A method for preparing a short-period PIP dense direct writing molding silicon carbide dot array ceramic

By using a solid-liquid composite impregnation system and a short-cycle PIP process, the problem of insufficient density in direct-write silicon carbide lattice ceramics was solved, achieving high density and uniform mechanical properties in complex structures, improving the material's hardness, toughness, and dynamic impact resistance, and shortening the preparation cycle.

CN123062271APending Publication Date: 2026-11-10QIANWAN INST OF CNITECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611568262.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-12
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing direct-write silicon carbide lattice ceramics suffer from insufficient density, excessive number of cycles in conventional PIP processes leading to lengthy preparation cycles, poor density gradient of components caused by gravity differentiation during impregnation, and low conversion rate of silicon carbide produced by pyrolysis.

Method used

By employing a solid-liquid composite impregnation system and a short-cycle PIP process, silicon carbide powder with graded particle sizes is combined in ceramic slurry and modified impregnation liquid. Silicon carbide lattice preforms are constructed using direct-write 3D printing. Through steps such as vacuum pre-sintering, vacuum negative pressure impregnation, curing, and pyrolysis, the high density and uniform mechanical properties of the complex lattice structure are achieved.

Benefits of technology

It significantly improves the density and mechanical property uniformity of silicon carbide lattice ceramics, shortens the preparation cycle, reduces the number of high-temperature thermal cycles and raw material loss, and enhances the hardness, toughness and dynamic impact resistance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123062271A_ABST
    Figure CN123062271A_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of silicon carbide ceramics, and relates to a preparation method of short-period PIP dense direct-writing forming silicon carbide lattice ceramics. The method comprises the following steps: (1) mixing first silicon carbide coarse powder, first silicon carbide fine powder and an additive and water to prepare ceramic slurry; (2) directly writing 3D printing to form a lattice blank; (3) vacuum pre-sintering to obtain a porous preform; (4) mixing an organic silicon precursor, second silicon carbide coarse powder, second silicon carbide fine powder, a surface modifier and an organic solvent to obtain a modified impregnating solution; (5) vacuum negative pressure impregnation, solidification and pyrolysis of the preform in the modified impregnating solution; (6) repeating the PIP cycle for 2-4 times; and (7) polishing after crystallization treatment to obtain the silicon carbide lattice ceramic. Through the cooperation of coarse and fine powder gradation and surface modification, the application realizes the combination of solid phase filling and precursor pyrolysis, significantly shortens the preparation period, improves the mechanical uniformity, and is suitable for lightweight protection, heat exchange and high-temperature bearing structural parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of silicon carbide ceramic technology and relates to a method for preparing short-cycle PIP dense direct-write molded silicon carbide lattice ceramics. Background Technology

[0002] Silicon carbide (SiC) ceramics possess ultra-high hardness, high temperature resistance, and strong chemical corrosion resistance. Lattice porous silicon carbide, with its three-dimensional controllable interconnected topology, achieves a synergistic effect of lightweighting and functionality, exhibiting irreplaceable application potential in impact protection and high-temperature heat exchange. Direct-write 3D printing technology, relying on ceramic slurries with shear-thinning properties, can digitally form arbitrarily complex lattice cell structures without custom molds. Pore size, porosity, and gradient structure can all be precisely designed, offering significant advantages in structure control compared to traditional porous ceramic preparation processes such as organic foam impregnation, solid-phase pore formation, and bio-templates.

[0003] However, simple direct-write printing combined with pre-sintered silicon carbide lattice preforms results in a high proportion of through-pores and low skeletal density. The material's hardness, toughness, and dynamic impact resistance are insufficient to meet the requirements of high-load-bearing and high-speed impact conditions. Currently, the mainstream densification method in the industry is PIP (Precursor Infiltration and Pyrolysis) process, which typically uses only a pure organosilicon precursor solution as the impregnation medium. Without solid ceramic particles filling the solution, the yield of newly generated SiC ceramic phases during a single pyrolysis is low. It requires 8 to 15 cycles of impregnation-curing-pyrolysis to slightly improve the component's density, resulting in a lengthy overall preparation cycle and high equipment energy and material consumption. Furthermore, the pure organosilicon precursor solution has high fluidity, and during the impregnation process, a wetting gradient forms along the vertical direction of the preform under gravity. This leads to full filling of pores at the bottom of the component, while leaving a large number of unfilled through-pores at the top. Consequently, the component's hardness and compressive strength fluctuate greatly along the thickness direction, resulting in extremely poor uniformity of mechanical properties.

[0004] Conventional PIP systems lack a solid-phase powder in-situ filling mechanism, and multiple rounds of high-temperature thermal cycling continuously induce and propagate microcracks within the component, significantly reducing the material's fracture toughness and dynamic compressive strength. Existing research largely focuses on PIP densification processes for fiber-reinforced silicon carbide composites, lacking a powder modification and impregnation system suitable for direct-write printing of pure silicon carbide lattice preforms, as well as an integrated, short-cycle PIP process. Furthermore, it cannot simultaneously meet the three core requirements of complex structure forming freedom, component density and uniformity, and high and low temperature mechanical stability. Summary of the Invention

[0005] The purpose of this invention is to address the problems in existing technologies, such as insufficient density of silicon carbide lattice ceramics formed by direct-write molding, excessive number of cycles in conventional PIP processes leading to lengthy preparation cycles, poor density gradients in components caused by gravity differentiation during impregnation, and low conversion rates of silicon carbide produced by pyrolysis. This invention provides a method for preparing dense direct-write molded silicon carbide lattice ceramics using a short-cycle PIP process. This method, by constructing a solid-liquid composite impregnation system and integrating it with a short-cycle PIP process, can achieve high density of complex lattice structures, uniform mechanical properties, and a significantly shortened preparation cycle.

[0006] The first objective of this invention is achieved through the following technical solution: A method for preparing short-cycle PIP dense direct-write molded silicon carbide lattice ceramics includes the following steps: (1) Mix the first coarse silicon carbide powder, the first fine silicon carbide powder, the additives and water to obtain a ceramic slurry; (2) Obtain a silicon carbide lattice green body by direct writing 3D printing of the ceramic slurry; (3) The silicon carbide lattice preform is vacuum pre-sintered to obtain a silicon carbide lattice porous preform; (4) Mix the organosilicon precursor, coarse second silicon carbide powder, fine second silicon carbide powder, surface modifier and organic solvent to obtain a modified impregnation solution; (5) The silicon carbide lattice porous preform is vacuum impregnated in the modified impregnation liquid, and then cured and pyrolyzed to complete one PIP cycle. (6) Repeat step (5) 2 to 4 times until the weight gain after a single PIP cycle is less than the preset threshold of 0.6 to 1.2 wt%, and the intermediate is obtained; (7) Under an inert atmosphere, the intermediate is crystallized to obtain silicon carbide lattice ceramic; In step (1), the median particle size of the first coarse silicon carbide powder is 1~2μm, the median particle size of the first fine silicon carbide powder is 200~500nm, and the amount of the first coarse silicon carbide powder added is ≥ the amount of the first fine silicon carbide powder added. In step (4), the median particle size of the second coarse silicon carbide powder is 1~2μm, the median particle size of the second fine silicon carbide powder is 200~500nm, and the amount of the second coarse silicon carbide powder added is ≤ the amount of the second fine silicon carbide powder added.

[0007] Preferably, in step (1), the total amount of the first coarse silicon carbide powder and the first fine silicon carbide powder added is 60-70 vol% of the volume fraction of the ceramic slurry.

[0008] Preferably, in step (1), the mass ratio of the first coarse silicon carbide powder to the first fine silicon carbide powder is 5:5 to 8:2.

[0009] In the ceramic slurry system, the amount of coarse silicon carbide powder added is greater than or equal to the amount of fine silicon carbide powder added. If too much fine powder is added, it will significantly increase the viscosity of the slurry and reduce its rheological stability, thereby affecting the extrusion uniformity and molding accuracy of direct-write 3D printing. At the same time, during the subsequent heating process, an excessively high content of fine powder will also lead to an increase in the sintering linear shrinkage rate, causing dimensional deviations and structural cracking risks.

[0010] Further preferred, in step (1), the amount of the first coarse silicon carbide powder added is greater than the amount of the first fine silicon carbide powder added.

[0011] Preferably, in step (1), the additives include dispersants, binders, and aqueous organic rheology modifiers; The dispersant is ammonium polycarboxylate, and its addition amount is 0.8~5 wt% of the total addition amount of the first coarse silicon carbide powder and the first fine silicon carbide powder; The binder is polyvinylpyrrolidone, and its addition amount is 0.3~3 wt% of the total addition amount of the first silicon carbide coarse powder and the first silicon carbide fine powder; The amount of the aqueous organic rheology modifier added is 0.1 to 0.3 wt% of the total amount of the first coarse silicon carbide powder and the first fine silicon carbide powder.

[0012] Preferably, in step (2), the parameters of the direct-write 3D printing include: nozzle outlet diameter of 1.0~2.0mm, extrusion pressure of 0.6~0.8MPa, printing speed of 18~22mm / s, and layer height of 0.9~1.0mm.

[0013] Preferably, in step (3), the vacuum pre-sintering is a two-stage sintering with a vacuum degree ≤10. -3 Pa, heating rate is 1~10℃ / min, first stage temperature is 500~700℃, time is 60~120min, second stage temperature is 1700~2000℃, time is 10~40min.

[0014] Preferably, in step (3), the porosity of the silicon carbide lattice porous preform is 35~45 vol.

[0015] This porosity range provides ample solid-phase filling space for the subsequent PIP impregnation process, ensuring that the impregnation liquid can fully penetrate to achieve densification, while maintaining sufficient structural strength of the precast skeleton to withstand the vacuum negative pressure and thermal stress during the impregnation process. This avoids insufficient densification due to insufficient impregnation liquid penetration caused by excessively low porosity, or insufficient skeleton strength due to excessively high porosity, which would affect the structural integrity of the component.

[0016] Preferably, in step (4), the amount of the second coarse silicon carbide powder added is less than the amount of the second fine silicon carbide powder added.

[0017] Preferably, in step (4), the mass ratio of the second coarse silicon carbide powder to the second fine silicon carbide powder is 2:8 to 5:5.

[0018] Further preferably, the mass ratio of the second coarse silicon carbide powder to the second fine silicon carbide powder is 3:7 to 4:6.

[0019] In the modified impregnation solution system, when the amount of fine silicon carbide powder added is greater than that of coarse silicon carbide powder added, it is beneficial to impregnation penetration and densification. The fine powder has a small particle size, which can penetrate deep into the micro-nano pores of the preform with the precursor solution to achieve full filling; at the same time, the fine powder has a large specific surface area, which can provide sufficient heterogeneous nucleation sites, promote the epitaxial growth of SiC ceramic phase, and improve the ceramic production efficiency and the overall density of the component.

[0020] Preferably, in step (4), the total mass of the second coarse silicon carbide powder and the second fine silicon carbide powder is 11 to 20 wt% of the mass of the modified impregnation liquid.

[0021] Preferably, in step (4), the amount of surface modifier added is 0.1 to 10 wt% of the mass of the modified impregnation solution.

[0022] Preferably, in step (4), the surface modifier includes a silane coupling agent or a silazane compound; The silane coupling agent is at least one of 3-aminopropyltriethoxysilane KH-550 and γ-glycidoxypropyltrimethoxysilane KH-560; The silazane compound is hexamethyldisilazane (HMDS).

[0023] Further preferably, the amount of the surface modifier added is 0.1~5wt% of the mass of the modified impregnation solution.

[0024] More preferably, the amount of the surface modifier added is 0.3 to 0.8 wt% of the mass of the modified impregnation liquid.

[0025] Preferably, in step (4), the organosilicon precursor includes at least one of polycarbosilane and polysilane.

[0026] Preferably, in step (4), the organic solvent includes at least one of n-hexane, xylene, toluene, cyclohexane, and ethyl acetate.

[0027] Preferably, in step (5), the absolute pressure of the vacuum negative pressure impregnation is ≤1kPa, the impregnation temperature is 40~60℃, and the impregnation time is 1.5~2h; The curing temperature is 180~260℃, and the curing time is 1~12h; The pyrolysis was carried out under an inert atmosphere, with the temperature increased to 1100-1600℃ at a heating rate of 1-10℃ / min and held for 0.5-2h.

[0028] Further preferably, the curing process includes ventilating and drying at 20~30℃ for 0.1~6 hours before curing.

[0029] If the uncrosslinked organic precursors are directly heated and decomposed without curing, they cannot form a stable solid framework. At high temperatures, they will be lost in large quantities due to rapid solvent evaporation and precursor melting and flow, resulting in a significant decrease in ceramic yield. At the same time, a large number of uncrosslinked organic components release small molecule volatiles in a concentrated and violent manner during decomposition. The gas cannot be slowly discharged through the pore channels in time, which will form local high pressure inside the component, causing defects such as blistering, delamination, or even cracking.

[0030] Preferably, in step (6), the preset threshold is 0.8wt%.

[0031] Preferably, in step (7), the crystallization treatment is carried out at a temperature of 1100~1600℃ for a time of 0.5~2h.

[0032] Preferably, step (7) includes post-processing, which includes polishing.

[0033] Preferably, the temperature of the crystallization treatment in step (7) is the same as the temperature of the pyrolysis in step (5).

[0034] Pyrolysis transforms the organic precursor into a SiC ceramic phase and releases small-molecule volatiles. Crystallization treatment allows the amorphous SiC phase generated by pyrolysis to fully crystallize and rearrange, eliminating residual organic components and thermal stress, and improving the crystallinity of the ceramic phase and the overall mechanical stability of the component. Reducing the temperature difference between the two processes avoids the introduction of new thermal stress cracks within the component due to sudden temperature changes during crystallization treatment, and allows the amorphous SiC phase generated by pyrolysis to rearrange into a crystalline state at similar temperatures, further eliminating residual thermal stress and improving the crystallinity of the ceramic phase. When both temperatures are the same, the transformation from amorphous to crystalline state can be completed directly at that temperature, avoiding thermal shock damage caused by secondary temperature rises and falls, thereby further reducing the number of microcracks within the component.

[0035] Preferably, in step (7), the relative density of the silicon carbide lattice ceramic is >90%.

[0036] Further preferred, in step (7), the relative density of the silicon carbide lattice ceramic is 92~99%.

[0037] Preferably, in step (7), the average Vickers hardness of the silicon carbide lattice ceramic is ≥19.7 GPa.

[0038] Preferably, in step (7), the difference in Vickers hardness between the upper and lower surfaces of the silicon carbide lattice ceramic in the vertical direction is ≤2.0 GPa.

[0039] The vertical direction refers to the layer-by-layer stacking direction during direct-write 3D printing (i.e., the Z-axis direction).

[0040] Preferably, in step (7), the fracture toughness of the silicon carbide lattice ceramic is ≥3.3 MPa·m. 1 / 2 .

[0041] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention introduces two grades of silicon carbide powder with different particle sizes into the ceramic slurry system and the modified impregnation liquid system, respectively. In the ceramic slurry system, the printing quality is ensured by combining graded particle sizes with direct-write 3D printing: coarse silicon carbide powder acts as a skeleton particle to construct the macroscopic support structure of the lattice porous preform, while fine silicon carbide powder fills the gaps between the coarse particles to optimize particle packing density, control pore size distribution, and improve the strength of the preform. In the modified impregnation liquid system, a silane coupling agent is used to solve the problem of incompatibility between inorganic powder and organic solution, preparing a stable, sedimentation-free impregnation liquid; coarse silicon carbide powder acts as a solid phase filler to increase the amount of solid phase introduced in a single impregnation, accelerating the densification process; fine silicon carbide powder further fills the gaps between the coarse particles, improving the stability and penetration depth of the slurry. During the impregnation process, the solid powder penetrates into the three-dimensional interconnected pores of the preform simultaneously with the precursor liquid. By relying on the solid particles to occupy the pore space, the gravity-driven impregnation stratification phenomenon is greatly reduced, which completely solves the performance gradient defect of the traditional PIP process components being dense at the bottom and loose at the top, thereby improving the impregnation efficiency and the density of the final component.

[0042] 2. This invention utilizes pre-loaded silicon carbide powder within pores as heterogeneous nucleation sites during the pyrolysis stage, improving the conversion efficiency and crystallinity quality of the SiC ceramic phase generated from the pyrolysis of organic precursors. Specifically, coarse powder fills larger pores to form a mechanical framework, while fine powder penetrates micro- and nano-scale gaps to achieve dense filling. Simultaneously, the fine powder provides ample heterogeneous nucleation sites, promoting the epitaxial growth of the SiC ceramic phase generated from the pyrolysis of organic precursors during the pyrolysis stage, with the pre-loaded powder surface as the nucleation center. The weight gain of samples in a single PIP cycle is significantly improved, requiring only 3 to 5 cycles to achieve the high densification target, greatly reducing the number of pyrolysis thermal cycles, minimizing internal microcracks caused by repeated heating and cooling, and simultaneously improving the material's toughness and dynamic impact resistance.

[0043] 3. This invention constructs an integrated matching process system for direct-write printing slurry preparation, lattice molding, graded drying, degreasing and pre-sintering, powder modification and impregnation, segmented curing, and temperature-controlled pyrolysis. All process parameters are mutually compatible, enabling digital customization of silicon carbide lattice preforms with arbitrary topologies and a dedicated short-cycle densification process. It balances the freedom of complex structure forming with the mechanical uniformity of components, meeting the needs of stable batch industrial production. The raw materials of the entire process have broad expansion and adaptability capabilities. The types of organosilicon precursors, organic solvents, and silicon carbide powder particle size ratios can be flexibly adjusted according to the operating conditions of the components. It can also prepare multi-component multiphase silicon carbide ceramics by compounding small amounts of boron-based and aluminum-based precursors in the impregnation solution, adapting to different application scenarios such as neutron shielding and high-temperature oxidation resistance.

[0044] 4. This invention generates a continuous silicon carbide ceramic matrix through powder filling combined with in-situ pyrolysis. The lattice cell walls are free of large-area pore defects, and multiple toughening effects occur during crack propagation, including crack deflection, grain bridging, and powder pull-out. This simultaneously improves the material's hardness, quasi-static compressive strength, high-strain-rate dynamic compressive strength, and fracture toughness, effectively addressing the inherent shortcomings of conventional PIP-prepared silicon carbide ceramics, such as brittleness and weak dynamic load-bearing capacity. The direct-write silicon carbide lattice ceramics obtained using this invention exhibit high overall relative density, small density difference between the upper and lower vertical regions, uniform pore filling, and no delamination or loose zones. The lattice does not experience localized stress concentration failure under stress, and its kinetic energy absorption capacity is significantly improved.

[0045] 5. This invention ensures printing quality through slurry gradation, precisely controls porosity during pre-sintering to reserve space for impregnation, achieves uniform penetration and efficient filling with a solid-liquid composite impregnation solution, reduces thermal damage through short cycle counts, and eliminates residual stress through crystallization treatment. Ultimately, it synergistically improves the overall density, mechanical uniformity, and dynamic and static compressive strength of the component. The entire process significantly reduces the number of high-temperature thermal cycles, substantially reduces the number of microcracks inside the component, exhibits excellent dimensional thermal stability, and can be stably used in high-temperature environments for extended periods without significant degradation of mechanical properties. The manufacturing cycle is shortened, and high-temperature energy consumption and raw material loss decrease simultaneously. It possesses outstanding engineering and economic value in the fields of lightweight individual soldier protective array armor, aerospace porous heat exchange arrays, and high-temperature load-bearing structural components. Attached Figure Description

[0046] Figure 1 This is a schematic diagram of the preparation process of short-cycle PIP dense direct-write molding silicon carbide lattice ceramics according to the present invention.

[0047] Figure 2 The images show SEM images of the silicon carbide lattice ceramic of Embodiment 1 of the present invention at different magnifications.

[0048] Figure 3 This is a SEM image of the two-phase interface in the silicon carbide lattice ceramic of Embodiment 1 of the present invention.

[0049] Figure 4 This is a SEM image of the silicon carbide lattice ceramic after the microcracks at the phase interface were repaired in Example 1 of the present invention. Detailed Implementation

[0050] The technical solution of the present invention will be further described and illustrated below through specific embodiments. It should be understood that the specific embodiments described herein are only for the purpose of helping to understand the present invention and are not intended to limit the present invention.

[0051] Unless otherwise specified, the raw materials used in this invention are all commonly used in the art, and the methods used are all conventional methods in the art.

[0052] In this invention, the raw materials include: First type of silicon carbide coarse powder, α-SiC, median particle size 1.37μm, purity ≥99.0%, type W1.5, purchased from Shandong Jinmeng New Materials; First, silicon carbide fine powder, α-SiC, median particle size 320nm, purity ≥99.0%, purchased from Huzhou Yuanqin New Materials; Second silicon carbide coarse powder, α-SiC, median particle size 1.50μm, purity ≥99.0%, model W1.5, purchased from Shandong Jinmeng New Materials; The second silicon carbide fine powder, α-SiC, with a median particle size of 350nm and a purity of ≥99.0%, was purchased from Huzhou Yuanqin New Materials. Ammonium polycarboxylate, dispersant, industrial grade, model HH-2054, purchased from Guangzhou Houhuan; Polyvinylpyrrolidone, PVP-K30, industrial grade, adhesive, purchased from Henan Pengfei New Materials; Aqueous organic rheology modifier, PA-670, purchased from Zhejiang Fenghong New Materials; Polycarbosilane, model ZR-PCS-100, purchased from Hunan Zerui New Materials; Polysilane, model MY-PMS-01, purchased from Anhui Mingyi Silicon Industry Co., Ltd. Silane coupling agent, KH-550, purchased from Nanjing Nengde New Materials.

[0053] In this invention, the test includes: Porosity: Archimedes drainage method was used; Relative density: Archimedes' displacement method was used; Vickers hardness average: Five tests were conducted under a fixed load of 9.8 N, and the average value was taken. Fracture toughness: The single-sided notched beam method was used; Quasi-static compressive strength: tested using 10mm cube specimens at a strain rate of 0.0025 / s; Dynamic compressive strength: Using a split Hopkinson bar (SHPB), at 1200s -1 Testing under strain rate; Hardness difference: The Vickers hardness of the upper and lower surfaces of the silicon carbide lattice ceramic component was measured separately, and the difference between the two was calculated.

[0054] In this invention, the room temperature is 25°C.

[0055] In this invention, Figure 1 This paper presents a schematic diagram of the process for preparing dense composite materials by combining direct-write 3D printing with precursor impregnation pyrolysis (PIP). A porous silicon carbide lattice preform with honeycomb-like interconnected pores, generated by direct-write printing, is impregnated under vacuum / pressure in an impregnation solution mixed with precursor and ceramic powder. Subsequently, it undergoes curing and high-temperature pyrolysis processes, gradually filling the internal pores through multiple cycles, ultimately yielding a high-density silicon carbide lattice ceramic composite material.

[0056] In this invention, the method for preparing short-period PIP dense direct-write molded silicon carbide lattice ceramics includes the following steps: (1) Mix the first silicon carbide coarse powder, the first silicon carbide fine powder, the additives and water to obtain a ceramic slurry; The median particle size of the first coarse silicon carbide powder is 1~2μm, and the median particle size of the first fine silicon carbide powder is 200~500nm. The mass ratio of the two is 7:3~5:5, and the total amount of both added accounts for 60~70% of the volume fraction of the ceramic slurry. (2) The ceramic slurry was directly written 3D printed to obtain a silicon carbide lattice green body; (3) When the vacuum degree is ≤10 -3 Under Pa, the silicon carbide lattice preform is vacuum pre-sintered, heated to the first stage temperature of 500~700℃ at a heating rate of 1~10℃ / min and held for 60~120min, and then continuously heated to the second stage temperature of 1700~2000℃ and held for 10~40min to obtain a silicon carbide lattice porous preform with a porosity of 35~45vol%. (4) Mix the organosilicon precursor, coarse second silicon carbide powder, fine second silicon carbide powder, surface modifier and organic solvent to obtain a modified impregnation solution; The median particle size of the second coarse silicon carbide powder is 1-2 μm, and the median particle size of the second fine silicon carbide powder is 200-500 nm. The mass ratio of the two is 3:7-5:5, and the total mass of the two is 11-20 wt% of the mass of the modified impregnation solution. The amount of the surface modifier added is 0.1~5 wt% of the mass of the modified impregnation solution; (5) The silicon carbide lattice porous preform is completely immersed in the modified impregnation liquid for vacuum negative pressure impregnation, cured at 180~260℃ and pyrolyzed at 1100~1600℃ to complete one round of PIP cycle; (6) Repeat step (5) 2 to 4 times until the weight gain after a single PIP cycle is less than 0.8 wt%, and obtain the intermediate; (7) Under an inert atmosphere, the intermediate is crystallized and polished at 1100~1600℃ to obtain silicon carbide lattice ceramic with a relative density of >92%.

[0057] Example 1 (1) 100 parts of coarse silicon carbide powder with a median particle size of 1.37 μm and fine silicon carbide powder with a median particle size of 320 nm, with a mass ratio of 7:3, were added to a 5L mixing tank. Then, 1 part of ammonium polycarboxylate dispersant (1 wt%), 0.5 parts of PVP-K30 binder (0.5 wt%), 0.15 parts of aqueous rheology modifier (0.15 wt%), and the remainder deionized water were added. The mixture was stirred at 350 r / min for 4 h at room temperature. The mixture was then transferred to an ultrasonic disperser and continuously ultrasonicated at 300 W and 20 kHz for 6 h, with a 10 min settling time every 2 h. The mixture was then transferred to a vacuum degassing tank and degassed under vacuum at -0.09 MPa for 2 h to obtain a ceramic slurry with a silicon carbide volume fraction of 65 vol%. The ceramic slurry showed no stratification or sedimentation after standing for 24 h. Its rheological curve exhibited standard shear thinning characteristics and a zero shear modulus of 12800 Pa, which met the requirements for direct-write extrusion molding.

[0058] (2) A regular hexagonal unit cell lattice model was constructed using SolidWorks, with a unit cell side length of 5mm and a target size of 100mm×100mm×20mm. The printing path code was generated using the slicing software Simplify3D. A direct-write 3D printer was used, with a nozzle outlet diameter of 1.2mm, a constant extrusion pressure of 0.7MPa, a printing speed of 20mm / s, a layer height of 1.0mm, and a constant printing platform temperature of 25℃. Layers were stacked one by one to obtain a silicon carbide lattice blank. After printing, the blank was left to stand in a dust-free room temperature environment for 24 hours to allow natural dehumidification. Then, it was transferred to a small hot air device and pre-dried with 50℃ constant temperature hot air for 30 minutes to slowly remove surface free moisture. After drying, the blank had no warping or surface crack defects.

[0059] (3) The obtained silicon carbide lattice blank is placed in a vacuum sintering furnace with a vacuum degree of 1×10⁻⁶. -3Pa was heated to the first stage temperature of 650℃ at a heating rate of 5℃ / min and held for 90 min. Then, the temperature was continuously increased to the second stage temperature of 1800℃ at a heating rate of 5℃ / min and held for 20 min. The furnace was then allowed to cool naturally to room temperature to obtain the preform. The preform had a porosity of 41 vol%. The lattice structure of the preform was intact without breakage or collapse, and all the pores were interconnected.

[0060] (4) A precursor solution with a solid content of 25 wt% was prepared by adding a polycarbosilane precursor to xylene. 16 parts of coarse silicon carbide powder with a median particle size of 1.5 μm and fine silicon carbide powder with a median particle size of 350 nm, and 0.5 parts of silane coupling agent were added to 100 parts of the precursor solution. The mixture was mechanically stirred at 400 r / min for 5 h, and simultaneously subjected to ultrasonic vibration at 250 W for 3 h to obtain the modified impregnation solution. After standing for 72 h, the bottom sediment thickness of the modified impregnation solution was less than 0.5 mm, indicating excellent suspension stability.

[0061] (5) The preform from step (3) is completely immersed in the modified impregnation solution from step (4), placed in a sealed vacuum impregnation tank, and evacuated until the pressure inside the tank is 0.8 kPa. It is then impregnated at a constant temperature of 50°C for 2 hours. After impregnation, it is removed and excess impregnation solution is drained off under normal temperature and ventilation conditions. Then it is transferred to a forced-air constant temperature oven and kept at 220°C for 6 hours to allow the precursor to crosslink and solidify. Subsequently, it is transferred to a vacuum carbon tube furnace and continuously purged with high-purity argon gas for protection. The temperature is increased to 1600°C at a rate of 4°C / min and held for 1 hour for pyrolysis. After pyrolysis, it is cooled to room temperature with the furnace and the weight gain is measured.

[0062] (6) The impregnation-curing-pyrolysis process in step (5) is counted as one PIP cycle. The PIP cycle is repeated. After the fourth pyrolysis cycle, the weight gain per cycle is only 0.67wt%, which is lower than the termination threshold of 0.8wt%. The densification process is stopped to obtain the intermediate.

[0063] (7) The intermediate that has completed 4 PIP cycles is placed in a high-temperature tube furnace and crystallized at 1600℃ for 1 hour under argon protection to eliminate the amorphous phase and residual thermal stress generated by cracking. After cooling, the loose areas on the upper and lower surfaces of the component are polished layer by layer with an 800-mesh diamond grinding wheel, then ultrasonically cleaned with deionized water for 30 minutes, and finally dried at 120℃ to obtain silicon carbide lattice ceramic.

[0064] The silicon carbide lattice ceramic of this embodiment was tested and found to have a relative density of 95.2%, an average Vickers hardness of 22.6 GPa, and a fracture toughness of 4.1 MPa·m. 1 / 2 The quasi-static compressive strength is 476 MPa; the dynamic compressive strength is 853 MPa; and the hardness difference between the upper and lower surfaces is 0.9 GPa.

[0065] Figure 2 The SiC framework substrate prepared by direct-write 3D printing exhibits a continuous three-dimensional network structure. After PIP densification, the large-size macroscopic through-holes and micron-sized micropores inside the original preform were filled and effectively filled with high density. Figure 3 The microscopic interface bonding is demonstrated. A clear, continuous and tightly bonded phase interface is formed between the coarse SiC skeleton matrix formed by direct-write 3D printing and the SiC gap-filling phase generated by subsequent PIP impregnation and pyrolysis, with no obvious debonding cracks or pore defects at the interface. Figure 4 Further evidence confirms that the modified impregnation solution and its pyrolysis products possess excellent penetration capabilities, reaching deep into the minute gaps and pits of the matrix. This process enables in-situ "gap repair" and bridging of microcracks and defects generated during direct-write printing and pre-sintering.

[0066] Example 2 (1) 100 parts of coarse silicon carbide powder with a median particle size of 1.37 μm and fine silicon carbide powder with a median particle size of 320 nm in a mass ratio of 7:3 were added to a 5L mixing tank. Then, 1 part of ammonium polycarboxylate dispersant (1 wt%), 0.5 parts of PVP-K30 binder (0.5 wt%), 0.15 parts of water-based rheology modifier (0.15 wt%) and the remainder of deionized water were added. The mixture was stirred at 350 r / min for 4 h at room temperature. The mixture was then transferred to an ultrasonic disperser and continuously ultrasonicated at 300 W and 20 kHz for 6 h, with the machine stopped every 2 h and allowed to stand for 10 min. The mixture was then transferred to a vacuum degassing tank and degassed under vacuum at -0.09 MPa for 2 h to obtain a ceramic slurry with a silicon carbide volume fraction of 63 vol%.

[0067] (2) A regular hexagonal unit cell lattice model was constructed using SolidWorks, with a unit cell side length of 5mm and a target size of 100mm×100mm×20mm. The printing path code was generated using the slicing software Simplify3D. A direct-write 3D printer was used with a nozzle size of 1.2mm, a constant extrusion pressure of 0.7MPa, a printing speed of 20mm / s, a layer height of 1.0mm, and a constant printing platform temperature of 25℃. Layers were stacked one by one to obtain a silicon carbide lattice blank. After printing, the blank was left to stand in a dust-free room temperature environment for 24 hours to allow natural dehumidification. Then, it was transferred to a small hot air device and pre-dried with 50℃ constant temperature hot air for 30 minutes to slowly remove surface free moisture. After drying, the blank had no warping or surface crack defects.

[0068] (3) The obtained silicon carbide lattice blank is placed in a vacuum sintering furnace with a vacuum degree of 1×10⁻⁶. -3Pa was heated to the first stage temperature of 650℃ at a heating rate of 5℃ / min and held for 90min. Then, the temperature was continuously increased to the second stage temperature of 1800℃ at a heating rate of 5℃ / min and held for 20min. The furnace was then allowed to cool naturally to room temperature to obtain a preform with a porosity of 43.6 vol%.

[0069] (4) Add the polysilane precursor to n-hexane to prepare a precursor solution with a precursor solid content of 23wt%. Add 13 parts of coarse second silicon carbide powder with a median particle size of 1.5μm and fine second silicon carbide powder with a mass ratio of 3:7 and 0.4 parts of silane coupling agent to 100 parts of the precursor solution. Stir mechanically at 400r / min for 5h and simultaneously apply ultrasonic vibration of 250W for 3h to obtain the modified impregnation solution.

[0070] (5) The preform from step (3) is completely immersed in the modified impregnation solution from step (4), placed in a sealed vacuum impregnation tank, and evacuated until the pressure inside the tank is 0.8 kPa. It is then impregnated at a constant temperature of 50°C for 2 hours. After impregnation, it is removed and excess impregnation solution is drained off under normal temperature and ventilation conditions. Then it is transferred to a forced-air constant temperature oven and kept at 220°C for 6 hours to allow the precursor to crosslink and solidify. Subsequently, it is transferred to a vacuum carbon tube furnace and continuously purged with high-purity argon gas for protection. The temperature is increased to 1600°C at a rate of 4°C / min and held for 1 hour for pyrolysis. After pyrolysis, it is cooled to room temperature with the furnace and the weight gain is measured.

[0071] (6) The impregnation-curing-pyrolysis process in step (5) is counted as one PIP cycle. The PIP cycle is repeated. After the third pyrolysis cycle, the weight gain per cycle is only 0.75wt%, which is lower than the termination threshold of 0.8wt%. The densification process is stopped to obtain the intermediate.

[0072] (7) The intermediate that has completed 3 PIP cycles is placed in a high-temperature tube furnace and crystallized at 1600℃ for 1 hour under argon protection to eliminate the amorphous phase and residual thermal stress generated by cracking. After cooling, the loose areas on the upper and lower surfaces of the component are polished layer by layer with an 800-mesh diamond grinding wheel, then ultrasonically cleaned with deionized water for 30 minutes, and finally dried at 120℃ to obtain silicon carbide lattice ceramic.

[0073] The silicon carbide lattice ceramic of this embodiment was tested and found to have a relative density of 93.8%, an average Vickers hardness of 21.7 GPa, and a fracture toughness of 3.8 MPa·m. 1 / 2 The quasi-static compressive strength is 421 MPa; the dynamic compressive strength is 791 MPa; and the hardness difference between the upper and lower surfaces is 1.1 GPa.

[0074] Example 3 Compared with Example 1, the difference is that in step (4), the polycarbosilane precursor is added to xylene to prepare a precursor solution with a precursor solid content of 25wt%. 16 parts of coarse second silicon carbide powder with a median particle size of 1.5μm and fine second silicon carbide powder with a median particle size of 350nm, and 0.5 parts of silane coupling agent are added to 100 parts of the precursor solution. The mixture is mechanically stirred at 400r / min for 5h and simultaneously subjected to ultrasonic vibration at 250W for 3h to obtain the modified impregnation solution.

[0075] The silicon carbide lattice ceramic of this embodiment was tested and found to have a relative density of 92.1%; an average Vickers hardness of 19.7 GPa; and a fracture toughness of 3.3 MPa·m. 1 / 2 The quasi-static compressive strength is 375 MPa; the dynamic compressive strength is 712 MPa; and the hardness difference between the upper and lower surfaces is 2.0 GPa.

[0076] In this embodiment, a density gradient appeared along the thickness direction of the silicon carbide lattice ceramic, resulting in a certain decrease in mechanical properties. This is because: in this embodiment, the ratio of coarse to fine powder in the modified impregnation solution was adjusted to 1:1, reducing the content of fine filler. This resulted in the inability to fully fill the micro-gaps in the pores, increasing the vertical gravity differentiation during impregnation, and widening the gradient difference between the hardness and density of the silicon carbide lattice ceramic component along the thickness direction. Simultaneously, the number of heterogeneous nucleation sites decreased during the pyrolysis stage, leading to a decrease in SiC generation per cycle, making it difficult to effectively improve the overall density after four cycles. Furthermore, the number of residual micro-closed pores and gaps inside the component increased, weakening the toughening effects such as crack deflection and powder pull-out, resulting in a simultaneous decrease in hardness, fracture toughness, and static / dynamic compressive strength.

[0077] Example 4 The process was carried out in accordance with Example 3, except that in step (4), the polycarbosilane precursor was added to xylene to prepare a precursor solution with a precursor solid content of 25 wt%. 16 parts of coarse silicon carbide powder with a median particle size of 1.37 μm and fine silicon carbide powder with a median particle size of 320 nm, and 0.5 parts of silane coupling agent were added to 100 parts of the precursor solution. The mixture was mechanically stirred at 400 r / min for 5 h and simultaneously subjected to ultrasonic vibration at 250 W for 3 h to obtain the modified impregnation solution.

[0078] The silicon carbide lattice ceramic of this embodiment was tested and found to have a relative density of 92.5%, an average Vickers hardness of 19.9 GPa, and a fracture toughness of 3.4 MPa·m. 1 / 2 The quasi-static compressive strength is 381 MPa; the dynamic compressive strength is 720 MPa; and the hardness difference between the upper and lower surfaces is 1.9 GPa.

[0079] Compared to Example 3, the silicon carbide lattice ceramic in this example exhibits slightly better density and stratification. This is because this example only reduces the particle size of both coarse and fine powders in the impregnation solution. The simultaneous reduction in particle size of both powders results in smaller particle sizes, making it easier for them to penetrate the micron-sized narrow channels inside the preform, weakening the gravity wetting and stratification effect, and slightly reducing the hardness difference between the upper and lower parts of the component. Simultaneously, the finer powder provides more heterogeneous nucleation sites for pyrolysis, which is beneficial for improving ceramic production efficiency. Furthermore, as the particle size decreases, the specific surface area of ​​the silicon carbide powder increases, which adsorbs some organosilicon precursors, reducing the content of effective precursors that can be pyrolyzed to generate silicon carbide within the system. This slightly offsets the filling gain brought about by the reduction in particle size, resulting in a slightly lower-than-expected weight gain per cycle.

[0080] Comparative Example 1 Compared with Example 1, the difference is that in step (4), the polycarbosilane precursor is added to xylene to prepare a precursor solution with a precursor solid content of 25wt% as a modified impregnation solution.

[0081] Using the modified impregnation solution of this comparative example, nine consecutive PIP cycles are required to meet the requirement that the weight gain per cycle is less than 0.8 wt%.

[0082] The silicon carbide lattice ceramic obtained in this comparative example was tested and found to have a relative density of 94.7%, an average Vickers hardness of 18.3 GPa, and a fracture toughness of 2.4 MPa·m. 1 / 2 The quasi-static compressive strength is 294 MPa; the dynamic compressive strength is 567 MPa; the bottom hardness is 21.5 GPa, the top hardness is 17.3 GPa, and the hardness difference between the upper and lower surfaces is 4.2 GPa.

[0083] The silicon carbide lattice ceramics in this comparative example exhibit significant dense layering defects and a noticeable number of internal microcracks.

[0084] Comparative Example 2 Compared with Example 1, the difference is that in step (4), the polycarbosilane precursor is added to xylene to prepare a precursor solution with a precursor solid content of 25wt%. 16 parts of coarse second silicon carbide powder with a median particle size of 1.5μm and fine second silicon carbide powder with a mass ratio of 3:7 are added to 100 parts of the precursor solution. The mixture is mechanically stirred at 400r / min for 5h and simultaneously subjected to ultrasonic vibration at 250W for 3h to obtain the modified impregnation solution.

[0085] The modified impregnation solution of this comparative example, without the addition of silane coupling agent, had a bottom sediment thickness of about 2.8 mm after standing for 72 hours, with severe powder agglomeration and sedimentation, and extremely poor suspension stability.

[0086] The silicon carbide lattice ceramic obtained in this comparative example was tested and found to have a relative density of 90.3%, an average Vickers hardness of 17.6 GPa, and a fracture toughness of 2.2 MPa·m. 1 / 2 The quasi-static compressive strength is 278 MPa; the dynamic compressive strength is 542 MPa; and the hardness difference between the upper and lower surfaces is 3.9 GPa.

[0087] The silicon carbide lattice ceramics in this comparative example exhibit significant density and delamination defects. This is due to several factors: poor compatibility between inorganic silicon carbide powder and organosilicon precursors; the powder's tendency to agglomerate and settle without silane coupling agent modification; decreased impregnation solution stability; excessive powder deposition during vacuum impregnation; reduced solid-phase filling; and a widening of the density and hardness gradient difference. Furthermore, the lack of coupling agent bridging results in weak interfacial bonding between the powder and matrix, leading to numerous gaps and debonding defects, failure of the toughening mechanism, and decreased fracture toughness. In addition, insufficient effective powder leads to a scarcity of heterogeneous nucleation sites, resulting in low ceramic yield per cycle. After four PIP cycles, density is difficult to improve, and the overall mechanical properties are even inferior to those of the pure precursor process.

[0088] Comparative Example 3 Compared with Example 1, the difference is that in step (4), the polycarbosilane precursor is added to xylene to prepare a precursor solution with a precursor solid content of 25wt%. 16 parts of coarse second silicon carbide powder with a median particle size of 1.37μm and fine second silicon carbide powder with a median particle size of 320nm, and 0.5 parts of silane coupling agent are added to 100 parts of the precursor solution. The mixture is mechanically stirred at 400r / min for 5h and simultaneously subjected to ultrasonic vibration at 250W for 3h to obtain the modified impregnation solution.

[0089] The silicon carbide lattice ceramic obtained in this comparative example was tested and found to have a relative density of 91.1%, an average Vickers hardness of 18.1 GPa, and a fracture toughness of 2.5 MPa·m. 1 / 2 The quasi-static compressive strength is 306 MPa; the dynamic compressive strength is 575 MPa; and the hardness difference between the upper and lower surfaces is 3.5 GPa.

[0090] In this comparative example, the median particle size and mass ratio of the coarse and fine silicon carbide powders added to the modified impregnation solution were consistent with those in the ceramic slurry. After four rounds of PIP cycles, the resulting silicon carbide lattice ceramic exhibited significant thickness-dense layering defects, and the component contained a large number of large-sized residual pores. Compared to Example 4, this comparative example further increased the amount of coarse silicon carbide powder added, resulting in further deterioration of the component's performance. The reasons are as follows: the modified impregnation solution contains an excessively high proportion of coarse powder and insufficient fine powder. Coarse particles have a small specific surface area and a fast settling rate, making them prone to deposition towards the bottom of the component under gravity during vacuum impregnation. This results in a lack of solid-phase particle filling in the top region, exacerbating vertical wetting segregation and density gradients. Simultaneously, the reduced fine powder content decreases the ability of the modified impregnation solution to penetrate narrow micro-nano pores. The lack of sufficient fine powder inside the pores serves as heterogeneous nucleation sites, leading to a decrease in the ceramic production efficiency of a single PIP cycle. After four cycles, a large number of unfilled, large-sized interconnected pores remain inside the component. Furthermore, excessive coarse powder easily forms localized particle accumulation and interface defects within the pores. The lack of secondary micro-filling of the gaps between coarse particles by fine powder prevents effective triggering of toughening mechanisms such as crack deflection and particle pull-out under stress, resulting in a significant deterioration in the component's hardness, fracture toughness, and dynamic and static compressive strength. Further reducing the particle size of the second silicon carbide coarse powder and the second silicon carbide fine powder increases the number of PIP cycles.

[0091] Comparative Example 4 Compared with Example 1, the difference is that in step (4), the polycarbosilane precursor is added to xylene to prepare a precursor solution with a precursor solid content of 25wt%. 16 parts of 350nm second silicon carbide fine powder and 0.5 parts of silane coupling agent are added to 100 parts of the precursor solution, and the mixture is mechanically stirred at 400r / min for 5h, while simultaneously subjected to ultrasonic vibration at 250W for 3h to obtain the modified impregnation solution.

[0092] The silicon carbide lattice ceramic obtained in this comparative example was tested and found to have a relative density of 91.6%, an average Vickers hardness of 18.6 GPa, and a fracture toughness of 2.7 MPa·m. 1 / 2 The quasi-static compressive strength is 322 MPa; the dynamic compressive strength is 614 MPa; and the hardness difference between the upper and lower surfaces is 3.1 GPa.

[0093] In this comparative example, the absence of coarse second silicon carbide powder in the modified impregnation solution resulted in localized powder enrichment and uneven pore filling within the component. This is because, while fine second silicon carbide powder can penetrate micropores, it lacks the skeletal support and volume-filling effect of coarse particles for the large-sized interconnected channels of the preform, leading to insufficient total solid phase introduction in a single impregnation. The use of fine powder alone drastically increases the specific surface area and viscosity of the modified impregnation solution, increasing penetration resistance. Fine powder easily accumulates and agglomerates in the lower pores of the preform, clogging the flow channels and hindering the continued transport of the impregnation solution to the upper part of the component. This exacerbates the gravity wetting stratification effect, resulting in a large number of unfilled pores remaining in the upper part of the component and a significant increase in the hardness difference between the upper and lower parts. Furthermore, the lack of a microscopic composite skeleton constructed from coarse particles means that after pyrolysis, the matrix lacks particle bridging and microscopic interlocking carriers, weakening the toughening effect and severely limiting fracture toughness and dynamic and static compressive strength.

[0094] Comparative Example 5 Compared with Example 1, the difference is that in step (4), the polycarbosilane precursor is added to xylene to prepare a precursor solution with a precursor solid content of 25wt%. 16 parts of second silicon carbide coarse powder with a median particle size of 1.5μm and 0.5 parts of silane coupling agent are added to 100 parts of the precursor solution, and the mixture is mechanically stirred at 400r / min for 5h, while simultaneously subjected to ultrasonic vibration at 250W for 3h to obtain the modified impregnation solution.

[0095] The silicon carbide lattice ceramic obtained in this comparative example was tested and found to have a relative density of 91.8%, an average Vickers hardness of 18.8 GPa, and a fracture toughness of 2.9 MPa·m. 1 / 2 The quasi-static compressive strength is 346 MPa; the dynamic compressive strength is 643 MPa; and the hardness difference between the upper and lower surfaces is 2.6 GPa.

[0096] In this comparative example, the modified impregnation solution lacked the second silicon carbide fine powder, resulting in the solid filler's inability to effectively fill the gaps between coarse particles and the narrow micro-nano-scale pores inside the preform. This is because the absence of fine powder reduces the suspension stability of the impregnation solution, causing coarse particles to settle rapidly under gravity and accumulate at the bottom of the component, severely exacerbating vertical wetting segregation and significantly widening the density and hardness gradient difference between the upper and lower surfaces of the component. Simultaneously, the lack of numerous heterogeneous nucleation sites provided by the fine powder reduces the SiC ceramic formation efficiency during the pyrolysis stage, resulting in insufficient weight gain per PIP cycle. After four PIP cycles, many unfilled gaps and closed pores remain inside, ultimately limiting the relative density of the component. Furthermore, the lack of fine particles within the matrix leads to multiple toughening effects such as particle bridging and microcrystalline interlocking, resulting in a significant decrease in fracture toughness and dynamic / static compressive strength. Even increasing the number of cycles cannot improve the density.

[0097] Comparative Example 6 Compared with Example 1, the difference is that in step (7), the intermediate that has completed 4 PIP cycles is placed in a high-temperature tube furnace and crystallized at 1200°C for 1 hour under argon protection to eliminate the amorphous phase and residual thermal stress generated by cracking. After cooling, the loose areas on the upper and lower surfaces of the component are polished layer by layer with an 800-mesh diamond grinding wheel, then ultrasonically cleaned with deionized water for 30 minutes, and finally dried at 120°C to obtain silicon carbide lattice ceramic.

[0098] The silicon carbide lattice ceramic obtained in this comparative example was tested and found to have a relative density of 94.5%, an average Vickers hardness of 17.6 GPa, and a fracture toughness of 3.0 MPa·m. 1 / 2 The quasi-static compressive strength is 392 MPa; the dynamic compressive strength is 708 MPa; and the hardness difference between the upper and lower surfaces is 1.1 GPa.

[0099] In this comparative example, the density uniformity of the component did not deteriorate significantly compared to Example 1, but a large amount of amorphous silicon carbide phase and thermal residual stress remained inside. This is because a large amount of amorphous silicon carbide is generated during the pyrolysis stage (1600℃), while the crystallization temperature is significantly lower than the pyrolysis temperature. The insufficient thermal activation energy cannot fully drive the amorphous silicon carbide to complete its crystal transformation, resulting in a high content of amorphous phase inside the component. The hardness and load-bearing capacity of amorphous silicon carbide are far lower than those of crystalline silicon carbide, directly weakening the overall hardness and compressive strength. Furthermore, the four pyrolysis cycles during the four PIP cycles accumulated significant thermal residual stress within the lattice framework, and the low-temperature crystallization treatment was insufficient to effectively release this stress. Under load, microcracks easily initiate and propagate rapidly at stress concentration points, significantly weakening fracture toughness and dynamic impact resistance.

[0100] Comparative Example 7 Compared with Example 1, the difference is that in step (4), the polycarbosilane precursor is added to xylene to prepare a precursor solution with a precursor solid content of 25wt%. 10 parts of coarse second silicon carbide powder with a median particle size of 1.5μm and fine second silicon carbide powder with a mass ratio of 3:7, and 0.5 parts of silane coupling agent are added to 100 parts of the precursor solution. The mixture is mechanically stirred at 400r / min for 5h and simultaneously subjected to ultrasonic vibration at 250W for 3h to obtain the modified impregnation solution.

[0101] The silicon carbide lattice ceramic obtained in this comparative example was tested and found to have a relative density of 92.3%, an average Vickers hardness of 19.1 GPa, and a fracture toughness of 3.1 MPa·m. 1 / 2 The quasi-static compressive strength is 370 MPa; the dynamic compressive strength is 689 MPa; and the hardness difference between the upper and lower surfaces is 2.3 GPa.

[0102] In this comparative example, the total solid content of silicon carbide powder in the modified impregnation solution was reduced to 10 wt%, resulting in a lower overall density of the component and obvious dense delamination defects along the thickness direction. The reason is that the total concentration of solid powder in the impregnation solution is too low, and the total amount of solid particles that simultaneously penetrate into the pores of the preform with the precursor solution is insufficient. This makes it difficult to effectively prevent the sedimentation and segregation of the precursor solution under gravity, and the vertical wetting gradient is intensified. As a result, the pores at the bottom of the component are filled more fully, while a large number of unfilled pores remain at the top, and the hardness difference between the top and bottom is widened. At the same time, the amount of silicon carbide powder preloaded in the pores is reduced, which weakens the heterogeneous nucleation effect and the single-cycle ceramic production efficiency. The single-cycle increment is significantly reduced, and deep densification cannot be achieved after the same 4 cycles of PIP. The residual pores inside cause the fracture toughness and dynamic and static load-bearing capacity to decrease simultaneously.

[0103] Comparative Example 8 Compared with Example 1, the difference is that in step (7), the intermediate body that has completed 4 rounds of PIP cycle is polished layer by layer with an 800-mesh diamond grinding wheel to remove the loose areas on the upper and lower surfaces of the component, then ultrasonically cleaned with deionized water for 30 minutes, and finally dried at 120°C to obtain silicon carbide lattice ceramic.

[0104] The silicon carbide lattice ceramic obtained in this comparative example was tested and found to have a relative density of 94.9%, an average Vickers hardness of 18.2 GPa, and a fracture toughness of 2.6 MPa·m. 1 / 2 The quasi-static compressive strength is 315 MPa; the dynamic compressive strength is 596 MPa; and the hardness difference between the upper and lower surfaces is 1.0 GPa.

[0105] In this comparative example, the absence of crystallization treatment resulted in a significant decrease in hardness, fracture toughness, and dynamic and static compressive strength of the component while maintaining high density. This is because omitting the crystallization step leaves the amorphous SiC phase generated by cracking directly within the component matrix. The amorphous phase has poor intrinsic hardness and resistance to deformation, reducing overall hardness and quasi-static compressive strength. More importantly, without high-temperature crystallization annealing, the enormous residual thermal stress accumulated within the skeleton and filling matrix after four rounds of PIP thermal cycles cannot be released. Under stress, this easily induces the initiation and unimpeded propagation of microcracks, significantly weakening toughening mechanisms such as grain bridging and crack deflection, leading to a substantial decrease in fracture toughness and dynamic impact resistance.

[0106] Comparative Example 9 Compared with Example 1, the difference is that in step (3), the silicon carbide lattice blank is placed in a vacuum sintering furnace with a vacuum degree of 1×10⁻⁶. -3 Pa is heated to 1800℃ at a heating rate of 5℃ / min and held for 20min; then naturally cooled to room temperature in the furnace to obtain the preform.

[0107] The silicon carbide lattice ceramic obtained in this comparative example was tested and found to have a relative density of 91.3%, an average Vickers hardness of 18.4 GPa, and a fracture toughness of 2.8 MPa·m. 1 / 2 The quasi-static compressive strength is 331 MPa; the dynamic compressive strength is 627 MPa; and the hardness difference between the upper and lower surfaces is 2.8 GPa.

[0108] In this comparative example, the pre-sintering process skipped the first stage of low-temperature insulation and directly increased the temperature to 1800℃, leading to an increase in preform quality defects and a significant deterioration in the subsequent PIP densification effect and overall mechanical properties. The reason is that the organic additives inside the printed preform, lacking the slow decomposition and degassing at low temperatures, rapidly decomposed and concentratedly generated gas at high temperatures, causing blistering, microcracks, and pore structure distortion within the preform. Some micropores were cracked, closed, or blocked by residual carbon. The primary micro-damage and pore blockage hindered the uniform penetration of the subsequent modified impregnation liquid, exacerbating the gravity differentiation effect of impregnation and widening the hardness difference between the upper and lower surfaces of the component. Simultaneously, the defects hindered the effective filling of the solid powder, resulting in low density after four PIP cycles. Furthermore, the primary microcracks in the preform became stress concentration sources, leading to a significant deterioration in fracture toughness and dynamic and static mechanical properties.

[0109] Comparative Example 10 Compared with Example 1, the difference is that in step (1), 100 parts of first silicon carbide coarse powder with a median particle size of 1.37 μm were added to a 5L mixing tank, and then 1 part of polycarboxylate ammonium dispersant (1 wt%), 0.5 parts of PVP-K30 binder (0.5 wt%), 0.15 parts of water-based rheology modifier (0.15 wt%) and the remainder of deionized water were added. The mixture was stirred at 350 r / min for 4 h at room temperature. It was then transferred to an ultrasonic disperser and continuously ultrasonicated at 300 W and 20 kHz for 6 h, with a stop and standing for 10 min every 2 h. It was then transferred to a vacuum degassing tank and degassed under vacuum at -0.09 MPa for 2 h to obtain a ceramic slurry with a silicon carbide volume fraction of 65 vol%.

[0110] The silicon carbide lattice ceramic obtained in this comparative example was tested and found to have a relative density of 91.5%, an average Vickers hardness of 18.2 GPa, and a fracture toughness of 2.8 MPa·m. 1 / 2 The quasi-static compressive strength is 335 MPa; the dynamic compressive strength is 620 MPa; and the hardness difference between the upper and lower surfaces is 2.9 GPa.

[0111] In this comparative example, the ceramic slurry system only used coarse silicon carbide powder, resulting in poor quality of the printed preform skeleton structure. After four PIP cycles, the density and overall mechanical properties of the component were limited. The reason is that the lack of fine powder in the slurry to fill the gaps between coarse particles led to a significant reduction in the particle packing density of the printed preform. After pre-sintering, the pore size inside the preform skeleton was larger and the uniformity of its distribution was worse, resulting in lower intrinsic strength of the skeleton. In the subsequent PIP impregnation stage, although the large pore size facilitated solution entry, the lack of fine powder to regulate suspension stability made it easier for solid particles in the impregnation solution to settle under gravity in the large pores and accumulate at the bottom of the component, thus expanding the density gradient in the thickness direction.

[0112] Comparative Example 11 Compared with Example 1, the difference is that in step (1), 100 parts of the first silicon carbide fine powder with a median particle size of 320 nm were added to a 5L mixing tank, and then 1 part of polycarboxylate ammonium dispersant (1 wt%), 0.5 parts of PVP-K30 binder (0.5 wt%), 0.15 parts of water-based rheology modifier (0.15 wt%) and the remainder of deionized water were added. The mixture was stirred at 350 r / min for 4 h at room temperature. It was then transferred to an ultrasonic disperser and continuously ultrasonicated at 300 W and 20 kHz for 6 h, with a stop and standing for 10 min every 2 h. It was then transferred to a vacuum degassing tank and degassed under vacuum at -0.09 MPa for 2 h to obtain a ceramic slurry with a silicon carbide volume fraction of 65 vol%.

[0113] The silicon carbide lattice ceramic obtained in this comparative example was tested and found to have a relative density of 89.2%, an average Vickers hardness of 16.5 GPa, and a fracture toughness of 2.1 MPa·m. 1 / 2 The quasi-static compressive strength is 252 MPa; the dynamic compressive strength is 495 MPa; and the hardness difference between the upper and lower surfaces is 3.8 GPa.

[0114] In this comparative example, the ceramic slurry system used only first-stage silicon carbide fine powder, resulting in severe sintering defects and dense delamination in the component, leading to a significant decrease in various mechanical properties. The reasons are as follows: the excessively large specific surface area of ​​the fine powder caused a dramatic increase in the viscosity of the ceramic slurry, reducing the smoothness and forming accuracy of direct-write printing extrusion, and making the green body prone to interlayer bonding defects; during the high-temperature pre-sintering process, the excessively high fine powder content triggered severe linear shrinkage during sintering, resulting in numerous sintering microcracks, localized distortion, and even localized closed pores within the lattice framework; the inherent defects in the preform framework hindered the deep penetration of subsequent modified impregnation liquid, and the extremely discrete distribution of residual interconnected channels exacerbated gravity segregation during PIP impregnation, further widening the hardness difference between the upper and lower parts; the severe inherent microcracks and high porosity within the framework acted as failure sources, causing a decrease in the component's relative density, hardness, fracture toughness, and dynamic and static compressive strength.

[0115] In summary, this invention introduces coarse and fine silicon carbide powders into ceramic slurry and modified impregnation liquid respectively, and modifies them with silane coupling agents to prepare a stable, non-settling impregnation liquid. Through powder filling combined with in-situ pyrolysis, and 3-5 short-cycle PIP, high densification of silicon carbide lattice preforms based on direct-write 3D printing is achieved. Crystallization treatment is then used to eliminate residual stress. Among these features, the coarse and fine powder gradation synergistically suppresses gravity segregation by solid particles, completely solving the defect of dense layering between the upper and lower parts of the component. The preloaded powder acts as a heterogeneous nucleation site to improve pyrolysis conversion efficiency, significantly shortening the preparation cycle and reducing thermal damage. Multiple toughening effects simultaneously improve hardness, fracture toughness, and dynamic impact resistance. The overall process is adaptable to digital customization of complex structures, and has both high mechanical uniformity and feasibility for industrial-scale mass production.

[0116] All aspects, embodiments, and features of this invention should be considered illustrative in all respects and not limiting of the invention; the scope of the invention is defined only by the claims. Other embodiments, modifications, and uses will become apparent to those skilled in the art without departing from the spirit and scope of the invention as claimed.

[0117] In the preparation method of this invention, the order of the steps is not limited to the listed order. For those skilled in the art, variations in the order of the steps without creative effort are also within the scope of protection of this invention. Furthermore, two or more steps or actions can be performed simultaneously.

[0118] Finally, it should be noted that the specific embodiments described herein are merely illustrative examples of the invention and are not intended to limit the implementation of the invention. Those skilled in the art can make various modifications or additions to the described specific embodiments or use similar methods to replace them; it is neither necessary nor possible to exemplify all embodiments here. However, these obvious variations or modifications derived from the essential spirit of the invention still fall within the scope of protection of the invention, and interpreting them as any additional limitation would contradict the spirit of the invention.

Claims

1. A method for preparing short-cycle PIP dense direct-write molded silicon carbide lattice ceramics, characterized in that, Includes the following steps: (1) Mix the first silicon carbide coarse powder, the first silicon carbide fine powder, the additives and water to obtain a ceramic slurry; (2) Obtain a silicon carbide lattice green body by direct writing 3D printing of the ceramic slurry; (3) The silicon carbide lattice blank is vacuum pre-sintered to obtain a silicon carbide lattice porous preform; (4) Mix the organosilicon precursor, coarse second silicon carbide powder, fine second silicon carbide powder, surface modifier and organic solvent to obtain a modified impregnation solution; (5) The silicon carbide lattice porous preform is vacuum impregnated in the modified impregnation liquid, and then cured and pyrolyzed to complete one PIP cycle. (6) Repeat step (5) 2 to 4 times until the weight gain after a single PIP cycle is less than 0.6 to 0.8 wt%, and obtain the intermediate; (7) Under an inert atmosphere, the intermediate is crystallized to obtain silicon carbide lattice ceramic; In step (1), the median particle size of the first coarse silicon carbide powder is 1~2μm, the median particle size of the first fine silicon carbide powder is 200~500nm, and the amount of the first coarse silicon carbide powder added is ≥ the amount of the first fine silicon carbide powder added. In step (4), the median particle size of the second coarse silicon carbide powder is 1~2μm, the median particle size of the second fine silicon carbide powder is 200~500nm, and the amount of the second coarse silicon carbide powder added is ≤ the amount of the second fine silicon carbide powder added.

2. The method for preparing short-period PIP dense direct-write molded silicon carbide lattice ceramics according to claim 1, characterized in that, In step (1), the total amount of the first coarse silicon carbide powder and the first fine silicon carbide powder added to the ceramic slurry accounts for 60~70% of the volume fraction. And / or, the mass ratio of the first coarse silicon carbide powder to the first fine silicon carbide powder is 5:5 to 8:

2.

3. The method for preparing short-period PIP dense direct-write molded silicon carbide lattice ceramics according to claim 1, characterized in that, In step (1), the additives include dispersants, binders, and aqueous organic rheology modifiers; The dispersant is ammonium polycarboxylate, and its addition amount is 0.8~5 wt% of the total addition amount of the first coarse silicon carbide powder and the first fine silicon carbide powder; The binder is polyvinylpyrrolidone, and its addition amount is 0.3~3 wt% of the total addition amount of the first silicon carbide coarse powder and the first silicon carbide fine powder; The amount of the aqueous organic rheology modifier added is 0.1 to 0.3 wt% of the total amount of the first coarse silicon carbide powder and the first fine silicon carbide powder.

4. The method for preparing short-period PIP dense direct-write molded silicon carbide lattice ceramics according to claim 1, characterized in that, In step (2), the parameters of the direct-write 3D printing include: nozzle outlet diameter of 1.0~2.0mm, extrusion pressure of 0.6~0.8MPa, printing speed of 18~22mm / s, and layer height of 0.9~1.0mm.

5. The method for preparing short-period PIP dense direct-write molded silicon carbide lattice ceramics according to claim 1, characterized in that, In step (3), the vacuum pre-sintering is a two-stage sintering process with a vacuum degree ≤10. -3 Pa, heating rate is 1~10℃ / min, first stage temperature is 500~700℃, time is 60~120min, second stage temperature is 1700~2000℃, time is 10~40min; And / or, the porosity of the silicon carbide lattice porous preform is 35~45 vol%.

6. The method for preparing short-period PIP dense direct-write molded silicon carbide lattice ceramics according to claim 1, characterized in that, In step (4), the mass ratio of the second coarse silicon carbide powder to the second fine silicon carbide powder is 2:8 to 5:5; And / or, the total mass of the second coarse silicon carbide powder and the second fine silicon carbide powder is 11-20 wt% of the mass of the modified impregnation solution; And / or, the amount of the surface modifier added is 0.1~10 wt% of the mass of the modified impregnation solution; And / or, the surface modifier includes a silane coupling agent or a silazane compound; the silane coupling agent is at least one of 3-aminopropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; the silazane compound is hexamethyldisilazane; And / or, the organosilicon precursor includes at least one of polycarbosilane and polysilane; And / or, the organic solvent includes at least one of n-hexane, xylene, toluene, cyclohexane, and ethyl acetate.

7. The method for preparing short-period PIP dense direct-write molded silicon carbide lattice ceramics according to claim 1, characterized in that, In step (5), the absolute pressure of the vacuum negative pressure impregnation is ≤1kPa, the impregnation temperature is 40~60℃, and the impregnation time is 1.5~2h; The curing temperature is 180~260℃, and the curing time is 1~12h; The pyrolysis was carried out under an inert atmosphere, with the temperature increased to 1100-1600℃ at a heating rate of 1-10℃ / min and held for 0.5-2h.

8. The method for preparing short-period PIP dense direct-write molded silicon carbide lattice ceramics according to claim 1, characterized in that, In step (7), the crystallization treatment is carried out at a temperature of 1100~1600℃ for 0.5~2h. And / or, step (7) may be followed by post-processing, which may include polishing.

9. The method for preparing short-period PIP dense direct-write molded silicon carbide lattice ceramics according to claim 1, characterized in that, The temperature of the crystallization process in step (7) is the same as the temperature of the pyrolysis process in step (5).

10. The method for preparing short-period PIP dense direct-write molded silicon carbide lattice ceramics according to claim 1, characterized in that, In step (7), the relative density of the silicon carbide lattice ceramic is >90%; in the vertical direction, the difference in Vickers hardness between the upper and lower surfaces of the silicon carbide lattice ceramic is ≤2.0GPa.