A method for preparing a moisture- and heat-resistant epoxy resin coating
By preparing fluorinated triphenylamine compounds and modified graphene oxide, the humid heat resistance of epoxy resin coatings is enhanced, solving the problem of poor protective effect of epoxy resin coatings in high temperature and high humidity environments, and achieving long-term protection under humid heat conditions.
Patent Information
- Application Number
- CN202611122327.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-28
- Publication Date
- 2026-11-10
AI Technical Summary
Existing epoxy resin coatings have poor resistance to damp heat in high temperature and high humidity environments, resulting in the failure of the coating's protective effect.
By preparing a moisture- and heat-resistant epoxy resin and a moisture- and heat-resistant reinforcing agent, triphenylamine was brominated using N-bromosuccinimide to introduce bromine atoms, which then reacted with 2,3-difluoro-4-butoxyphenylboronic acid to form a fluorinated triphenylamine compound. Epoxy groups were then introduced by reacting the polyhydroxy fluorinated triphenylamine with epichlorohydrin to prepare the moisture- and heat-resistant epoxy resin. Simultaneously, graphene oxide was modified using a POSS structure formed by the hydrolysis of γ-aminopropyltriethoxysilane to prepare a moisture- and heat-resistant reinforcing agent, which enhanced the crosslinking density and hydrophobicity of the coating.
In high temperature and high humidity environments, the coating maintains excellent performance, inhibits the penetration of water vapor, oxygen and corrosive ions, and ensures long-term protection of the substrate.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of coatings, and more specifically to a method for preparing a moisture- and heat-resistant epoxy resin coating. Background Technology
[0002] Epoxy resin coatings are widely used in substrate protection due to their excellent adhesion, mechanical strength, and chemical resistance. However, in harsh environments with high temperature and humidity, such as marine climates, tropical regions, or inside enclosed equipment, water molecules can easily penetrate into the coating and the coating / substrate interface under thermal drive. This causes the coating to swell and soften, reducing its physical barrier function. It can also trigger hydrolysis of the resin matrix and breakage of chemical bonds, resulting in loss of coating adhesion, blistering, peeling, and ultimately, failure of protection.
[0003] Therefore, developing a method for preparing a moisture- and heat-resistant epoxy resin coating is of significant practical importance. Summary of the Invention
[0004] In order to overcome the above-mentioned technical problems, the purpose of this invention is to provide a method for preparing a moisture- and heat-resistant epoxy resin coating, which solves the problem that existing epoxy resin coatings have poor moisture- and heat resistance and are prone to coating protection failure in harsh environments with high temperature and high humidity.
[0005] The objective of this invention can be achieved through the following technical solutions: In a first aspect, this application provides a method for preparing a moisture- and heat-resistant epoxy resin coating, comprising the following steps: Step 1: Weigh out 25-30 parts of epoxy resin, 1-11 parts of moisture-resistant epoxy resin, 36-38 parts of curing agent, 0.5-1.7 parts of moisture-resistant reinforcing agent, 20-25 parts of solvent, 0.3-0.5 parts of wetting and dispersing agent, 0.2-0.4 parts of antioxidant, and 0.1-0.3 parts of leveling agent according to the following proportions, and set aside. Step 2: Add epoxy resin, moisture-heat resistant epoxy resin, moisture-heat resistant reinforcing agent, solvent, wetting and dispersing agent, antioxidant and leveling agent to a mixer, and stir and react for 20-30 minutes at a temperature of 20-25℃ and a stirring speed of 2000-3000r / min to obtain the coating base material. Step 3: When using, add the curing agent to the coating base and stir evenly to obtain a moisture- and heat-resistant epoxy resin coating.
[0006] In a preferred embodiment of the present invention, the moisture-resistant epoxy resin is prepared by the following steps: Step a1: Triphenylamine, N-bromosuccinimide, and tetrahydrofuran were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Nitrogen gas was introduced for protection. The mixture was stirred for 20-30 min at a temperature of 0-5℃ and a stirring rate of 200-300 r / min. Then, the temperature was raised to 50-60℃ and the mixture was stirred for 3-6 h. After the reaction was completed, the reaction product was cooled to room temperature and then poured into a saturated sodium thiosulfate solution. The product was then extracted 2-3 times with dichloromethane. The extracts were combined and dried with anhydrous sodium sulfate. The product was then filtered under vacuum. The solvent was removed by rotary evaporation of the filtrate. The product was then recrystallized with a mixture of ethyl acetate and petroleum ether to obtain the tribromotriphenylamine compound. Step a2: Tribromotriphenylamine compound, 2,3-difluoro-4-butoxyphenylboronic acid, potassium carbonate, palladium chloride, and N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Nitrogen gas was introduced for protection, and the reaction was stirred at 20-25℃ and 200-300 r / min for 20-30 min. Then, the temperature was raised to 80-90℃ and the reaction was stirred for 1-2 h. After that, the temperature was raised to 130-140℃ and the reaction was stirred for 3-6 h. After the reaction was completed, the reaction product was cooled to room temperature and then vacuum filtered. The filter cake was washed 2-3 times with distilled water and then placed in a vacuum drying oven and dried at 60-70℃ for 3-5 h to obtain butoxyfluorotriphenylamine compound. Step a3: Add butoxy-fluorinated triphenylamine compound, boron tribromide, aluminum chloride and dichloromethane to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir the reaction at 20-25℃ and 200-300 r / min for 10-15 h. After the reaction is complete, pour the reaction product into distilled water, let it stand to separate into layers, dry the organic phase with anhydrous sodium sulfate, then filter under vacuum, remove the solvent by rotary evaporation of the filtrate, and then recrystallize with N,N-dimethylformamide to obtain polyhydroxy fluorinated triphenylamine compound. Step a4: Add the polyhydroxy fluorinated triphenylamine compound, benzyltriethylammonium chloride, and epichlorohydrin to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Purge with nitrogen for protection and stir the reaction at 20-25℃ and 200-300 r / min for 10-20 min. Then raise the temperature to 100-110℃ and continue stirring for 3-5 h. After that, lower the temperature to 50-60℃ and add sodium hydroxide solution and continue stirring for 3-4 h. After the reaction is complete, cool the reaction product to room temperature, then vacuum filter it. Wash the filtrate 2-3 times with distilled water, then dry it with anhydrous sodium sulfate, then vacuum filter it again. Rotary evaporate the filtrate to remove the solvent, and obtain the moisture-resistant epoxy resin.
[0007] In a preferred embodiment of the present invention, the epoxy resin is epoxy resin E-44.
[0008] In a preferred embodiment of the present invention, the curing agent is 650 low molecular weight polyamide.
[0009] In a preferred embodiment of the present invention, the solvent is acetone.
[0010] In a preferred embodiment of the present invention, the wetting and dispersing agent is TEGO Dispers 655.
[0011] In a preferred embodiment of the present invention, the antioxidant is antioxidant 1010.
[0012] In a preferred embodiment of the present invention, the leveling agent is BY-333 leveling agent.
[0013] In a preferred embodiment of the present invention, the ratio of triphenylamine, N-bromosuccinimide and tetrahydrofuran in step a1 is 10 mmol: 30 mmol: 40-50 mL.
[0014] In a preferred embodiment of the present invention, the ethyl acetate / petroleum ether mixture in step a1 is a mixture of ethyl acetate and petroleum ether in a volume ratio of 7-8:1.
[0015] In a preferred embodiment of the present invention, the ratio of the tribromotriphenylamine compound, 2,3-difluoro-4-butoxyphenylboronic acid, potassium carbonate, palladium chloride and N,N-dimethylformamide used in step a2 is 10 mmol: 35-40 mmol: 50-60 mmol: 0.01-0.12 g: 100-110 mL.
[0016] In a preferred embodiment of the present invention, the ratio of the butoxy-fluorinated triphenylamine compound, boron tribromide, aluminum chloride and dichloromethane in step a3 is 10 mmol: 40-45 mmol: 20-25 mmol: 100-110 mL.
[0017] In a preferred embodiment of the present invention, the ratio of the polyhydroxy fluorinated triphenylamine compound, benzyltriethylammonium chloride, epichlorohydrin and sodium hydroxide solution in step a4 is 3g:0.4-0.5g:40-50g:10-12mL.
[0018] In a preferred embodiment of the present invention, the sodium hydroxide solution in step a4 has a mass fraction of 30-35%.
[0019] In a preferred embodiment of the present invention, the moisture-heat resistance enhancer is prepared by the following steps: Step b1: Deionized water, propanol, acetonitrile, and tetraethylammonium hydroxide were added to a four-necked flask equipped with a stirrer, thermometer, reflux condenser, constant pressure dropping funnel, and gas delivery tube. Nitrogen gas was introduced for protection. The mixture was stirred for 10-20 min at a temperature of 20-25℃ and a stirring rate of 200-300 r / min. Then, γ-aminopropyltriethoxysilane was added dropwise while stirring, with the dropping rate controlled at 1-3 drops / s. After the addition was completed, the temperature was raised to 50-60℃ and the reaction was stirred for 20-30 h. After the reaction was completed, the reaction product was cooled to room temperature, and the solvent was removed by rotary evaporation. The product was then washed 2-3 times with distilled water and cyclohexane, and then freeze-dried to obtain amination POSS. Step b2: Add graphene oxide and dimethyl sulfoxide to the reaction vessel, purge with nitrogen for protection, and stir for 20-30 min at a temperature of 20-25℃ and a stirring rate of 200-300 r / min. Then add aminated POSS and paraformaldehyde and continue stirring for 20-30 min. After that, raise the temperature to 170-180℃ and continue stirring for 20-30 h. After the reaction is completed, cool the reaction product to room temperature, centrifuge, and wash the precipitate 2-3 times with distilled water. Then freeze-dry to obtain the moisture-heat resistant reinforcing agent.
[0020] In a preferred embodiment of the present invention, the ratio of deionized water, propanol, acetonitrile, tetraethylammonium hydroxide and γ-aminopropyltriethoxysilane in step b1 is 10-12 mL: 5-6 mL: 1-2 mL: 0.2-0.3 g: 20-25 g.
[0021] In a preferred embodiment of the present invention, the ratio of graphene oxide, dimethyl sulfoxide, aminated POSS and paraformaldehyde in step b2 is 0.5g: 280-300mL: 3-9g: 1.8-2.2g.
[0022] In a preferred embodiment of the present invention, the graphene oxide in step b2 is TNGO-3 graphene oxide from Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences.
[0023] The beneficial effects of this invention are: This invention discloses a method for preparing a moisture-heat resistant epoxy resin coating. The method involves stirring and reacting epoxy resin, moisture-heat resistant epoxy resin, moisture-heat resistant reinforcing agent, solvent, wetting and dispersing agent, antioxidant, and leveling agent to obtain a coating base. During use, a curing agent is added to the coating base and stirred until homogeneous, resulting in the moisture-heat resistant epoxy resin coating. This epoxy resin coating, by adding moisture-heat resistant epoxy resin and moisture-heat resistant reinforcing agent, achieves excellent protective effects through their synergistic effect. It exhibits excellent moisture-heat resistance, inhibiting the penetration of water vapor, oxygen, and corrosive ions, ensuring the coating maintains excellent performance under moisture-heat aging, and providing long-term protection for the substrate.
[0024] In the preparation of moisture- and heat-resistant epoxy resin coatings, a moisture- and heat-resistant epoxy resin was first prepared. Triphenylamine was brominated using N-bromosuccinimide as a brominating agent, introducing bromine atoms onto the benzene ring of triphenylamine to obtain a tribromotriphenylamine compound. The tribromotriphenylamine compound reacted with 2,3-difluoro-4-butoxyphenylboronic acid, resulting in a Suzuki coupling reaction between the bromine atom on the tribromotriphenylamine compound and the phenylboronic acid group on the 2,3-difluoro-4-butoxyphenylboronic acid, introducing fluorine atoms and a butoxy group to obtain a butoxy-fluorinated triphenylamine compound. The butoxy-fluorinated triphenylamine compound was then treated with boron tribromide and aluminum chloride to achieve ether bond cleavage. The removal of alkyl groups yields hydroxyl groups, resulting in a polyhydroxy fluorinated triphenylamine compound. The hydroxyl groups on this compound react with the epoxy groups on epichlorohydrin via a ring-opening-ring-closing reaction, introducing multiple epoxy groups to obtain a moisture-resistant epoxy resin. This moisture-resistant epoxy resin contains multiple epoxy groups in its molecular structure, significantly enhancing the crosslinking density and thermal stability of the coating. Furthermore, the presence of multiple benzene rings and fluorine atoms in its molecular structure endows it with excellent heat resistance, and the abundance of fluorine atoms provides excellent hydrophobic and water-resistant properties. This allows the epoxy resin coating to maintain its integrity and stability for a long time in high-temperature and high-humidity environments, effectively protecting the functional groups.
[0025] In the process of preparing a moisture-resistant epoxy resin coating, a moisture-resistant reinforcing agent was also prepared. This agent was formed by hydrolyzing γ-aminopropyltriethoxysilane to form a silanol intermediate, which then underwent a dehydration condensation reaction to form a POSS structure, resulting in aminated POSS. The aminated POSS was then used to modify graphene oxide. The amino groups on the aminated POSS reacted with the carboxyl groups on the graphene oxide, achieving grafting of POSS onto the graphene oxide, thus obtaining the moisture-resistant reinforcing agent. The sheet-like structure of graphene oxide dispersed in the epoxy resin coating can fill its internal defects. After POSS grafting modification, the dispersibility of graphene oxide is improved, allowing it to be uniformly distributed within the coating, forming a good barrier. Furthermore, the abundant silicon content in the POSS structure improves the hydrophobicity of the coating, reducing the contact between corrosive media and the coating surface, further enhancing the moisture-resistant properties of the epoxy resin coating. Detailed Implementation
[0026] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0027] Example 1:
[0028] This embodiment describes a method for preparing a moisture- and heat-resistant epoxy resin coating, comprising the following steps: Step S1: 10 mmol of triphenylamine, 30 mmol of N-bromosuccinimide and 40 mL of tetrahydrofuran were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Nitrogen gas was introduced for protection. The mixture was stirred at 0 °C and 200 r / min for 20 min. Then the temperature was raised to 50 °C and the mixture was stirred for 3 h. After the reaction was completed, the reaction product was cooled to room temperature and then poured into a saturated sodium thiosulfate solution. The product was then extracted twice with dichloromethane. The extracts were combined and dried with anhydrous sodium sulfate. The product was then filtered under vacuum. The solvent was removed by rotary evaporation of the filtrate. The product was then recrystallized from an ethyl acetate / petroleum ether mixture in a volume ratio of 7:1 to obtain the tribromotriphenylamine compound. Step S2: 10 mmol of tribromotriphenylamine compound, 35 mmol of 2,3-difluoro-4-butoxyphenylboronic acid, 50 mmol of potassium carbonate, 0.01 g of palladium chloride, and 100 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred at 20 °C and 200 r / min for 20 min. The temperature was then raised to 80 °C and the mixture was stirred for 1 h. The temperature was then raised to 130 °C and the mixture was stirred for 3 h. After the reaction was completed, the reaction product was cooled to room temperature and then vacuum filtered. The filter cake was washed twice with distilled water and then placed in a vacuum drying oven and dried at 60 °C for 3 h to obtain butoxyfluorotriphenylamine compound. Step S3: 10 mmol of butoxy-fluorinated triphenylamine compound, 40 mmol of boron tribromide, 20 mmol of aluminum chloride and 100 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Nitrogen gas was introduced for protection. The reaction was stirred at 20 °C and 200 r / min for 10 h. After the reaction was completed, the reaction product was poured into distilled water and allowed to stand for separation. The organic phase was dried with anhydrous sodium sulfate and then vacuum filtered. The solvent was removed by rotary evaporation of the filtrate and then recrystallized with N,N-dimethylformamide to obtain the polyhydroxy fluorinated triphenylamine compound. Step S4: Add 3g of polyhydroxy fluorinated triphenylamine compound, 0.4g of benzyltriethylammonium chloride and 40g of epichlorohydrin to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 20℃ and 200r / min for 10min. Then raise the temperature to 100℃ and continue stirring for 3h. Then lower the temperature to 50℃ and add 10mL of 30% sodium hydroxide solution and continue stirring for 3h. After the reaction is complete, cool the reaction product to room temperature and then filter under vacuum. Wash the filtrate twice with distilled water and then dry it with anhydrous sodium sulfate. Then filter under vacuum and remove the solvent by rotary evaporation to obtain a moisture-resistant epoxy resin. Step S5: Add 10 mL of deionized water, 5 mL of propanol, 1 mL of acetonitrile, and 0.2 g of tetraethylammonium hydroxide to a four-necked flask equipped with a stirrer, thermometer, reflux condenser, constant pressure dropping funnel, and gas delivery tube. Purge with nitrogen for protection and stir the reaction at 20 °C and 200 r / min for 10 min. Then, while stirring, add 20 g of γ-aminopropyltriethoxysilane dropwise at a rate of 1 drop / s. After the addition is complete, raise the temperature to 50 °C and continue stirring for 20 h. After the reaction is complete, cool the reaction product to room temperature, then remove the solvent by rotary evaporation. Wash the product twice with distilled water and cyclohexane, and then freeze-dry to obtain amination-modified POSS. Step S6: Add 0.5g of graphene oxide TNGO-3 and 280mL of dimethyl sulfoxide to the reaction vessel, purge with nitrogen for protection, and stir for 20min at 20℃ and 200r / min. Then add 3g of aminated POSS and 1.8g of paraformaldehyde and continue stirring for 20min. Then raise the temperature to 170℃ and continue stirring for 20h. After the reaction is completed, cool the reaction product to room temperature, centrifuge, wash the precipitate twice with distilled water, and freeze dry to obtain the moisture and heat resistance enhancer. Step S7: Weigh out 25 parts by weight of epoxy resin, 1 part by weight of moisture-resistant epoxy resin, 36 parts by weight of curing agent, 0.5 parts by weight of moisture-resistant reinforcing agent, 20 parts by weight of solvent, 0.3 parts by weight of wetting and dispersing agent, 0.2 parts by weight of antioxidant, and 0.1 parts by weight of leveling agent, and set aside; the epoxy resin is epoxy resin E-44; the curing agent is 650 low molecular weight polyamide; the solvent is acetone; the wetting and dispersing agent is TEGO Dispers 655; the antioxidant is antioxidant 1010; and the leveling agent is BY-333 leveling agent; Step S8: Add epoxy resin, moisture-resistant epoxy resin, moisture-resistant reinforcing agent, solvent, wetting and dispersing agent, antioxidant and leveling agent to a mixer, and stir and react for 20 minutes at a temperature of 20℃ and a stirring speed of 2000r / min to obtain coating base material; Step S9: When using, add the curing agent to the coating base and stir evenly to obtain a moisture-resistant epoxy resin coating.
[0029] Example 2:
[0030] This embodiment describes a method for preparing a moisture- and heat-resistant epoxy resin coating, comprising the following steps: Step S1: 10 mmol of triphenylamine, 30 mmol of N-bromosuccinimide, and 45 mL of tetrahydrofuran were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred at 3 °C and 250 r / min for 25 min. Then, the temperature was raised to 55 °C and the mixture was stirred for another 4.5 h. After the reaction was completed, the product was cooled to room temperature and then poured into a saturated sodium thiosulfate solution. The product was then extracted twice with dichloromethane, and the extracts were combined and dried with anhydrous sodium sulfate. The product was then filtered under vacuum, and the solvent was removed by rotary evaporation of the filtrate. The product was then recrystallized from an ethyl acetate / petroleum ether mixture in a volume ratio of 7.5:1 to obtain the tribromotriphenylamine compound. Step S2: 10 mmol of tribromotriphenylamine compound, 38 mmol of 2,3-difluoro-4-butoxyphenylboronic acid, 55 mmol of potassium carbonate, 0.011 g of palladium chloride, and 105 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Nitrogen gas was introduced for protection, and the reaction was stirred at 22 °C and 250 r / min for 25 min. Then, the temperature was raised to 85 °C and the reaction was stirred for 1.5 h. After that, the temperature was raised to 135 °C and the reaction was stirred for 4.5 h. After the reaction was completed, the reaction product was cooled to room temperature, then vacuum filtered, and the filter cake was washed twice with distilled water. Then, it was placed in a vacuum drying oven and dried at 65 °C for 4 h to obtain butoxyfluorotriphenylamine compound. Step S3: 10 mmol of butoxy-fluorinated triphenylamine compound, 42 mmol of boron tribromide, 22 mmol of aluminum chloride and 105 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Nitrogen gas was introduced for protection. The mixture was stirred and reacted for 12 h at 22 °C and 250 r / min. After the reaction was completed, the reaction product was poured into distilled water and allowed to stand for separation. The organic phase was dried with anhydrous sodium sulfate and then filtered under vacuum. The solvent was removed by rotary evaporation of the filtrate and then recrystallized with N,N-dimethylformamide to obtain the polyhydroxy fluorinated triphenylamine compound. Step S4: Add 3g of polyhydroxy fluorinated triphenylamine compound, 0.45g of benzyltriethylammonium chloride and 45g of epichlorohydrin to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 22℃ and 250r / min for 15min. Then raise the temperature to 105℃ and continue stirring for 4h. Then lower the temperature to 55℃ and add 11mL of 32% sodium hydroxide solution and continue stirring for 3.5h. After the reaction is complete, cool the reaction product to room temperature, then vacuum filter. Wash the filtrate twice with distilled water, then dry with anhydrous sodium sulfate, then vacuum filter again. Rotary evaporate the filtrate to remove the solvent, and obtain a moisture-resistant epoxy resin. Step S5: Add 11 mL of deionized water, 5.5 mL of propanol, 1.5 mL of acetonitrile, and 0.25 g of tetraethylammonium hydroxide to a four-necked flask equipped with a stirrer, thermometer, reflux condenser, constant pressure dropping funnel, and gas delivery tube. Purge with nitrogen for protection and stir the reaction at 22 °C and 250 r / min for 15 min. Then, while stirring, add 22 g of γ-aminopropyltriethoxysilane dropwise at a rate of 2 drops / s. After the addition is complete, raise the temperature to 55 °C and continue stirring for 25 h. After the reaction is complete, cool the reaction product to room temperature, then remove the solvent by rotary evaporation. Wash twice with distilled water and cyclohexane, and then freeze-dry to obtain amination POSS. Step S6: Add 0.5g of graphene oxide TNGO-3 and 290mL of dimethyl sulfoxide to the reaction vessel, purge with nitrogen for protection, and stir for 25min at 22℃ and 250r / min. Then add 6g of aminated POSS and 2.0g of paraformaldehyde and continue stirring for 25min. Then raise the temperature to 175℃ and continue stirring for 25h. After the reaction is completed, cool the reaction product to room temperature, centrifuge, wash the precipitate twice with distilled water, and freeze dry to obtain the moisture and heat resistance enhancer. Step S7: Weigh out 28 parts by weight of epoxy resin, 6 parts by weight of moisture-resistant epoxy resin, 37 parts by weight of curing agent, 1.1 parts by weight of moisture-resistant reinforcing agent, 22 parts by weight of solvent, 0.4 parts by weight of wetting and dispersing agent, 0.3 parts by weight of antioxidant, and 0.2 parts by weight of leveling agent, and set aside; the epoxy resin is epoxy resin E-44; the curing agent is 650 low molecular weight polyamide; the solvent is acetone; the wetting and dispersing agent is TEGO Dispers 655; the antioxidant is antioxidant 1010; and the leveling agent is BY-333 leveling agent; Step S8: Add epoxy resin, moisture-resistant epoxy resin, moisture-resistant reinforcing agent, solvent, wetting and dispersing agent, antioxidant and leveling agent to a mixer, and stir and react for 25 minutes at a temperature of 22℃ and a stirring speed of 2500r / min to obtain coating base material; Step S9: When using, add the curing agent to the coating base and stir evenly to obtain a moisture-resistant epoxy resin coating.
[0031] Example 3:
[0032] This embodiment describes a method for preparing a moisture- and heat-resistant epoxy resin coating, comprising the following steps: Step S1: 10 mmol of triphenylamine, 30 mmol of N-bromosuccinimide and 50 mL of tetrahydrofuran were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Nitrogen gas was introduced for protection. The mixture was stirred at 5 °C and 300 r / min for 30 min. Then the temperature was raised to 60 °C and the mixture was stirred for 6 h. After the reaction was completed, the reaction product was cooled to room temperature and poured into a saturated sodium thiosulfate solution. The product was then extracted three times with dichloromethane. The extracts were combined and dried with anhydrous sodium sulfate. The product was then filtered under vacuum. The solvent was removed by rotary evaporation of the filtrate. The product was then recrystallized from an ethyl acetate / petroleum ether mixture in a volume ratio of 8:1 to obtain the tribromotriphenylamine compound. Step S2: 10 mmol of tribromotriphenylamine compound, 40 mmol of 2,3-difluoro-4-butoxyphenylboronic acid, 60 mmol of potassium carbonate, 0.12 g of palladium chloride, and 110 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred at 25 °C and a stirring rate of 300 r / min for 30 min. The temperature was then raised to 90 °C and the mixture was stirred for 2 h. The temperature was then raised to 140 °C and the mixture was stirred for 6 h. After the reaction was completed, the reaction product was cooled to room temperature and then vacuum filtered. The filter cake was washed three times with distilled water and then placed in a vacuum drying oven and dried at 70 °C for 5 h to obtain butoxyfluorotriphenylamine compound. Step S3: 10 mmol of butoxy-fluorinated triphenylamine compound, 45 mmol of boron tribromide, 25 mmol of aluminum chloride and 110 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Nitrogen gas was introduced for protection. The mixture was stirred and reacted for 15 h at 25 °C and a stirring rate of 300 r / min. After the reaction was completed, the reaction product was poured into distilled water and allowed to stand for separation. The organic phase was dried with anhydrous sodium sulfate and then vacuum filtered. The solvent was removed by rotary evaporation of the filtrate. The filtrate was then recrystallized with N,N-dimethylformamide to obtain the polyhydroxy fluorinated triphenylamine compound. Step S4: Add 3g of polyhydroxy fluorinated triphenylamine compound, 0.5g of benzyltriethylammonium chloride and 50g of epichlorohydrin to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 25℃ and 300r / min for 20min. Then raise the temperature to 110℃ and continue stirring for 5h. Then lower the temperature to 60℃ and add 12mL of 35% sodium hydroxide solution and continue stirring for 4h. After the reaction is completed, cool the reaction product to room temperature and then filter under vacuum. Wash the filtrate three times with distilled water and then dry it with anhydrous sodium sulfate. After vacuum filtration, remove the solvent by rotary evaporation of the filtrate to obtain a moisture-resistant epoxy resin. Step S5: Add 12 mL of deionized water, 6 mL of propanol, 2 mL of acetonitrile, and 0.3 g of tetraethylammonium hydroxide to a four-necked flask equipped with a stirrer, thermometer, reflux condenser, constant pressure dropping funnel, and gas delivery tube. Purge with nitrogen for protection and stir the reaction at 25 °C and a stirring rate of 300 r / min for 20 min. Then, while stirring, add 25 g of γ-aminopropyltriethoxysilane dropwise at a rate of 3 drops / s. After the addition is complete, raise the temperature to 60 °C and continue stirring for 30 h. After the reaction is complete, cool the reaction product to room temperature, then remove the solvent by rotary evaporation. Wash the product three times with distilled water and cyclohexane, and then freeze-dry to obtain amination-modified POSS. Step S6: Add 0.5g of graphene oxide TNGO-3 and 300mL of dimethyl sulfoxide to the reaction vessel, purge with nitrogen for protection, and stir for 30min at 25℃ and 300r / min. Then add 9g of aminated POSS and 2.2g of paraformaldehyde and continue stirring for 30min. Then raise the temperature to 180℃ and continue stirring for 30h. After the reaction is completed, cool the reaction product to room temperature, centrifuge, wash the precipitate three times with distilled water, and freeze-dry to obtain the moisture and heat resistance enhancer. Step S7: Weigh out 30 parts by weight of epoxy resin, 11 parts by weight of moisture-resistant epoxy resin, 38 parts by weight of curing agent, 1.7 parts by weight of moisture-resistant reinforcing agent, 25 parts by weight of solvent, 0.5 parts by weight of wetting and dispersing agent, 0.4 parts by weight of antioxidant, and 0.3 parts by weight of leveling agent, and set aside; the epoxy resin is epoxy resin E-44; the curing agent is 650 low molecular weight polyamide; the solvent is acetone; the wetting and dispersing agent is TEGO Dispers 655; the antioxidant is antioxidant 1010; and the leveling agent is BY-333 leveling agent; Step S8: Add epoxy resin, moisture-resistant epoxy resin, moisture-resistant reinforcing agent, solvent, wetting and dispersing agent, antioxidant and leveling agent to a mixer, and stir and react for 30 minutes at a temperature of 25℃ and a stirring speed of 3000r / min to obtain coating base material; Step S9: When using, add the curing agent to the coating base and stir evenly to obtain a moisture-resistant epoxy resin coating.
[0033] Comparative Example 1: This comparative example illustrates a method for preparing a moisture- and heat-resistant epoxy resin coating, comprising the following steps: Step S1: Weigh out 30 parts by weight of epoxy resin, 38 parts by weight of curing agent, 25 parts by weight of solvent, 0.5 parts by weight of wetting and dispersing agent, 0.4 parts by weight of antioxidant, and 0.3 parts by weight of leveling agent, and set aside; the epoxy resin is epoxy resin E-44; the curing agent is 650 low molecular weight polyamide; the solvent is acetone; the wetting and dispersing agent is TEGO Dispers 655; the antioxidant is antioxidant 1010; and the leveling agent is BY-333 leveling agent; Step S2: Add epoxy resin, solvent, wetting and dispersing agent, antioxidant and leveling agent to a mixer, and stir and react for 30 minutes at a temperature of 25℃ and a stirring speed of 3000r / min to obtain coating base material; Step S3: When using, add the curing agent to the coating base and stir evenly to obtain a moisture-resistant epoxy resin coating.
[0034] Comparative Example 2: This comparative example illustrates a method for preparing a moisture- and heat-resistant epoxy resin coating, comprising the following steps: Step S1: 10 mmol of triphenylamine, 30 mmol of N-bromosuccinimide and 50 mL of tetrahydrofuran were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Nitrogen gas was introduced for protection. The mixture was stirred at 5 °C and 300 r / min for 30 min. Then the temperature was raised to 60 °C and the mixture was stirred for 6 h. After the reaction was completed, the reaction product was cooled to room temperature and poured into a saturated sodium thiosulfate solution. The product was then extracted three times with dichloromethane. The extracts were combined and dried with anhydrous sodium sulfate. The product was then filtered under vacuum. The solvent was removed by rotary evaporation of the filtrate. The product was then recrystallized from an ethyl acetate / petroleum ether mixture in a volume ratio of 8:1 to obtain the tribromotriphenylamine compound. Step S2: 10 mmol of tribromotriphenylamine compound, 40 mmol of 2,3-difluoro-4-butoxyphenylboronic acid, 60 mmol of potassium carbonate, 0.12 g of palladium chloride, and 110 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred at 25 °C and a stirring rate of 300 r / min for 30 min. The temperature was then raised to 90 °C and the mixture was stirred for 2 h. The temperature was then raised to 140 °C and the mixture was stirred for 6 h. After the reaction was completed, the reaction product was cooled to room temperature and then vacuum filtered. The filter cake was washed three times with distilled water and then placed in a vacuum drying oven and dried at 70 °C for 5 h to obtain butoxyfluorotriphenylamine compound. Step S3: 10 mmol of butoxy-fluorinated triphenylamine compound, 45 mmol of boron tribromide, 25 mmol of aluminum chloride and 110 mL of dichloromethane were added to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Nitrogen gas was introduced for protection. The mixture was stirred and reacted for 15 h at 25 °C and a stirring rate of 300 r / min. After the reaction was completed, the reaction product was poured into distilled water and allowed to stand for separation. The organic phase was dried with anhydrous sodium sulfate and then vacuum filtered. The solvent was removed by rotary evaporation of the filtrate. The filtrate was then recrystallized with N,N-dimethylformamide to obtain the polyhydroxy fluorinated triphenylamine compound. Step S4: Add 3g of polyhydroxy fluorinated triphenylamine compound, 0.5g of benzyltriethylammonium chloride and 50g of epichlorohydrin to a three-necked flask equipped with a stirrer, thermometer, reflux condenser and gas delivery tube. Purge with nitrogen for protection and stir at 25℃ and 300r / min for 20min. Then raise the temperature to 110℃ and continue stirring for 5h. Then lower the temperature to 60℃ and add 12mL of 35% sodium hydroxide solution and continue stirring for 4h. After the reaction is completed, cool the reaction product to room temperature and then filter under vacuum. Wash the filtrate three times with distilled water and then dry it with anhydrous sodium sulfate. After vacuum filtration, remove the solvent by rotary evaporation of the filtrate to obtain a moisture-resistant epoxy resin. Step S5: Weigh out 30 parts by weight of epoxy resin, 11 parts by weight of moisture-resistant epoxy resin, 38 parts by weight of curing agent, 25 parts by weight of solvent, 0.5 parts by weight of wetting and dispersing agent, 0.4 parts by weight of antioxidant, and 0.3 parts by weight of leveling agent, and set aside; the epoxy resin is epoxy resin E-44; the curing agent is 650 low molecular weight polyamide; the solvent is acetone; the wetting and dispersing agent is TEGO Dispers 655; the antioxidant is antioxidant 1010; and the leveling agent is BY-333 leveling agent; Step S6: Add epoxy resin, moisture-resistant epoxy resin, solvent, wetting and dispersing agent, antioxidant and leveling agent to a mixer, and stir and react for 30 minutes at a temperature of 25℃ and a stirring speed of 3000r / min to obtain the coating base material. Step S7: When using, add the curing agent to the coating base and stir evenly to obtain a moisture-resistant epoxy resin coating.
[0035] Comparative Example 3: This comparative example illustrates a method for preparing a moisture- and heat-resistant epoxy resin coating, comprising the following steps: Step S1: 12 mL of deionized water, 6 mL of propanol, 2 mL of acetonitrile, and 0.3 g of tetraethylammonium hydroxide were added to a four-necked flask equipped with a stirrer, thermometer, reflux condenser, constant pressure dropping funnel, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred at 25 °C and a stirring rate of 300 r / min for 20 min. Then, 25 g of γ-aminopropyltriethoxysilane was added dropwise while stirring, with the dropping rate controlled at 3 drops / s. After the addition was completed, the temperature was raised to 60 °C and the reaction was stirred for another 30 h. After the reaction was completed, the reaction product was cooled to room temperature, and the solvent was removed by rotary evaporation. The product was then washed three times with distilled water and cyclohexane, and then freeze-dried to obtain amination POSS. Step S2: Add 0.5g of graphene oxide TNGO-3 and 300mL of dimethyl sulfoxide to the reaction vessel, purge with nitrogen for protection, and stir for 30min at 25℃ and 300r / min. Then add 9g of aminated POSS and 2.2g of paraformaldehyde and continue stirring for 30min. Then raise the temperature to 180℃ and continue stirring for 30h. After the reaction is completed, cool the reaction product to room temperature, centrifuge, wash the precipitate three times with distilled water, and freeze-dry to obtain the moisture and heat resistance enhancer. Step S3: Weigh out 30 parts by weight of epoxy resin, 38 parts by weight of curing agent, 1.7 parts by weight of moisture-heat resistant reinforcing agent, 25 parts by weight of solvent, 0.5 parts by weight of wetting and dispersing agent, 0.4 parts by weight of antioxidant, and 0.3 parts by weight of leveling agent, and set aside; the epoxy resin is epoxy resin E-44; the curing agent is 650 low molecular weight polyamide; the solvent is acetone; the wetting and dispersing agent is TEGO Dispers 655; the antioxidant is antioxidant 1010; and the leveling agent is BY-333 leveling agent; Step S4: Add epoxy resin, moisture-heat resistant reinforcing agent, solvent, wetting and dispersing agent, antioxidant and leveling agent to a mixer, and stir and react for 30 minutes at a temperature of 25℃ and a stirring speed of 3000r / min to obtain coating base material; Step S5: When using, add the curing agent to the coating base and stir evenly to obtain a moisture-resistant epoxy resin coating.
[0036] Performance testing The moisture-resistant epoxy resin coatings of Examples 1-3 and Comparative Examples 1-3 were applied to tinplate with a thickness of 100 μm. The coatings were cured at room temperature and the pencil hardness of the coatings was measured. The tinplate containing the coatings was then immersed in distilled water for 48 hours to observe the coating condition. The coatings were weighed and placed in a constant temperature and humidity aging test chamber for 21 days of moisture aging at 100°C and 85% humidity. After being naturally drained for 12 hours, the coatings were weighed again. The water absorption rate was measured by (weight after immersion - weight before immersion) / weight before immersion × 100%.
[0037] The test results are shown in the table below:
[0038] Referring to the data in the table above, and based on the comparison between Examples 1-3 and Comparative Examples 1-3, it can be seen that adding moisture-resistant epoxy resin and moisture-resistant reinforcing agent can significantly improve the water resistance and moisture-resistant properties of epoxy resin coatings.
[0039] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0040] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in this application, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing a moisture- and heat-resistant epoxy resin coating, characterized in that, Includes the following steps: Step 1: Weigh out 25-30 parts of epoxy resin, 1-11 parts of moisture-resistant epoxy resin, 36-38 parts of curing agent, 0.5-1.7 parts of moisture-resistant reinforcing agent, 20-25 parts of solvent, 0.3-0.5 parts of wetting and dispersing agent, 0.2-0.4 parts of antioxidant, and 0.1-0.3 parts of leveling agent according to the following proportions, and set aside. Step 2: Stir and react the epoxy resin, moisture-heat resistant epoxy resin, moisture-heat resistant reinforcing agent, solvent, wetting and dispersing agent, antioxidant, and leveling agent to obtain the coating base material; Step 3: When using, add the curing agent to the coating base and stir evenly to obtain a moisture-resistant and heat-resistant epoxy resin coating; The moisture- and heat-resistant epoxy resin is prepared by the following steps: Step a1: Triphenylamine, N-bromosuccinimide and tetrahydrofuran were stirred and reacted. After the reaction was completed, the reaction product was cooled and then poured into a saturated sodium thiosulfate solution. The product was then extracted, the extracts were combined and dried, then vacuum filtered, the filtrate was evaporated by rotary evaporation, and then recrystallized to obtain tribromotriphenylamine compound. Step a2: Tribromotriphenylamine compound, 2,3-difluoro-4-butoxyphenylboronic acid, potassium carbonate, palladium chloride and N,N-dimethylformamide were stirred and reacted. After the reaction was completed, the reaction product was cooled and then filtered under vacuum. The filter cake was washed and dried to obtain butoxyfluorotriphenylamine compound. Step a3: The butoxy-fluorinated triphenylamine compound, boron tribromide, aluminum chloride and dichloromethane were stirred and reacted. After the reaction was completed, the reaction product was poured into distilled water, then allowed to stand and separate into layers. The organic phase was dried, then vacuum filtered, the filtrate was evaporated by rotary evaporation, and then recrystallized to obtain the polyhydroxy fluorinated triphenylamine compound. Step a4: The polyhydroxy fluorinated triphenylamine compound, benzyltriethylammonium chloride and epichlorohydrin are stirred and reacted. Then sodium hydroxide solution is added and the reaction is continued. After the reaction is completed, the reaction product is cooled and then vacuum filtered. The filtrate is washed and dried, then vacuum filtered again and the filtrate is rotary evaporated to obtain a moisture-resistant epoxy resin.
2. The method for preparing a moisture- and heat-resistant epoxy resin coating according to claim 1, characterized in that, The epoxy resin is epoxy resin E-44; The curing agent is 650 low molecular weight polyamide; The solvent is acetone; The wetting and dispersing agent is TEGO Dispers 655; The antioxidant is antioxidant 1010; The leveling agent is BY-333 leveling agent.
3. The method for preparing a moisture- and heat-resistant epoxy resin coating according to claim 1, characterized in that, The ratio of triphenylamine, N-bromosuccinimide, and tetrahydrofuran in step a1 is 10 mmol: 30 mmol: 40-50 mL.
4. The method for preparing a moisture- and heat-resistant epoxy resin coating according to claim 1, characterized in that, The ratio of the tribromotriphenylamine compound, 2,3-difluoro-4-butoxyphenylboronic acid, potassium carbonate, palladium chloride, and N,N-dimethylformamide used in step a2 is 10 mmol: 35-40 mmol: 50-60 mmol: 0.01-0.12 g: 100-110 mL.
5. The method for preparing a moisture- and heat-resistant epoxy resin coating according to claim 1, characterized in that, The ratio of the butoxy-fluorinated triphenylamine compound, boron tribromide, aluminum chloride, and dichloromethane used in step a3 is 10 mmol: 40-45 mmol: 20-25 mmol: 100-110 mL.
6. The method for preparing a moisture- and heat-resistant epoxy resin coating according to claim 1, characterized in that, In step a4, the ratio of the polyhydroxy fluorinated triphenylamine compound, benzyltriethylammonium chloride, epichlorohydrin, and sodium hydroxide solution is 3g:0.4-0.5g:40-50g:10-12mL; the mass fraction of the sodium hydroxide solution is 30-35%.
7. The method for preparing a moisture- and heat-resistant epoxy resin coating according to claim 1, characterized in that, The moisture-heat resistance enhancer is prepared by the following steps: Step b1: Deionized water, propanol, acetonitrile and tetraethylammonium hydroxide were stirred and reacted. Then γ-aminopropyltriethoxysilane was added and the reaction was stirred and reacted. After the reaction was completed, the reaction product was cooled, then rotary evaporated, then washed, and then freeze-dried to obtain aminated POSS. Step b2: Graphene oxide and dimethyl sulfoxide are stirred and reacted, then aminated POSS and paraformaldehyde are added and the reaction is continued. After the reaction is completed, the reaction product is cooled, then centrifuged, the precipitate is washed, and then freeze-dried to obtain the moisture and heat resistance enhancer.
8. The method for preparing a moisture- and heat-resistant epoxy resin coating according to claim 7, characterized in that, The ratio of deionized water, propanol, acetonitrile, tetraethylammonium hydroxide and γ-aminopropyltriethoxysilane used in step b1 is 10-12 mL: 5-6 mL: 1-2 mL: 0.2-0.3 g: 20-25 g.
9. The method for preparing a moisture- and heat-resistant epoxy resin coating according to claim 7, characterized in that, The ratio of graphene oxide, dimethyl sulfoxide, aminated POSS, and paraformaldehyde in step b2 is 0.5g: 280-300mL: 3-9g: 1.8-2.2g.