min, more preferably 450 r / min, and the ball milling time is 1~5h, more preferably 3.0h.

[0020] Preferably, in step (2), the mass fraction of concentrated sulfuric acid is 75%~95%, preferably 90%.

[0021] Preferably, in step (2), the solid-liquid weight ratio is 1:3 to 1:6, and more preferably 1:4.5 to 1:5.

[0022] Preferably, in step (2), the reflux temperature is 120~180 ℃, more preferably 160 ℃, and the reflux reaction time is 1~6h, more preferably 4.0 h.

[0023] Preferably, in step (3), the solid-liquid weight ratio is 1:2.5~1:8, more preferably 1:3.5~1:4, and the sodium hydroxide solution concentration is 1.5~6 mol / L, more preferably 5 mol / L.

[0024] Preferably, in step (3), the reflux temperature is 100~150 ℃, more preferably 110 ℃, and the reflux reaction time is 1~5h, more preferably 3.0 h.

[0025] Preferably, in step (4), the volume ratio of sodium silicate aqueous solution to hydrogen peroxide is 1:2.5 to 1:8, and more preferably 1:10.

[0026] Preferably, in step (4), the mixing time is 10~60 min, preferably 30 min.

[0027] Preferably, in step (5), the photothermal reaction temperature is preferably 130~140 ℃, more preferably 135 ℃; the atomization particle size, carrier gas flow rate and material residence time are set according to the scale of the photofluidized bed device, with the solvent evaporation time of droplets in the reaction zone and the nucleation time of silicon species matching each other as the criterion.

[0028] Beneficial effects Compared with the prior art, the present invention has the following advantages: Firstly, this invention achieves source reduction of silicon slag solid waste and full utilization of mineral resources. Addressing the industry pain point of large-scale silicon slag stockpiling resulting from traditional acid beneficiation of low-grade ilmenite, this invention employs a two-stage selective acid leaching process: ball milling with dilute hydrochloric acid for pre-removal and reflux with concentrated sulfuric acid. This process leaches and recovers valuable metal components such as iron, aluminum, and titanium from the ore in stages. The silicon component, originally discarded as solid waste, is no longer stockpiled as waste residue but is transformed into nano-silica products after alkali dissolution. This reduces the amount of silicon slag solid waste generated at the source, avoiding environmental risks such as land occupation, dust pollution, and salt rainwater leaching caused by silicon slag stockpiling.

[0029] Secondly, it breaks through the limitation that peroxidation-photochemical synthesis technology is only applicable to acidic d 0 Application boundaries of metal oxide systems. Existing peroxide-photochemical synthesis techniques are all based on acidic sol systems, relying on d... 0 After metals form soluble peroxide complexes, oxides are precipitated. This invention extends the peroxide-photochemical synthesis approach to silicon-based alkaline systems. A peroxide silicate precursor solution is directly prepared using a mineral-derived sodium silicate solution obtained under alkaline conditions. The nucleation and precipitation of silicon species are achieved in one step using a photofluidized bed photothermal spraying method, avoiding the technical path of direct gelation of silica under acidic conditions and the need to form a sol and then dry it in the sol-gel method.

[0030] Third, the product exhibits excellent dispersibility and structural properties, resulting in high added value. The nano-silica powder prepared via photochemical spray decomposition allows for in-situ decomposition of hydrogen peroxide within a photofluidized bed. Silicon species can undergo controllable nucleation and growth within the confined micro-units of the droplets, effectively suppressing hard bridging and hard agglomeration between particles. This yields silica powder with good monodispersity, no obvious hard agglomeration, and well-developed pore structure.

[0031] Fourth, it has strong raw material adaptability and does not require complex physical mineral processing pretreatment. Targeting the mineral characteristics of tightly embedded titanium, iron, aluminum, and silicon within ilmenite, this invention utilizes the differences in the solubility behavior of each component in dilute hydrochloric acid and concentrated sulfuric acid systems to achieve selective stepwise impurity removal. It has good applicability to low-grade, difficult-to-process symbiotic ilmenite. Simultaneously, the residual sodium aluminate impurity allowed in the alkali dissolution process allows the process to directly accept mineral-sourced sodium silicate solutions, eliminating the need for deep purification methods such as ion exchange resins and reducing silicon source costs. Attached Figure Description

[0032] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0033] Figure 1 This is a flowchart illustrating the overall process flow of anatase-associated silica extraction and nano-silica photochemical synthesis process according to the present invention.

[0034] Figure 2 This is a transmission electron microscope (TEM) image of the nano-silica powder prepared in Example 1.

[0035] Figure 3 This is a schematic diagram of the optical fluidized bed device used in this invention.

[0036] Figure 4 This is a schematic diagram of the structure of the photofluidized bed reaction tube in the multi-source photofluidized bed device of the present invention.

[0037] Figure 5 This is a partial isometric view of the multi-source optical fluidized bed device.

[0038] Figure 6 This is a partial cross-sectional view of the multi-source optical fluidized bed device.

[0039] Figure 1 Process flow description: Low-grade ilmenite ore (1) enters the dilute hydrochloric acid ball mill pre-purification unit (2) to separate iron and aluminum-containing acidic leachate (3) and silicon-titanium enriched solid material (4); silicon-titanium enriched solid material (4) is sent to the concentrated sulfuric acid reflux removal unit (5) to separate titanium and iron-containing sulfuric acid leachate (6) and silicon-rich residue (7); silicon-rich residue (7) enters the alkaline dissolution reaction unit (8) and is filtered to remove impurities (9) to obtain sodium silicate aqueous solution (10); sodium silicate aqueous solution (10) is sent to the hydrogen peroxide mixing unit (11) to prepare peroxide silicate precursor solution (12); precursor solution is passed into the photofluidized bed photothermal spray synthesis unit (13) and collected after reaction to obtain nano-silica powder product (14); iron and aluminum-containing acidic leachate (3) and titanium-containing iron-containing sulfuric acid leachate (6) are both used to recover valuable metal components of iron, aluminum and titanium.

[0040] Figure 3-6 The device structure is described in detail. For specific structure and process, please refer to the applicant's previous patent CN202611050770.6: 1. Air source; 2. Feeder; 3. Atomizing nozzle; 4. Photofluidized bed reactor; 41. Photofluidized bed reaction tube; 40. Discharge port; 42. Light source; 43. Concentrating lens jacket; 5. Primary cyclone separator; 6. Secondary cyclone separator; 7. Dust collection bag; and 8. Storage silo. Detailed Implementation

[0041] The present invention will now be described in detail. Before proceeding with the description, it should be understood that the terminology used in this specification and the appended claims should not be construed as limited to its general or dictionary meaning, but rather should be interpreted according to the meaning and concept corresponding to the technical aspects of the invention, based on the principle that the inventors are allowed to appropriately define the terms for the best interpretation. Therefore, the description presented herein is merely a preferred example for illustrative purposes and is not intended to limit the scope of the invention. It should be understood that other equivalents or modifications can be obtained from it without departing from the spirit and scope of the invention.

[0042] In this document, the terms “comprising,” “including,” “having,” “containing,” or any other similar terms are open-ended conjunctions intended to cover non-exclusive inclusions. For example, a composition or article containing a plurality of elements is not limited to those listed herein, but may also include other elements not explicitly listed but typically inherent to the composition or article. Furthermore, unless explicitly stated to the contrary, the term “or” is inclusive, not exclusive. For example, the condition “A or B” is satisfied in any of the following cases: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); A and B are both true (or exist). Moreover, in this document, the terms “comprising,” “including,” “having,” and “containing” should be interpreted as specifically disclosed and simultaneously cover closed or semi-closed conjunctions such as “composed of” and “substantially composed of.”

[0043] In this document, all features or conditions defined in the form of numerical ranges or percentage ranges are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible secondary ranges and individual values ​​within those ranges, particularly integer values. For example, a range description of "1 to 8" should be considered as specifically disclosing all secondary ranges such as 1 to 7, 2 to 8, 2 to 6, 3 to 6, 4 to 8, 3 to 8, etc., particularly secondary ranges defined by all integer values, and should be considered as specifically disclosing individual values ​​within those ranges such as 1, 2, 3, 4, 5, 6, 7, 8, etc. Unless otherwise specified, the foregoing interpretation applies to all content throughout this invention, regardless of its scope.

[0044] If a quantity or other numerical value or parameter is expressed as a range, a preferred range, or a series of upper and lower limits, it should be understood that this document has specifically disclosed all ranges consisting of any upper or preferred value of that range and the lower or preferred value of that range, regardless of whether such ranges are separately disclosed. Furthermore, when a range of numerical values ​​is mentioned herein, unless otherwise stated, the range shall include its endpoints and all integers and fractions within the range.

[0045] In this document, numerical values ​​are to be understood as having a precision with significant digits, provided that the purpose of the invention can be achieved. For example, the number 40.0 should be understood to cover a range from 39.50 to 40.49.

[0046] In the synthesis process according to the present invention: The purpose of step 1.2 is to achieve efficient dissolution of iron and aluminum impurities under mild acidity under the conditions of continuous new surface exposure and enhanced mass transfer provided by mechanical ball milling, while avoiding the loss of silicon and titanium components, thus creating a compositional prerequisite for subsequent selective separation. The preferred concentration of dilute hydrochloric acid is 5-6 mol / L: when the concentration is below 3 mol / L, the leaching rate and leaching percentage of aluminum and iron impurities decrease significantly, and simply extending the ball milling time is insufficient to compensate; when the concentration is above 6 mol / L, the increase in iron and aluminum leaching rates tends to plateau, while acid mist emission and equipment corrosion problems intensify, leading to decreased economic efficiency.

[0047] The purpose of step (3) is to achieve selective dissolution of silicon components and final separation of silicon and titanium, while bringing the small amount of aluminum that was not completely removed in the previous process into the liquid phase in the form of sodium aluminate, leaving a unified interface for impurity control in subsequent processes.

[0048] The purpose of step (4) is to introduce hydrogen peroxide into the alkaline silicate liquid phase system in advance to form an oxidizing precursor liquid, so that the in-situ decomposition of hydrogen peroxide and the nucleation and precipitation of silicon species occur synchronously in time and space during the subsequent photothermal spraying process, avoiding excessive local supersaturation caused by nucleation before decomposition.

[0049] The process of this invention targets low-grade ilmenite with associated aluminum, where the content of iron, aluminum, titanium, etc., is relatively low. Taking Yanxigou anatase ilmenite ore as an example, the component content is shown in Table 1 below: Table 1: Results of Multi-Element Chemical Analysis of Raw Ore

[0050] In addition, unless otherwise stated, the reagents and solvents disclosed below were purchased from Tianjin Zhiyuan Chemical Reagent Co., Ltd., Beijing Innocare Technology Co., Ltd., and Langfang Tuodi Chemical Co., Ltd.; the detection instruments used were a Varian 710-OES inductively coupled plasma atomic emission spectrometer, a Hitachi S-4800 scanning electron microscope, and a Bruker D8 Advance XRD diffractometer; the ball mill used was a Henan Tianwei Industrial Co., Ltd. planetary ball mill XQM-2A, and the centrifuge used was a Henan Beihong Industrial Co., Ltd. low-speed centrifuge TD5D.

[0051] The following embodiments are merely examples illustrating implementations of the present invention and do not constitute any limitation on the present invention. Those skilled in the art will understand that modifications made without departing from the spirit and concept of the present invention fall within the protection scope of the present invention. Unless otherwise specified, the reagents and instruments used in the following embodiments are commercially available products.

[0052] Example 1 1. Pre-treatment of ore: Take 1 kg of low-grade anatase ilmenite from Yanxigou, Ya'an, and crush it to particles with a diameter of less than 3 mm.

[0053] 2. Pre-removal of impurities by hydrochloric acid ball milling: Pretreated ilmenite particles are mixed with hydrochloric acid at a solid-liquid ratio of 1:6 and fed into a ball mill. The hydrochloric acid concentration is 6 mol / L, the ball mill speed is 450 r / min, and the ball milling time is 3.0 h. After ball milling, solid and liquid are separated, and the acidic leaching solution containing iron and aluminum is discarded, yielding silicon-titanium enriched solid phase material. ICP analysis shows that this step can leach more than 85% of aluminum and iron impurities in the ore, while titanium and silicon components remain in the solid phase.

[0054] 3. Deep Removal of Titanium and Iron by Concentrated Sulfuric Acid Reflux: The silicon-titanium enriched solid material obtained in the above steps was mixed with 90% concentrated sulfuric acid at a solid-liquid weight ratio of 1:5, and heated under reflux at 160 °C for 4.0 h. After the reaction was completed and cooled, the solid and liquid phases were separated, and the titanium-iron sulfuric acid leachate was removed to obtain a silicon-rich residue. ICP analysis showed that the SiO2 content in the silicon-rich residue reached 92.1%, and the total residual titanium and iron was less than 2.3%.

[0055] 4. Preparation of silicate solution by alkaline dissolution: Take 200 g of the silica-rich residue obtained in the above steps, mix it with sodium hydroxide solution at a solid-liquid weight ratio of 1:4, heat under reflux (5 mol / L sodium hydroxide solution concentration, reflux temperature 110 ℃, reflux reaction for 3.0 h). After the reaction is complete, separate the solid and liquid phases, remove the insoluble titanium-containing solid phase residue, and obtain an aqueous solution of sodium silicate containing a small amount of sodium aluminate impurities (mass fraction ≤1.5%).

[0056] 5. Preparation of peroxide silicate precursor solution: The sodium silicate aqueous solution obtained in the above steps is mixed with hydrogen peroxide (mass percentage concentration of 30%) at a volume ratio of 1:10 and stirred thoroughly for 30 min to obtain a clear peroxide silicate aqueous solution.

[0057] 6. Photothermal spray photochemical synthesis in a photofluidized bed: The silicate peroxide precursor liquid is transported to the photofluidized bed device, the photothermal reaction temperature is controlled at 135 ℃, and the precursor liquid is sprayed out using an atomizing nozzle; under photothermal conditions, hydrogen peroxide decomposes rapidly, silicon species are controlled to agglomerate and precipitate, and nano-silica powder is obtained by gas-solid separation.

[0058] The product obtained in this embodiment is monodisperse nano-silica, without obvious hard agglomerates, and has a narrow particle size distribution. It can be directly used in coatings, fillers, and adsorbent materials. See the appendix for details. Figure 2 .

[0059] Example 2 This embodiment examines the preparation of nano-silica powder under different solid-liquid ratios and hydrochloric acid concentrations.

[0060] 1. Mineral pretreatment: Same as the mineral pretreatment operation steps in Example 1.

[0061] 2. Pre-removal of impurities by hydrochloric acid ball milling: The pretreated ilmenite particles were mixed with hydrochloric acid at a solid-liquid weight ratio of 1:5 and fed into a ball mill. The hydrochloric acid concentration was 3 mol / L, the ball mill speed was 450 r / min, and the milling time was 3.0 h. Solid-liquid separation was performed, and the acidic leaching solution containing iron and aluminum was discarded, yielding a silicon-titanium enriched solid phase. ICP analysis showed that this step could leach more than 81% of aluminum and iron impurities from the ore, while titanium and silicon components remained in the solid phase.

[0062] 3. Deep Removal of Titanium-Iron by Concentrated Sulfuric Acid Reflux: The silicon-titanium enriched solid material obtained in the above steps was mixed with 90% concentrated sulfuric acid at a solid-liquid weight ratio of 1:4.5, and heated under reflux at 160 °C for 4.0 h. After cooling following the reaction, the solid and liquid phases were separated. Titanium and iron entered the sulfuric acid leaching solution, which can be used for subsequent recovery of titanium-iron resources. The solid phase was the silicon-rich residue. ICP analysis showed that the silicon-rich residue contained 90.4% SiO2 and 2.8% total titanium-iron residue.

[0063] 4. Preparation of silicate solution by alkaline dissolution: Take 200 g of the silica-rich residue obtained in the above steps, mix it with sodium hydroxide solution at a solid-liquid ratio of 1:3.5, heat under reflux (5 mol / L sodium hydroxide solution concentration, reflux temperature 110 ℃, reflux reaction for 3.0 h). After the reaction is complete, separate the solid and liquid phases, remove the titanium-containing solid phase residue, collect the filtrate to obtain sodium silicate solution, the filtrate contains a small amount of sodium aluminate impurity.

[0064] 5. Preparation of peroxide silicate precursor solution: Same as the operation steps for preparing peroxide silicate precursor solution in Example 1.

[0065] 6. Photohydrodynamic fluidized bed photothermal spray photochemical synthesis: Same as the operation steps of photohydrodynamic fluidized bed photothermal spray photochemical synthesis in Example 1.

[0066] The obtained nano-silica powder has good monodispersity, no hard agglomerates, and uniform particle size distribution, and can be used as a rubber reinforcing filler.

[0067] Example 3 1. Mineral pretreatment: Same as the mineral pretreatment operation steps in Example 1.

[0068] 2. Pre-removal of impurities by ball milling with hydrochloric acid: The operation steps for pre-removal of impurities by ball milling with hydrochloric acid are the same as those in Example 1.

[0069] 3. Removal of ferrotitanium by concentrated sulfuric acid reflux: The same procedure as in Example 1 for removing ferrotitanium by concentrated sulfuric acid reflux.

[0070] 4. Preparation of silicate solution by alkaline dissolution: The operation steps for preparing silicate solution by alkaline dissolution are the same as in Example 1.

[0071] 5. Preparation of peroxide silicate precursor solution: Same as the operation steps for preparing peroxide silicate precursor solution in Example 1.

[0072] 6. Photochemical synthesis by photothermal spraying in a photofluidized bed: The peroxide silicate precursor solution is fed into a photofluidized bed device, the photothermal reaction temperature is controlled at 100 ℃, and the photochemical reaction is carried out by atomization spraying; hydrogen peroxide decomposes, silicon species are precipitated in a controllable manner, and nano-silica powder is collected.

[0073] The obtained nano-silica powder has a small amount of slight agglomeration, and the overall particle size distribution is relatively uniform. The monodispersity is slightly lower than that under the conditions of Example 1, but it can still be used as a rubber reinforcing filler.

[0074] Comparative Example 1: Preparation of Silica by Traditional Acidification Precipitation Method 1. Mineral pretreatment: Same as the mineral pretreatment operation steps in Example 1.

[0075] 2. Pre-removal of impurities by ball milling with hydrochloric acid: The operation steps for pre-removal of impurities by ball milling with hydrochloric acid are the same as those in Example 1.

[0076] 3. Removal of ferrotitanium by concentrated sulfuric acid reflux: The same procedure as in Example 1 for removing ferrotitanium by concentrated sulfuric acid reflux.

[0077] 4. Preparation of silicate solution by alkaline dissolution: The operation steps for preparing silicate solution by alkaline dissolution are the same as in Example 1.

[0078] 5. Preparation of silica by conventional acid precipitation: Under stirring conditions at room temperature, a 10% (w / w) dilute sulfuric acid solution is slowly added dropwise to an aqueous sodium silicate solution, controlling the dropping rate and monitoring the pH of the system in real time, adjusting the pH to 8-9; after the addition is complete, the reaction is continued at a constant temperature and stirred for 1.5 h, during which sodium silicate undergoes a hydrolysis reaction to precipitate silica hydrate; after the reaction is completed, the mixture is allowed to stand for 2 h, the suspension is filtered, and the filter cake is washed multiple times with deionized water until the conductivity of the filtrate is stable; the filter cake is dried in an oven at 105 ℃ for 12 h, and then ground to obtain ordinary silica powder.

[0079] The resulting silica powder exhibited significant hard agglomeration and a wide particle size distribution. Comparative Example 1 used the exact same raw materials, pretreatment process, and sodium silicate solution as Example 1, differing only in the final silicon precipitation process. Therefore, the difference in product morphology between the two examples can be directly attributed to the difference in the precipitation process route.

[0080] Comparative Example 2 uses a conventional hydrofluoric acid leaching process (without ball milling). 1. Raw materials and leaching agents: High-silicon ilmenite with a SiO2 content of 2%~3.5% by mass is selected as raw material, and the ilmenite raw material is not subjected to ball milling pretreatment; hydrofluoric acid with a mass concentration of 40%~45% by mass is selected as leaching agent, wherein the silicon content is 0.7%~1.2% by mass.

[0081] 2. Hydrofluoric acid leaching: The above-mentioned ilmenite is added to the above-mentioned hydrofluoric acid for leaching. The molar amount of hydrofluoric acid is 1.08~1.12 times the total molar amount of titanium and silicon in the ilmenite. The reaction is carried out for 0.5~1.5 h, and then allowed to stand for 2~4 h. The feeding rate is 0.4~0.6 t / h. The leachate is obtained by filtration. Water is added during the leaching process. The amount of water added is based on the precipitation of unsaturated titanium crystals in the leachate. The TiO2 content in the leachate is controlled to be 155~170 g / L.

[0082] 3. Leachate purification and desiliconization: Take the above 3 m 3 Mix the leachate and add 0.44 mg of a saturated potassium chloride solution with a concentration of 259 g / L. 3 (The molar ratio of potassium chloride to silicon in the leachate was 1.6). The feeding time was controlled at 1.8 h, and after standing for 3 h, the solution was filtered and separated. 3.52 m³ of purified solution was obtained. 3 The SiO2 content was 1.12 g / L and the TiO2 content was 141.21 g / L; the by-product potassium fluorosilicate filter residue was 92.03 kg, and the potassium fluorosilicate purity was 98.7%.

[0083] In Comparative Example 2, silicon is removed by precipitation in the form of potassium fluorosilicate, which is a technical route of "removing silicon" rather than "using silicon", and requires the use of a hydrofluoric acid system.

[0084] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

[0085] References [1] Weng Yi, Wang Zhijian, Zheng Siwen, et al. A method for preparing potassium fluorotitanate with adjustable grade from high-silicon ilmenite [P]. Chinese Patent: CN102515261A, 2012-06-27.

Claims

1. A process for extracting anatase-associated silica and photochemically synthesizing nano-silica, comprising the following steps: (1) Pre-removal of impurities by ball milling with dilute hydrochloric acid 1.1 Ore pretreatment: The low-grade anatase-type ilmenite ore is coarsely crushed to obtain ilmenite particles; 1.2 Pre-removal of impurities by hydrochloric acid ball milling: The ilmenite particles obtained in step 1.1 are simultaneously added to a planetary ball mill with dilute hydrochloric acid, and ball milling leaching is carried out under normal temperature conditions. During the leaching process, aluminum and iron impurities in the ore are leached out by dilute hydrochloric acid and enter the liquid phase, while silicon and titanium components are resistant to dilute acid and remain in the solid residue. After ball milling, solid-liquid separation is carried out, and the acidic leaching solution containing iron and aluminum is discarded to obtain silicon-titanium enriched solid material. (2) Deep titanium extraction and iron removal by concentrated sulfuric acid reflux The silicon-titanium enriched solid material obtained in step (1) is mixed with a concentrated sulfuric acid system and refluxed. During the reaction, the iron and titanium components in the material are leached out by concentrated sulfuric acid and enter the liquid phase, while the silicon component remains in the solid phase. After the reaction is completed, the mixture is cooled and the solid and liquid are separated to remove the titanium-iron sulfuric acid leaching solution and obtain silicon-rich residue. (3) Preparation of silicate solution by alkaline dissolution The silicon-rich residue obtained in step (2) is added to sodium hydroxide solution for atmospheric pressure reflux reaction. During the reaction, the silicon dioxide in the silicon-rich residue reacts with sodium hydroxide to generate sodium silicate and enters the liquid phase. The titanium component is retained in the solid phase. The small amount of aluminum impurities remaining in the ore generates sodium aluminate and enters the liquid phase together. After the reaction is completed, the insoluble titanium-containing solid phase residue is removed by filtration to obtain an aqueous solution of sodium silicate containing a small amount of sodium aluminate impurities. (4) Preparation of peroxide silicate precursor solution The sodium silicate aqueous solution obtained in step (3) is thoroughly mixed with hydrogen peroxide at a mass percentage concentration of 30% to obtain a peroxide silicate aqueous solution, i.e., peroxide silicate precursor solution. (5) Photothermal spray photochemical synthesis of nano-silica in a fluidized bed The peroxide silicate precursor liquid obtained in step (4) is fed into the photofluidized bed device and sprayed out through the atomizing nozzle. Under photothermal conditions, hydrogen peroxide decomposes rapidly, and peroxide species undergo controllable nucleation and agglomeration precipitation. The gas-solid mixture after the reaction is collected by gas-solid separation to obtain monodisperse nano silica powder.

2. The process for extracting anatase-associated silica and photochemically synthesizing nano-silica according to claim 1, characterized in that, In step 1.1, the ilmenite ore is coarsely crushed into particles with a particle size of less than 3 mm.

3. The process for extracting anatase-associated silica and photochemically synthesizing nano-silica according to claim 1, characterized in that, In step 1.2, the solid-liquid weight ratio of ilmenite particles to dilute hydrochloric acid is 1:5 to 1:20, preferably 1:5 to 1:10, and more preferably 1:5 to 1:

6. Preferably, in step 1.2, the concentration of hydrochloric acid is 1.0~6.5 mol / L, more preferably 3.0~6.0 mol / L; Preferably, in step 1.2, the ball mill speed is 120~800 r / min, more preferably 450 r / min, and the ball milling time is 1~5h, more preferably 3.0h.

4. The process for extracting anatase-associated silica and photochemically synthesizing nano-silica according to claim 1, characterized in that, In step (2), the concentrated sulfuric acid has a mass fraction of 75% to 95%, preferably 90%; Preferably, in step (2), the solid-liquid weight ratio is 1:3 to 1:6, and more preferably 1:4.5 to 1:5; Preferably, in step (2), the reflux temperature is 120~180 ℃, more preferably 160 ℃, and the reflux reaction time is 1~6h, more preferably 4.0 h.

5. The process for extracting anatase-associated silica and photochemically synthesizing nano-silica according to claim 1, characterized in that, In step (3), the solid-liquid weight ratio is 1:2.5~1:8, preferably 1:3.5~1:4, and the sodium hydroxide solution concentration is 1.5~6 mol / L, preferably 5 mol / L; Preferably, in step (3), the reflux temperature is 100~150 ℃, more preferably 110 ℃, and the reflux reaction time is 1~5h, more preferably 3.0 h.

6. The process for extracting anatase-associated silica and photochemically synthesizing nano-silica according to claim 1, characterized in that, In step (4), the volume ratio of sodium silicate aqueous solution to hydrogen peroxide is 1:2.5 to 1:8, preferably 1:10; Preferably, in step (4), the mixing time is 10~60 min, preferably 30 min.

7. The process for extracting anatase-associated silica and photochemically synthesizing nano-silica according to claim 1, characterized in that, In step (5), the photothermal reaction temperature is preferably 130~140 ℃, more preferably 135 ℃.

Citation Information

Patent Citations

  • Method for preparing grade-adjustable potassium fluotitanate through using high-silicon-titanium iron ore

    CN102515261A

  • A method for low-temperature preparation of catalysts using a multi-source photofluidized bed and a multi-source photofluidized bed device

    CN122850280A

  • A method for preparing a silica nanocomposite thermal insulation material using iron tailings and the silica nanocomposite thermal insulation material

    CN122853846A