A low-density thermal protective coating, its preparation method and application

Through the synergistic effect of components such as hydroxyl-terminated silicone rubber and glass microspheres, combined with the condensation reaction of hydrogen-containing silicone oil, the density of the thermal protective coating is reduced while its toughness and adhesion strength are improved. This solves the problems of high density and high cost of existing coatings, and achieves low-cost, high-performance thermal protection.

CN123063069APending Publication Date: 2026-11-10BEIJING JIUTIANXINGGE AEROSPACE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611302064.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing thermal protective coatings have excessive density, high cost, and poor thermal protection performance, making it difficult to meet the requirements of low density, low thermal conductivity, and high toughness for spacecraft.

Method used

The coating uses hydroxyl-terminated silicone rubber, glass microspheres, alkali-free glass fiber, high-temperature resistant fillers, and other components, combined with hydrogen-containing silicone oil and crosslinking agents. Through condensation reaction, the density is reduced and the toughness and adhesion strength of the coating are improved. Hydrophobic silica is used to increase the physicochemical adsorption sites and construct a stable three-dimensional network structure.

Benefits of technology

Low-density thermal protective coatings have been developed at low cost, with density reduced to below 0.75 g/cm3, tensile strength greater than 2.0 MPa, high bonding strength, and cost only 1/10 of commercially available products, meeting the safety requirements of spacecraft.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063069A_ABST
    Figure CN123063069A_ABST
Patent Text Reader

Abstract

This invention provides a low-density thermal protective coating, comprising components A, B, C, and a solvent. Component A includes hydroxyl-terminated silicone rubber, a reinforcing agent, silicone resin, glass microspheres, alkali-free glass fiber, and high-temperature resistant filler. Component B is hydrogen-containing silicone oil. Component C includes a crosslinking agent and a catalyst. The low-density thermal protective coating provided by this invention significantly reduces the coating density while maintaining tensile strength, improves the coating's adhesion strength to aluminum alloys, titanium alloys, and stainless steel, and greatly enhances the coating's toughness, ensuring that the spacecraft does not crack or detach during aerodynamic heating and erosion during ascent. Furthermore, the preparation method of the low-density thermal protective coating provided by this invention is easy to operate and low-cost, facilitating large-scale commercial application. It has already been applied to the instrument compartment, nose cone, inverted cone section, nose cone, booster tail section, and interstage section of spacecraft, providing strong technical support for obtaining safer and more reliable thermal protection for high-payload spacecraft.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of special thermal protective coatings technology, and in particular relates to a low-density thermal protective coating, its preparation method and application. Background Technology

[0002] With the rapid development of the aerospace industry, spacecraft have seen significant improvements in flight speed, maneuverability, load-bearing capacity, and safety performance. Under normal flight conditions, the environmental heating of a spacecraft consists of both convection and radiation, with radiation heating playing a relatively minor role; convection heating of the gas is the primary factor. During high-speed flight, the overall structure of a spacecraft typically faces a harsh aerodynamic heating environment. To achieve good aerodynamic characteristics, most spacecraft adopt a sharp aerodynamic shape at the nose, which results in a high aerodynamic heat flux density during flight. Excessive aerodynamic heat flux density can have serious multi-dimensional impacts on the sharp structure, internal equipment, and flight safety of the spacecraft. Developing a low-density, low-thermal-conductivity, tough, high-bonding-strength, and easy-to-apply thermal protective coating has always been a key research and application focus worldwide. Glass microspheres, possessing high compressive strength, extremely low thermal conductivity, chemical stability, corrosion resistance, and excellent insulation properties, are commonly used in the fabrication of lightweight aerospace components. Hydrogen-containing silicone oils are a class of organosilicon polymers containing active silicon-hydrogen bonds in their molecules, and are typically used as crosslinking agents under suitable conditions. Currently, my country's private commercial aerospace industry is still in its early stages of development, and the development of aerospace products is primarily market-oriented. Therefore, developing a lower-cost thermal protective coating while ensuring high toughness, high strength, and low density is of great significance. Summary of the Invention

[0003] The purpose of this invention is to provide a low-density thermal protective coating, its preparation method, and its application, so as to solve the technical problems of excessively high production costs, excessively high density of thermal protective coatings, and poor thermal protection performance in the prior art.

[0004] To solve the above-mentioned technical problems, the present invention provides a low-density thermal protection coating, wherein the thermal protection coating comprises component A, component B, component C, and solvent;

[0005] Component A specifically includes: 100 parts of hydroxyl-terminated silicone rubber, 10-50 parts of reinforcing agent, 0-10 parts of organosilicon resin, 20-60 parts of glass microspheres, 10-40 parts of alkali-free glass fiber, and 10-40 parts of high-temperature resistant filler.

[0006] Component B is 1-15 parts of hydrogen-containing silicone oil;

[0007] Component C specifically includes: 1-20 parts of crosslinking agent and 1-10 parts of catalyst;

[0008] The solvent is 25-150 parts;

[0009] The reinforcing agent is hydrophobic silica;

[0010] The hydrogen content of the hydrogen-containing silicone oil is 0.35%-1.6%; the hydrogen in the hydrogen-containing silicone oil can be in the chain or at the chain end.

[0011] All components are listed in parts by mass.

[0012] The main chain of macromolecular hydroxyl-terminated silicone rubber has a highly compliant -Si-O- structure, and the molecular chain can rotate freely, absorbing impact energy and significantly improving the mechanical strength and impact toughness of the coating. On the other hand, the terminal hydroxyl groups of macromolecular hydroxyl-terminated silicone rubber can also have a synergistic effect with hydrogen-containing silicone oil. That is, under the reaction conditions provided in this application, the terminal hydroxyl groups can undergo a condensation reaction with hydrogen to generate hydrogen gas, thereby further reducing the density of the coating film.

[0013] Furthermore, the molecular weight of the hydroxyl-terminated silicone rubber is 10,000 to 1,000,000;

[0014] Preferably, the hydroxyl-terminated silicone rubber is hydroxyl-terminated methyl silicone rubber and / or hydroxyl-terminated methylphenyl silicone rubber;

[0015] The molecular weight of the silicone resin is 3000-6000.

[0016] Both macromolecular silicone rubber and organosilicon resin have high specific heat capacity, and can effectively absorb heat during thermal decomposition, phase change and sublimation, thus playing a role in thermal protection.

[0017] Furthermore, the specific surface area of ​​the hydrophobic silica is ≥150 m² / g; the pH value is 6-8.

[0018] Preferably, the hydrophobic silica is selected from hydrophobically modified fumed silica and hydrophobically modified nano silica.

[0019] Under the premise of the same amount of addition, using hydrophobic silica with a larger specific surface area can, on the one hand, increase the number of active sites on the surface of hydrophobic silica particles, increase the probability of physicochemical adsorption, facilitate the construction of a more stable three-dimensional network structure, and improve the mechanical strength of the coating; on the other hand, it can reduce the particle size of hydrophobic silica, increase the gap between particles, and reduce the density of the coating.

[0020] Furthermore, the glass microspheres are a mixture of one or more types of glass microspheres selected from low-density glass microspheres, medium-density glass microspheres, and high-density glass microspheres;

[0021] The density of the low-density glass microspheres is 0.10 g / cm³ to 0.15 g / cm³.

[0022] The density of the medium-density glass microspheres is 0.20 g / cm³ to 0.29 g / cm³.

[0023] The density of the high-density glass microspheres is 0.30 g / cm3-0.39 g / cm3.

[0024] Using glass microspheres as fillers can effectively reduce coating density. When glass microspheres with a particle size ≤20μm are used as fillers, the microspheres are densely packed, which is beneficial for enhancing coating strength, but the coating density is relatively high. Preferably, a mixture of glass microspheres with large, medium, and small particle sizes is used as fillers. The larger glass microspheres have more gaps between them, which can effectively reduce the coating density, while the smaller glass microspheres can fill some of the gaps to ensure that the coating strength is not significantly reduced.

[0025] Furthermore, the glass microspheres are unmodified glass microspheres and / or modified glass microspheres;

[0026] The modified glass microspheres are selected from amino-modified glass microspheres, epoxy-modified glass microspheres, and methyl-modified glass microspheres.

[0027] Using surface-treated modified glass microspheres can improve the tensile strength of coatings and the tensile-shear strength of metal bonding components. Therefore, modified glass microspheres are preferred.

[0028] Furthermore, the diameter of the single filament of the alkali-free glass fiber is 10μm-14μm;

[0029] Furthermore, the alkali-free glass fiber is unmodified glass fiber and / or silane-modified glass fiber.

[0030] Preferably, the alkali-free glass fiber is silane-modified chopped glass fiber.

[0031] The use of glass fiber in coatings can effectively provide support for silicone rubber and decomposition products during heating, and slow down the deformation of the coating due to heat.

[0032] Furthermore, the high-temperature resistant filler is one or more of the following: zirconium oxide powder, alumina powder, titanium dioxide powder, quartz powder, mullite powder, ferric oxide powder, zinc oxide powder, mica powder, and silicon carbide powder.

[0033] Furthermore, the crosslinking agent is selected from silane coupling agents, titanate coupling agents, aluminate coupling agents, siloxane coupling agents, and hydrogen-containing silazanes;

[0034] The catalyst is one or more of the following: dibutyltin dilaurate, dibutyltin diacetate, dioctyltin dilaurate, dimethyltin dioleate, stannous isooctanoate, stannous isodecanoate, and stannous isooctanoate.

[0035] The solvent is one or more of the following: n-heptane, gasoline, butyl acetate, ethyl acetate, and xylene.

[0036] The present invention also provides a method for preparing the above-mentioned thermal protective coating, wherein the specific steps of the preparation method are as follows:

[0037] Step 1: Take 100 parts of hydroxyl-terminated silicone rubber, 10-50 parts of reinforcing agent, 0-10 parts of organosilicon resin, 10-40 parts of alkali-free glass fiber, and 10-40 parts of high-temperature resistant filler, mix them, and after grinding and dispersing, add solvent to adjust the viscosity to obtain a reinforcing mixture.

[0038] Step 2: Take 20-60 parts of the glass microspheres and mix them with the reinforcing mixture. After high-speed dispersion, add solvent to adjust the viscosity to obtain component A mixture.

[0039] Step 3: Take 1-20 parts of crosslinking agent and 1-10 parts of catalyst and stir thoroughly to obtain component B mixture;

[0040] Step 4: Take 1-15 parts of hydrogen-containing silicone oil and mix it with the mixture of component A and component B. Add solvent to adjust the viscosity and stir at a speed of 200 rpm to 1000 rpm for 5-15 minutes to obtain the thermal protective coating.

[0041] All components are listed in parts by mass.

[0042] Adding glass microspheres after the reinforcing mixture has been ground and dispersed can prevent the glass microspheres from being crushed by the three-roll mill during the grinding process, allowing the glass microspheres to better exert their function of reducing coating density and improving tensile strength and shear strength.

[0043] On the other hand, the present invention also provides an application of the above-mentioned thermal protective coating or the thermal protective coating obtained by the above preparation method, wherein the thermal protective coating is applied to the aluminum alloy substrate of the instrument compartment, nose cap, inverted cone section, nose cone, booster tail section, and interstage section of a spacecraft.

[0044] The coating method is selected from spraying, scraping, and brushing.

[0045] The thickness of a single coating layer is 200μm-400μm; the interval between each layer is 15-60min.

[0046] The curing temperature of the coating is 20℃-70℃; the curing time is 12h-15h.

[0047] To ensure that the hydrogen gas generated by the condensation reaction between the hydroxyl-terminated silicone rubber and the hydrogen-containing silicone oil does not damage the coating and can be smoothly discharged, a thin-coat, multi-layer spraying method is preferred to achieve the specified coating thickness.

[0048] By adopting the above technical solution, the present invention has the following beneficial effects:

[0049] This invention provides a low-density thermal protective coating, comprising component A, component B, component C, and solvent. Component A includes hydroxyl-terminated silicone rubber, a reinforcing agent, silicone resin, glass microspheres, alkali-free glass fiber, and high-temperature resistant filler. Component B is hydrogen-containing silicone oil. Component C includes a crosslinking agent and a catalyst. Through the combined use of glass microspheres and glass fiber, a synergistic effect is achieved, reducing the coating's density while improving its tensile strength, and also enhancing its adhesion strength to aluminum alloys, titanium alloys, and stainless steel substrates. This invention also creatively employs high-molecular-weight hydroxyl-terminated silicone rubber, which not only significantly improves the coating's toughness but also undergoes a condensation reaction with the crosslinking agent, hydrogen-containing silicone oil, releasing hydrogen gas and achieving a synergistic effect, further reducing the coating's density while ensuring optimal overall performance. Furthermore, the preparation method of the low-density thermal protective coating provided by this invention is low-cost and easy to operate, facilitating large-scale production and providing strong technical support for obtaining safer and more reliable thermal protection for heavy-load spacecraft. Attached Figure Description

[0050] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0051] Figure 1 This is an image showing the appearance of the thermal protective coating obtained in Example 1 applied to an aluminum alloy substrate.

[0052] Figure 2 This is a schematic diagram showing the appearance change of sample 1 after 2 minutes of ablation in a flame ablation experiment.

[0053] Figure 3 This is a schematic diagram showing the appearance changes of sample 1 after 6 minutes of ablation in a flame ablation experiment.

[0054] Figure 4 This is a schematic diagram of the bending experiment of test sample 1. Detailed Implementation

[0055] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0056] The present invention will be further explained below with reference to specific embodiments.

[0057] The low-density thermal protective coating is prepared using the method provided by this invention. The specific steps are as follows:

[0058] Step 1: Take 100 parts of hydroxyl-terminated silicone rubber, 10-50 parts of hydrophobic silica, 0-10 parts of organosilicon resin, 10-40 parts of alkali-free glass fiber, and 10-40 parts of high-temperature resistant filler, mix them, grind and disperse them through a three-roll mill, add solvent to adjust the viscosity, and obtain a reinforcing mixture.

[0059] The molecular weight of hydroxyl-terminated silicone rubber is 10,000 to 1,000,000; hydroxyl-terminated silicone rubber is hydroxyl-terminated methyl silicone rubber and / or hydroxyl-terminated methylphenyl silicone rubber.

[0060] The molecular weight of silicone resin is 3000-6000;

[0061] The specific surface area of ​​hydrophobic silica is ≥150 m² / g;

[0062] The diameter of a single filament of alkali-free glass fiber is 10μm-14μm;

[0063] The high-temperature resistant filler is one or more of the following: zirconium oxide powder, alumina powder, titanium dioxide powder, quartz powder, mullite powder, ferric oxide powder, zinc oxide powder, mica powder, and silicon carbide powder.

[0064] Step 2: Take 20-60 parts of glass microspheres and mix them with the reinforcing mixture. After high-speed dispersion, add solvent to adjust the viscosity to obtain component A mixture.

[0065] The glass microspheres are one or more mixtures of unmodified glass microspheres, amino-modified glass microspheres, epoxy-modified glass microspheres, and methyl-modified glass microspheres.

[0066] Step 3: Take 1-20 parts of crosslinking agent and 1-10 parts of catalyst and stir thoroughly to obtain component B mixture;

[0067] The crosslinking agent is selected from silane coupling agents, titanate coupling agents, aluminate coupling agents, siloxane coupling agents, and hydrogen-containing silazane;

[0068] The catalyst is one or more of the following: dibutyltin dilaurate, dibutyltin diacetate, dioctyltin dilaurate, dimethyltin dioleate, stannous isooctanoate, stannous isodecanoate, and stannous isooctanoate-decanoate.

[0069] Step 4: Take 1-15 parts of hydrogen-containing silicone oil and mix it with mixture of component A and mixture of component B. Add solvent to adjust the viscosity and stir at a speed of 200 rpm to 1000 rpm for 5-15 minutes to obtain a heat-protective coating.

[0070] Hydrogen-containing silicone oils have a hydrogen content of 0.35%-1.6%;

[0071] The solvent is one or more of the following: n-heptane, gasoline, butyl acetate, ethyl acetate, and xylene.

[0072] All components are listed in parts by mass.

[0073] Example 1

[0074] This embodiment demonstrates the preparation of a low-density thermal protective coating using the method provided by this invention.

[0075] Step 1: Weigh 1 kg of hydroxyl-terminated polydimethylsiloxane with a molecular weight of 583,000, 0.3 kg of hydrophobic silica H2000, 0.2 kg of chopped glass fiber, and 0.1 kg of titanium dioxide, mix them evenly, and then add ethyl acetate to adjust the viscosity after grinding evenly through a three-roll mill to obtain a reinforcing mixture.

[0076] Step 2: Take 0.4 kg of low-density unmodified glass microspheres, mix them with the reinforcing mixture, add ethyl acetate to adjust the viscosity, and stir at high speed of 1000 r / min for 1 h to obtain component A mixture;

[0077] Step 3: Weigh 0.1 kg of tetraethyl orthosilicate and 0.04 kg of tin dibutyl dilaurate, mix and stir evenly to obtain component B mixture;

[0078] Step 4: Weigh 0.4 kg of component A mixture, mix it with 0.01 kg of hydrogen-containing silicone oil with a hydrogen content of 1.6%, add butyl acetate to adjust the viscosity, stir evenly, then add 0.12 kg of component B mixture, stir evenly to obtain a low-density thermal protective coating.

[0079] Example 2

[0080] Step 1: Weigh 1 kg of hydroxyl-terminated polydimethylsiloxane with a molecular weight of 122,000, 0.2 kg of hydrophobic silica H2000, 0.2 kg of chopped glass fiber, 0.1 kg of sericite, and 0.1 kg of silicone resin, mix them evenly, and then add butyl acetate to adjust the viscosity after grinding evenly with a three-roll mill to obtain a reinforcing mixture.

[0081] Step 2: Take 0.25 kg of low-density unmodified glass microspheres, 0.13 kg of medium-density unmodified glass microspheres, and 0.02 kg of high-density unmodified glass microspheres, mix them with the reinforcing mixture, add butyl acetate to adjust the viscosity, and stir at 1000 r / min for 1 h to obtain component A mixture;

[0082] Step 3: Weigh 0.1 kg of tetraethyl orthosilicate and 0.04 kg of tin dibutyl dilaurate, mix and stir evenly to obtain component B mixture;

[0083] Step 4: Weigh 0.4 kg of component A mixture, mix it with 0.01 kg of hydrogen-containing silicone oil with a hydrogen content of 1.6%, add butyl acetate to adjust the viscosity, stir evenly, then add 0.06 kg of component B mixture, stir evenly to obtain a low-density thermal protective coating.

[0084] Example 3

[0085] Step 1: Weigh 1 kg of hydroxyl-terminated polydimethylsiloxane with a molecular weight of 341,000, 0.25 kg of hydrophobic silica H2000, 0.2 kg of chopped glass fiber, 0.1 kg of iron oxide, 0.1 kg of titanium dioxide, and 0.05 kg of hydroxyl silicone oil DT-2, mix them evenly, and then add gasoline to adjust the viscosity after uniform grinding through a three-roll mill to obtain a reinforcing mixture.

[0086] Step 2: Take 0.4 kg of low-density amino-modified glass microspheres, mix them with the reinforcing mixture, add gasoline to adjust the viscosity, and stir at high speed of 1000 r / min for 1 h to obtain component A mixture;

[0087] Step 3: Weigh 0.1 kg of tetraethyl orthosilicate, 0.02 kg of tin dibutyl dilaurate, and 0.02 kg of stannous isooctanoate, mix and stir evenly to obtain component B mixture;

[0088] Step 4: Weigh 0.4 kg of component A mixture, mix it with 0.01 kg of hydrogen-containing silicone oil with a hydrogen content of 1.6%, add gasoline to adjust the viscosity, stir evenly, then add 0.08 kg of component B mixture, stir evenly to obtain a low-density thermal protective coating.

[0089] Example 4

[0090] This embodiment verifies the effect of glass microsphere modification on the performance of low-density thermal protective coatings.

[0091] The preparation steps of the low-density thermal protective coating in this embodiment are basically the same as those in Example 1. The difference is that in step 2, 0.4 kg of low-density glass microspheres modified with KH550 are used to obtain the low-density thermal protective coating.

[0092] Example 5

[0093] As attached Figure 1 - Appendix Figure 4 As shown, this embodiment uses the low-density thermal protective coating obtained in Example 1 for spraying and verifies its performance.

[0094] Step S1: Take the aluminum alloy substrate of the launch vehicle stage section, wipe it clean with degreased gauze soaked in acetone, and spray the primer PR1200 onto the aluminum alloy substrate in an environment of not less than 20°C, and cure for 24 hours.

[0095] Step S2: Weigh 500g of the low-density thermal protection coating obtained in Example 1, adjust the viscosity of the coating with ethyl acetate to achieve 30s-40s in a Forco 4 cup, and then filter the diluted low-density thermal protection coating through a 40-mesh metal filter to obtain the low-density thermal protection coating for later use.

[0096] Step S3: In an environment not lower than 20℃, use a compressed air spray gun to spray the prepared low-density thermal protective coating onto the aluminum alloy substrate coated with a primer in multiple applications. The thickness of each spray is 200μm-400μm, with an interval of 15-60 minutes between each spray. After the total film thickness reaches 4mm, cure for 72 hours to obtain the desired result. Figure 1 The test sample 1 shown is shown.

[0097] Tests showed that the coating had a specific heat capacity of 1500 J / kgK; a linear ablation rate of 0.030 mm / s at 800℃ and 300 Pa; a density of only 0.66 g / cm3; a Shore A hardness of 73; a tensile strength of 2.9 MPa; a thermal conductivity of 0.16 W / mK; and a tensile-shear strength of 2.7 MPa for the bonded aluminum alloy specimen.

[0098] A flame ablation experiment was conducted on test sample 1 obtained in this embodiment: Test sample 1 was placed in the flame of a liquefied natural gas stove for ablation, and the changes in appearance were observed and recorded. (See attached...) Figure 2 As shown, after being burned in a flame for 2 minutes, test sample 1 showed no obvious changes in appearance, without cracking or peeling; as shown in the attached image. Figure 3 As shown, another test sample 1 was ablated in a flame for 6 minutes, and its appearance remained intact, without cracking or peeling, with only a small amount of powdering on the surface. The aerodynamic heating high-temperature phase during the actual launch of a carrier rocket typically lasts only a few tens of seconds. From the above experimental results, it can be seen that the low-density thermal protective coating provided by this invention fully meets the safety requirements of spacecraft.

[0099] A bending test was conducted on the remaining portion of test sample 1: as shown in the attached diagram. Figure 4 As shown, when the material is folded at nearly 180°, the coating does not break, proving that the low-density thermal protective coating provided by this invention has excellent toughness.

[0100] Example 6

[0101] This embodiment verifies the effect of glass microsphere density on the performance of low-density thermal protective coatings.

[0102] The experimental steps in this embodiment are basically the same as those in Embodiment 5, except that the low-density thermal protective coatings obtained in Embodiments 2-4 are used to spray aluminum alloy substrates to obtain test samples, which are labeled as Test Sample 2, Test Sample 3, and Test Sample 4, respectively. The performance test results of Test Samples 1-4 are listed in Table 1 below:

[0103] Table 1. Test results of various performance parameters for samples 1-4

[0104] Test sample Bending test Shore A hardness Coating density (g / cm3) Tensile strength (MPa) Thermal conductivity W / mK Tensile shear strength (MPa) 1 180° without breaking 73 0.66 2.9 0.16 2.7 2 90° without breaking 60 0.56 2.4 0.13 2.6 3 90° without breaking 63 0.56 2.5 0.14 2.6 4 180° without breaking 73 0.66 3.1 0.16 2.9

[0105] As can be seen from the test results in Table 1, the tensile and shear strengths of test sample 4 are significantly higher than those of test sample 1. This fully demonstrates that, under the premise that other components remain unchanged, adding amino-modified glass microspheres to the coating can increase the tensile strength of the coating and the tensile and shear strength of the metal bonded specimen.

[0106] Regarding tensile strength, sample 1 > sample 3 > sample 2. This is because both modified fumed silica and hydroxyl-terminated silicone rubber significantly improve the tensile strength of the coating. Under otherwise unchanged conditions, the higher the amount of modified fumed silica added, the higher the tensile strength of the resulting coating; appropriately increasing the molecular weight of the added hydroxyl-terminated silicone rubber can also improve the tensile strength of the coating.

[0107] In the bending test, we can see that test samples 1 and 4 both used hydroxyl-terminated polydimethylsiloxane with a molecular weight as high as 538,000, and the resulting coatings showed significantly better toughness than the other test samples. This proves that appropriately increasing the molecular weight of the added hydroxyl-terminated rubber can not only improve the tensile strength of the coating, but also effectively improve its toughness.

[0108] In summary, this invention provides a low-density thermal protective coating comprising component A, component B, component C, and solvent. Component A includes hydroxyl-terminated silicone rubber, reinforcing agent, silicone resin, glass microspheres, alkali-free glass fiber, and high-temperature resistant filler. Component B is hydrogen-containing silicone oil. Component C includes a crosslinking agent and a catalyst. Through the combined use of glass microspheres and glass fiber, a synergistic effect is achieved, reducing the coating's density while improving its tensile strength, and also enhancing its adhesion strength to aluminum alloys, titanium alloys, and stainless steel. This invention also creatively employs hydroxyl-terminated silicone rubber, which not only significantly improves the coating's toughness but also undergoes a condensation reaction with the hydrogen-containing silicone oil (acting as a crosslinking agent) to release hydrogen gas, further reducing the coating's density while ensuring optimal overall performance. The low-density thermal protective coating provided by this invention has a density not exceeding 0.75 g / cm³, a tensile strength greater than 2.0 MPa, an adhesion strength greater than 2.0 MPa to aluminum alloys, titanium alloys, and stainless steel, and a Shore A hardness not less than 60. All performance tests show significant improvements over commercially available similar products. In addition, the cost of commercially available similar thermal protective coatings is 2,000-3,000 yuan / kg, while the thermal protective coating prepared according to the method provided by this invention not only has better comprehensive performance, but also costs only 100-200 yuan / kg. It has the characteristics of low cost and easy operation, which is conducive to large-scale production. It has made a great contribution to improving quality and reducing costs in the thermal protective coating industry, and provided strong technical support for obtaining safer and more reliable thermal protection for heavy-load spacecraft.

[0109] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A low-density thermal protective coating, characterized in that, The thermal protective coating comprises component A, component B, component C, and solvent; Component A specifically includes: 100 parts of hydroxyl-terminated silicone rubber, 10-50 parts of reinforcing agent, 0-10 parts of organosilicon resin, 20-60 parts of glass microspheres, 10-40 parts of alkali-free glass fiber, and 10-40 parts of high-temperature resistant filler. Component B is 1-15 parts of hydrogen-containing silicone oil; Component C specifically includes: 1-20 parts of crosslinking agent and 1-10 parts of catalyst; The solvent is 25-150 parts; The reinforcing agent is hydrophobic silica; The hydrogen content of the hydrogen-containing silicone oil is 0.35%-1.6%; All components are listed in parts by mass.

2. The thermal protective coating according to claim 1, characterized in that, The molecular weight of the hydroxyl-terminated silicone rubber is 10,000 to 1,000,000. The hydroxyl-terminated silicone rubber is hydroxyl-terminated methyl silicone rubber and / or hydroxyl-terminated methylphenyl silicone rubber; The molecular weight of the silicone resin is 3000-6000.

3. The thermal protective coating according to claim 1, characterized in that, The specific surface area of ​​the hydrophobic silica is ≥150 m² / g.

4. The thermal protective coating according to claim 1, characterized in that, The glass microspheres are a mixture of one or more types of glass microspheres selected from low-density glass microspheres, medium-density glass microspheres, and high-density glass microspheres; The density of the low-density glass microspheres is 0.10 g / cm³ to 0.15 g / cm³. The density of the medium-density glass microspheres is 0.20 g / cm³ to 0.29 g / cm³. The density of the high-density glass microspheres is 0.30 g / cm3-0.39 g / cm3.

5. The thermal protective coating according to claim 4, characterized in that... The glass microspheres are unmodified glass microspheres and / or modified glass microspheres; The modified glass microspheres are selected from amino-modified glass microspheres, epoxy-modified glass microspheres, and methyl-modified glass microspheres.

6. The thermal protective coating according to claim 1, characterized in that, The alkali-free glass fiber has a single filament diameter of 10μm-14μm; The alkali-free glass fiber is unmodified glass fiber and / or silane-modified glass fiber.

7. The thermal protective coating according to claim 1, characterized in that, The high-temperature resistant filler is one or more of the following: zirconium oxide powder, alumina powder, titanium dioxide powder, quartz powder, mullite powder, ferric oxide powder, zinc oxide powder, mica powder, and silicon carbide powder.

8. The thermal protective coating according to claim 1, characterized in that, The crosslinking agent is selected from silane coupling agents, titanate coupling agents, aluminate coupling agents, siloxane coupling agents, and hydrogen-containing silazane; The catalyst is one or more of the following: dibutyltin dilaurate, dibutyltin diacetate, dioctyltin dilaurate, dimethyltin dioleate, stannous isooctanoate, stannous isodecanoate, and stannous isooctanoate. The solvent is one or more of the following: n-heptane, gasoline, butyl acetate, ethyl acetate, and xylene.

9. A method for preparing a thermal protective coating according to any one of claims 1-8, characterized in that, The specific steps of the preparation method are as follows: The following components are all in parts by mass; Step 1: Take 100 parts of hydroxyl-terminated silicone rubber, 10-50 parts of reinforcing agent, 0-10 parts of organosilicon resin, 10-40 parts of alkali-free glass fiber, and 10-40 parts of high-temperature resistant filler, mix them, and after grinding and dispersing, add solvent to adjust the viscosity to obtain a reinforcing mixture. Step 2: Take 20-60 parts of the glass microspheres and mix them with the reinforcing mixture. After high-speed dispersion, add solvent to adjust the viscosity to obtain component A mixture. Step 3: Take 1-20 parts of crosslinking agent and 1-10 parts of catalyst and stir thoroughly to obtain component B mixture; Step 4: Take 1-15 parts of hydrogen-containing silicone oil and mix it with the mixture of component A and component B. Add solvent to adjust the viscosity and stir at a speed of 200 rpm to 1000 rpm for 5-15 minutes to obtain the thermal protective coating.

10. The application of a thermal protective coating according to any one of claims 1-8 or a thermal protective coating obtained by the preparation method according to claim 9, characterized in that, The thermal protective coating is applied to the aluminum alloy substrate of the instrument compartment, nose cone, inverted cone section, nose cone, booster tail section, and interstage section of the spacecraft. The coating method is selected from spraying, scraping, and brushing. The thickness of a single coating layer is 200 μm-400 μm; the interval between each layer is 15-60 min. The curing temperature of the coating is 20℃-70℃; the curing time is 12h-15h.