A corrosion-resistant paint for pedestrian walkway steel structures and its preparation method
By using a modified waterborne acrylic resin and waterborne epoxy emulsion compound system and an anti-corrosion paint made of ultrafine modified zinc phosphate and mica iron oxide ash composite anti-rust filler, the problems of insufficient weather resistance and adhesion of pedestrian walkway steel structures have been solved, achieving high-efficiency anti-corrosion performance and environmentally friendly construction.
Patent Information
- Application Number
- CN202611399387.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-10
AI Technical Summary
Existing anti-corrosion coatings have insufficient weather resistance and adhesion on pedestrian walkway steel structures, and are prone to blistering, loss of gloss and peeling of the paint film, resulting in reduced structural strength and increased maintenance costs.
A modified waterborne acrylic resin and waterborne epoxy emulsion compound system, combined with ultrafine modified zinc phosphate and mica iron oxide ash composite anti-rust filler, is used to prepare an anti-corrosion paint through a refined preparation process, which improves the density and adhesion of the paint film.
It significantly improves the water resistance, salt spray resistance, and damp heat resistance of anti-corrosion paint, extends the service life of steel structures, reduces maintenance frequency and cost, and ensures environmental friendliness and ease of construction.
Smart Images

Figure CN123063018A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of anti-corrosion coating technology, and more specifically, to an anti-corrosion paint for pedestrian walkway steel structures and its preparation method. Background Technology
[0002] As a crucial component of municipal infrastructure, urban pedestrian walkway steel structures are constantly exposed to the outdoor natural environment, enduring year-round erosion from rainwater, alternating day-night temperature and humidity changes, and corrosion from atmospheric dust and trace amounts of salt spray. These steel structural components are mostly made of Q235 ordinary carbon steel, which inherently has poor corrosion resistance. During long-term service, they are prone to problems such as paint peeling, substrate corrosion, and component aging. This not only reduces the overall structural strength and service life of the steel structure but can also, in severe cases, affect the safety of pedestrian walkways. Therefore, extremely high requirements are placed on the corrosion resistance, weather resistance, and adhesion of protective coatings on the steel structure surface.
[0003] Currently, most anti-corrosion coatings used on pedestrian walkway steel structures are traditional oil-based coatings or ordinary single-component water-based coatings. Oil-based coatings suffer from high VOC content, significant pollution, strong odor during application, and failure to meet green municipal construction standards. Conventional water-based anti-corrosion coatings often use a single resin system with a simple formula and limited filler combinations. This results in insufficient film density and poor resistance to water, salt spray, and damp heat under complex outdoor conditions. Long-term use can easily lead to problems such as blistering, loss of gloss, and peeling of the film. The protection cycle is short, requiring frequent recoating, which significantly increases the maintenance costs and manpower required for municipal facilities. Summary of the Invention
[0004] (a) Technical problems to be solved To address the shortcomings of existing technologies, this invention provides an anti-corrosion paint for pedestrian walkway steel structures and its preparation method, thus solving the aforementioned problems.
[0005] (II) Technical Solution To achieve the above-mentioned objectives, the present invention provides the following technical solution: an anti-corrosion paint for pedestrian walkway steel structures and its preparation method, comprising the following raw materials in parts by weight: 55-65 parts of modified waterborne acrylic resin dispersion, 12-18 parts of waterborne epoxy emulsion, 6-10 parts of zinc phosphate anti-rust pigment, 3-6 parts of mica iron oxide ash, 4-7 parts of ultrafine talc powder, 0.3-0.8 parts of fumed silica, 0.5-1.2 parts of wetting and dispersing agent, 0.2-0.6 parts of organosilicon leveling agent, 0.1-0.4 parts of defoamer, 0.4-0.9 parts of waterborne adhesion promoter, 2-4 parts of propylene glycol methyl ether acetate, and 10-16 parts of deionized water, wherein the modified waterborne acrylic resin dispersion is a hydroxyl-modified acrylic resin aqueous dispersion with a solid content of 42%.
[0006] Preferably, the mixture also includes the following raw materials in parts by weight: 60 parts modified waterborne acrylic resin dispersion, 15 parts waterborne epoxy emulsion, 8 parts zinc phosphate anti-rust pigment, 4.5 parts mica iron oxide ash, 5.5 parts ultrafine talc powder, 0.5 parts fumed silica, 0.8 parts wetting and dispersing agent, 0.4 parts organosilicon leveling agent, 0.25 parts defoamer, 0.6 parts waterborne adhesion promoter, 3 parts propylene glycol methyl ether acetate, and 13 parts deionized water.
[0007] Preferably, the aqueous epoxy emulsion is a bisphenol A type aqueous epoxy emulsion with a solid content of 50%, and the emulsion particle size is controlled at 0.1-0.3 μm.
[0008] Preferably, the zinc phosphate anti-rust pigment is ultrafine modified zinc phosphate with a particle size range of 800-1200 mesh.
[0009] Preferably, the wetting and dispersing agent is Disperbyk-163 wetting and dispersing agent, and the silicone leveling agent is BYK-333 leveling agent.
[0010] Preferably, the defoamer is BYK-024 water-based defoamer, and the water-based adhesion promoter is silane coupling agent KH-550.
[0011] A method for preparing an anti-corrosion paint for steel structures of pedestrian walkways, the method comprising the following steps: (1) At room temperature, the amount of deionized water and propylene glycol methyl ether acetate in the formula are added to the high-speed dispersion mixing tank in sequence. The stirring equipment is turned on and the stirring speed is adjusted to 300 r / min. After stirring and mixing for 5 min, the amount of wetting and dispersing agent and defoamer in the formula are added and stirred for 10 min to obtain a uniform mixed solvent system for later use.
[0012] (2) Keep the stirring speed of the paint mixing tank at 300 r / min, add zinc phosphate anti-rust pigment, mica iron oxide ash, ultrafine talc powder and fumed silica in batches to the mixed solvent system obtained in step (1). The interval between each addition is 3 min. After all the materials are added, increase the stirring speed to 1200 r / min and disperse and grind at high speed for 35 min. After grinding, check the fineness of the material and control the fineness of the material to ≤35 μm to obtain a uniform pigment filler slurry.
[0013] (3) Reduce the stirring speed of the paint mixing kettle to 500 r / min, slowly add the modified waterborne acrylic resin dispersion and waterborne epoxy emulsion of the formula to the pigment filler slurry obtained in step (2), add at a uniform rate, control the addition time to 15 min, and continue stirring for 20 min after the addition is completed, so that the resin and slurry are fully mixed and blended to obtain the primary mixed paint liquid.
[0014] (4) Keep the stirring speed of the paint mixing kettle at 500 r / min, add water-based adhesion promoter and organosilicon leveling agent to the primary mixed paint liquid obtained in step (3) in sequence, and continue stirring for 15 min after the addition is completed. During the stirring process, the paint mixing kettle is sealed to avoid impurities from being mixed in, and the intermediate mixed paint liquid is obtained.
[0015] (5) Adjust the stirring speed of the intermediate mixed paint liquid obtained in step (4) to 400 r / min and continue stirring for 25 min at room temperature. After stirring, use a Forte 4 cup to test the viscosity of the paint liquid. Adjust the viscosity of the paint liquid by using deionized water to control the viscosity at 75-95 s. At the same time, test the pH value of the paint liquid and use a weak water neutralizer to adjust the pH value to 7.8-8.5. After filtering to remove trace impurities, the anti-corrosion paint for pedestrian walkway steel structure is obtained.
[0016] (III) Beneficial Effects Compared with the prior art, the present invention provides an anti-corrosion paint for pedestrian walkway steel structures and its preparation method, which has the following beneficial effects: 1. This invention relates to an anti-corrosion paint for pedestrian walkway steel structures and its preparation method. The invention employs a modified waterborne acrylic resin and waterborne epoxy emulsion compound system, combined with ultrafine modified zinc phosphate and mica iron oxide ash composite anti-rust filler, which effectively improves the density, adhesion and mechanical strength of the paint film, significantly improves the anti-corrosion performance of pedestrian walkway steel structures under outdoor working conditions such as water resistance, salt spray resistance and damp heat resistance, and can resist the erosion of outdoor rainwater, moisture and atmospheric corrosive media for a long time, effectively delaying the rust aging of steel structures, and meeting the long-term service requirements of outdoor pedestrian walkway steel structures.
[0017] 2. This invention relates to an anti-corrosion paint for pedestrian walkway steel structures and its preparation method. The invention adopts a water-based formulation system, supplemented by a reasonable ratio of additives and a refined preparation process. The raw materials are environmentally friendly and non-toxic, and the application is convenient. The prepared paint has uniform fineness and a smooth, defect-free film, effectively avoiding the problems of bubbling, loss of gloss, and poor adhesion of traditional anti-corrosion paints. At the same time, the formulation system has strong stability, controllable production costs, and is suitable for batch coating construction of pedestrian walkway steel structures, making it more practical and valuable for promotion. Attached Figure Description
[0018] Figure 1 This is a schematic diagram of the structure of the present invention; Figure 2 This is a flowchart illustrating the preparation process of the present invention. Detailed Implementation
[0019] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example 1
[0020] This embodiment provides an anti-corrosion paint for pedestrian walkway steel structures. The raw material components, by weight, are: 55 parts modified waterborne acrylic resin dispersion, 12 parts waterborne epoxy emulsion, 6 parts zinc phosphate anti-rust pigment, 3 parts mica iron oxide ash, 4 parts ultrafine talc powder, 0.3 parts fumed silica, 0.5 parts Disperbyk-163 wetting and dispersing agent, 0.2 parts BYK-333 organosilicon leveling agent, 0.1 parts BYK-024 waterborne defoamer, 0.4 parts KH-550 waterborne adhesion promoter, 2 parts propylene glycol methyl ether acetate, and 10 parts deionized water.
[0021] Among them, the modified waterborne acrylic resin dispersion is a hydroxyl-modified acrylic resin water dispersion with a solid content of 42%; the waterborne epoxy emulsion is a bisphenol A type waterborne epoxy emulsion with a solid content of 50% and a particle size of 0.1-0.3μm; and the zinc phosphate anti-rust pigment is an 800-mesh ultrafine modified zinc phosphate.
[0022] In this embodiment, the anti-corrosion paint was prepared using a specific method. The entire process was conducted at room temperature, and the stirring speed, feeding interval, dispersion time, and grinding parameters for each step strictly followed the preparation procedure. Finally, the paint viscosity was adjusted to 75 s (Ford cup 4) with deionized water, and the pH was adjusted to 8.0 using a weak aqueous neutralizing agent. The product was then filtered to obtain the finished anti-corrosion paint. The preparation method is as follows: Step (1) Stirring and mixing at room temperature with low speed throughout to avoid local agglomeration of solvent and additives; Step (2) Filler is added in batches in equal amounts, with four equal additions at 3-minute intervals. After high-speed grinding, the measured fineness is 32μm, which meets the requirement of ≤35μm; Step (3) Resin is added slowly and uniformly, with the flow rate controlled to be stable throughout the addition process to avoid local flocculation of resin; Step (4) Stirring is carried out in a closed manner throughout the process to prevent external dust and impurities from falling into the paint liquid; Step (5) Finally, a weak water-based neutralizer is used to finely adjust the pH to 8.0, and the measured viscosity of the Forecast-4 cup is 75s. After filtering through a 200-mesh filter to remove impurities, the anti-corrosion paint product of this embodiment is obtained. Example 2
[0023] This embodiment provides an anti-corrosion paint for pedestrian walkway steel structures. The raw material components, by weight, are: 60 parts modified waterborne acrylic resin dispersion, 15 parts waterborne epoxy emulsion, 8 parts zinc phosphate anti-rust pigment, 4.5 parts mica iron oxide ash, 5.5 parts ultrafine talc powder, 0.5 parts fumed silica, 0.8 parts Disperbyk-163 wetting and dispersing agent, 0.4 parts BYK-333 organosilicon leveling agent, 0.25 parts BYK-024 waterborne defoamer, 0.6 parts KH-550 waterborne adhesion promoter, 3 parts propylene glycol methyl ether acetate, and 13 parts deionized water.
[0024] Among them, the modified waterborne acrylic resin dispersion is a hydroxyl-modified acrylic resin aqueous dispersion with a solid content of 42%; the waterborne epoxy emulsion is a bisphenol A type waterborne epoxy emulsion with a solid content of 50% and a particle size of 0.1-0.3μm; and the zinc phosphate anti-rust pigment is a 1000-mesh ultrafine modified zinc phosphate.
[0025] In this embodiment, the anti-corrosion paint was prepared using a specific method. The entire process was conducted at room temperature, and all parameters followed the standard preparation procedures. The final viscosity of the paint was adjusted to 85 s (Ford Cup 4), the pH value was adjusted to 8.2, and the paint was filtered to obtain the finished anti-corrosion paint. The preparation process is as follows: Step (1) Observe the liquid surface state during stirring to ensure that the additives are completely dissolved and the system is free of floating oil; Step (2) During the filler fine dispersion process, extend the uniform dispersion time appropriately. After grinding, the material fineness uniformity is higher, and the measured fineness is 30μm; Step (3) Strictly control the 15min dripping time during the resin compounding and mixing stage to ensure that the acrylic resin and epoxy emulsion are fully cross-linked and fused; Step (4) After the additives are added, knead at a low speed to improve the leveling and adhesion performance of the paint film; Step (5) Finally, adjust the pH value to 8.2, adjust the viscosity to 85s, and filter with a 200-mesh precision filter.
[0026] The anti-corrosion paint is composed of the following components in parts by weight: 60 parts modified waterborne acrylic resin dispersion, 15 parts waterborne epoxy emulsion, 8 parts zinc phosphate anti-rust pigment, 4.5 parts mica iron oxide ash, 5.5 parts ultrafine talc powder, 0.5 parts fumed silica, 0.8 parts Disperbyk-163 wetting and dispersing agent, 0.4 parts BYK-333 organosilicon leveling agent, 0.25 parts BYK-024 waterborne defoamer, 0.6 parts KH-550 waterborne adhesion promoter, 3 parts propylene glycol methyl ether acetate, and 13 parts deionized water; the parameters of each raw material are consistent with those in Example 1, wherein the zinc phosphate anti-rust pigment is 1000 mesh ultrafine modified zinc phosphate; the anti-corrosion paint is prepared by the preparation method described in claim 7, and the final viscosity of the paint is adjusted to 85s and the pH value to 8.2. Example 3
[0027] This embodiment provides an anti-corrosion paint for pedestrian walkway steel structures. The raw material components, by weight, are: 65 parts modified waterborne acrylic resin dispersion, 18 parts waterborne epoxy emulsion, 10 parts zinc phosphate anti-rust pigment, 6 parts mica iron oxide ash, 7 parts ultrafine talc powder, 0.8 parts fumed silica, 1.2 parts Disperbyk-163 wetting and dispersing agent, 0.6 parts BYK-333 organosilicon leveling agent, 0.4 parts BYK-024 waterborne defoamer, 0.9 parts KH-550 waterborne adhesion promoter, 4 parts propylene glycol methyl ether acetate, and 16 parts deionized water.
[0028] Among them, the modified waterborne acrylic resin dispersion is a hydroxyl-modified acrylic resin aqueous dispersion with a solid content of 42%; the waterborne epoxy emulsion is a bisphenol A type waterborne epoxy emulsion with a solid content of 50% and a particle size of 0.1-0.3μm; and the zinc phosphate anti-rust pigment is a 1200-mesh ultrafine modified zinc phosphate.
[0029] In this embodiment, the anti-corrosion paint is prepared using a specific method. The entire process is carried out at room temperature, and all process parameters follow the preparation standard. The final viscosity of the paint is adjusted to 95s (Ford cup 4), the pH value is adjusted to 8.5, and the material is filtered to obtain the finished anti-corrosion paint. The preparation method is as follows: Step (1) For the ratio of excessive additives, extend the static fusion time to ensure the uniformity and stability of the system; Step (2) Strictly control the high-speed dispersion speed and time of the high filler system to completely disperse the powder agglomerates, with a measured fineness of 28μm; Step (3) Reduce the drip rate of the high resin content system to prevent the paint viscosity from rising suddenly and causing uneven mixing; Step (4) Add the leveling agent and coupling agent step by step at a slow speed to effectively improve the density of the paint film; Step (5) Finally adjust the pH value to 8.5, control the viscosity at 95s, and filter through a 200-mesh filter to obtain a high-hardness, high-weather-resistant anti-corrosion paint product.
[0030] The anti-corrosion paint is composed of the following components in parts by weight: 65 parts modified waterborne acrylic resin dispersion, 18 parts waterborne epoxy emulsion, 10 parts zinc phosphate anti-rust pigment, 6 parts mica iron oxide ash, 7 parts ultrafine talc powder, 0.8 parts fumed silica, 1.2 parts Disperbyk-163 wetting and dispersing agent, 0.6 parts BYK-333 organosilicon leveling agent, 0.4 parts BYK-024 waterborne defoamer, 0.9 parts KH-550 waterborne adhesion promoter, 4 parts propylene glycol methyl ether acetate, and 16 parts deionized water; the parameters of each raw material are consistent with those in Example 1, wherein the zinc phosphate anti-rust pigment is 1200 mesh ultrafine modified zinc phosphate; the anti-corrosion paint is prepared by the preparation method described in claim 7, and the final viscosity of the paint is adjusted to 95s and the pH value to 8.5.
[0031] The above situations are shown in Table 1.
[0032] Table 1:
[0033] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely preferred examples and are not intended to limit the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of the present invention is defined by the appended claims and their equivalents.
Claims
1. An anti-corrosion paint for steel structures of pedestrian walkways, characterized in that, The raw materials include the following parts by weight: 55-65 parts of modified waterborne acrylic resin dispersion, 12-18 parts of waterborne epoxy emulsion, 6-10 parts of zinc phosphate anti-rust pigment, 3-6 parts of mica iron oxide ash, 4-7 parts of ultrafine talc powder, 0.3-0.8 parts of fumed silica, 0.5-1.2 parts of wetting and dispersing agent, 0.2-0.6 parts of organosilicon leveling agent, 0.1-0.4 parts of defoamer, 0.4-0.9 parts of waterborne adhesion promoter, 2-4 parts of propylene glycol methyl ether acetate, and 10-16 parts of deionized water. The modified waterborne acrylic resin dispersion is a hydroxyl-modified acrylic resin aqueous dispersion with a solid content of 42%.
2. The anti-corrosion paint for pedestrian walkway steel structures according to claim 1, characterized in that, It also includes the following raw materials in parts by weight: 60 parts modified waterborne acrylic resin dispersion, 15 parts waterborne epoxy emulsion, 8 parts zinc phosphate anti-rust pigment, 4.5 parts mica iron oxide ash, 5.5 parts ultrafine talc powder, 0.5 parts fumed silica, 0.8 parts wetting and dispersing agent, 0.4 parts organosilicon leveling agent, 0.25 parts defoamer, 0.6 parts waterborne adhesion promoter, 3 parts propylene glycol methyl ether acetate, and 13 parts deionized water.
3. The anti-corrosion paint for pedestrian walkway steel structures according to claim 1 or 2, characterized in that, The aqueous epoxy emulsion is a bisphenol A type aqueous epoxy emulsion with a solid content of 50%, and the emulsion particle size is controlled at 0.1-0.3μm.
4. The anti-corrosion paint for pedestrian walkway steel structures according to claim 1 or 2, characterized in that, The zinc phosphate anti-rust pigment is an ultrafine modified zinc phosphate with a particle size range of 800-1200 mesh.
5. The anti-corrosion paint for pedestrian walkway steel structures according to claim 1 or 2, characterized in that, The wetting and dispersing agent is Disperbyk-163, and the silicone leveling agent is BYK-333.
6. The anti-corrosion paint for pedestrian walkway steel structures according to claim 1 or 2, characterized in that, The defoamer is BYK-024 water-based defoamer, and the water-based adhesion promoter is silane coupling agent KH-550.
7. The method for preparing the anti-corrosion paint for pedestrian walkway steel structures according to any one of claims 1-6, characterized in that: The preparation method includes the following steps: (1) At room temperature, the amount of deionized water and propylene glycol methyl ether acetate in the formula are added to the high-speed dispersion mixing tank in sequence. The stirring equipment is turned on and the stirring speed is adjusted to 300 r / min. After stirring and mixing for 5 min, the amount of wetting and dispersing agent and defoamer in the formula are added. Stirring is continued for 10 min to obtain a uniform mixed solvent system for later use. (2) Keep the stirring speed of the paint mixing tank at 300 r / min, add zinc phosphate anti-rust pigment, mica iron oxide ash, ultrafine talc powder and fumed silica to the mixed solvent system obtained in step (1) in batches, with a 3 min interval between each addition. After all the materials are added, increase the stirring speed to 1200 r / min and disperse and grind at high speed for 35 min. After grinding, check the fineness of the material and control the fineness of the material to ≤35 μm to obtain a uniform pigment filler slurry. (3) Reduce the stirring speed of the paint mixing kettle to 500 r / min, slowly add the modified waterborne acrylic resin dispersion and waterborne epoxy emulsion of the formula to the pigment filler slurry obtained in step (2), add at a uniform rate, control the addition time to 15 min, and continue stirring for 20 min after the addition is completed to make the resin and slurry fully mixed and blended to obtain the primary mixed paint liquid. (4) Keep the stirring speed of the paint mixing tank at 500 r / min, add water-based adhesion promoter and organosilicon leveling agent to the primary mixed paint liquid obtained in step (3) in sequence, and continue stirring for 15 min after the addition is completed. During the stirring process, the paint mixing tank is sealed to avoid impurities from being mixed in, and the intermediate mixed paint liquid is obtained. (5) Adjust the stirring speed of the intermediate mixed paint liquid obtained in step (4) to 400 r / min and continue stirring for 25 min at room temperature. After stirring, use a Forte 4 cup to test the viscosity of the paint liquid. Adjust the viscosity of the paint liquid by using deionized water to control the viscosity at 75-95 s. At the same time, test the pH value of the paint liquid and use a weak water neutralizer to adjust the pH value to 7.8-8.
5. After filtering to remove trace impurities, the anti-corrosion paint for pedestrian walkway steel structure is obtained.