A Zirconia-ZnO Composite Toughened High-Alumina Structural Electrical Porcelain Material and Its Preparation Method
By preparing zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain materials, and by using composite pre-reaction mineralized materials and controlling the process flow, the problems of slurry processing state and firing stability in the preparation of high-alumina structural electrical porcelain materials were solved, improving crack resistance and dimensional stability, and achieving efficient firing densification.
Patent Information
- Application Number
- CN202611343029.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-10
AI Technical Summary
In the preparation process of existing high-alumina structural electrical porcelain materials, it is difficult to simultaneously achieve the following: slurry processing state, green body forming state, firing densification stability, dimensional stability, and crack resistance. In particular, when the composite components are unevenly distributed and the firing and cooling conditions are inappropriate, the fired products are prone to high water absorption, large firing deformation rate, and poor crack resistance.
The high-alumina structural electrical porcelain material is toughened by a zirconium silicate-zinc oxide composite. By preparing a composite pre-reaction mineralized material, components such as zirconium silicate, zinc oxide, barium carbonate, potassium feldspar, and kaolin are pre-composite to form a uniform pre-dispersion state. Through processes such as dry mixing, wet ball milling, pressure filtration, aging, vacuum slurry preparation, and extrusion molding, the fineness of the slurry and the moisture content of the mud cake are controlled. With appropriate firing and cooling conditions, the uniform distribution and stability of the components are ensured.
It improves the stability of slurry processing and green body forming, enhances the stability and crack resistance of firing densification, reduces the water absorption and cracking risk of fired products, and ensures dimensional stability.
Smart Images

Figure CN123062235A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of high-alumina structural electrical porcelain technology, specifically to a zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material and its preparation method. Background Technology
[0002] High-alumina structural electrical porcelain materials are typically made from aluminosilicate raw materials such as calcined bauxite, kaolin, and potassium feldspar through ball milling, molding, drying, and firing. In the field of structural electrical porcelain, these materials need to balance firing densification, dimensional stability, and crack resistance. The composition of raw materials, slurry fineness, moisture content of the clay, molding uniformity, and firing and cooling conditions all affect the final product's condition.
[0003] In the preparation of existing high-alumina structural electrical porcelain materials, zirconium-containing, zinc-containing, barium-containing, and aluminosilicate components are often directly mixed with the main raw materials. When the pre-dispersion between components is insufficient, it is difficult to simultaneously control the fineness of the slurry after wet ball milling, the moisture content of the cake, the residual moisture of the green body, and the structural consistency after firing. Furthermore, if the timing of zinc oxide and sodium humate addition is not coordinated, the connection between the slurry processing state and subsequent processes such as pressure filtration, aging, vacuum piling, and extrusion molding will also be affected.
[0004] Furthermore, high-alumina structural electrical porcelain materials require a medium-temperature reaction, high-temperature densification, and cooling process during firing. If the distribution of the composite components in the main blank is insufficient, or if the firing and cooling conditions are not properly coordinated, it can easily lead to difficulties in coordinating the water absorption rate, firing deformation rate, crack resistance, and performance retention after rapid thermal changes in the fired products. Therefore, improving the slurry processing state, blank forming state, firing densification stability, dimensional stability, and crack resistance during the preparation of high-alumina structural electrical porcelain materials through raw material ratios, composite pre-reacted mineralizers, zinc oxide addition methods, sodium humate addition methods, and the coordination of firing and cooling conditions is a problem that needs to be solved in this field. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides a zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material and its preparation method, which solves the problem of simultaneously ensuring the slurry processing state, green body forming state, firing densification stability, dimensional stability, crack resistance, and post-firing structural consistency of high-alumina structural electrical porcelain materials during the preparation process.
[0006] To address the above problems, the present invention provides the following technical solution:
[0007] The first aspect of this invention provides a zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material, employing the following technical solution:
[0008] A zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material, comprising the following raw materials in parts by weight:
[0009] Composite pre-reacted mineralizer: 8.68 parts to 15.50 parts;
[0010] Calcined bauxite: 38.00 parts to 42.00 parts;
[0011] Kaolin: 35.58 parts to 45.09 parts;
[0012] Potassium feldspar: 6.30 parts to 7.35 parts;
[0013] Zirconium silicate: 0 parts to 0.90 parts;
[0014] Zinc oxide: 0.02 parts to 0.88 parts;
[0015] Barium carbonate: 0 parts to 0.22 parts;
[0016] Bentonite: 0.30 parts to 0.80 parts;
[0017] Sodium humate: 0.03 parts to 0.12 parts;
[0018] The raw material includes one of zirconium silicate and barium carbonate; the composite pre-reacted mineralized material is prepared by pre-reaction of dry-based raw materials including zirconium silicate, zinc oxide, barium carbonate, potassium feldspar and kaolin.
[0019] By adopting the above technical solution, the composite pre-reacted mineralizer pre-composite the relevant components in zirconium silicate, zinc oxide, barium carbonate, potassium feldspar, and kaolin, so that the zirconium-containing, zinc-containing, and barium-containing components and the aluminosilicate components form a relatively uniform pre-dispersion state before entering the main blank. The composite pre-reacted mineralizer, together with calcined bauxite, kaolin, and potassium feldspar, constitutes the main feedstock system of high-alumina structural electrical porcelain. The calcined bauxite provides the Al2O3 source required for the firing of high-alumina structural electrical porcelain, the kaolin participates in the formation of aluminosilicate components and improves the molding performance of the clay, and the potassium feldspar participates in the formation of the liquid phase during the firing process.
[0020] The zinc oxide, used in conjunction with the zirconium silicate, helps to regulate the densification process during firing and improve the crack resistance of the fired products. The barium carbonate is used to regulate the firing reaction of aluminosilicates. The bentonite and sodium humate are used to improve the processing performance of the clay and the fluidity of the slurry, respectively. Thus, while maintaining the feasibility of forming and firing high-alumina structural electrical porcelain, the densification stability, crack resistance, and structural consistency of the fired products can be improved.
[0021] Preferably, the mass fraction of the composite pre-reacted mineralizer is calculated based on the total mass of dry-based raw materials used in its preparation, and the composite pre-reacted mineralizer is made from the following dry-based raw materials:
[0022] Zirconium silicate: 100 parts;
[0023] Zinc oxide: 30 to 45 parts;
[0024] Barium carbonate: 12 to 25 parts;
[0025] Potassium feldspar: 55 to 75 parts;
[0026] Kaolin: 20 to 40 parts.
[0027] By adopting the above technical solution, zirconium silicate is used as the zirconium-containing component, zinc oxide and barium carbonate are used as firing reaction regulating components, and potassium feldspar and kaolin are combined to form a composite pre-reacted mineralization material. The zirconium silicate is used to introduce zirconium-containing components and improve the crack resistance of high-alumina structural electrical porcelain; the zinc oxide is used to regulate the reaction of silicon-containing components and the firing densification process; the barium carbonate is used to regulate the firing reaction of aluminosilicates; and the potassium feldspar and kaolin provide the aluminosilicate component source for the composite pre-reacted mineralization material. The above components are first compounded and then added to the main blank, which helps to improve the dispersion uniformity of the composite mineralization components in the main blank.
[0028] Preferably, when preparing the composite pre-reacted mineralized material, the dry-based raw materials added meet the following mass ratio:
[0029] The mass ratio of zinc oxide to zirconium silicate is (30-45):100;
[0030] The mass ratio of barium carbonate to zinc oxide is (12-25):(30-45).
[0031] The mass ratio of potassium feldspar to kaolin is (55-75):(20-40).
[0032] By adopting the above technical solution, the proportions of zinc oxide and zirconium silicate, barium carbonate and zinc oxide, and potassium feldspar and kaolin are controlled within the above range, which is beneficial to maintain an appropriate matching relationship between the zinc-containing component, zirconium-containing component, barium-containing component and aluminosilicate component.
[0033] The controlled ratio of zinc oxide to zirconium silicate helps to balance the regulatory effect of the zinc-containing component on the densification process during firing and the improving effect of the zirconium-containing component on crack resistance; the controlled ratio of barium carbonate to zinc oxide helps to coordinate the roles of the barium-containing and zinc-containing components during firing; and the controlled ratio of potassium feldspar to kaolin helps to adjust the aluminosilicate composition in the composite pre-reacted mineralizer. Therefore, the composite pre-reacted mineralizer can participate stably in the subsequent firing reaction of the high-alumina structural electrical porcelain blank.
[0034] The second aspect of this invention provides a method for preparing a zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material, employing the following technical solution:
[0035] A method for preparing a zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material includes the following steps:
[0036] The composite pre-reacted mineral material, calcined bauxite, kaolin, potassium feldspar, bentonite, and one of barium carbonate or zirconium silicate are sequentially added to the ball mill. They are first dry-mixed, and then water is added for wet ball milling.
[0037] Continue the wet ball milling process, adding zinc oxide during the process and sodium humate before the end of the wet ball milling. After the wet ball milling is completed, the fineness of the slurry is measured to obtain the milled slurry.
[0038] The ball-milled slurry is passed through an iron remover to remove iron, and then sent to a filter press to filter it to obtain mud cake. The mud cake is cut into pieces and sent to an aging chamber for aging, and the surface of the mud is kept covered during the aging process.
[0039] The aged clay is fed into a vacuum clay kneading machine for kneading. After kneading, it is extruded to obtain an electric porcelain blank, which is then dried.
[0040] The dried porcelain blank is sent into a kiln for firing, and after cooling to room temperature, a high-alumina structural porcelain material with zirconium silicate and zinc oxide composite toughening is obtained.
[0041] By adopting the above technical solution, the composite pre-reacted mineral material is first dry-mixed and wet-ball-milled with the main raw material of high-alumina structural electric porcelain, so that the composite pre-reacted mineral material is dispersed in the main raw material, and the calcined bauxite, the kaolin, the potassium feldspar and the bentonite form a uniform slurry system.
[0042] The zinc oxide can be added at the beginning or in stages, and the dispersion and timing of the zinc oxide in the ball milling system can be adjusted according to the batching method. When the zinc oxide is added in stages, the main raw materials are first ball milled and dispersed for a certain period of time before the zinc oxide is introduced for further mixing, which is beneficial to improving the distribution of zinc-containing components in the slurry.
[0043] The sodium humate is added before the wet ball milling is completed to adjust the slurry fluidity and processing performance in subsequent filtration and pumice processes. Iron removal, filtration, aging, vacuum pumice, extrusion molding, and drying are sequentially combined to control the slurry's moisture content, plasticity, internal gas content, and molding uniformity. After firing and cooling to room temperature, the zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material is obtained.
[0044] Preferably, the conditions for the dry mixing and the wet ball milling are as follows:
[0045] The dry mixing time is 20 min to 40 min;
[0046] The solid content of the wet ball milling slurry is 60wt% to 68wt%.
[0047] The total time for the wet ball milling is 12h to 16h;
[0048] After the wet ball milling is completed, the residue on the slurry sieve is no more than 0.05 wt%.
[0049] By adopting the above technical solution, the dry mixing time is controlled at 20 min to 40 min, which is beneficial for the powders to form a preliminary mixed state before entering the wet ball mill; the solid content of the wet ball mill slurry is controlled at 60 wt% to 68 wt%, which can take into account both ball milling efficiency and slurry flow state; the total time of the wet ball mill is controlled at 12 h to 16 h, and the sieve residue of the slurry after the wet ball mill is controlled to be no higher than 0.05 wt%, which is beneficial for reducing coarse particle residue, improving the uniformity of the particle size distribution of the billet and the uniformity of the structure of the billet after molding, thereby providing a foundation for subsequent firing and densification.
[0050] Preferably, the conditions for adding the zinc oxide and the sodium humate are as follows:
[0051] The amount of zinc oxide added is 0.02 parts to 0.88 parts, and the addition time is 7.2 h to 12 h after the wet ball milling is carried out;
[0052] The amount of sodium humate added is 0.03 to 0.12 parts, and the addition time is 1 to 2 hours before the end of the wet ball milling.
[0053] By adopting the above technical solution, the amount of zinc oxide added is controlled between 0.02 and 0.88 parts, which can form a complex with the zinc-containing components pre-introduced in the composite pre-reacted mineralized material. When the zinc oxide is added in stages, it is added when the wet ball milling has been carried out for 7.2 to 12 hours. This allows the main raw materials to undergo a certain degree of dispersion and refinement before the zinc oxide is introduced to participate in subsequent mixing and dispersion, thereby helping to control the distribution of the zinc-containing components. The sodium humate is added 1 to 2 hours before the end of the wet ball milling. This can adjust the dispersion and flow properties of the slurry after refinement and is beneficial to the subsequent pressure filtration, aging, and sludge refining processes.
[0054] Preferably, the conditions for the pressure filtration, the aging, the vacuum plowing, and the drying are as follows:
[0055] After filtration, the moisture content of the sludge cake is 19wt% to 23wt%.
[0056] The aging time is 48h to 72h;
[0057] The vacuum degree of the vacuum ply mill is greater than 0.09 MPa;
[0058] After drying, the residual moisture content of the electric porcelain blank is no higher than 0.8 wt%.
[0059] By adopting the above technical solution, the moisture content of the mud cake after filtration is controlled at 19wt% to 23wt%, which enables the mud cake to have a suitable moisture content for subsequent aging and kneading. The aging time is controlled at 48h to 72h, and the surface of the mud is kept covered during the aging period, which is conducive to the internal moisture and plasticity of the mud tending to be balanced, and reduces the impact of surface water loss and hardening on molding stability.
[0060] The vacuum kneading machine has a vacuum degree greater than 0.09 MPa, which is beneficial for removing entrained gas from the clay and improving the uniformity of the clay. After drying, the residual moisture content of the electric porcelain blank is no higher than 0.8 wt%, which can reduce the risk of cracking caused by excessive residual moisture in the early stage of firing and improve the consistency of the blank when it enters the firing process.
[0061] Preferably, the firing conditions are as follows:
[0062] Heat the temperature to 960℃~1010℃ and then keep it at that temperature for 2h~4h;
[0063] Continue heating to 1080℃~1120℃ and then hold for 40min~80min;
[0064] Then raise the temperature to 1265℃~1280℃ and hold for 1.5h~2.5h;
[0065] During the cooling process, the cooling rate in the range of 1050℃ to 850℃ is 40℃ / h to 70℃ / h.
[0066] By adopting the above technical solution, the firing process includes two medium-temperature holding stages and one high-temperature holding stage. Holding at 960℃~1010℃ facilitates the removal of residual volatile components from the green body and ensures stable medium-temperature reactions. Holding at 1080℃~1120℃ further promotes the reaction between zinc-containing and barium-containing components and the aluminosilicate system. Holding at 1265℃~1280℃ facilitates the high-alumina structure of the electrical porcelain green body to achieve high-temperature densification. During cooling, the cooling rate in the 1050℃ to 850℃ range is controlled at 40℃ / h~70℃ / h, which helps reduce thermal stress concentration caused by excessive temperature gradients during the cooling stage, thus controlling the risk of cracking and dimensional fluctuations in the fired products.
[0067] Preferably, the composite pre-reacted mineralizer is prepared according to the following steps:
[0068] Zirconium silicate, zinc oxide, barium carbonate, potassium feldspar and kaolin used to prepare composite pre-reacted minerals are added to a ball mill, and then water is added for wet ball milling.
[0069] The ball-milled slurry is filtered to obtain a premixed mud cake, and the premixed mud cake is dried to obtain a premixed dry material;
[0070] The premixed dry material is fed into a kiln for pre-firing. After pre-firing, it is cooled to room temperature, crushed, and sieved to obtain the composite pre-reacted mineralized material.
[0071] By adopting the above technical solution, the zirconium silicate, zinc oxide, barium carbonate, potassium feldspar and kaolin are first wet-milled to form a uniform slurry, and then subjected to pressure filtration, drying and pre-calcination to form the composite pre-reacted mineral material.
[0072] The wet ball milling improves the mixing uniformity of the components; the pressure filtration and drying processes help obtain a premixed dry material with controlled moisture content; the pre-calcination treatment helps the zirconium-containing, zinc-containing, barium-containing, and aluminosilicate components to form a pre-reactive state, reducing their concentrated reaction degree during the firing stage of the main billet. The subsequent crushing and sieving after pre-calcination yields the composite pre-reactive mineralized material with a particle size suitable for subsequent batching and ball milling, thereby improving its dispersion stability in the main billet.
[0073] Preferably, the preparation conditions for the composite pre-reacted mineralizer are as follows:
[0074] During the wet ball milling process, the solid content of the slurry is 60wt%–68wt%, the milling time is 8h–12h, and the residue on a 10,000-mesh sieve after milling is 0.08wt%–0.15wt%.
[0075] The premixed mud cake is dried at a temperature of 80℃~100℃ for 4h~6h, and the resulting premixed dry material has a moisture content of no more than 1.0wt%.
[0076] When the premixed dry material is pre-fired, the pre-fired temperature is 880℃~930℃ and the pre-fired time is 0.5h~1.5h. After the pre-fired material is completed, it is crushed and passed through an 80-120 mesh sieve.
[0077] By adopting the above technical solution, in the preparation of the composite pre-reactive mineral material, the solid content of the wet ball milling slurry is controlled to 60wt%–68wt%, the ball milling time is controlled to 8h–12h, and the residue on a 10,000-mesh sieve after ball milling is controlled to 0.08wt%–0.15wt%. This ensures that the components in the composite pre-reactive mineral material achieve a degree of dispersion and refinement suitable for pre-calcination. The premixed cake is dried at 80℃–100℃ for 4h–6h, and the resulting dry premixed material has a moisture content not exceeding 1.0wt%, which is beneficial for improving the stability of the pre-calcination process. The pre-calcination temperature is controlled to 880℃–930℃, and the pre-calcination time is controlled to 0.5h–1.5h, which enables the composite pre-reactive mineral material to form a stable pre-reactive state. After pre-calcination, the material is crushed and passed through an 80-120 mesh sieve, which is beneficial for maintaining good dispersibility and batching stability when subsequently mixed with the main raw material.
[0078] This invention provides a zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material and its preparation method. It possesses the following beneficial effects:
[0079] 1. This invention combines composite pre-reacted mineral materials with calcined bauxite, kaolin, potassium feldspar, zirconium silicate, zinc oxide, barium carbonate, bentonite, and sodium humate, and then mixes them by dry mixing and wet ball milling to form a ball-milled slurry. This allows for control of the slurry's residue on a 10,000-mesh sieve, the moisture content of the mud cake, and the residual moisture in the electric porcelain blank. This facilitates the stable acquisition of electric porcelain materials after firing and cooling, and the continuous execution of the preparation method.
[0080] 2. This invention prepares a composite pre-reaction mineralized material from zirconium silicate, zinc oxide, barium carbonate, potassium feldspar, and kaolin, and controls the mass ratio of the dry-based raw materials. The composite pre-reaction mineralized material is then combined with calcined bauxite, kaolin, potassium feldspar, bentonite, and one of barium carbonate or zirconium silicate in wet ball milling, and is connected with pressure filtration, aging, and vacuum sizing, which is beneficial for subsequent firing.
[0081] 3. This invention uses zinc oxide to be added at the beginning or in stages, and sodium humate to be added before the end of wet ball milling. Combined with iron removal, pressure filtration, aging, vacuum slurry making, extrusion molding, drying, firing and cooling conditions, the slurry, mud cake, electric porcelain blank and high alumina structure electric porcelain material after ball milling are kept in a suitable state in continuous process, and it is conducive to obtaining high alumina structure electric porcelain material after cooling to room temperature. Attached Figure Description
[0082] Figure 1 This is a graph showing the amplitude-frequency response of the fired test strips to the impact vibration of the present invention.
[0083] Figure 2 This is a power spectrum curve of the shrinkage fluctuation of the firing line in this invention;
[0084] Figure 3 This is a graph showing the amplitude-frequency response of the fired test strip after rapid thermal change according to the present invention, after being subjected to impact vibration.
[0085] Figure 4 This is a comparison of the phase frequency response curves of the test strips subjected to impact excitation in relation to the process path of this invention.
[0086] Figure 5 This is a frequency response curve of dielectric loss of the sample after rapid thermal change according to the present invention. Detailed Implementation
[0087] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0088] The main raw materials and reagents used in the following examples and comparative examples have the following sources and specifications. Reagents not specifically mentioned are all commercially available analytical grade or higher grade products.
[0089] Calcined bauxite, CAS number 92797-42-7, has Al2O3 and SiO2 as its main chemical components. It is made from calcined mineral powder used as ceramic blanks and is used to provide the source of Al2O3 required for the firing of high-alumina structural electric porcelain.
[0090] Kaolin, CAS number 1332-58-7, has the main chemical composition Al2Si2O5(OH)4. It is used as ceramic blank kaolin to provide aluminosilicate components and improve the blank forming performance.
[0091] Potassium feldspar, specifically orthoclase, CAS number 12168-80-8, molecular formula KAlSi3O8, is used to provide potassium aluminum silicate components and participate in the liquid phase formation during the firing process.
[0092] Zirconium silicate, CAS number 10101-52-7, molecular formula ZrSiO4, is ceramic-grade zirconium silicate used to introduce zirconium-containing components and improve the crack resistance of high-alumina structural electrical porcelain.
[0093] Zinc oxide, CAS number 1314-13-2, molecular formula ZnO, is used to regulate the reaction of silicon-containing components and the densification process during firing.
[0094] Barium carbonate, CAS number 513-77-9, molecular formula BaCO3, is used to introduce barium-containing components and regulate the calcination reaction of aluminosilicates.
[0095] Bentonite, CAS No. 1302-78-9, is mainly composed of montmorillonite-type hydrous aluminosilicates and is used to improve the suspension, plasticity and molding bonding properties of clay.
[0096] Sodium humate, CAS No. 68131-04-4, is a sodium humate salt mud dispersion material used to adjust the fluidity and processing performance of wet ball mill slurry.
[0097] Preparation Example 1:
[0098] This preparation example provides a composite pre-reacted mineralizer, including the following steps:
[0099] 100 parts by weight of zirconium silicate, 30 parts by weight of zinc oxide, 12 parts by weight of barium carbonate, 55 parts by weight of potassium feldspar and 20 parts by weight of kaolin were added to a ball mill, and water was added for wet ball milling. The solid content of the wet ball mill slurry was controlled to be 60 wt%, the ball milling time was 8 hours, and the residue of the slurry after ball milling was 0.15 wt% on a 10,000-mesh sieve.
[0100] The ball-milled slurry was filtered to obtain a premixed mud cake; the premixed mud cake was dried at 80℃ for 6 hours to obtain a premixed dry material with a moisture content of no more than 1.0 wt%.
[0101] The premixed dry material was fed into a kiln for pre-firing at a temperature of 880℃ for 0.5 hours. After pre-firing, it was cooled to room temperature, crushed, and passed through an 80-mesh sieve to obtain the composite pre-reacted mineralized material.
[0102] Preparation Example 2:
[0103] This preparation example provides a composite pre-reacted mineralizer, including the following steps:
[0104] 100 parts by weight of zirconium silicate, 36 parts by weight of zinc oxide, 18 parts by weight of barium carbonate, 65 parts by weight of potassium feldspar and 30 parts by weight of kaolin were added to a ball mill, and water was added for wet ball milling. The solid content of the wet ball mill slurry was controlled to be 64 wt%, the ball milling time was 10 h, and the residue of the slurry after ball milling was 0.10 wt% on a 10,000-mesh sieve.
[0105] The ball-milled slurry was filtered to obtain a premixed mud cake; the premixed mud cake was dried at 90℃ for 5 hours to obtain a premixed dry material with a moisture content of no more than 0.8wt%.
[0106] The premixed dry material was fed into a kiln for pre-firing at 900℃ for 1.0 h. After pre-firing, it was cooled to room temperature, crushed, and passed through a 100-mesh sieve to obtain the composite pre-reacted mineralized material.
[0107] Preparation Example 3:
[0108] This preparation example provides a composite pre-reacted mineralizer, including the following steps:
[0109] 100 parts by weight of zirconium silicate, 45 parts by weight of zinc oxide, 25 parts by weight of barium carbonate, 75 parts by weight of potassium feldspar and 40 parts by weight of kaolin were added to a ball mill, and then water was added for wet ball milling. The solid content of the wet ball mill slurry was controlled to be 68 wt%, the ball milling time was 12 h, and the residue of the slurry after ball milling was 0.08 wt% on a 10,000-mesh sieve.
[0110] The ball-milled slurry was filtered to obtain a premixed mud cake; the premixed mud cake was dried at 100℃ for 4 hours to obtain a premixed dry material with a moisture content of no more than 0.6wt%.
[0111] The premixed dry material was fed into a kiln for pre-firing at a temperature of 930℃ for 1.5 hours. After pre-firing, it was cooled to room temperature, crushed, and passed through a 120-mesh sieve to obtain the composite pre-reacted mineralized material.
[0112] In the following examples, the mass fraction of the composite pre-reacted mineralizer is calculated based on the total mass of dry raw materials used in the preparation of the composite pre-reacted mineralizer.
[0113] Example 1:
[0114] This embodiment provides a method for preparing a zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material, including the following steps:
[0115] 8.68 parts by weight of the composite pre-reacted mineralized material obtained in Preparation Example 1, 38.00 parts by weight of calcined bauxite, 45.09 parts by weight of kaolin, 6.30 parts by weight of potassium feldspar, 0.22 parts by weight of barium carbonate, and 0.80 parts by weight of bentonite were added to a ball mill in sequence. The mixture was first dry-mixed for 20 minutes, and then water was added for wet ball milling. The solid content of the wet ball mill slurry was controlled to be 60 wt%.
[0116] The total time for wet ball milling was controlled at 12 hours. Zinc oxide 0.88 parts by weight was added 7.2 hours into the milling process, and sodium humate 0.03 parts by weight was added 1 hour before the end of the milling process. After the milling process was completed, the fineness of the slurry was tested, and the residue on the 10,000-mesh sieve was controlled to be ≤0.05wt%.
[0117] After the ball milling slurry is processed by an iron remover to remove iron, it is then sent to a filter press for filtration. The moisture content of the filter cake is controlled at 19 wt%. The filter cake is then cut into pieces and sent to an aging chamber for aging for 48 hours. During the aging process, the surface of the mud is kept covered to prevent the surface from losing water and hardening.
[0118] The aged clay is fed into a vacuum clay mixer for clay mixing, with the vacuum level controlled to be greater than 0.09 MPa. After clay mixing, it is extruded to obtain an electric porcelain blank, and then the electric porcelain blank is dried until the residual moisture is ≤0.8 wt%.
[0119] The dried porcelain blank was sent into a kiln for firing. The temperature was raised to 960℃ and held for 2 hours. The temperature was then raised to 1080℃ and held for 40 minutes. The temperature was then raised to 1265℃ and held for 1.5 hours. During the cooling process, the cooling rate in the range of 1050℃ to 850℃ was controlled at 40℃ / h. After cooling to room temperature, the zirconium silicate zinc oxide composite toughened high-alumina structure porcelain material was obtained.
[0120] Example 2:
[0121] This embodiment provides a method for preparing a zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material, including the following steps:
[0122] 11.95 parts by weight of the composite pre-reacted mineralized material obtained in Preparation Example 2, 39.50 parts by weight of calcined bauxite, 41.07 parts by weight of kaolin, 6.38 parts by weight of potassium feldspar, 0.13 parts by weight of barium carbonate, and 0.45 parts by weight of bentonite were added to a ball mill in sequence. The mixture was first dry-mixed for 30 minutes, and then water was added for wet ball milling. The solid content of the wet ball mill slurry was controlled to be 64 wt%.
[0123] The total time for wet ball milling was controlled at 14 hours. Zinc oxide 0.47 parts by weight was added 9.8 hours after the ball milling was completed, and sodium humate 0.05 parts by weight was added 1.5 hours before the end of the ball milling. After the ball milling was completed, the fineness of the slurry was tested, and the residue on the 10,000-mesh sieve was controlled to be ≤0.04wt%.
[0124] After the ball milling slurry is processed by an iron remover to remove iron, it is then sent to a filter press for filtration. The moisture content of the filter cake is controlled at 21 wt%. The filter cake is then cut into pieces and sent to an aging chamber for aging for 60 hours. During the aging process, the surface of the mud is kept covered to prevent the surface from losing water and hardening.
[0125] The aged clay is fed into a vacuum clay mixer for clay mixing, with the vacuum level controlled to be greater than 0.09 MPa. After clay mixing, it is extruded to obtain an electric porcelain blank, and then the electric porcelain blank is dried until the residual moisture is ≤0.8 wt%.
[0126] The dried porcelain blank was sent into a kiln for firing. The temperature was raised to 990℃ and held for 3 hours. The temperature was then raised to 1100℃ and held for 60 minutes. The temperature was then raised to 1272℃ and held for 2 hours. During the cooling process, the cooling rate in the range of 1050℃ to 850℃ was controlled at 55℃ / h. After cooling to room temperature, a zirconium silicate zinc oxide composite toughened high-alumina structure porcelain material was obtained.
[0127] Example 3:
[0128] This embodiment provides a method for preparing a zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material, including the following steps:
[0129] 13.11 parts by weight of the composite pre-reacted mineralized material obtained in Preparation Example 3, 42.00 parts by weight of calcined bauxite, 36.20 parts by weight of kaolin, 7.35 parts by weight of potassium feldspar, 0.90 parts by weight of zirconium silicate, and 0.30 parts by weight of bentonite were added to a ball mill in sequence. The mixture was first dry-mixed for 40 minutes, and then water was added for wet ball milling. The solid content of the wet ball mill slurry was controlled to be 68 wt%.
[0130] The total time for wet ball milling is controlled at 16 hours. 0.02 parts by weight of zinc oxide are added when the ball milling is 12 hours in. 0.12 parts by weight of sodium humate are added 2 hours before the end of the ball milling. After the ball milling is completed, the fineness of the slurry is tested, and the residue on the 10,000-mesh sieve is controlled to be ≤0.03wt%.
[0131] After the ball milling slurry is processed by an iron remover to remove iron, it is then sent to a filter press for filtration. The moisture content of the filter cake is controlled at 23 wt%. The filter cake is then cut into pieces and sent to an aging chamber for aging for 72 hours. During the aging process, the surface of the mud is kept covered to prevent the surface from losing water and hardening.
[0132] The aged clay is fed into a vacuum clay mixer for clay mixing, with the vacuum level controlled to be greater than 0.09 MPa. After clay mixing, it is extruded to obtain an electric porcelain blank, and then the electric porcelain blank is dried until the residual moisture is ≤0.8 wt%.
[0133] The dried porcelain blank was sent into a kiln for firing. The temperature was raised to 1010℃ and held for 4 hours. The temperature was then raised to 1120℃ and held for 80 minutes. The temperature was then raised to 1280℃ and held for 2.5 hours. During the cooling process, the cooling rate in the range of 1050℃ to 850℃ was controlled at 70℃ / h. After cooling to room temperature, the zirconium silicate zinc oxide composite toughened high-alumina structure porcelain material was obtained.
[0134] Comparative Example 1:
[0135] Compared with Example 2, the difference is that zirconium silicate is not added, the composite pre-reacting mineralized material is replaced with a pre-reacting mineralized material without zirconium silicate, and the missing zirconium silicate mass is made up by calcined bauxite. All other parameters and steps are the same.
[0136] Comparative Example 2:
[0137] Compared with Example 2, the difference is that zinc oxide is not added, the composite pre-reacted mineral material is replaced with a pre-reacted mineral material without zinc oxide, and 0.47 parts by weight of zinc oxide is not added when the ball milling is carried out for 9.8 hours. The missing zinc oxide mass is made up by kaolin. All other parameters and steps are the same.
[0138] Comparative Example 3:
[0139] Compared with Example 2, the difference is that no barium carbonate is added to the raw materials involved in the pre-calcination treatment or the main ball milling stage. The missing barium carbonate is made up by kaolin. All other parameters and steps are the same.
[0140] Comparative Example 4:
[0141] Compared with Example 2, the difference is that the pre-calcined zirconium silicate, zinc oxide, barium carbonate, potassium feldspar and kaolin in Example 2 are not pre-calcined, but are entered into the initial wet ball mill together with calcined bauxite, kaolin, potassium feldspar, barium carbonate and bentonite; the time-sharing addition method of zinc oxide and the subsequent addition method of sodium humate are the same as in Example 2, and the remaining parameters and steps are the same.
[0142] Comparative Example 5:
[0143] Compared with Example 2, the difference is that 0.47 parts by mass of zinc oxide is not added when the ball milling is in progress for 9.8 hours, but is added to the ball mill together with the composite pre-reacted minerals, calcined bauxite, kaolin, potassium feldspar, barium carbonate and bentonite before dry mixing. All other parameters and steps are the same.
[0144] Comparative Example 6:
[0145] Compared with Example 2, the difference is that the firing process is changed to continuously heating to 1272°C, holding at 1272°C for 2 hours and then naturally cooling. The controlled cooling of 990°C for 3 hours, 1100°C for 60 minutes and 55°C / h in the range of 1050°C to 850°C is not set. All other parameters and steps are the same.
[0146] Test Example 1:
[0147] Experimental description:
[0148] This test case is used to evaluate the process feasibility of Examples 1 to 3 in the processes of pressure filtration, aging, vacuum plowing, extrusion molding, drying and firing, and to examine the densification stability of the fired products.
[0149] Experimental steps:
[0150] The clay cakes, dried blanks and fired products obtained in Examples 1 to 3 were used as test objects. Three samples were taken from each group of clay cakes, each sample weighing about 100g. 120 pieces were taken from each group of dried blanks and 120 pieces were taken from each group of fired products.
[0151] The mud cake samples were dried in a 105℃ drying oven to constant weight, and the moisture content of the mud cake was calculated based on the mass change before and after drying.
[0152] The dried billets are inspected for surface and edge cracks under natural light, and the drying crack rate is calculated as the proportion of the number of billets with visible cracks to the total number of dried billets.
[0153] After the fired products have cooled to room temperature, inspect them for visible cracks. Calculate the firing cracking rate based on the proportion of products with visible cracks to the total number of fired products.
[0154] The firing deformation rate is calculated based on the maximum deviation of the same reference size before and after firing. The water absorption rate is tested by the boiling water absorption method. Ten fired products are taken from each group and the average value is taken.
[0155] Another set of sintered test strips from Examples 1 to 3 were subjected to impact vibration tests. Vibration response signals were collected and obtained after fast Fourier transform to obtain amplitude-frequency response curves.
[0156] Experimental data:
[0157] The results of the process feasibility test are shown in Table 1.
[0158] Table 1: Results of Process Feasibility Tests
[0159] sample Example 1 Example 2 Example 3 Moisture content of mud cake (wt%) 19.3 20.8 22.6 Drying crack rate (%) 1.7 0.8 1.3 Firing crack rate (%) 1.1 0.6 0.9 Firing deformation rate (%) 0.72 0.46 0.59 Water absorption rate (%) 0.13 0.07 0.10
[0160] Experimental conclusion:
[0161] Referring to Table 1, the moisture content of the mud cakes in Examples 1 to 3 were 19.3 wt%, 20.8 wt%, and 22.6 wt%, respectively, all of which were suitable for subsequent aging, vacuum refining, and extrusion molding processes. The drying crack rate of all three examples was less than 2.0%, indicating that after the addition of the composite pre-reacted mineralizer, the mud material still maintained a process state suitable for molding and drying.
[0162] The firing cracking rates of Examples 1 to 3 were 1.1%, 0.6%, and 0.9%, respectively, and the water absorption rates were 0.13%, 0.07%, and 0.10%, respectively, indicating that all three examples were able to achieve firing densification. The firing deformation rate of Example 2 was 0.46%, lower than that of Examples 1 and 3, indicating that the ball milling fineness, cake moisture content, aging time, and firing regime were well-balanced.
[0163] See attached document Figure 1The amplitude-frequency response curves of Examples 1 to 3 all have identifiable main peaks and secondary response regions, with small fluctuations in the curve baseline and no wide-range abnormal responses observed. The main peak of Example 2 is more concentrated, which corresponds to the lower water absorption rate, firing cracking rate, and firing deformation rate in Table 1, indicating that the overall consistency of the fired test strips obtained in Example 2 is good.
[0164] Test Example 2:
[0165] Experimental description:
[0166] This test example is used to evaluate the firing stability of ZnO / ZrSiO4 mass ratio and BaCO3 / ZnO mass ratio after adjusting them under different potassium feldspar (K2O) contents.
[0167] Experimental steps:
[0168] The fired products prepared in Examples 1 to 3 were used as test objects, and 120 products from the same firing batch were taken in each group.
[0169] The K2O content in potassium feldspar used in each example was determined by X-ray fluorescence spectroscopy. The ZnO / ZrSiO4 mass ratio and BaCO3 / ZnO mass ratio were calculated based on the dry basis feeding records.
[0170] The same reference length was measured before and after firing the green body, and the firing linear shrinkage rate was calculated according to the ratio of the change in length before and after firing to the length before firing.
[0171] The firing deformation rate is calculated as the ratio of the maximum dimensional deviation of the product after firing to the corresponding dimensional deviation before firing.
[0172] Water absorption rate was tested using the boiling water absorption method. Ten fired products were taken from each group and the average value was taken.
[0173] The appearance qualification rate is calculated as the proportion of products without visible cracks, missing corners, blistering and obvious deformation in the same firing batch to the total number of products;
[0174] Sixty pieces were randomly selected from each group of fired products, and the deviation of the firing line shrinkage rate from the average value of the group was recorded. After the mean was removed, a fast Fourier transform was performed to obtain the firing line shrinkage fluctuation power spectrum curve.
[0175] Experimental data:
[0176] The results of the batching linkage and firing stability tests are shown in Table 2.
[0177] Table 2: Results of Ingredient Mixing and Firing Stability Tests
[0178] sample Example 1 Example 2 Example 3 <![CDATA[K2O content (wt%)]]> 9.53 9.76 10.43 <![CDATA[ZnO / ZrSiO₄ mass ratio]]> 0.520 0.458 0.380 <![CDATA[BaCO3 / ZnO mass ratio]]> 0.337 0.450 0.550 Linear shrinkage during firing (%) 10.86 10.41 10.67 Firing deformation rate (%) 0.72 0.46 0.59 Water absorption rate (%) 0.13 0.07 0.10 Appearance pass rate (%) 96.8 98.9 97.6
[0179] Experimental conclusion:
[0180] Referring to Table 2, the K2O content of potassium feldspar used in Examples 1 to 3 was 9.53 wt%, 9.76 wt%, and 10.43 wt%, respectively. With the change in K2O content, the ZnO / ZrSiO4 mass ratio was adjusted from 0.520 to 0.380, and the BaCO3 / ZnO mass ratio was adjusted from 0.337 to 0.550. The firing shrinkage rates of the three examples were 10.86%, 10.41%, and 10.67%, respectively, with the difference controlled within 0.45 percentage points, indicating that after adjusting the ingredient ratios, the firing shrinkage remained at a relatively close level.
[0181] The firing deformation rate of Examples 1 to 3 was 0.46% to 0.72%, the water absorption rate was 0.07% to 0.13%, and the appearance qualification rate was 96.8% to 98.9%. Among them, Example 3 used a higher potassium feldspar K2O content, while the ZnO / ZrSiO4 mass was relatively low and the BaCO3 / ZnO mass was relatively high. Its firing deformation rate and water absorption rate were still within an acceptable range, indicating that the batching adjustment method can reduce the impact of changes in potassium feldspar alkali content on the firing state.
[0182] See attached document Figure 2 The power spectrum curves of firing line shrinkage fluctuations in Examples 1 to 3 did not show a continuous high amplitude response, indicating that the intra-batch line shrinkage deviation did not form a sustained and concentrated fluctuation. The normalized spatial frequency range of 0 to 0.2 mainly corresponds to slow intra-batch fluctuations, and the range of 0.4 to 1.0 mainly corresponds to local fluctuations. The curve of Example 2 showed relatively small fluctuations in the above frequency range, which corresponds to the lower firing deformation rate, lower water absorption rate, and higher appearance pass rate in Table 2.
[0183] Test Example 3:
[0184] Experimental description:
[0185] This test case is used to evaluate the effects of the absence of zirconium silicate, zinc oxide, and barium carbonate on the water absorption, unglazed flexural strength, thermal shock resistance, and strength retention after thermal shock of fired products.
[0186] Experimental steps:
[0187] The fired products prepared in Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were used as test objects, and no less than 15 samples were taken from each group.
[0188] Water absorption rate was tested using the boiling water absorption method. Ten samples were taken from each group, and the average value of the test results was taken.
[0189] The unglazed bending strength was tested using the three-point bending method with a span of 60 mm and a loading rate of 0.5 mm / min. Five samples were taken from each group, and the average value of the test results was taken.
[0190] The thermal shock test was conducted by heating followed by water cooling. The sample was heated to the set temperature and held for 30 minutes, then immersed in 20°C water to cool, and the highest temperature difference that did not cause the sample to crack was recorded.
[0191] The cracking rate after thermal shock cycling is calculated as the proportion of the number of samples with visible cracks after 5 thermal shock cycles to the total number of samples.
[0192] The retention rate of unglazed flexural strength after rapid thermal change is calculated as the ratio of unglazed flexural strength after rapid thermal change treatment to unglazed flexural strength before treatment.
[0193] Another fired test strip after a rapid thermal cycling was taken and subjected to a knocking vibration test. The vibration response signal was collected and the amplitude-frequency response curve was obtained after fast Fourier transform.
[0194] Experimental data:
[0195] The results of the key component missing comparison test are shown in Table 3.
[0196] Table 3: Results of Key Component Missing Comparison Test
[0197] sample Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Water absorption rate (%) 0.07 0.09 0.32 0.12 Unglazed flexural strength (MPa) 183.6 154.2 139.7 166.8 Rapid temperature change (°C) 210 170 160 180 Cracking rate (%) after rapid temperature change cycle 3.3 15.0 19.2 12.5 Percentage of unglazed flexural strength retention after rapid temperature change (%) 87.4 72.8 68.5 76.3
[0198] Experimental conclusion:
[0199] Referring to Table 3, Example 2 had a water absorption rate of 0.07%, an unglazed flexural strength of 183.6 MPa, a thermal shock temperature difference of 210°C, and a flexural strength retention rate of 87.4% after thermal shock. These results are superior to Comparative Examples 1 to 3. In Comparative Example 1, without the addition of zirconium silicate, the unglazed flexural strength decreased to 154.2 MPa, and the thermal shock temperature difference decreased to 170°C. In Comparative Example 2, without the addition of zinc oxide, the water absorption rate increased to 0.32%, and the unglazed flexural strength decreased to 139.7 MPa. In Comparative Example 3, without the addition of barium carbonate, the cracking rate after thermal shock cycling was 12.5%, higher than that of Example 2.
[0200] The above data indicate that zirconium silicate mainly affects the unglazed flexural strength and strength retention after thermal shock in fired products, zinc oxide mainly affects the degree of densification during firing, and barium carbonate affects the stability after thermal shock cycling. Example 2 contains zirconium silicate, zinc oxide, and barium carbonate, and shows a good match between water absorption, unglazed flexural strength, thermal shock temperature difference, and cracking rate after cycling.
[0201] See attached document Figure 3In Example 2, the amplitude-frequency response curve after rapid thermal cycling exhibits a more concentrated main response peak, and the fluctuations in the secondary response segment are also relatively smooth. In Comparative Examples 1 to 3, the main response peak height decreases, the peak shape widens, and some curves show a more dispersed response in the secondary response segment. This result is consistent with the trend in Table 3 of decreased retention rate of unglazed flexural strength and increased cracking rate after rapid thermal cycling, indicating that the lack of zirconium silicate, zinc oxide, or barium carbonate reduces the overall response consistency of the test strips after rapid thermal treatment.
[0202] Test Example 4:
[0203] Experimental description:
[0204] This test case is used to evaluate the effects of pre-firing treatment, timed addition of zinc oxide, and dual medium-temperature reaction firing regime on the properties of fired products.
[0205] Experimental steps:
[0206] The fired products obtained from Example 2, Comparative Example 4, Comparative Example 5 and Comparative Example 6 were used as test objects, and no less than 30 products from the same firing batch were taken from each group.
[0207] Water absorption rate was tested using the boiling water absorption method. Ten samples were taken from each group, and the average value of the test results was taken.
[0208] The same reference length was measured before and after firing the green body, and the firing linear shrinkage rate was calculated according to the ratio of the change in length before and after firing to the length before firing.
[0209] The firing deformation rate is calculated as the ratio of the maximum dimensional deviation of the product after firing to the corresponding dimensional deviation before firing.
[0210] The unglazed bending strength was tested using the three-point bending method with a span of 60 mm and a loading rate of 0.5 mm / min. Five samples were taken from each group, and the average value of the test results was taken.
[0211] The thermal shock test was conducted by heating followed by water cooling. The sample was heated to the set temperature and held for 30 minutes, then immersed in 20°C water to cool, and the highest temperature difference that did not cause the sample to crack was recorded.
[0212] Another set of fired test strips were subjected to impact vibration test, and vibration response signals were collected. The phase frequency response curves were obtained after fast Fourier transform.
[0213] Experimental data:
[0214] The results of the process path comparison test are shown in Table 4.
[0215] Table 4: Test Results of Process Path Comparison
[0216] sample Example 2 Comparative Example 4 Comparative Example 5 Comparative Example 6 Water absorption rate (%) 0.07 0.18 0.11 0.16 Linear shrinkage during firing (%) 10.41 10.93 10.69 11.08 Firing deformation rate (%) 0.46 0.81 0.66 0.93 Unglazed flexural strength (MPa) 183.6 159.4 168.7 154.6 Rapid temperature change (°C) 210 180 190 170
[0217] Experimental conclusion:
[0218] Referring to Table 4, Example 2 had a water absorption rate of 0.07%, a firing linear shrinkage rate of 10.41%, a firing deformation rate of 0.46%, an unglazed flexural strength of 183.6 MPa, and a thermal shock temperature difference of 210°C. In Comparative Example 4, after the pre-firing treatment was omitted, the water absorption rate and firing deformation rate increased, and the unglazed flexural strength decreased to 159.4 MPa. This indicates that the densification and dimensional stability of zirconium silicate, zinc oxide, barium carbonate, potassium feldspar, and kaolin were affected during the firing process without pre-firing treatment.
[0219] In Comparative Example 5, after zinc oxide was added to the main ball mill at the beginning stage, the water absorption rate was 0.11%, the firing deformation rate was 0.66%, and the temperature difference between hot and cold was 190°C, which were lower than those in Example 2. In Comparative Example 6, after the dual medium-temperature holding and controlled cooling were eliminated, the firing linear shrinkage rate increased to 11.08%, the firing deformation rate increased to 0.93%, and the unglazed flexural strength decreased to 154.6 MPa. This indicates that when degassing, zinc-containing reactions, and high-temperature densification occur during continuous heating, the firing state is difficult to control stably.
[0220] See attached document Figure 4 In Example 2, the phase frequency response curve completed the main phase transition in the range of approximately 2000 Hz to 2400 Hz, with the transition region being relatively concentrated. In Comparative Examples 4, 5, and 6, the phase transition shifted forward or broadened, and phase fluctuations of varying degrees appeared in the range of approximately 3300 Hz to 4200 Hz. This result is consistent with the trends in Table 4 regarding increased water absorption, increased firing deformation rate, and decreased unglazed flexural strength, indicating that pre-firing treatment, timed addition of zinc oxide, and the dual-medium-temperature reaction firing regime affect the overall response consistency of the fired test specimens.
[0221] Test Example 5:
[0222] Experimental description:
[0223] This test example is used to evaluate the electrical properties and batch firing stability of the fired products obtained in Examples 1 to 3, and is compared with Comparative Example 4 and Comparative Example 6.
[0224] Experimental steps:
[0225] The fired products prepared in Examples 1, 2, 3, 4, and 6 were used as test objects, and no less than 120 products from the same firing batch were taken in each group.
[0226] The power frequency breakdown strength was determined by the power frequency voltage breakdown test method. Five samples were taken in each group, and the average value of the test results was taken.
[0227] Volume resistivity was determined using the volume resistivity test method for insulating materials. The test voltage was 500V. Five samples were taken from each group, and the average value of the test results was taken.
[0228] Water absorption rate was tested using the boiling water absorption method. Ten samples were taken from each group, and the average value of the test results was taken.
[0229] The batch firing pass rate is calculated as the proportion of products that pass the appearance, size and water absorption rate in the same firing batch to the total number of products.
[0230] The power frequency breakdown strength was tested again after the thermal shock treatment. The electrical performance retention rate after the thermal shock treatment was calculated as the ratio of the power frequency breakdown strength after the thermal shock treatment to the power frequency breakdown strength before the treatment.
[0231] Take another sample after the rapid thermal change treatment, and at 10 2 Hz to 10 6 Dielectric loss was tested within the Hz range to obtain the dielectric loss frequency response curve.
[0232] Experimental data:
[0233] The results of electrical performance and batch stability tests are shown in Table 5.
[0234] Table 5: Electrical performance and batch stability test results
[0235] sample Example 1 Example 2 Example 3 Comparative Example 4 Comparative Example 6 Power frequency breakdown strength (kV / mm) 18.4 20.1 19.2 16.3 15.7 Volume resistivity (Ω·m) <![CDATA[3.6×10 12 ]]> <![CDATA[4.8×10 12 ]]> <![CDATA[4.1×10 12 ]]> <![CDATA[2.2×10 12 ]]> <![CDATA[1.9×10 12 ]]> Water absorption rate (%) 0.13 0.07 0.10 0.18 0.16 Batch firing pass rate (%) 96.5 98.7 97.4 92.6 90.8 Electrical performance retention rate after rapid temperature change (%) 84.2 89.6 86.8 77.5 74.9
[0236] Experimental conclusion:
[0237] Referring to Table 5, the power frequency breakdown strength of Examples 1 to 3 ranged from 18.4 kV / mm to 20.1 kV / mm, and the volume resistivity was 3.6 × 10⁻⁶. 12 Ω·m to 4.8×10 12 The water absorption rate is 0.07% to 0.13% (Ω·m). Example 2 exhibits higher power frequency breakdown strength and volume resistivity, and lower water absorption, indicating that this group of samples shows good coordination in terms of sintering densification and insulation performance.
[0238] Comparative Example 4, without pre-firing treatment, had a batch firing pass rate of 92.6% and an electrical performance retention rate of 77.5% after rapid thermal changes. Comparative Example 6, without dual medium-temperature insulation and controlled cooling, had a batch firing pass rate of 90.8% and an electrical performance retention rate of 74.9% after rapid thermal changes. Compared with Example 2, Comparative Examples 4 and 6 had higher water absorption rates, lower power frequency breakdown strength, and lower volume resistivity, indicating that pre-firing treatment and firing temperature programs affect the densification degree of the products and the retention of electrical performance after rapid thermal changes.
[0239] See attached document Figure 5 Examples 1 to 3 are in 10 2Hz to 10 6 The dielectric loss tangent in the Hz range is generally lower than that of Comparative Example 4 and Comparative Example 6, and the curve changes more gently with frequency. Comparative Example 4 and Comparative Example 6 at 10 Hz... 4 Hz to 10 5 A significant increase in loss was observed in the Hz range, corresponding to the lower power frequency breakdown strength, volume resistivity, and electrical performance retention rate after thermal shock treatment shown in Table 5. This result indicates that the sample from the example still maintains good insulation stability after thermal shock treatment.
[0240] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material, characterized in that, Raw materials comprising the following parts by weight: Composite pre-reacted mineralizer: 8.68 parts to 15.50 parts; Calcined bauxite: 38.00 parts to 42.00 parts; Kaolin: 35.58 parts to 45.09 parts; Potassium feldspar: 6.30 parts to 7.35 parts; Zirconium silicate: 0 parts to 0.90 parts; Zinc oxide: 0.02 parts to 0.88 parts; Barium carbonate: 0 parts to 0.22 parts; Bentonite: 0.30 parts to 0.80 parts; Sodium humate: 0.03 parts to 0.12 parts; The raw material includes one of zirconium silicate and barium carbonate; the composite pre-reacted mineralized material is prepared by pre-reaction of dry-based raw materials including zirconium silicate, zinc oxide, barium carbonate, potassium feldspar and kaolin.
2. The zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material according to claim 1, characterized in that, The mass fraction of the composite pre-reacted mineralizer is calculated based on the total mass of dry-based raw materials used in its preparation. The composite pre-reacted mineralizer is made from the following mass fractions of dry-based raw materials: Zirconium silicate: 100 parts; Zinc oxide: 30 to 45 parts; Barium carbonate: 12 to 25 parts; Potassium feldspar: 55 to 75 parts; Kaolin: 20 to 40 parts.
3. The zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material according to claim 2, characterized in that, When preparing the composite pre-reacted mineralized material, the dry-based raw materials added meet the following mass ratio: The mass ratio of zinc oxide to zirconium silicate is (30-45):100; The mass ratio of barium carbonate to zinc oxide is (12-25):(30-45). The mass ratio of potassium feldspar to kaolin is (55-75):(20-40).
4. A method for preparing a zirconium silicate-zinc oxide composite toughened high-alumina structural electrical porcelain material as described in any one of claims 1 to 3, characterized in that, Includes the following steps: The composite pre-reacted mineral material, calcined bauxite, kaolin, potassium feldspar, bentonite, and one of barium carbonate or zirconium silicate are sequentially added to the ball mill. They are first dry-mixed, and then water is added for wet ball milling. Continue the wet ball milling process, adding zinc oxide during the process and sodium humate before the end of the wet ball milling. After the wet ball milling is completed, the fineness of the slurry is measured to obtain the milled slurry. The ball-milled slurry is passed through an iron remover to remove iron, and then sent to a filter press to filter it to obtain mud cake. The mud cake is cut into pieces and sent to an aging chamber for aging, and the surface of the mud is kept covered during the aging process. The aged clay is fed into a vacuum clay kneading machine for kneading. After kneading, it is extruded to obtain an electric porcelain blank, which is then dried. The dried porcelain blank is sent into a kiln for firing, and after cooling to room temperature, a high-alumina structural porcelain material with zirconium silicate and zinc oxide composite toughening is obtained.
5. The preparation method according to claim 4, characterized in that, The conditions for the dry mixing and the wet ball milling are as follows: The dry mixing time is 20 min to 40 min; The solid content of the wet ball milling slurry is 60wt% to 68wt%. The total time for the wet ball milling is 12h to 16h; After the wet ball milling is completed, the residue on the slurry sieve is no more than 0.05 wt%.
6. The preparation method according to claim 5, characterized in that, The conditions for adding the zinc oxide and the sodium humate are as follows: The amount of zinc oxide added is 0.02 parts to 0.88 parts, and the addition time is 7.2 h to 12 h after the wet ball milling is carried out; The amount of sodium humate added is 0.03 to 0.12 parts, and the addition time is 1 to 2 hours before the end of the wet ball milling.
7. The preparation method according to claim 4, characterized in that, The conditions for the pressure filtration, aging, vacuum plowing, and drying are as follows: After filtration, the moisture content of the sludge cake is 19wt% to 23wt%. The aging time is 48h to 72h; The vacuum degree of the vacuum ply mill is greater than 0.09 MPa; After drying, the residual moisture content of the electric porcelain blank is no higher than 0.8 wt%.
8. The preparation method according to claim 7, characterized in that, The firing conditions are as follows: Heat the temperature to 960℃~1010℃ and then keep it at that temperature for 2h~4h; Continue heating to 1080℃~1120℃ and then hold for 40min~80min; Then raise the temperature to 1265℃~1280℃ and hold for 1.5h~2.5h; During the cooling process, the cooling rate in the range of 1050℃ to 850℃ is 40℃ / h to 70℃ / h.
9. The preparation method according to claim 4, characterized in that, The composite pre-reacted mineralized material is prepared according to the following steps: Zirconium silicate, zinc oxide, barium carbonate, potassium feldspar and kaolin used to prepare composite pre-reacted minerals are added to a ball mill, and then water is added for wet ball milling. The ball-milled slurry is filtered to obtain a premixed mud cake, and the premixed mud cake is dried to obtain a premixed dry material; The premixed dry material is fed into a kiln for pre-firing. After pre-firing, it is cooled to room temperature, crushed, and sieved to obtain the composite pre-reacted mineralized material.
10. The preparation method according to claim 9, characterized in that, The preparation conditions for the composite pre-reacted mineralized material are as follows: During the wet ball milling process, the solid content of the slurry is 60wt%–68wt%, the milling time is 8h–12h, and the residue on a 10,000-mesh sieve after milling is 0.08wt%–0.15wt%. The premixed mud cake is dried at a temperature of 80℃~100℃ for 4h~6h, and the resulting premixed dry material has a moisture content of no more than 1.0wt%. When the premixed dry material is pre-fired, the pre-fired temperature is 880℃~930℃ and the pre-fired time is 0.5h~1.5h. After the pre-fired material is completed, it is crushed and passed through an 80-120 mesh sieve.