A method for preparing tungsten carbide composite powder from waste tungsten wires
Tungsten carbide composite powder can be prepared in one step by flame calcination and spray drying technology, which solves the problems of incomplete oxidation and agglomeration in traditional calcination methods, and realizes efficient and environmentally friendly tungsten wire recycling and high-value utilization.
Patent Information
- Application Number
- CN202611351263.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-10
AI Technical Summary
Existing waste tungsten wire recycling technologies suffer from high costs, environmental pollution, and low recycling efficiency. In particular, the traditional calcination method leads to incomplete oxidation and clumping of the tungsten wire, requiring complex wet grinding and separation processes.
Waste tungsten wire is burned with a flame to generate gaseous tungsten oxide, which is then mixed with rare earth oxides, carbon sources and additives. Tungsten carbide composite powder is prepared in one step through spray drying and reduction carbonization treatment, avoiding the oxide layer from hindering internal oxidation and agglomeration.
This technology enables efficient and environmentally friendly recycling of waste tungsten wires, significantly improving recycling efficiency, simplifying the process, and producing high-quality tungsten carbide composite powder for use in cemented carbide products, thereby enhancing the value of resource utilization.
Smart Images

Figure CN123062279A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of tungsten wire recycling technology, specifically relating to a method for preparing tungsten carbide composite powder from waste tungsten wire. Background Technology
[0002] Tungsten-diamond wire possesses excellent properties such as high hardness, high strength, high temperature resistance, and corrosion resistance, making it widely used in the silicon wafer cutting industry. With the continued expansion of the photovoltaic industry and the increasing demand for silicon wafers, the demand for tungsten-diamond wire is growing rapidly. However, the current yield rate of tungsten-diamond wire production is only around 60%, resulting in a large amount of waste tungsten wire. As a vital strategic resource, the recycling of metallic tungsten is of great strategic significance. Therefore, developing efficient and clean waste tungsten wire recycling technologies is of great importance.
[0003] Currently, the mainstream process for recycling waste tungsten wire is hydrometallurgical technology. Related technology 1 proposes a process for recycling nickel-plated tungsten wire diamond cutting wire, using concentrated sulfuric acid for acid leaching to remove nickel from the tungsten wire surface, and then utilizing hydrogen peroxide as a catalytic reaction to separate the tungsten wire main body. However, this method requires a large amount of solution reagents, resulting in high costs and potential environmental pollution risks. Related technology 2 proposes an electrolytic method for recycling tungsten wire, which reduces the use of solution reagents to some extent, but still requires alkaline solutions for the final recycling process. Overall, existing hydrometallurgical processes generally rely on chemical reagents such as concentrated sulfuric acid, hydrogen peroxide, and sodium hydroxide, leading not only to high recycling costs but also to environmental pollution problems, significantly hindering their industrial development.
[0004] To address the shortcomings of hydrometallurgy, existing technology 3 proposes a method for recycling waste tungsten wire from diamond wire, employing calcination to process the waste tungsten wire. This method first calcines the cleaned waste tungsten wire to obtain calcined tungsten wire; then, the calcined tungsten wire is wet-milled and sieved under dispersant conditions to obtain a mixed powder of tungsten trioxide powder and tungsten particles; subsequently, tungsten particles and tungsten trioxide powder are obtained separately through ultrasonic and centrifugal separation; the tungsten particles are then repeatedly calcined, wet-milled, sieved, ultrasonically separated, and centrifuged; finally, the obtained tungsten trioxide powder is de-dispersed and reduced in a reducing gas to obtain regenerated tungsten powder. Related technology 4 proposes a method for preparing tungsten-containing waste into oxides using a kiln. The tungsten waste is placed in a kiln, rapidly heated, and oxygen is continuously introduced into the kiln, causing the tungsten waste to calcine and oxidize in an oxygen atmosphere. The calcined tungsten waste is then ball-milled and gravity-screened to obtain tungsten oxide powder. However, this method produces a large amount of lumps during the calcination process, the interior of which contains unoxidized tungsten wire, resulting in low recycling efficiency. The problem stems from the fact that in traditional calcination methods, the oxide layer formed on the surface of the tungsten wire after oxidation hinders the diffusion of oxygen into the interior, making it difficult for the internal tungsten wire to be further oxidized. The incompletely oxidized material must be processed through subsequent complex wet grinding and separation processes, resulting in a lengthy process.
[0005] In summary, existing waste tungsten wire recycling technologies have the following shortcomings: hydrometallurgical processes rely on a large amount of chemical reagents, resulting in high costs and a heavy environmental burden; traditional calcination methods suffer from severe agglomeration problems, making it difficult to fully oxidize the internal tungsten wires, requiring complex wet grinding and separation processes, resulting in low recycling efficiency and a long process. Summary of the Invention
[0006] The purpose of this invention is to provide a method for preparing tungsten carbide composite powder from waste tungsten wire. The method provided by this invention can effectively solve the problem of calcination agglomeration, achieve rapid and complete oxidation of waste tungsten wire, effectively connect with the tungsten carbide preparation process, and has a short preparation process that is easy to industrialize. It has important practical significance and application value.
[0007] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a method for preparing tungsten carbide composite powder from waste tungsten wire, comprising the following steps: Waste tungsten wire and oxidant are burned under flame conditions to obtain gaseous tungsten oxide; The gaseous tungsten oxide is introduced into water via a carrier gas to obtain a tungsten oxide suspension; The tungsten oxide suspension, rare earth oxides, carbon source, and additives are mixed to obtain a mixture. The mixture was spray-dried to obtain a composite powder precursor; The composite powder precursor was subjected to reduction and carbonization treatment under inert gas conditions to obtain a pre-passivated material. The pre-passivated material is passivated in a hydrogen atmosphere to obtain the tungsten carbide composite powder.
[0008] Preferably, the oxidant includes sodium nitrite; the mass ratio of the waste tungsten wire to the oxidant is (10~20):1; the gaseous tungsten oxide includes tungsten; and the carrier gas is air or nitrogen.
[0009] Preferably, the rare earth oxide includes lanthanum oxide, and the mass ratio of the rare earth oxide to tungsten oxide in the tungsten oxide suspension is 1:(100~200).
[0010] Preferably, the carbon source includes carbon black and / or an organic carbon source, wherein the organic carbon source includes glucose and / or maltose; the molar ratio of carbon in the carbon source to tungsten oxide in the tungsten oxide suspension is (2.5~3.5):1.
[0011] Preferably, the additive includes a binder; the binder includes polyethylene glycol (PEG); and the mass ratio of the additive to tungsten oxide in the tungsten oxide suspension is 1:(50~100).
[0012] Preferably, the inert gas is nitrogen; the temperature of the reduction carbonization treatment is 900~1000℃, and the time is 20~40min.
[0013] Preferably, the passivation treatment is performed at a temperature of 900~1300℃ for a time of 20~60 minutes.
[0014] Preferably, the tungsten carbide composite powder has a Fisher's standard particle size (FSSS size) of 1.9~2.6 μm.
[0015] Preferably, the mixing is ball milling, and the ball milling time is 240~300 min; after the passivation treatment is completed, the passivation product is further crushed.
[0016] Preferably, the reduction carbonization treatment is carried out in a tube furnace or a rotary furnace; the passivation treatment is carried out in a molybdenum wire furnace.
[0017] This invention provides a method for preparing tungsten carbide composite powder from waste tungsten wire, comprising the following steps: calcining waste tungsten wire and an oxidant under flame conditions to obtain gaseous tungsten oxide; introducing the gaseous tungsten oxide into water through a carrier gas to obtain a tungsten oxide suspension; mixing the tungsten oxide suspension, rare earth oxides, a carbon source, and additives to obtain a mixture; spray-drying the mixture to obtain a composite powder precursor; subjecting the composite powder precursor to reduction carbonization under inert gas conditions to obtain a pre-passivated material; and passivating the pre-passivated material in a hydrogen atmosphere to obtain the tungsten carbide composite powder. Compared with the prior art, this invention has the following beneficial effects: This invention solves the problem of caking caused by incomplete oxidation of tungsten wire in traditional calcination processes, significantly improving the recycling efficiency of waste tungsten wire. Existing pyrometallurgical recycling technologies, when calcining waste tungsten wire, suffer from an oxide layer formed on the surface that hinders oxygen diffusion, resulting in insufficient oxidation of the internal tungsten wire and the formation of large amounts of lumps. This necessitates complex wet grinding and separation processes to handle the incompletely oxidized material, leading to a lengthy process and low recycling efficiency. This invention employs the addition of an oxidant and flame combustion (i.e., flame gasification). The high temperature of the flame instantly oxidizes the waste tungsten wire into gaseous tungsten oxide, effectively avoiding the caking problem caused by the oxide layer covering the internal tungsten wire during traditional calcination. This achieves a one-step, highly efficient conversion of waste tungsten wire into tungsten oxide, significantly shortening the process flow.
[0018] This invention eliminates the reliance on large amounts of chemical reagents in hydrometallurgical technology, achieving green and environmentally friendly recycling. Current mainstream processes for recycling waste tungsten wires are hydrometallurgical techniques, which generally require large amounts of solutions such as concentrated sulfuric acid, hydrogen peroxide, and sodium hydroxide. This not only leads to high recycling costs but also poses potential environmental pollution risks, severely hindering its industrial development. This invention uses a pyrometallurgical process to replace the hydrometallurgical process, eliminating the need for corrosive chemical reagents such as acids and alkalis throughout the entire process. The recycling and conversion of waste tungsten wires can be completed solely through flame oxidation and carrier gas collection. The process is short, the equipment is simple, the cost is low, and it is environmentally friendly, making it easy to promote industrialization.
[0019] This invention achieves a short-process, integrated preparation of high-quality tungsten carbide composite powder from waste tungsten filaments. Most existing recycling technologies only convert waste tungsten filaments into recycled tungsten powder or tungsten oxide powder. Further preparation of tungsten carbide products requires additional carbonization and other processes, resulting in poor process integration and a lengthy workflow. This invention organically combines the recycling of waste tungsten filaments with the preparation of tungsten carbide composite powder: the recovered tungsten oxide suspension is directly introduced into rare earth oxides, carbon sources, and additives, followed by spray drying, reduction, and carbonization treatment to obtain high-quality tungsten carbide composite powder in one step. The method provided by this invention achieves a short-process conversion from waste tungsten filaments to end products, reducing intermediate steps and improving resource utilization efficiency and economic added value.
[0020] The method provided by this invention can prepare tungsten carbide composite powder with excellent properties, realizing the high-value utilization of waste tungsten resources. This invention introduces rare earth oxides as grain growth inhibitors during the recycling process and combines this with spray drying technology to achieve uniform mixing of the components. After subsequent reduction carburization and passivation treatments, tungsten carbide composite powder with complete grains and uniform composition distribution can be obtained. The tungsten carbide composite powder obtained by this invention can be used to prepare cemented carbide products, possessing excellent properties such as high strength and high hardness, realizing a leap from low-value recycling to high-value utilization of waste tungsten wire. Attached Figure Description
[0021] Figure 1 A flowchart illustrating the process of preparing tungsten carbide composite powder from waste tungsten wires, provided by this invention. Figure 2 This is a photograph of the waste tungsten wire used in this invention. Figure 3 This is a photograph of the agglomerated sample of the waste tungsten wire used in the comparative example of this invention. Figure 4 The waste tungsten wires in the comparative example of this invention were calcined, agglomerated, ball-milled, and sieved without being oxidized. Detailed Implementation
[0022] This invention provides a method for preparing tungsten carbide composite powder from waste tungsten wire, comprising the following steps: Waste tungsten wire and oxidant are burned under flame conditions to obtain gaseous tungsten oxide; The gaseous tungsten oxide is introduced into water via a carrier gas to obtain a tungsten oxide suspension; The tungsten oxide suspension, rare earth oxides, carbon source, and additives are mixed to obtain a mixture. The mixture was spray-dried to obtain a composite powder precursor; The composite powder precursor was subjected to reduction and carbonization treatment under inert gas conditions to obtain a pre-passivated material. The pre-passivated material is passivated in a hydrogen atmosphere to obtain the tungsten carbide composite powder.
[0023] In this invention, unless otherwise specified, all raw materials / components are commercially available products well-known to those skilled in the art. The flowchart of the method for preparing tungsten carbide composite powder from waste tungsten wire provided by this invention is as follows: Figure 1 As shown below, in conjunction with Figure 1 The present invention provides a detailed description of the method for preparing tungsten carbide composite powder from waste tungsten wire.
[0024] This invention involves burning waste tungsten wire and an oxidant under flame conditions (i.e., flame vaporization) to obtain gaseous tungsten oxide. In this invention, the oxidant is preferably sodium nitrite. The mass ratio of the waste tungsten wire to the oxidant is preferably (10~20):1, more preferably (10~15):1, and in the examples, it can be 10:1.
[0025] In this invention, residue is obtained after burning under flame conditions. Preferably, the invention further includes leaching and filtering the residue sequentially to obtain recovered nickel products. The leaching solution is preferably an aqueous solution, the leaching temperature can be room temperature, and the leaching time is preferably 10-20 hours.
[0026] After obtaining gaseous tungsten oxide, the present invention introduces the gaseous tungsten oxide into water via a carrier gas to obtain a tungsten oxide suspension. In the present invention, the main component of the gaseous tungsten oxide is tungsten trioxide (WO3), which may contain tungsten trioxide and / or tungsten blue phases after condensation. The carrier gas is preferably air or nitrogen.
[0027] After obtaining the tungsten oxide suspension, the present invention mixes the tungsten oxide suspension, rare earth oxides, carbon source, and additives to obtain a mixture. In the present invention, the tungsten oxide suspension comprises tungsten oxide and water. The mass ratio of tungsten oxide to water in the tungsten oxide suspension is (15~20):30, and in the examples it can be 19:30. The rare earth oxide comprises lanthanum oxide, and the mass ratio of the rare earth oxide to tungsten oxide in the tungsten oxide suspension is preferably 1:(100~200), more preferably 1:(100~180), and even more preferably 1:(120~180). The carbon source preferably comprises carbon black and / or an organic carbon source. The organic carbon source preferably comprises glucose and / or maltose. The molar ratio of carbon in the carbon source to tungsten oxide in the tungsten oxide suspension is preferably (2.5~3.5):1, more preferably (2.7~3.2):1. The additive preferably comprises a binder. The binder preferably comprises polyethylene glycol (PEG). The preferred mass ratio of the additive to the tungsten oxide in the tungsten oxide suspension is 1:(50~100), more preferably 1:(50~70).
[0028] In this invention, the mixing is preferably ball milling, and the ball milling time is preferably 240-300 min. The ball milling conditions preferably include: a ball-to-material ratio of 10-12:1; a rotation speed of 200-400 rpm, which can be 300 rpm in the embodiment; and water as the milling medium.
[0029] After obtaining the mixture, the present invention performs spray drying on the mixture to obtain a composite powder precursor. The present invention does not have specific requirements for the specific implementation method of the spray drying.
[0030] After obtaining the composite powder precursor, the present invention performs a reduction carbonization treatment on the composite powder precursor under inert gas conditions to obtain a pre-passivated material. In the present invention, the inert gas is preferably nitrogen. The reduction carbonization treatment is preferably carried out in a tube furnace or a rotary furnace. The temperature of the reduction carbonization treatment is preferably 900~1000℃, and in the embodiments it can be 900, 950 or 1000℃. The time of the reduction carbonization treatment is preferably 20~40 min, and in the embodiments it can be 20, 25, 30, 35 or 40 min.
[0031] In this invention, during the reduction carbonization process: carbonization refers to the main reaction that occurs: W + C = WC.
[0032] After obtaining the pre-passivated material, the present invention performs passivation treatment on the pre-passivated material in a hydrogen atmosphere to obtain the tungsten carbide composite powder. In the present invention, the passivation treatment is preferably performed in a molybdenum wire furnace. The passivation treatment temperature is preferably 900~1300℃, and in the embodiments it can be 1000, 1100, 1200 or 1260℃. The passivation treatment time is preferably 20~60 min, and in the embodiments it can be 30, 40, 50 or 60 min.
[0033] In this invention, the passivation treatment preferably further includes crushing the passivation product after the passivation treatment is completed. The specific implementation of the crushing treatment is not particularly required in this invention. The FSSS of the tungsten carbide composite powder is preferably 1.9~2.6μm, and in the embodiments it can be 1.90, 2.19, 2.45, 2.47, 2.53 or 2.60μm.
[0034] To further illustrate the present invention, the technical solutions provided by the present invention will be described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0035] Example 1 This embodiment provides a method for preparing tungsten carbide composite powder from waste tungsten wire, specifically including the following steps: (1) Place 1550g of waste tungsten wire and 150g of sodium nitrite in a flame and burn them in air atmosphere to form gaseous tungsten trioxide; (2) The gaseous tungsten trioxide in step (1) is introduced into water through a carrier gas (nitrogen) to obtain a tungsten trioxide suspension. The mass of tungsten trioxide in the obtained tungsten trioxide suspension is 1890g and the mass of water is 3000g. (3) Add 19g of rare earth oxide (lanthanum oxide), 342g of carbon source (carbon black) and 38g of additive (binder, PEG) to the 4890g tungsten trioxide suspension obtained in step (2), and place it in a ball mill for ball milling (ball-to-material ratio of 12:1, rotation speed of 300 rpm, ball milling medium of water) for 240 min to obtain a mixture. (4) The mixture obtained in step (3) is spray-dried to obtain a composite powder precursor; (5) The composite powder precursor obtained in step (4) is placed in a rotary kiln and subjected to reduction carbonization under inert gas (nitrogen) conditions. The heating rate is 10℃ / min, the reduction temperature is 900℃, and the reduction time is 40min to obtain pre-passivated material. (6) The pre-passivated material obtained in step (5) was placed in a molybdenum wire furnace for passivation (in a hydrogen atmosphere). The passivation temperature was 1260℃, the heating rate was 10℃ / min, and the passivation time was 60min. After crushing, it was sieved to obtain tungsten carbide composite powder. The FSSS particle size of the tungsten carbide composite powder prepared in Example 1 was 1.90μm.
[0036] Example 2 Example 2 provides a method for preparing tungsten carbide composite powder from waste tungsten wire, which is basically the same as the preparation method in Example 1, except that the parameters in Table 1 are used for preparation.
[0037] Example 3 Example 3 provides a method for preparing tungsten carbide composite powder from waste tungsten wire, which is basically the same as the preparation method in Example 1, except that the parameters in Table 1 are used for preparation.
[0038] Example 4 Example 4 provides a method for preparing tungsten carbide composite powder from waste tungsten wire, which is basically the same as the preparation method in Example 1, except that the parameters in Table 1 are used for preparation.
[0039] Example 5 Example 5 provides a method for preparing tungsten carbide composite powder from waste tungsten wire, which is basically the same as the preparation method in Example 1, except that the parameters in Table 1 are used for preparation.
[0040] Example 6 Example 6 provides a method for preparing tungsten carbide composite powder from waste tungsten wire, which is basically the same as the preparation method in Example 1, except that the parameters in Table 1 are used for preparation.
[0041] Table 1. Operating parameters of the methods provided in Examples 1-6
[0042] Comparative Example 1 (1) 1000g of waste diamond wire tungsten wire (50μm in diameter) was ultrasonically cleaned to obtain cleaned waste tungsten wire.
[0043] (2) The cleaned waste tungsten wire was calcined in a calcining furnace at a temperature of 1100℃ (heating rate of 10℃ / min) for 2 h, yielding 1190g of calcined tungsten wire. A physical image of the calcined tungsten wire product obtained in step 2 of Comparative Example 1 is shown below. Figure 3 As shown, Figure 3 It can be seen that there is obvious clumping in the calcined tungsten wire.
[0044] (3) The calcined tungsten wire obtained in step (2) and 8.3g of isopropanol were mixed and wet-milled using a high-energy ball milling device. The ball-to-material ratio was 12:1, the rotation speed was 300 rpm, the wet milling medium was water, and the ball milling time was 60 min.
[0045] (4) The material after ball milling in step (3) is passed through a 150-mesh sieve to obtain the undersize material, which is a mixed powder containing tungsten trioxide powder and tungsten particles. 1195g of the mixed powder containing tungsten trioxide powder and tungsten particles is obtained. 17.93kg of water is added to the mixed powder, and ultrasonic centrifugation is performed (ultrasonic frequency of 50 Hz, time of 60 min) and centrifugation (speed of 5000 rpm, time of 30 min) to obtain tungsten particles and tungsten trioxide powder, respectively. The oversize product after sieving in step (4) of Comparative Example 1 is as follows: Figure 4 As shown, it can be observed that a significant amount of tungsten wire was not completely oxidized and could not be processed into tungsten oxide powder during ball milling.
[0046] (5) Using a calcining furnace, the tungsten particles obtained in step (4) are returned to step (2) for calcination, and the process of steps (3) and (4) is repeated once.
[0047] (6) Place the tungsten trioxide powder from steps (4) and (5) in a calcining furnace for calcination to remove the dispersant and obtain tungsten trioxide powder. The calcination temperature is 900℃ (heating rate is 10℃ / min) and the calcination time is 30 min.
[0048] (7) Using a rotary reduction furnace, the tungsten trioxide powder in steps (4) and (5) is reduced in hydrogen to obtain 998.6g of regenerated tungsten powder. The reduction temperature is 900℃ (heating rate is 10℃ / min) and the reduction time is 60min.
[0049] Comparative Example 2: Referring to Example 1 disclosed in Chinese Patent CN202510473567.9 (1) Place the tungsten waste on the silicon carbide rack in the kiln and close the kiln.
[0050] (2) Turn on the electric heating so that the temperature inside the kiln rises rapidly to 750~1250℃.
[0051] (3) Introduce oxygen into the kiln, exhaust the air in the kiln, continue to introduce oxygen, control the electric heating power of the kiln under the oxygen atmosphere, maintain the temperature in the kiln at 750~1250℃, and calcine the oxidation reaction at 750~1250℃ for 2~6 hours.
[0052] (4) After the calcination oxidation reaction is completed, the electric heating is stopped and oxygen is continuously introduced. Under the oxygen atmosphere, the temperature inside the kiln drops to 100℃~200℃ and then the furnace is opened to cool naturally to room temperature, resulting in calcined tungsten waste with obvious agglomeration.
[0053] (5) The calcined tungsten waste from step four is ball-milled and gravity-screened to obtain tungsten oxide powder.
[0054] As can be seen from the above embodiments, the present invention employs a simple and efficient tungsten wire oxidation technology under flame conditions, solving the problem of tungsten wire agglomeration caused by traditional calcination, optimizing the cumbersome ball milling and gravity screening processes, and improving the efficiency of tungsten wire recycling. Simultaneously, the recovered tungsten trioxide powder can be directly used to prepare tungsten carbide composite powder, resulting in a short process flow, low cost, and enabling rapid industrial-scale recycling and reuse of diamond wire tungsten wire waste.
[0055] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, and not all embodiments. Other embodiments can be obtained based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing tungsten carbide composite powder from waste tungsten wire, characterized in that, Includes the following steps: Waste tungsten wire and oxidant are burned under flame conditions to obtain gaseous tungsten oxide; The gaseous tungsten oxide is introduced into water via a carrier gas to obtain a tungsten oxide suspension; The tungsten oxide suspension, rare earth oxides, carbon source and additives are mixed to obtain a mixture. The mixture is spray-dried to obtain a composite powder precursor; The composite powder precursor was subjected to reduction and carbonization treatment under inert gas conditions to obtain a pre-passivated material. The pre-passivated material is passivated in a hydrogen atmosphere to obtain the tungsten carbide composite powder.
2. The method for preparing tungsten carbide composite powder from waste tungsten wire according to claim 1, characterized in that, The oxidant includes sodium nitrite; the mass ratio of the waste tungsten wire to the oxidant is (10~20):1; the gaseous tungsten oxide includes yellow tungsten; the carrier gas is air or nitrogen.
3. The method for preparing tungsten carbide composite powder from waste tungsten wire according to claim 1, characterized in that, The rare earth oxide includes lanthanum oxide, and the mass ratio of the rare earth oxide to tungsten oxide in the tungsten oxide suspension is 1:(100~200).
4. The method for preparing tungsten carbide composite powder from waste tungsten wire according to claim 1, characterized in that, The carbon source includes carbon black and / or an organic carbon source, wherein the organic carbon source includes glucose and / or maltose; the molar ratio of carbon in the carbon source to tungsten oxide in the tungsten oxide suspension is (2.5~3.5):
1.
5. The method for preparing tungsten carbide composite powder from waste tungsten wire according to claim 1, characterized in that, The additive includes a binder; the binder includes polyethylene glycol; the mass ratio of the additive to tungsten oxide in the tungsten oxide suspension is 1:(50~100).
6. The method for preparing tungsten carbide composite powder from waste tungsten wire according to claim 1, characterized in that, The inert gas is nitrogen; the reduction carbonization treatment is carried out at a temperature of 900~1000℃ for a time of 20~40 minutes.
7. The method for preparing tungsten carbide composite powder from waste tungsten wire according to claim 1, characterized in that, The passivation treatment is performed at a temperature of 900~1300℃ for a time of 20~60 minutes.
8. The method for preparing tungsten carbide composite powder from waste tungsten wire according to claim 1, characterized in that, The tungsten carbide composite powder has a Fisher particle size of 1.9~2.6μm.
9. The method for preparing tungsten carbide composite powder from waste tungsten wire according to claim 1, characterized in that, The mixing process involves ball milling for 240-300 minutes; after the passivation treatment is completed, the passivation product is further subjected to crushing.
10. The method for preparing tungsten carbide composite powder from waste tungsten wire according to claim 1, characterized in that, The reduction carbonization treatment is carried out in a tube furnace or a rotary furnace; the passivation treatment is carried out in a molybdenum wire furnace.
Citation Information
Patent Citations
A method for producing an oxide from tungsten-containing waste material using a kiln
CN120097385B