A low-carbon interface-reactivated barium slag-based semi-solid backfill material and its preparation method

By using copolymer hydrogel particles and chemical reagents to form an interfacial spacer phase in barium slag-based semi-solid backfill material, the problems of agglomeration and redispersion caused by the surface covering layer of barium slag particles were solved, thereby improving the pumping performance of the material and the strength of the backfill.

CN123062231APending Publication Date: 2026-11-10GUIZHOU REDSTAR DEVING +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611520079.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

After the barium slag-based semi-solid backfill material is premixed with water, the barium slag particles undergo ion dissolution, migration and deposition, and initial gelation reaction to form a low-activity covering layer. This leads to particle agglomeration and a reduction in effective reaction sites, making it difficult to fully redisperse and reactivate. The gel phase is also difficult to continuously nucleate at the particle interface, resulting in a decrease in the material's pumpability and a reduction in the strength of the backfill.

Method used

Copolymer hydrogel particles are distributed on the surface of barium slag particles and in adjacent contact areas. The copolymer hydrogel particles are prepared by acylation reaction, cross-linking polymerization and wet shearing. Combined with aqueous solutions of sodium sulfite and sodium hydroxide and sodium silicate solution, an interfacial spacer phase is formed to limit direct contact between particles, promote gelation reaction and improve redispersibility and pumpability.

Benefits of technology

The use of copolymer hydrogel particles reduces particle agglomeration and the activity of the capping layer, improves the redispersibility and pumpability of the material, and enhances the interfacial bonding between particles and the strength of the backfill.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention belongs to the technical field of low-carbon backfill materials, and provides a low-carbon interface-reactivated barium slag-based semi-solid backfill material and its preparation method. The material contains three mutually separated components: the first component is an aqueous semi-solid containing barium slag, granulated blast furnace slag powder, metakaolin, water, and copolymer hydrogel particles, with the copolymer hydrogel particles distributed on the surface of the barium slag particles and in the contact area between adjacent particles; the second component is an aqueous solution containing sodium sulfite and sodium hydroxide; and the third component is an aqueous solution of sodium silicate. The three components are prepared by acylation reaction of cystamine dihydrochloride with methacrylic anhydride. After the barium slag is premixed with water, ion dissolution, migration deposition, and initial gelation reaction form a low-activity capping layer and cause particle agglomeration, resulting in difficulty in interface redispersibility and hindered growth of the gel phase interface. This promotes particle redispersibility and interface exposure, improving the strength of the backfill.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of low-carbon backfill materials, and relates to a low-carbon interface-reactivated barium slag-based semi-solid backfill material and its preparation method. Background Technology

[0002] Barium slag is an industrial solid waste generated during barium salt production. Its solid phase typically contains insoluble mineral phases, residual reactive phases, and small amounts of soluble barium and calcium. When barium slag comes into contact with water, the soluble components and residual reactive phases on the particle surface dissolve. The dissolved ions migrate with the pore liquid and redeposit when the ion concentration, alkalinity, or local saturation state on the particle surface changes. Simultaneously, the reactive components in the barium slag and the coexisting active powders may undergo initial gelation reactions, and the resulting sediments and early gelation products gradually cover the particle surface. This covering layer has lower reactivity and mass transfer capacity than the fresh particle surface, hindering the continued entry of water and reactive components into the particle interface and reducing effective reaction sites available for subsequent gelation nucleation.

[0003] During settling, aqueous semi-solid materials undergo particle approach, flocculation, and aggregation, and the sediment and initial cementation products may form connections between adjacent particles. Re-stirring primarily disrupts the weakly bonded slurry structure, but for particle interfaces with existing capping layers or connected regions, simple mechanical shearing is insufficient to restore them to their initial dispersed state. When particle surfaces are not adequately re-exposed, subsequent cementation reactions tend to occur in the pore fluid or outside the particles. The nucleation of the cemented phase at the particle interface lacks continuity and is difficult to grow across adjacent particle interfaces, thus forming weakly bonded regions and residual pores.

[0004] The technical problem to be solved by this invention is that during the short-term storage and transportation of barium slag-based semi-solid backfill material after premixing with water, a low-activity covering layer is formed on the surface of barium slag particles due to ion dissolution, migration and deposition, and initial gelation reaction. This is accompanied by particle agglomeration and a reduction in effective reaction sites. As a result, when the particles are stirred again after storage, it is difficult for them to be fully redispersed and reactivated. The gel phase is difficult to continuously nucleate at the particle interface and grow across the interface, which in turn leads to a decrease in the pumping performance of the material, insufficient inter-particle bonding, and a reduction in the strength of the backfill. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide a low-carbon, interface-reactivated barium slag-based semi-solid backfill material and its preparation method. Addressing the problem of low-activity capping and agglomeration formed by the premixing of barium slag with water, which hinders redispersion and the growth of the cementitious phase interface, the invention employs a three-component system. The first component contains copolymer hydrogel particles distributed at the barium slag interface; the second component contains sodium sulfite and sodium hydroxide; and the third component contains sodium silicate. The copolymer hydrogel particles are obtained through acylation, cross-linking polymerization, and wet shearing. The first component is then prepared through predispersion, and the three components are encapsulated.

[0006] To achieve this objective, the present invention adopts the following technical solution: In a first aspect, the present invention provides an interface-reactivated barium slag-based semi-solid backfill material, comprising a first component, a second component, and a third component that are separated from each other; The first component is an aqueous semi-solid material, including barium slag, granulated blast furnace slag powder, metakaolin, water, and copolymer hydrogel particles. The copolymer hydrogel particles are distributed on the surface of the barium slag particles and in the contact area between adjacent barium slag particles. The copolymer hydrogel particles are N,N′-bis(methacryloyl)cysteine ​​crosslinked acrylic-2-acrylamido-2-methylpropanesulfonic acid copolymer hydrogel particles. The second component is an aqueous solution containing sodium sulfite and sodium hydroxide; the third component is an aqueous solution of sodium silicate.

[0007] Preferably, based on a total mass of 100 parts by mass of the barium slag, granulated blast furnace slag powder, and metakaolin, the barium slag comprises 60-75 parts by mass, the granulated blast furnace slag powder comprises 18-30 parts by mass, and the metakaolin comprises 7-15 parts by mass. The copolymer hydrogel particles are 0.2-0.8 parts by weight based on the dry polymer, and the water in the first component is 22-30 parts by weight; The mass of the barium slag is calculated on a dry basis, and the water contained in the barium slag and the copolymer hydrogel particles is included in the water in the first component.

[0008] Preferably, the D50 of the barium slag is 15-90 μm; based on the dry basis weight of the barium slag, the mass fraction of water-soluble barium in the barium slag is not higher than 0.03 wt.%, and the mass fraction of water-soluble calcium is not higher than 0.15 wt.%. The granulated blast furnace slag powder has a D50 of 5-25 μm and a glass phase content of 80-98 wt.%; the metakaolin has a D50 of 2-20 μm and a total SiO2 and Al2O3 content of 80-95 wt.%.

[0009] Preferably, based on a total mass of 100 wt.% of the monomers used to prepare the copolymer hydrogel particles, the monomers are: acrylic acid 45-65 wt.%, 2-acrylamido-2-methylpropanesulfonic acid 32-52 wt.%, and N,N′-bis(methacryloyl)cysteine ​​1-3 wt.%. The degree of neutralization of the acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid is 99-100 mol; the wet D50 of the copolymer hydrogel particles is 5-50 μm, and the gel fraction is 75-95 wt. based on the dry polymer mass of the copolymer hydrogel particles.

[0010] Preferably, the mass fraction of sodium sulfite in the second component is 15-20 wt.%; each 1 mol of N,N′-bis(methacryloyl)cysteine ​​used to prepare the copolymer hydrogel particles corresponds to 4-8 mol of sodium sulfite, and according to the total amount of water-soluble barium and water-soluble calcium in the barium slag, each 1 mol of water-soluble barium and water-soluble calcium corresponds to an additional 1.0-1.3 mol of sodium sulfite; The total mass of the second component is determined based on the mass of sodium sulfite and its mass fraction in the second component. The total mass of sodium hydroxide and water in the second component is the difference between the total mass of the second component and the mass of sodium sulfite. The mass of sodium hydroxide is determined according to the following conditions: using a first component containing 100 parts by mass of the barium slag, granulated blast furnace slag powder and metakaolin, and all the second components that are matched with it as the test object, while keeping the total mass of the second component unchanged, the water in the second component is replaced by an equal mass of sodium hydroxide. The first component and the second component are mixed at 25°C and 120 rpm for 10 min, filtered through a filter membrane with a pore size of 0.45 μm, and the pH value of the resulting filtrate is 9.0-11.5. The third component contains 35-45 wt.% sodium silicate, expressed as Na₂O·nSiO₂, where n is the molar ratio of SiO₂ to Na₂O and is 1.5-1.8. The mass of sodium silicate in the third component, calculated as Na₂O, is 3-4.5 wt.% of the total mass of the granulated blast furnace slag powder and metakaolin. With the total mass of the barium slag, granulated blast furnace slag powder and metakaolin being 100 parts by mass, the total water content in the first, second and third components is 30-45 parts by mass, and the water introduced by the second and third components is included in the total mass of the water.

[0011] Secondly, the present invention provides a method for preparing the interface-reactivated barium slag-based semi-solid backfill material as described in the first aspect, comprising the following steps: S1, Cystamine dihydrochloride is acylated with methacrylic anhydride to obtain N,N′-bis(methacryloyl)cystamine; S2, acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid are added to water and neutralized with sodium hydroxide respectively. Then, N,N′-bis(methacryloyl)cysteine ​​and ammonium persulfate are added to carry out cross-linking polymerization to obtain the reaction product. The reaction product is washed with water and wet sheared to obtain copolymer hydrogel particles. S3, the copolymer hydrogel particles are pre-dispersed with water in the first stage, then barium slag is added for the first mixing, followed by the addition of granulated blast furnace slag powder, metakaolin and remaining water for the second mixing to obtain the first component; S4, sodium sulfite and sodium hydroxide are added to water in sequence and mixed to obtain the second component; sodium silicate is added to water and mixed to obtain the third component; the first component, the second component and the third component are sealed and packaged separately to obtain the interface reactivated barium slag-based semi-solid backfill material.

[0012] Preferably, in S1, the molar ratio of cystamine dihydrochloride to methacrylic anhydride is 1:2.0-2.4; The cystamine dihydrochloride was dissolved in water, and the methacrylic anhydride was dissolved in acetone, with a water to acetone mass ratio of 1:0.3-1.0; the pH of the reaction solution was maintained at 8.0-9.5 using sodium hydroxide, and the acetone solution containing methacrylic anhydride was added over 0.5-2 hours at 0-10°C. After the addition was completed, the reaction was carried out at 15-25°C for 2-6 hours. After extraction with ethyl acetate and concentration under reduced pressure, the reaction solution was crystallized at 0-5℃ for 4-12 hours. The filtered solid was dried at 30-45℃ and 5-20 kPa absolute pressure for 4-12 hours.

[0013] Preferably, in step S2, after neutralizing acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid with sodium hydroxide, the pH of the aqueous phase is adjusted to 7.5-9.0, and then N,N′-bis(methacryloyl)cysteine ​​is added; the total mass fraction of acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid, and N,N′-bis(methacryloyl)cysteine ​​in the polymerization reaction solution is 10-25 wt.%, and the mass of ammonium persulfate is 0.2-0.8 wt.% of the total mass of the three monomers. Before polymerization, argon gas is introduced into the reactor gas phase until the oxygen volume fraction is no higher than 1 vol.%, and the reaction is carried out at 50-70℃ for 2-6 hours under argon atmosphere. The resulting reaction product is cut and replaced with deionized water 2-4 times, with the mass ratio of deionized water to reaction product being 2-5:1 each time. Then, it is wet-sheared at 2000-6000 rpm for 5-20 minutes.

[0014] Preferably, in S3, the water used in the first stage is 60-80 wt.% of the total water mass in the first component; the copolymer hydrogel particles are added to the water used in the first stage and pre-dispersed at 500-1500 rpm for 5-15 min, and then barium slag is added within 3-10 min under stirring at 60-180 rpm. After the addition is completed, the first mixing is continued for 10-20 min. After mixing granulated blast furnace slag powder and metakaolin at 20-60 rpm for 2-5 minutes, add them together with the remaining water to the material obtained from the first mixing, and then carry out a second mixing at 60-180 rpm for 5-15 minutes.

[0015] Preferably, in step S4, sodium sulfite is added to water and mixed at 15-30°C for 3-10 minutes, then sodium hydroxide is added and mixed for another 5-15 minutes to obtain the second component; sodium silicate is mixed with water at 50-80°C for 20-60 minutes, and the resulting third component is cooled to 15-30°C; the first, second, and third components are then sealed and packaged separately.

[0016] When cystamine dihydrochloride dissolves in water, the ammonium salt groups at both ends of the cystamine molecule are converted into nucleophilic amino groups under the action of sodium hydroxide. The amino group attacks the carbonyl carbon of methacrylic anhydride, breaking the anhydride bond and forming an amide bond, introducing methacryloyl groups at both ends of the cystamine molecule to yield N,N′-bis(methacryloyl)cystamine. This reaction retains the disulfide bond in the middle of the cystamine molecule while simultaneously introducing carbon-carbon double bonds at both ends of the molecule that can participate in free radical polymerization. After neutralization of acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid with sodium hydroxide, the carboxylic acid group and sulfonic acid group are converted into carboxylate group and sulfonate group, respectively, increasing the solubility of the monomer in the aqueous phase. The thermal decomposition of ammonium persulfate produces sulfate radicals, which add to the carbon-carbon double bonds of acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid, and N,N′-bis(methacryloyl)cystamine, initiating a chain propagation reaction. The double bonds at both ends of N,N′-bis(methacryloyl)cysteine ​​enter different polymer segments, forming covalent cross-linking points containing disulfide bonds between the segments, thus forming a water-insoluble cross-linked copolymer network. The carboxylate and sulfonate groups undergo ion hydration with water molecules, causing the cross-linked network to absorb water, swell, and form a copolymer hydrogel.

[0017] The copolymerized hydrogel particles are first dispersed in water during the first stage, with the carboxylate, sulfonate, and amide groups on the outer layer of the particles forming a hydrated layer with water. After the barium slag is added, the hydrogel particles contact the barium slag before the granulated blast furnace slag powder and metakaolin. The carboxylate groups can interact electrostatically or coordinately with the barium and calcium sites on the surface of the barium slag, while the sulfonate and amide groups can participate in interfacial adsorption through ionic and hydrogen bonding interactions, causing the hydrogel particles to tend to remain on the surface of the barium slag particles and in the contact area with adjacent particles. When the granulated blast furnace slag powder and metakaolin are subsequently added, the hydrogel particles that have already contacted the barium slag form a water-containing interstitial phase, restricting the direct adhesion of the barium slag particles and maintaining an interfacial gap between adjacent particles that can accommodate the water phase.

[0018] After the first component is formed, soluble components on the surface of the barium slag enter the pore water. Barium ions, calcium ions, and other dissolved components migrate along the aqueous phase and can deposit on the particle surface due to local changes in ion concentration and alkalinity. The residual reactive phase of the barium slag, as well as the granulated blast furnace slag powder and metakaolin surface layer, can undergo initial dissolution and gelation reactions, resulting in inorganic deposits and early gelation products forming a covering area on the particle surface. The hydrated layer of the interfacial hydrogel reduces the direct contact area between adjacent barium slag particles and restricts the formation of continuous hard bridges at particle contact points by early gelation products. The covalent cross-linking points in the hydrogel network also restrict the large-scale migration of polymer segments from the interface, allowing the aqueous spacer phase to remain on the surface of the barium slag particles and in the particle contact area during settling.

[0019] After the first and second components come into contact, sodium hydroxide maintains the alkalinity of the mixed aqueous phase, limiting the conversion of sulfite to bisulfite and preserving the nucleophilic ability of sulfite to disulfide bonds. Sulfite attacks the disulfide bonds at the crosslinking points of the copolymer hydrogel, breaking the covalent bonds between sulfur atoms and forming thiol or thiol anion end groups and thiosulfate-type end groups. This causes the crosslinking points that originally connected different polymer segments to lose their interchain bridging effect. With the decrease in the number of crosslinking points, the elastic constraint and shape retention of the hydrogel network decrease, reducing the resistance to water migration into the network interior. Under shearing, the hydrogel particles deform, split, and redistribute. The aqueous spacer phase originally located in the contact area with the barium slag particles unfolds as the network relaxes, the interparticle connections are disrupted by shearing, and some interfaces below the capping layer or at particle contact points re-contact the aqueous phase.

[0020] The water-soluble barium and calcium released from barium slag can form sulfites with low solubility with sulfite ions, and can also form ionic bridges with carboxylate groups in the hydrogel. The addition of sodium sulfite includes a corresponding replenishment amount for water-soluble barium and calcium, which can compensate for the consumption of sulfite ions due to inorganic salt deposition, allowing the remaining sulfite ions to participate in the sulfite decomposition of disulfide bonds. After the concentration of water-soluble barium and calcium decreases, the bridging between carboxylate groups mediated by polyvalent ions is restricted. The polymer chain segments after network relaxation are restricted from approaching barium slag particles again by the hydration layer and steric hindrance. The size and bonding strength of the particle agglomerates decrease with shear. The continuous aqueous phase between particles is restored, the particle bonds that need to be broken during slurry flow are reduced, and the yield resistance and shear resistance generated along the transport interface decrease accordingly.

[0021] After the third component comes into contact with the material that has undergone the aforementioned interfacial changes, sodium silicate provides alkaline components and soluble silicate ions to the aqueous phase. The alkaline aqueous phase attacks the silicon-oxygen-silicon bonds and silicon-oxygen-aluminum bonds in the granulated blast furnace slag powder and the amorphous phase of metakaolin, allowing silicon and aluminum species to enter the pore water, while the granulated blast furnace slag powder simultaneously releases calcium species. The dissolved silicon and aluminum species undergo condensation, and the calcium species participate in the formation of calcium aluminum silicate hydrates. Alkali metal ions participate in charge balance and can form aluminosilicate gels. After the surface of the barium slag particles and the particle contact area are re-exposed, the dissolved reactive species can diffuse to these interfaces and nucleate near surface hydroxyl groups, residual mineral edges, and the vicinity of the existing cemented phase. The cemented phase grows from the particle surface into the interparticle spaces, gradually crossing the interfaces between adjacent barium slag particles and between the barium slag and the active powder.

[0022] With the increase in interfacial nucleation sites and the formation of interfacial cementitious bonds, when particles are subjected to load, shear stress can be transferred from barium slag particles through the cementitious phase to the bonded phase formed by the reaction of granulated blast furnace slag powder and metakaolin. The unbonded areas on the particle surface and the residual gaps between particles decrease, limiting the initiation of cracks caused by interfacial debonding under stress. When cracks propagate along the particle interface, they need to pass through the cementitious bonds or change their propagation direction, increasing the interfacial resistance that particles need to overcome for pull-out. The weak areas formed by low-activity capping layers, particle agglomeration, and discontinuous nucleation decrease with interface re-exposure and the growth of the cementitious phase across the interface, expanding the interfacial load transfer range when the backfill is subjected to compressive loads.

[0023] Compared with the prior art, the beneficial effects of the present invention are as follows: The present invention pre-disperses the copolymer hydrogel particles, distributing them on the surface of barium slag particles and in the contact area between adjacent particles. This allows hydrated segments to form an interfacial spacer phase, reducing direct particle contact and limiting the formation of continuous connections between sediments and initial cementitious products at particle contact points. This weakens particle agglomeration and reduces the covering of reactive interfaces. After the first component contacts the second component, the alkaline aqueous phase maintains the reaction mode of sulfite ions. Sulfite ions cleave the disulfide bond crosslinking structure in the copolymer hydrogel, reducing the degree of network crosslinking. Under shear action, the sulfite ions deform, split, and redistribute, releasing particle connections and allowing the covered interfaces to re-contact the aqueous phase. This reduces the particle connection and shear resistance that needs to be overcome during slurry flow, improving redispersibility and pumpability. The third component provides alkaline components and soluble silicates, which promote the dissolution and cementation reaction of silica and aluminum species in granulated blast furnace slag powder and metakaolin. This allows the cementitious phase to nucleate on the re-exposed particle surface and grow into the interparticle gaps, reducing unconnected areas and residual gaps at the interface, expanding the load transfer range, limiting interface debonding and crack propagation, and improving the interparticle bonding and backfill strength. Detailed Implementation

[0024] The technical solution of the present invention will be described in detail below with reference to specific embodiments. The embodiments described herein are specific implementations of the present invention and are used to illustrate the concept of the present invention; these descriptions are explanatory and exemplary and should not be construed as limiting the implementation of the present invention or the scope of protection of the present invention. In addition to the embodiments described herein, those skilled in the art can also adopt other obvious technical solutions based on the content disclosed in the claims and the specification of this application. These technical solutions include those that make any obvious substitutions and modifications to the embodiments described herein.

[0025] The chemical reagents used in the embodiments and comparative examples of this invention are all commercially available products and have not undergone any further purification treatment.

[0026] Example 1 This embodiment provides a method for preparing a low-carbon, interface-reactivated barium slag-based semi-solid backfill material, the preparation method specifically including the following steps: S1, 1.2 g of cystamine dihydrochloride was dissolved in 40 g of water, and 1.73 g of methacrylic anhydride was dissolved in 24 g of acetone. The molar ratio of cystamine dihydrochloride to methacrylic anhydride was 1:2.1, and the mass ratio of water to acetone was 1:0.6. The pH of the reaction solution was maintained at 8.5 using 0.9 g of sodium hydroxide. The acetone solution containing methacrylic anhydride was added over 1 h at 5 °C. After the addition was completed, the reaction was carried out at 20 °C for 4 h. The reaction solution was extracted with 60 g of ethyl acetate and concentrated under reduced pressure. The solution was crystallized at 3 °C for 8 h. The filtered solid was dried at 35 °C and 10 kPa absolute pressure for 8 h to obtain 1.2 g of N,N′-bis(methacryloyl)cystamine. S2, 31.2g of acrylic acid and 27.6g of 2-acrylamido-2-methylpropanesulfonic acid were added to 317.0g of water, and neutralized with 17.3g of sodium hydroxide and 5.3g of sodium hydroxide, respectively. The neutralization degrees of acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid were 99.9mol% and 99.5mol%, respectively. The pH of the aqueous phase was adjusted to 8.0, and then 1.2g of [unspecified substance] was added. N,N′-bis(methacryloyl)cysteamine and 0.36 g ammonium persulfate, the total mass fraction of the three monomers in the polymerization reaction solution was 15 wt.%, and the mass of ammonium persulfate was 0.6 wt.% of the total mass of the three monomers. Argon gas was introduced into the reactor gas phase to produce 0.7 vol.% oxygen. The reaction was carried out at 60 °C for 4 h under an argon atmosphere to obtain the reaction product. The reaction product was cut and replaced with deionized water three times, with a deionized water to reaction product mass ratio of 3:1 each time. Then, it was wet-sheared at 4000 rpm for 12 min to obtain 500 g of copolymer hydrogel particles, of which 60 g was dry polymer. The wet D50 of the copolymer hydrogel particles was 25 μm, and the gel fraction was 85 wt.%. S3, 500g of the copolymer hydrogel particles are added to 1820g of water for the first stage, pre-dispersed at 1000rpm for 10min, and then 6300g of barium slag is added within 6min under stirring at 120rpm. The barium slag has a dry basis weight of 6000g, a water content of 300g, and a D50 of 50μm. Based on the dry basis weight of the barium slag, the mass fraction of water-soluble barium is 0.015wt.%, and the mass fraction of water-soluble calcium is 0.08wt.%. After the barium slag is added, the first mixing continues for 15min. 2800g of granulated blast furnace slag powder and 1 200g of metakaolin was mixed at 40rpm for 3min. The granulated blast furnace slag powder had a D50 of 15μm and a glass phase content of 90wt.%, while the metakaolin had a D50 of 10μm and a total SiO2 and Al2O3 content of 88wt.%. The mixed granulated blast furnace slag powder and metakaolin, along with 40g of remaining water, were added to the material obtained from the first mixing. The mixture was then mixed again at 120rpm for 10min to obtain the first component. The water used in the first stage was 70wt.% of the total water mass in the first component, and the total water mass in the first component was 2600g. S4. Following the principle that 1 mol of N,N′-bis(methacryloyl)cysteine ​​corresponds to 6 mol of sodium sulfite, and based on the total amount of water-soluble barium and water-soluble calcium in the barium slag, 1 mol of water-soluble barium and water-soluble calcium corresponds to an additional 1.1 mol of sodium sulfite. 20.7 g of sodium sulfite was added to 93.8 g of water and mixed at 20°C for 5 min. Then, 0.5 g of sodium hydroxide was added and mixing continued for 5 min, yielding 115.0 g of the second component. The mass fraction of sodium sulfite in the second component was 18 wt.%. The pH of the filtrate obtained after mixing the first component and all of the second component was 10.0. 357.2g of sodium silicate and 535.8g of water were mixed at 65℃ for 40min. The sodium silicate had a modulus of 1.6 and a mass of 140.0g as Na2O, accounting for 3.5wt.% of the total mass of granulated blast furnace slag powder and metakaolin. A third component with a sodium silicate mass fraction of 40wt.% was obtained. The third component was cooled to 20℃. The total water content of the first, second, and third components was 3229.6g. The first, second, and third components were sealed and packaged separately to obtain a low-carbon interface reactivated barium slag-based semi-solid backfill material.

[0027] Example 2 This embodiment provides a method for preparing a low-carbon, interface-reactivated barium slag-based semi-solid backfill material, the preparation method specifically including the following steps: S1, 0.6 g of cystamine dihydrochloride was dissolved in 30 g of water, and 0.99 g of methacrylic anhydride was dissolved in 30 g of acetone. The molar ratio of cystamine dihydrochloride to methacrylic anhydride was 1:2.4, and the mass ratio of water to acetone was 1:1.0. The pH of the reaction solution was maintained at 9.5 using 0.5 g of sodium hydroxide. The acetone solution containing methacrylic anhydride was added over 2 h at 0 °C. After the addition was completed, the reaction was carried out at 15 °C for 6 h. The reaction solution was extracted with 50 g of ethyl acetate and concentrated under reduced pressure. The solution was crystallized at 0 °C for 12 h. The filtered solid was dried at 45 °C and 5 kPa absolute pressure for 4 h to obtain 0.6 g of N,N′-bis(methacryloyl)cystamine. S2, 9.0g of acrylic acid and 10.4g of 2-acrylamido-2-methylpropanesulfonic acid were added to 53.0g of water, and neutralized with 5.00g of sodium hydroxide and 2.01g of sodium hydroxide, respectively. The neutralization degree of acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid was 100 mol%. The pH of the aqueous phase was adjusted to 8.5, and then 0.6g of [unspecified substance] was added. N,N′-bis(methacryloyl)cysteamine and 0.04 g ammonium persulfate, the total mass fraction of the three monomers in the polymerization reaction solution was 25 wt.%, and the mass of ammonium persulfate was 0.2 wt.% of the total mass of the three monomers. Argon gas was introduced into the reactor gas phase to produce 1.0 vol.% oxygen. The reaction was carried out at 50 °C for 6 h under an argon atmosphere to obtain the reaction product. The reaction product was cut and replaced with deionized water four times, each time with a deionized water to reaction product mass ratio of 2:1. Then, it was wet-sheared at 6000 rpm for 20 min to obtain 200 g of copolymer hydrogel particles, of which 20 g was dry polymer. The wet D50 of the copolymer hydrogel particles was 5 μm, and the gel fraction was 95 wt.%. S3, 200g of the copolymer hydrogel particles are added to 1760g of water for the first stage, pre-dispersed at 1500rpm for 5min, and then 6565g of barium slag is added within 10min under stirring at 60rpm. The barium slag has a dry basis weight of 6500g, a water content of 65g, and a D50 of 15μm. Based on the dry basis weight of the barium slag, the mass fraction of water-soluble barium is 0.03wt.%, and the mass fraction of water-soluble calcium is 0.15wt.%. After the barium slag is added, the first mixing continues for 20min. 2000g of granulated blast furnace slag powder and 150g of... 0g of metakaolin was mixed at 20rpm for 5min. The granulated blast furnace slag powder had a D50 of 25μm and a glass phase content of 80wt.%, while the metakaolin had a D50 of 20μm and a total SiO2 and Al2O3 content of 95wt.%. The mixed granulated blast furnace slag powder and metakaolin, along with 195g of remaining water, were added to the first mixture. The mixture was then mixed again at 180rpm for 5min to obtain the first component. The water used in the first stage was 80wt.% of the total water mass in the first component, and the total water mass in the first component was 2200g. S4. Following the principle that 1 mol of N,N′-bis(methacryloyl)cysteine ​​corresponds to 4 mol of sodium sulfite, and based on the total amount of water-soluble barium and water-soluble calcium in the barium slag, 1 mol of water-soluble barium and water-soluble calcium corresponds to an additional 1.3 mol of sodium sulfite. 43.2 g of sodium sulfite was added to 172.6 g of water and mixed at 30°C for 3 minutes. Then, 0.2 g of sodium hydroxide was added and mixing continued for 5 minutes, yielding 216.0 g of the second component. The mass fraction of sodium sulfite in the second component was 20 wt.%. The pH of the filtrate obtained after mixing the first component and all of the second component was 9.0. 432.3g of sodium silicate and 802.8g of water were mixed at 50℃ for 60min. The sodium silicate had a modulus of 1.8 and a mass of 157.5g as Na2O, accounting for 4.5wt.% of the total mass of granulated blast furnace slag powder and metakaolin. A third component with a sodium silicate mass fraction of 35wt.% was obtained. The third component was cooled to 30℃. The total water content of the first, second, and third components was 3175.4g. The first, second, and third components were sealed and packaged separately to obtain a low-carbon interface reactivated barium slag-based semi-solid backfill material.

[0028] Example 3 This embodiment provides a method for preparing a low-carbon, interface-reactivated barium slag-based semi-solid backfill material, the preparation method specifically including the following steps: S1, 0.8 g of cystamine dihydrochloride was dissolved in 40 g of water, and 1.10 g of methacrylic anhydride was dissolved in 12 g of acetone. The molar ratio of cystamine dihydrochloride to methacrylic anhydride was 1:2.0, and the mass ratio of water to acetone was 1:0.3. The pH of the reaction solution was maintained at 8.0 using 0.6 g of sodium hydroxide. The acetone solution containing methacrylic anhydride was added over 0.5 h at 10 °C. After the addition was completed, the reaction was carried out at 25 °C for 2 h. The reaction solution was extracted with 50 g of ethyl acetate and concentrated under reduced pressure. It was crystallized at 5 °C for 4 h. The obtained solid was filtered and dried at 30 °C and 20 kPa absolute pressure for 12 h to obtain 0.8 g of N,N′-bis(methacryloyl)cystamine. S2, 48.0g of acrylic acid and 31.2g of 2-acrylamido-2-methylpropanesulfonic acid were added to 686.8g of water, and neutralized with 26.64g and 6.02g of sodium hydroxide, respectively. The neutralization degree of both acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid was 100 mol%. The pH of the aqueous phase was adjusted to 9.0, and then 0.8g of [unspecified substance] was added. N,N′-bis(methacryloyl)cysteamine and 0.64 g ammonium persulfate, the total mass fraction of the three monomers in the polymerization reaction solution was 10 wt.%, and the mass of ammonium persulfate was 0.8 wt.% of the total mass of the three monomers. Argon gas was introduced into the reactor gas phase to produce oxygen with a volume fraction of 0.2 vol.%. The reaction was carried out at 70 °C for 2 h under an argon atmosphere to obtain the reaction product. The reaction product was cut and replaced twice with deionized water, each time with a deionized water to reaction product mass ratio of 5:1. Then, it was wet-sheared at 2000 rpm for 5 min to obtain 640 g of copolymer hydrogel particles, of which 80 g was dry polymer. The wet D50 of the copolymer hydrogel particles was 50 μm, and the gel fraction was 75 wt.%. S3, 640g of the copolymer hydrogel particles are added to 1800g of water for the first stage, pre-dispersed at 500rpm for 15min, and then 7875g of barium slag is added within 3min under stirring at 180rpm. The barium slag has a dry basis weight of 7500g, a water content of 375g, and a D50 of 90μm. Based on the dry basis weight of the barium slag, the mass fraction of water-soluble barium is 0.005wt.%, and the mass fraction of water-soluble calcium is 0.03wt.%. After the barium slag is added, the first mixing continues for 10min. 1800g of granulated blast furnace slag powder and... 700g of metakaolin was mixed at 60rpm for 2min. The granulated blast furnace slag powder had a D50 of 5μm and a glass phase content of 98wt.%, while the metakaolin had a D50 of 2μm and a total SiO2 and Al2O3 content of 80wt.%. The mixed granulated blast furnace slag powder and metakaolin, along with 265g of remaining water, were added to the material obtained from the first mixing. The mixture was then mixed again at 60rpm for 15min to obtain the first component. The water used in the first stage was 60wt.% of the total water mass in the first component, and the total water mass in the first component was 3000g. S4. Based on the principle that 1 mol of N,N′-bis(methacryloyl)cysteine ​​corresponds to 8 mol of sodium sulfite, and based on the total amount of water-soluble barium and water-soluble calcium in the barium slag, 1 mol of water-soluble barium and water-soluble calcium corresponds to 1.0 mol of sodium sulfite. Take 10.2 g of sodium sulfite and add it to 55.8 g of water. Mix at 15°C for 10 min, then add 2.0 g of sodium hydroxide and continue mixing for 15 min to obtain 68.0 g of the second component. The mass fraction of sodium sulfite in the second component is 15 wt.%. The pH value of the filtrate obtained after mixing the first component and all of the second component is 11. 5. Mix 184.1g of sodium silicate with 225.0g of water at 80℃ for 20min. The sodium silicate has a modulus of 1.5 and a mass of 75.0g as Na2O, accounting for 3.0wt.% of the total mass of granulated blast furnace slag powder and metakaolin. A third component with a sodium silicate mass fraction of 45wt.% is obtained. The third component is cooled to 15℃. The total water content of the first, second, and third components is 3280.8g. The first, second, and third components are sealed and packaged separately to obtain a low-carbon interface reactivated barium slag-based semi-solid backfill material.

[0029] Example 4 This embodiment provides a method for preparing a low-carbon, interface-reactivated barium slag-based semi-solid backfill material, the preparation method specifically including the following steps: S1, 1.2 g of cystamine dihydrochloride was dissolved in 40 g of water, and 1.89 g of methacrylic anhydride was dissolved in 32 g of acetone. The molar ratio of cystamine dihydrochloride to methacrylic anhydride was 1:2.3, and the mass ratio of water to acetone was 1:0.8. The pH of the reaction solution was maintained at 9.0 using 0.9 g of sodium hydroxide. The acetone solution containing methacrylic anhydride was added over 1.5 h at 7 °C. After the addition was completed, the reaction was carried out at 20 °C for 5 h. The reaction solution was extracted with 60 g of ethyl acetate and concentrated under reduced pressure. The solution was crystallized at 2 °C for 10 h. The filtered solid was dried at 40 °C and 15 kPa absolute pressure for 10 h to obtain 1.2 g of N,N′-bis(methacryloyl)cystamine. S2, 26.0g of acrylic acid and 12.8g of 2-acrylamido-2-methylpropanesulfonic acid were added to 142.9g of water, and neutralized with 14.4g and 2.47g of sodium hydroxide, respectively. The neutralization degrees of acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid were 99.8mol% and 99.9mol%, respectively. The pH of the aqueous phase was adjusted to 7.5, and then 1.2g of [unspecified substance] was added. N,N′-bis(methacryloyl)cysteamine and 0.16 g ammonium persulfate, the total mass fraction of the three monomers in the polymerization reaction solution was 20 wt.%, and the mass of ammonium persulfate was 0.4 wt.% of the total mass of the three monomers. Argon gas was introduced into the reactor gas phase to produce oxygen with a volume fraction of 0.5 vol.%. The reaction was carried out at 65 °C for 5 h under an argon atmosphere to obtain the reaction product. The reaction product was cut and replaced with deionized water three times, with a deionized water to reaction product mass ratio of 4:1 each time. Then, it was wet-sheared at 5000 rpm for 15 min to obtain 320 g of copolymer hydrogel particles, of which 40 g was dry polymer. The wet D50 of the copolymer hydrogel particles was 15 μm, and the gel fraction was 92 wt.%. S3, 320g of the copolymer hydrogel particles were added to 1875g of water for the first stage, and pre-dispersed at 1200rpm for 8min. Then, 6552g of barium slag was added within 8min under stirring at 150rpm. The dry basis weight of the barium slag was 6300g, the water content was 252g, and the D50 was 35μm. Based on the dry basis weight of the barium slag, the mass fraction of water-soluble barium was 0.02wt.%, and the mass fraction of water-soluble calcium was 0.10wt.%. After the barium slag was added, the first mixing was continued for 18min. 3000g of granulated blast furnace slag powder and 7 00g of metakaolin was mixed at 50rpm for 4min. The granulated blast furnace slag powder had a D50 of 20μm and a glass phase content of 94wt.%, while the metakaolin had a D50 of 15μm and a total SiO2 and Al2O3 content of 92wt.%. The mixed granulated blast furnace slag powder and metakaolin, along with 93g of remaining water, were added to the first mixture. The mixture was then mixed again at 150rpm for 8min to obtain the first component. The water used in the first stage was 75wt.% of the total water mass in the first component, and the total water mass in the first component was 2500g. S4. Based on the principle that 1 mol of N,N′-bis(methacryloyl)cysteine ​​corresponds to 7 mol of sodium sulfite, and based on the total amount of water-soluble barium and water-soluble calcium in the barium slag, 1 mol of water-soluble barium and water-soluble calcium corresponds to an additional 1.2 mol of sodium sulfite. 28.8 g of sodium sulfite was added to 139.6 g of water and mixed at 25°C for 5 min. Then, 1.0 g of sodium hydroxide was added and mixing continued for 8 min, yielding 169.4 g of the second component. The mass fraction of sodium sulfite in the second component was 17 wt.%. The pH of the filtrate obtained after mixing the first component and all of the second component was 10.5. 391.9g of sodium silicate and 541.2g of water were mixed at 70℃ for 50min. The sodium silicate had a modulus of 1.7 and a mass of 148.0g as Na2O, accounting for 4.0wt.% of the total mass of granulated blast furnace slag powder and metakaolin. A third component with a sodium silicate mass fraction of 42wt.% was obtained. The third component was cooled to 25℃. The total water content of the first, second, and third components was 3180.8g. The first, second, and third components were sealed and packaged separately to obtain a low-carbon interface reactivated barium slag-based semi-solid backfill material.

[0030] Comparative Example 1 This comparative example provides a method for preparing a low-carbon interface-reactivated barium slag-based semi-solid backfill material. The difference between this method and Example 1 is that copolymer hydrogel particles are not added in S3, and 440g of water is used to replenish the water introduced by the copolymer hydrogel particles. Since copolymer hydrogel particles are not prepared and used, S1 and S2 are cancelled accordingly. Other process parameters and operating conditions are exactly the same as in Example 1.

[0031] Comparative Example 2 This comparative example provides a method for preparing a low-carbon interface-reactivated barium slag-based semi-solid backfill material. The difference between this method and Example 1 is that in S3, after the copolymer hydrogel particles are pre-dispersed with water in the first stage, the barium slag is added simultaneously with the pre-mixed granulated blast furnace slag powder and metakaolin. The separate pre-contact process between the copolymer hydrogel particles and the barium slag is not set. Other process parameters and operating conditions are exactly the same as in Example 1.

[0032] Comparative Example 3 This comparative example provides a method for preparing a low-carbon interface-reactivated barium slag-based semi-solid backfill material. The difference between this method and Example 1 is that the amount of sodium sulfite in S4 is determined only according to the ratio of 6 mol of sodium sulfite to 1 mol of N,N′-bis(methacryloyl)cysteine, and the amount of sodium sulfite is no longer increased according to the total amount of water-soluble barium and water-soluble calcium in the barium slag. The amount of sodium hydroxide and water in the second component remains unchanged, and other process parameters and operating conditions are exactly the same as in Example 1.

[0033] Comparative Example 4 This comparative example provides a method for preparing a low-carbon interface-reactivated barium slag-based semi-solid backfill material. The difference between this method and Example 1 is that sodium sulfite is not added when preparing the second component in S4, the amount of sodium hydroxide and water in the second component remains unchanged, and other process parameters and operating conditions are exactly the same as in Example 1.

[0034] Test method: Storage and subsequent stirring: Three parallel samples were prepared. The first component was placed in a sealed container and left at 25°C for 12 hours. Then, the entire second component was added over 2 minutes at 120 rpm, and stirring continued for 20 minutes. After stirring, 100.0 g of the slurry from each sample was weighed and placed in a pre-weighed drying pan. The sample was dried at 105°C for 4 hours, cooled for 30 minutes, and then weighed to determine the solid mass fraction. Another 500.0 g of the same slurry was weighed and placed on a 0.60 mm aperture, 200 mm diameter sieve. Deionized water was continuously added at a flow rate of 500 mL / min to rinse the sieve for 4 minutes, without squeezing or rubbing the material on the sieve during rinsing. The material on the sieve was transferred to a pre-weighed drying pan, dried at 105°C for 4 hours, cooled for 30 minutes, and then weighed. The wet sieve residue rate is defined as the percentage of the dry mass of the material remaining on the sieve relative to the solid mass of 500.0g of slurry. The result is expressed as a percentage (%), and the arithmetic mean of the results from three samples is taken, accurate to 0.1%.

[0035] Post-storage slurry flowability: Refer to GB / T 2419-2005 "Method for Determination of Flowability of Cement Mortar". Prepare three parallel samples. Place the first component in a sealed container and let it stand at 25℃ for 12 hours. Add all of the second component within 2 minutes at 120 rpm and continue stirring for 20 minutes. Then add all of the third component within 3 minutes at 160 rpm and continue stirring for 5 minutes. Use a truncated conical mold with an upper inner diameter of 70 mm, a lower inner diameter of 100 mm, and a height of 60 mm, and a cement mortar flowability tester. Complete the mold filling within 2 minutes after the second stirring. Fill the slurry into the truncated conical mold in two layers. Fill the first layer to two-thirds of the mold height, make 5 marks in each of two mutually perpendicular directions, and tamp 15 times from the edge to the center. Fill the second layer to 20 mm above the mold opening, make 5 marks in each of the same directions, and tamp 10 times. Scrape off the slurry above the mold opening and lift the truncated conical mold vertically. The slurry table completes 25 jumps within 25 seconds. Then, the two diameters of the slurry extension that are perpendicular to each other are measured. The arithmetic mean of the two diameters is taken as the flowability of a single sample. The result is expressed in mm. The arithmetic mean of the results of 3 samples is taken, accurate to 1 mm.

[0036] Splitting tensile strength: Tested according to GB / T 50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete". The first component was placed in a sealed container and left at 25℃ for 12 hours. The second component was added over 2 minutes at 120 rpm and stirred for another 20 minutes. The third component was then added over 3 minutes at 160 rpm and stirred for another 5 minutes. The resulting slurry was poured into 150mm×150mm×150mm cubic molds within 10 minutes, vibrated on a vibrating table for 30 seconds, covered with a polyethylene film, and left at 20℃ for 24 hours. After demolding, the specimens were cured at 20±2℃ and a relative humidity of not less than 95%RH for 28 days. Three specimens were prepared for each group. Before the test, wipe off any moisture from the specimen surface. Mark the loading lines at the center of two opposite sides. Place the specimen in the center of the compression testing machine. Place 20mm wide and 3mm thick plywood strips along the loading lines between the specimen and the upper and lower pressure plates. Continuously load the specimen at a stress rate of 0.05MPa / s until it splits, and record the maximum load. Calculate the splitting tensile strength by dividing twice the maximum load by the product of pi, the splitting width, and the splitting height. The result is expressed in MPa, and the arithmetic mean of the results from three specimens is taken, accurate to 0.01MPa.

[0037] Compressive strength: Tested according to GB / T 50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete". The first component was placed in a sealed container and left at 25℃ for 12 hours. The second component was added over 2 minutes at 120 rpm and stirred for another 20 minutes. The third component was then added over 3 minutes at 160 rpm and stirred for another 5 minutes. The resulting slurry was poured into 150mm×150mm×150mm cubic molds within 10 minutes, vibrated on a vibrating table for 30 seconds, covered with a polyethylene film, and left at 20℃ for 24 hours. After demolding, the specimens were cured at 20±2℃ and a relative humidity of not less than 95%RH for 28 days. Three specimens were prepared for each group. Before the test, the surface moisture of the specimens was wiped off. Using the two opposite sides perpendicular to the pouring direction as the bearing surfaces, the specimens were placed in the center of the pressure plate of the compression testing machine and continuously loaded at a stress rate of 0.5 MPa / s until failure. The maximum load was recorded. The compressive strength is calculated by dividing the maximum load by the measured bearing area. The result is expressed in MPa and is the arithmetic mean of the results of three specimens, accurate to 0.1 MPa.

[0038] The test results are shown in Table 1.

[0039] Table 1. Test results of low-carbon interface-reactivated barium slag-based semi-solid backfill materials in Examples 1-4 and Comparative Examples 1-4

[0040] As shown in Table 1, compared to Example 1, Comparative Example 1 showed an increase in wet sieve residue after storage and re-stirring, and a decrease in slurry fluidity, splitting tensile strength, and compressive strength. Comparative Example 1 did not include copolymer hydrogel particles, resulting in a lack of spatial isolation between the barium slag particles and adjacent particle contact areas. During storage, particle connections formed by ion migration deposition and initial gelation reactions were not restricted. Upon re-stirring, the formed agglomerates were difficult to disintegrate, leading to an increase in sieve residue and a decrease in slurry fluidity. Insufficient exposure of the effective reaction interface of the barium slag limited the continuous formation of the subsequent gel phase at the particle interface, increasing the number of weak interface areas and thus reducing splitting tensile strength and compressive strength.

[0041] As shown in Table 1, compared to Example 1, Comparative Example 2 showed an increase in wet sieve residue after storage and re-stirring, and a decrease in slurry fluidity, splitting tensile strength, and compressive strength after storage. Comparative Example 2 altered the feeding and pre-dispersion sequence in S3, failing to pre-disperse the copolymer hydrogel particles with water in the first stage before pre-contacting them with barium slag. When the copolymer hydrogel particles entered the system containing granulated blast furnace slag powder and metakaolin, they were simultaneously distributed on the surfaces of different powders, reducing their distribution on the surface of barium slag particles and in the particle contact area. Increased agglomeration and particle bonding in the barium slag contact area during storage led to increased sieve residue and decreased fluidity; the reduced exposed barium slag interface after re-stirring affected interparticle gelation and load transfer, thus reducing both strengths.

[0042] As shown in Table 1, compared to Example 1, Comparative Example 3 showed an increase in wet sieve residue after storage and subsequent stirring, and a decrease in slurry fluidity, splitting tensile strength, and compressive strength. In Comparative Example 3, the sodium sulfite was not increased according to the amount of water-soluble barium and calcium in the barium slag; it was only added for disulfide bonds in the copolymer hydrogel. During barium slag storage, the barium and calcium ions dissolved can consume sulfite ions and form sulfite precipitates, reducing the amount of sulfite ions participating in disulfide bond sulfite decomposition, thus limiting the relaxation and redistribution of the copolymer hydrogel network. The increase in residual agglomerates hindered slurry flow, leading to an increase in sieve residue and a decrease in fluidity. The insufficiently relaxed hydrogel continued to occupy part of the particle interface, limiting the migration of subsequent reactants to the interface and the cross-interface growth of the gel phase, thus reducing both strengths.

[0043] As shown in Table 1, compared to Example 1, the wet sieve residue of Comparative Example 4 increased after storage and re-stirring, while the slurry fluidity, splitting tensile strength, and compressive strength all decreased after storage. In Comparative Example 4, sodium sulfite was not added during the preparation of the second component; only sodium hydroxide and water were retained. Sodium hydroxide provides an alkaline environment but cannot initiate the sulfite dissociation of disulfide bonds in the copolymer hydrogel, making it difficult for the crosslinked network to relax and redistribute during re-stirring after storage. The continuous coverage of the particle interface by the hydrogel and the connection between adjacent particles increased the residual agglomerates and restricted slurry flow, leading to increased sieve residue and decreased fluidity. Simultaneously, the migration of sodium silicate and dissolved ions to the barium slag interface was restricted, reducing interfacial gelation and thus decreasing the splitting tensile strength and compressive strength.

[0044] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.

Claims

1. A low-carbon, interface-reactivated barium slag-based semi-solid backfill material, characterized in that, It includes a first component, a second component, and a third component that are separated from each other; The first component is an aqueous semi-solid material, including barium slag, granulated blast furnace slag powder, metakaolin, water, and copolymer hydrogel particles. The copolymer hydrogel particles are distributed on the surface of the barium slag particles and in the contact area between adjacent barium slag particles. The copolymer hydrogel particles are N,N′-bis(methacryloyl)cysteine ​​crosslinked acrylic-2-acrylamido-2-methylpropanesulfonic acid copolymer hydrogel particles. The second component is an aqueous solution containing sodium sulfite and sodium hydroxide; the third component is an aqueous solution of sodium silicate.

2. The low-carbon interface-reactivated barium slag-based semi-solid backfill material according to claim 1, characterized in that, Based on a total mass of 100 parts by mass of the barium slag, granulated blast furnace slag powder, and metakaolin, the barium slag comprises 60-75 parts by mass, the granulated blast furnace slag powder comprises 18-30 parts by mass, and the metakaolin comprises 7-15 parts by mass. The copolymer hydrogel particles are 0.2-0.8 parts by weight based on the dry polymer, and the water in the first component is 22-30 parts by weight; The mass of the barium slag is calculated on a dry basis, and the water contained in the barium slag and the copolymer hydrogel particles is included in the water in the first component.

3. The low-carbon interface-reactivated barium slag-based semi-solid backfill material according to claim 2, characterized in that, The barium slag has a D50 of 15-90 μm; based on the dry weight of the barium slag, the mass fraction of water-soluble barium in the barium slag is not higher than 0.03 wt.%, and the mass fraction of water-soluble calcium in the barium slag is not higher than 0.15 wt.%. The granulated blast furnace slag powder has a D50 of 5-25 μm and a glass phase content of 80-98 wt.%; the metakaolin has a D50 of 2-20 μm and a total SiO2 and Al2O3 content of 80-95 wt.%.

4. The low-carbon interface-reactivated barium slag-based semi-solid backfill material according to claim 2, characterized in that, Based on a total mass of 100 wt.% of the monomers used to prepare the copolymer hydrogel particles, the monomers are: acrylic acid 45-65 wt.%, 2-acrylamido-2-methylpropanesulfonic acid 32-52 wt.%, and N,N′-bis(methacryloyl)cysteine ​​1-3 wt.%. The degree of neutralization of the acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid is 99-100 mol; the wet D50 of the copolymer hydrogel particles is 5-50 μm, and the gel fraction is 75-95 wt. based on the dry polymer mass of the copolymer hydrogel particles.

5. The low-carbon interface-reactivated barium slag-based semi-solid backfill material according to claim 4, characterized in that, The second component contains 15-20 wt.% sodium sulfite; each 1 mol of N,N′-bis(methacryloyl)cysteine ​​used to prepare the copolymer hydrogel particles corresponds to 4-8 mol of sodium sulfite, and according to the total amount of water-soluble barium and water-soluble calcium in the barium slag, each 1 mol of water-soluble barium and water-soluble calcium corresponds to 1.0-1.3 mol of sodium sulfite. The total mass of the second component is determined based on the mass of sodium sulfite and its mass fraction in the second component. The total mass of sodium hydroxide and water in the second component is the difference between the total mass of the second component and the mass of sodium sulfite. The mass of sodium hydroxide is determined according to the following conditions: using a first component containing 100 parts by mass of the barium slag, granulated blast furnace slag powder and metakaolin, and all the second components that are matched with it as the test object, while keeping the total mass of the second component unchanged, the water in the second component is replaced by an equal mass of sodium hydroxide. The first component and the second component are mixed at 25°C and 120 rpm for 10 min, filtered through a filter membrane with a pore size of 0.45 μm, and the pH value of the resulting filtrate is 9.0-11.

5. The third component contains 35-45 wt.% sodium silicate, expressed as Na₂O·nSiO₂, where n is the molar ratio of SiO₂ to Na₂O and is 1.5-1.

8. The mass of sodium silicate in the third component, calculated as Na₂O, is 3-4.5 wt.% of the total mass of the granulated blast furnace slag powder and metakaolin. With the total mass of the barium slag, granulated blast furnace slag powder and metakaolin being 100 parts by mass, the total water content in the first, second and third components is 30-45 parts by mass, and the water introduced by the second and third components is included in the total mass of the water.

6. A method for preparing a low-carbon interface-reactivated barium slag-based semi-solid backfill material as described in any one of claims 1-5, characterized in that, Includes the following steps: S1, Cystamine dihydrochloride is acylated with methacrylic anhydride to obtain N,N′-bis(methacryloyl)cystamine; S2, acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid are added to water and neutralized with sodium hydroxide respectively. Then, N,N′-bis(methacryloyl)cysteine ​​and ammonium persulfate are added to carry out cross-linking polymerization to obtain the reaction product. The reaction product is washed with water and wet sheared to obtain copolymer hydrogel particles. S3, the copolymer hydrogel particles are pre-dispersed with water in the first stage, then barium slag is added for the first mixing, followed by the addition of granulated blast furnace slag powder, metakaolin and remaining water for the second mixing to obtain the first component; S4, sodium sulfite and sodium hydroxide are added to water in sequence and mixed to obtain the second component; sodium silicate is added to water and mixed to obtain the third component; the first component, the second component and the third component are sealed and packaged separately to obtain the low-carbon interface reactivated barium slag-based semi-solid backfill material.

7. The preparation method of the low-carbon interface-reactivated barium slag-based semi-solid backfill material according to claim 6, characterized in that, In S1, the molar ratio of cystamine dihydrochloride to methacrylic anhydride is 1:2.0-2.4; The cystamine dihydrochloride was dissolved in water, and the methacrylic anhydride was dissolved in acetone, with a water to acetone mass ratio of 1:0.3-1.0; the pH of the reaction solution was maintained at 8.0-9.5 using sodium hydroxide, and the acetone solution containing methacrylic anhydride was added over 0.5-2 hours at 0-10°C. After the addition was completed, the reaction was carried out at 15-25°C for 2-6 hours. After extraction with ethyl acetate and concentration under reduced pressure, the reaction solution was crystallized at 0-5℃ for 4-12 hours. The filtered solid was dried at 30-45℃ and 5-20 kPa absolute pressure for 4-12 hours.

8. The preparation method of the low-carbon interface-reactivated barium slag-based semi-solid backfill material according to claim 6, characterized in that, In S2, acrylic acid and 2-acrylamido-2-methylpropanesulfonic acid are neutralized with sodium hydroxide, and the pH of the aqueous phase is adjusted to 7.5-9.

0. Then, N,N′-bis(methacryloyl)cysteine ​​is added. The total mass fraction of acrylic acid, 2-acrylamido-2-methylpropanesulfonic acid, and N,N′-bis(methacryloyl)cysteine ​​in the polymerization reaction solution is 10-25 wt.%, and the mass of ammonium persulfate is 0.2-0.8 wt.% of the total mass of the three monomers. Before polymerization, argon gas is introduced into the reactor gas phase until the oxygen volume fraction is no higher than 1 vol.%, and the reaction is carried out at 50-70℃ for 2-6 hours under argon atmosphere. The resulting reaction product is cut and replaced with deionized water 2-4 times, with the mass ratio of deionized water to reaction product being 2-5:1 each time. Then, it is wet-sheared at 2000-6000 rpm for 5-20 minutes.

9. The preparation method of the low-carbon interface-reactivated barium slag-based semi-solid backfill material according to claim 6, characterized in that, In S3, the water used in the first stage is 60-80 wt.% of the total water mass in the first component; the copolymer hydrogel particles are added to the water used in the first stage and pre-dispersed at 500-1500 rpm for 5-15 min, and then barium slag is added within 3-10 min under stirring at 60-180 rpm. After the addition is completed, the first mixing is continued for 10-20 min. After mixing granulated blast furnace slag powder and metakaolin at 20-60 rpm for 2-5 minutes, add them together with the remaining water to the material obtained from the first mixing, and then carry out a second mixing at 60-180 rpm for 5-15 minutes.

10. The preparation method of the low-carbon interface-reactivated barium slag-based semi-solid backfill material according to claim 6, characterized in that, In S4, sodium sulfite is added to water and mixed at 15-30℃ for 3-10 minutes, then sodium hydroxide is added and mixed for another 5-15 minutes to obtain the second component; sodium silicate is mixed with water at 50-80℃ for 20-60 minutes, and the resulting third component is cooled to 15-30℃; the first, second and third components are then sealed and packaged separately.