A method for preparing a flame retardant for thermally conductive potting compound

By reacting aluminum hydroxide with silane and washing it before mixing it with boron nitride, the problem of powder agglomeration during the co-treatment of aluminum hydroxide and boron nitride was solved, thus improving the dispersibility and thermal conductivity of the thermally conductive potting compound.

CN123063097APending Publication Date: 2026-11-10YANTAI GRACE POLYMER MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611579259.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In existing technologies, when aluminum hydroxide and boron nitride are treated together with silane, dispersion and powder agglomeration during the silane reaction process are likely to occur, affecting the dispersion and processing performance of the thermally conductive potting compound.

Method used

First, aluminum hydroxide undergoes a silane surface reaction. Before adding boron nitride, it is washed, separated into solid and liquid components, and dried. Then, it is mixed with boron nitride in a solid state. During the mixing process, hydrolysis of hydrolyzable alkoxy groups and silanol condensation reactions are carried out, while controlling the amount of water and reaction conditions.

Benefits of technology

It effectively reduces the degree to which silane continues to participate in hydrolysis and condensation, improves the dispersibility and viscosity of composite powder, and enhances the thermal conductivity and flame retardant properties of thermally conductive potting compound.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063097A_ABST
    Figure CN123063097A_ABST
Patent Text Reader

Abstract

This invention relates to the field of thermally conductive and flame-retardant adhesive materials, and discloses a method for preparing a flame retardant for thermally conductive potting compounds. The method involves a surface reaction of aluminum hydroxide with a hydrolyzable silane coupling agent. The reactants are then washed, separated from solids, and dried to obtain an aluminum hydroxide intermediate containing hydrolyzable alkoxy groups. The hydrolyzable alkoxy groups in the washed and dried aluminum hydroxide intermediate are quantified. Then, plate-like boron nitride with hydroxyl groups on its surface is mixed with the aluminum hydroxide intermediate in a solid state. This invention first involves a silane surface reaction of aluminum hydroxide, and then washing, separating from solids, and drying the treated aluminum hydroxide before adding boron nitride. This reduces the amount of silane components that can be extracted again by organic solvents before the addition of boron nitride, thereby reducing the extent to which this portion of silane continues to enter subsequent mixing and aqueous treatment processes and participates in hydrolysis and condensation. This is beneficial for reducing the coarsening and agglomeration of the composite powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of thermally conductive and flame-retardant adhesive materials technology, specifically a method for preparing a flame retardant for thermally conductive potting compound. Background Technology

[0002] Thermally conductive potting compounds are used for potting, bonding, and insulating electronic devices, power modules, and battery components. To balance thermal conductivity and flame retardancy, inorganic fillers such as aluminum hydroxide and boron nitride are typically added to the adhesive matrix. Aluminum hydroxide absorbs heat and releases moisture when heated, while boron nitride has high thermal conductivity and electrical insulation properties. The combination of the two can meet both flame retardancy and thermal conductivity requirements.

[0003] As the amount of inorganic filler added increases, the interfacial compatibility between different fillers and between the filler and the adhesive matrix affects the flowability, filler dispersion, and thermal conductivity of the potting compound. Existing technologies typically employ silane coupling agents to surface-treat aluminum hydroxide and boron nitride. For example, CN102585506A discloses a method where a silane coupling agent is pre-hydrolyzed in a system composed of ethanol and water before being added to aluminum hydroxide and boron nitride for co-treatment; CN119570115B discloses a method where boron nitride and aluminum hydroxide are first mixed, and then a silane coupling agent is added to the mixed filler for surface treatment.

[0004] When silane coupling agents treat inorganic powders, alkoxyl hydrolysis, condensation between silanols, and reactions between silanols and hydroxyl groups on inorganic surfaces occur simultaneously. When aluminum hydroxide and boron nitride are present together from the beginning of silane treatment, silanes may simultaneously participate in reactions on different filler surfaces and in condensation between silanols. When silanes undergo significant hydrolysis and condensation before the addition of boron nitride, the number of hydrolyzable groups that can continue to participate in subsequent reactions is correspondingly reduced.

[0005] Furthermore, aluminum hydroxide, even after silane surface treatment, may still contain silane components that can be extracted again by organic solvents. These components, carried along with the aluminum hydroxide intermediate into subsequent mixing and aqueous treatment stages, may continue to undergo hydrolysis and condensation, increasing powder agglomeration and affecting the dispersion and processing performance of the resulting composite flame retardant in thermally conductive potting compounds. Summary of the Invention

[0006] This invention provides a method for preparing a flame retardant for thermally conductive potting compound, which has the beneficial effect of balancing thermal conductivity and flame retardancy. It solves the problem mentioned in the background art that dispersion and powder agglomeration easily occur during the silane reaction process when aluminum hydroxide and boron nitride are treated together.

[0007] This invention provides the following technical solution: a method for preparing a flame retardant for thermally conductive potting compound, wherein aluminum hydroxide is reacted with a hydrolyzable silane coupling agent on the surface, and the reactants are washed, separated from solids and liquids and dried to obtain an aluminum hydroxide intermediate containing hydrolyzable alkoxy groups; Quantitative analysis of hydrolyzable alkoxy groups in the washed and dried aluminum hydroxide intermediate; Boron nitride flakes with hydroxyl groups on their surface were mixed with aluminum hydroxide intermediate in a solid mixture at a mass ratio of 25:100 to 35:100. The water content of the aluminum hydroxide intermediate and boron nitride was measured before solid mixing. After the solids are mixed, water is introduced and mixing continues. During the mixing process, hydrolysis of hydrolyzable alkoxy groups and condensation of silanols occur. The reactants were dried to obtain a composite flame retardant for thermally conductive potting compound.

[0008] As an optional method for preparing a flame retardant for a thermally conductive potting compound according to the present invention, wherein: the hydrolyzable silane coupling agent is an organosilane coupling agent containing a trialkoxysilane group, and the amount of the hydrolyzable silane coupling agent is 1.0% to 3.0% of the mass of aluminum hydroxide.

[0009] As an optional method for preparing a flame retardant for a thermally conductive potting compound according to the present invention, the reactants after surface reaction are washed 2 to 3 times with anhydrous acetone, and the mass ratio of anhydrous acetone to solid material used in each wash is 1:1 to 3:1; after solid-liquid separation, they are vacuum dried at 50 to 70°C for 1 to 3 hours.

[0010] As an optional method for preparing a flame retardant for a thermally conductive potting compound according to the present invention, the content of hydrolyzable alkoxy groups is 0.08-0.25 mmol / g.

[0011] As an optional method for preparing a flame retardant for a thermally conductive potting compound according to the present invention, wherein the hydrolyzable alkoxy group is quantified by alcohol exchange and gas chromatography.

[0012] As an optional method for preparing a flame retardant for a thermally conductive potting compound according to the present invention, boron nitride is added to a 3-5 mol / L sodium hydroxide solution, treated at 80-95°C for 12-24 hours, washed with water until neutral, and then dried.

[0013] As an optional method for preparing a flame retardant for a thermally conductive potting compound according to the present invention, the surface reaction temperature is 55-65°C, the reaction time is 25-35 min, and the ratio of the molar amount of water added to the treatment solution used for the surface reaction to the molar amount of alkoxy groups contained in the hydrolyzable silane coupling agent is 0.15:1 to 0.45:1.

[0014] As an optional embodiment of the preparation method of the flame retardant for thermally conductive potting compound described in this invention, the total molar amount of water introduced by the two solid materials is determined according to the water content of the aluminum hydroxide intermediate and boron nitride, and the total molar amount of water introduced by the two solid materials is lower than the predetermined total molar amount of water; the predetermined total molar amount of water is 0.8 to 1.0 times the molar amount of hydrolyzable alkoxy groups; the amount of water added is determined according to the difference between the predetermined total molar amount of water and the total molar amount of water introduced by the two solid materials.

[0015] As an optional method for preparing a flame retardant for a thermally conductive potting compound according to the present invention, wherein: external water is added in an atomized manner within 10 to 30 minutes, and after the water is added, mixing is continued at 40 to 70°C for 20 to 60 minutes.

[0016] As an optional embodiment of the preparation method of the flame retardant for thermally conductive potting compound described in this invention, wherein the hydrolyzable silane coupling agent is vinyltrimethoxysilane.

[0017] The present invention has the following beneficial effects: 1. The preparation method of the flame retardant for thermally conductive potting compound involves first reacting aluminum hydroxide with silane on its surface, and then washing, separating solids and liquids, and drying the treated aluminum hydroxide before adding boron nitride. This reduces the amount of silane components that can be extracted again by organic solvents before the addition of boron nitride, thereby reducing the extent to which this portion of silane continues to enter the subsequent mixing and water-containing treatment processes and participates in hydrolysis and condensation. This is beneficial for reducing the coarsening and agglomeration of the composite powder.

[0018] 2. The preparation method of the flame retardant for thermally conductive potting compound involves adding boron nitride after completing the surface treatment and washing of aluminum hydroxide, and first mixing boron nitride with aluminum hydroxide intermediate in a solid state, followed by water treatment, thereby avoiding premature initiation of subsequent hydrolysis and condensation of hydrolyzable alkoxy groups before the addition of boron nitride. Attached Figure Description

[0019] Figure 1 This is a flowchart of the preparation method of the present invention. Detailed Implementation

[0020] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0021] Please see Figure 1This invention provides a method for preparing a flame retardant for thermally conductive potting compounds, which improves the problems of powder agglomeration that occur when aluminum hydroxide and boron nitride are treated together with silane, as well as the increase in viscosity and storage stratification of thermally conductive potting compounds under high filling conditions. Aluminum hydroxide was reacted with a hydrolyzable silane coupling agent on the surface. The reactants were washed, separated from solids and liquids and dried to obtain an aluminum hydroxide intermediate containing hydrolyzable alkoxy groups. Solid mixing of plate-shaped boron nitride with hydroxyl groups on its surface and aluminum hydroxide intermediate; After the solids are mixed, water is introduced and mixing continues. During the mixing process, hydrolysis of hydrolyzable alkoxy groups and condensation of silanols occur. The reactants were dried to obtain a composite flame retardant for thermally conductive potting compound.

[0022] The preferred mass ratio of boron nitride to aluminum hydroxide intermediate is 25:100 to 35:100. The hydrolyzable silane coupling agent is preferably an organosilane coupling agent containing a trialkoxysilane group, and the preferred amount is 1.0% to 3.0% of the mass of aluminum hydroxide.

[0023] The reactants after the surface reaction are preferably washed 2-3 times with anhydrous acetone, with the mass ratio of anhydrous acetone to solid material being 1:1 to 3:1 for each wash; after solid-liquid separation, they are vacuum dried at 50-70°C for 1-3 hours. The hydrolyzable alkoxy groups in the washed and dried aluminum hydroxide intermediate are preferably 0.08-0.25 mmol / g.

[0024] The preferred surface reaction temperature is 55–65°C, and the preferred reaction time is 25–35 min. The preferred ratio of the molar amount of water added to the treatment solution to the molar amount of alkoxy groups in the hydrolyzable silane coupling agent is 0.15:1–0.45:1. Here, the water amount refers to the actual amount of water added to the treatment solution, not the total water content of the surface reaction system. Aluminum hydroxide is preferably pre-dried before the surface reaction.

[0025] Boron nitride can be added to a 3-5 mol / L sodium hydroxide solution and treated at 80-95℃ for 12-24 hours, then washed with water until neutral and dried.

[0026] In the following examples, the amount of sodium hydroxide solution used is calculated as 20 mL per 1 g of boron nitride. The water content of the aluminum hydroxide intermediate and boron nitride was measured separately before mixing the solids. The predetermined total molar amount of water is preferably 0.8 to 1.0 times the molar amount of hydrolyzable alkoxy groups. When the total molar amount of water introduced by the two solid materials is lower than the predetermined total molar amount of water, the amount of water added is determined according to the difference between the predetermined total molar amount of water and the total molar amount of water introduced by the two solid materials.

[0027] When the total molar amount of water introduced by the two solid materials reaches or exceeds the predetermined total molar amount of water, one or both of the aluminum hydroxide intermediate and boron nitride are dried further, and the water content is re-measured; solid mixing is then carried out only when the total molar amount of water introduced by the two solid materials is lower than the predetermined total molar amount of water. The added water is preferably added via atomization over 10–30 minutes, and mixing continues at 40–70°C for 20–60 minutes after the water addition is complete.

[0028] By adopting the above processing sequence, aluminum hydroxide is first treated with silane and then washed before adding boron nitride. This can reduce the content of extractable silane components in the aluminum hydroxide intermediate, thereby reducing the amount of these components entering the subsequent boron nitride mixing and water treatment stages. By mixing boron nitride and aluminum hydroxide intermediates in a solid state followed by aqueous treatment, the hydrolysis and condensation of hydrolyzable alkoxy groups before the addition of boron nitride can be reduced. The resulting composite flame retardant, when used in thermally conductive potting compounds, improves powder dispersion, viscosity, and storage stratification under high-filling conditions, while also maintaining both thermal conductivity and flame retardant properties.

[0029] Specifically, before the second stage of water treatment, the present invention quantifies the hydrolyzable alkoxy groups in the washed and dried aluminum hydroxide intermediate, as well as the water introduced by the aluminum hydroxide intermediate and boron nitride. The predetermined total water amount is determined based on the amount of hydrolyzable alkoxy groups, and the amount of water already introduced by the two solid materials is deducted from the predetermined total water amount to determine the amount of water to be added. This ensures that the amount of water in the subsequent water treatment corresponds to the actual state of the intermediate, reducing powder coarsening and increased system viscosity caused by excessive water content.

[0030] Raw materials and testing methods: Aluminum hydroxide was used as powder with a D50 of approximately 12 μm. Flaky hexagonal boron nitride also had a D50 of approximately 12 μm; the same batch of boron nitride was used in all examples and comparative examples. Unless otherwise stated, the isopropanol used in the surface treatment solution was anhydrous isopropanol.

[0031] Hydrolyzable alkoxy groups were quantified using alcohol exchange and gas chromatography.

[0032] Weigh 0.50 g of washed and dried aluminum hydroxide intermediate, add 20 mL of anhydrous ethanol, seal and maintain at 60 °C for 24 h, then perform solid-liquid separation. Determine the alcohols in the liquid phase using gas chromatography with external standard method. When using vinyltrimethoxysilane, methanol is the primary quantitative target; if other corresponding alcohols formed by alkoxy exchange are detected simultaneously, their molar amounts are included, and the molar amount of hydrolyzable alkoxy groups per unit mass of aluminum hydroxide intermediate is calculated accordingly.

[0033] The water content of aluminum hydroxide intermediates and boron nitride was determined by the Karl Fischer furnace method at a furnace temperature of 105°C, and the same test endpoint criteria were used for all groups.

[0034] The method for determining extractable Si is as follows: 2.00 g of the composite flame retardant is added to 20 mL of anhydrous acetone, stirred at 25 °C for 30 min, and then filtered. A quantitative amount of the filtrate is placed in a sealed digestion container and oxidized and digested using nitric acid and hydrogen peroxide. After cooling, the volume is adjusted, and the Si content is determined by ICP-OES and converted to the extractable Si content per unit mass of the composite flame retardant.

[0035] The method for determining the dispersion D90 is as follows: 5 wt% of the composite flame retardant is added to vinyl silicone oil with a viscosity of 1000 ± 100 mPa·s at 25℃, and mixed at 1000 r / min for 5 min. Subsequently, the particle size distribution is determined using laser particle size distribution method, and the particle size D90 corresponding to the cumulative volume distribution reaching 90% is recorded. All samples use the same dispersion medium and pretreatment conditions.

[0036] The performance of the thermally conductive potting compound was evaluated using a standardized addition-type silicone adhesive system. The vinyl-terminated polydimethylsiloxane had a viscosity of 5000±500 mPa·s at 25°C, with a vinyl content of 0.18% by mass; the active hydrogen content in the hydrogen-containing silicone oil was 0.75% by mass. 100 parts by mass of vinyl-terminated polydimethylsiloxane and 220 parts by mass of a composite flame retardant were vacuum-mixed and degassed. The hydrogen-containing silicone oil was added at a Si-H to vinyl molar ratio of 1.15:1, and the platinum catalyst was added at 20 ppm (Pt). After mixing, the mixture was cured at 80°C for 60 min and then left to stand at room temperature for 24 h.

[0037] Viscosity at 25℃ was measured using a rotational rheometer at a shear rate of 10 s⁻¹; thermal conductivity was measured using the transient plane heat source method; 7-day stratification rate was calculated as the ratio of the height of the upper low-filled region formed after standing at 25℃ for 7 days to the total height of the sample; limiting oxygen index was measured according to GB / T 2406.2; vertical combustion performance was measured on a 3.2 mm thick sample according to GB / T 2408.

[0038] Example 1

[0039] Take 1000g of aluminum hydroxide, dry it at 105℃ for 2h, and cool it to 60℃. Prepare a surface treatment solution: 20g of vinyltrimethoxysilane, 80g of anhydrous isopropanol, 2.20g of water and 0.10g of glacial acetic acid. The molar ratio of water to methoxyl in the treatment solution is approximately 0.30:1.

[0040] The dried aluminum hydroxide was added to a mixer and stirred at 250 rpm. The surface treatment solution was added within 10 minutes, and the reaction was continued at 60°C for 30 minutes. The reactants were washed three times with anhydrous acetone at a mass ratio of 2:1 to solids each time, and filtered after each wash. After washing, the reactants were vacuum dried at 60°C for 2 hours. 1000 g of the obtained aluminum hydroxide intermediate was weighed for subsequent steps. The content of hydrolyzable alkoxy groups in the aluminum hydroxide intermediate was determined to be 0.160 mmol / g using the aforementioned alcohol exchange-gas chromatography method.

[0041] The washing procedure following the surface reaction of aluminum hydroxide is arranged before the addition of boron nitride to reduce the silane components in the aluminum hydroxide intermediate that can be extracted again by organic solvents.

[0042] 300g of flake-shaped hexagonal boron nitride was added to 6000mL of 4mol / L sodium hydroxide solution and treated at 90℃ for 18h. After washing with water until neutral, it was dried at 100℃ for 3h. The water content of the aluminum hydroxide intermediate and boron nitride was determined to be 0.10wt% and 0.12wt%, respectively, using the Karl Fischer furnace method.

[0043] 1000g of aluminum hydroxide intermediate contains 0.160 mol of hydrolyzable alkoxy groups. Based on a predetermined ratio of total water molars to hydrolyzable alkoxy molars of 0.90:1, the predetermined total water amount is 0.144 mol, or 2.59g. 1000g of aluminum hydroxide intermediate introduces approximately 1.00g of water, and 300g of boron nitride introduces approximately 0.36g of water, for a total of 1.36g of water introduced by the two solid materials. Therefore, the amount of water added is 1.23g.

[0044] 1000g of aluminum hydroxide intermediate and 300g of boron nitride were mixed in a solid state at 200 rpm for 20 min. 1.23g of water was atomized and added over 15 min, while maintaining mixing; then mixing was continued at 50℃ for 30 min. The reactants were vacuum dried at 80℃ for 3 h to obtain the composite flame retardant.

[0045] The resulting composite flame retardant has an extractable Si content of 34 μg / g and a dispersion D90 of 26.8 μm. When used in the aforementioned addition-type silicone thermally conductive potting compound system, it exhibits a viscosity of 35.6 Pa·s at 25°C, a thermal conductivity of 1.80 W / (m·K), a 7-day delamination rate of 1.0%, a limiting oxygen index of 31.8%, and a vertical flammability rating of V-0 for a 3.2 mm sample.

[0046] Example 2

[0047] The aluminum hydroxide intermediate was prepared, washed, and dried according to the method in Example 1, and 1000g was weighed; the amount of boron nitride was adjusted to 250g. Except for the amount of boron nitride, the surface reaction of aluminum hydroxide, washing, boron nitride treatment, solid mixing, and subsequent reaction conditions were the same as in Example 1.

[0048] The aluminum hydroxide intermediate contains 0.160 mmol / g of hydrolyzable alkoxy groups and 0.10 wt% water; 250g of boron nitride contains 0.12 wt% water. The total amount of water is 2.59g, the combined water introduced by the two solids is 1.30g, and the amount of added water is 1.29g.

[0049] The resulting composite flame retardant has an extractable Si content of 35 μg / g and a D90 of 24.9 μm. The corresponding thermally conductive potting compound has a viscosity of 33.8 Pa·s at 25℃, a thermal conductivity of 1.68 W / (m·K), a 7-day delamination rate of 1.1%, a limiting oxygen index of 32.4%, and a vertical flammability rating of V-0 for a 3.2 mm sample.

[0050] Example 3

[0051] The aluminum hydroxide intermediate was prepared, washed, and dried according to the method in Example 1, and 1000g was weighed; the amount of boron nitride was adjusted to 350g. Except for the amount of boron nitride, the other conditions were the same as in Example 1.

[0052] The aluminum hydroxide intermediate contained 0.160 mmol / g of hydrolyzable alkoxy groups and 0.10 wt% water; 350g of boron nitride contained 0.12 wt% water. The total amount of water was planned to be 2.59g, the water carried in by the two solids totaled 1.42g, and the amount of water added was 1.17g.

[0053] The resulting composite flame retardant has an extractable Si content of 35 μg / g and a D90 of 29.7 μm. The corresponding thermally conductive potting compound has a viscosity of 39.4 Pa·s at 25℃, a thermal conductivity of 1.91 W / (m·K), a 7-day delamination rate of 1.4%, a limiting oxygen index of 30.9%, and a vertical flammability rating of V-0 for a 3.2 mm sample.

[0054] Example 4

[0055] Except for the process parameters explicitly listed below, the aluminum hydroxide, hydrolyzable silane coupling agent, treatment solution addition method, washing method, boron nitride treatment method, solid mixing method, detection method, and final drying method used in Example 4 are all the same as those in Example 1.

[0056] Take 1000g of aluminum hydroxide, 1.2% vinyltrimethoxysilane (by mass of aluminum hydroxide), 80g of anhydrous isopropanol, 0.10g of glacial acetic acid, and 0.66g of water. Add water to the treatment solution at a molar ratio of approximately 0.15:1 for alkoxy groups, and react at 55℃ for 25 min. Wash the reactants twice with anhydrous acetone and dry under vacuum at 50℃ for 3 h. Weigh 1000g of the obtained aluminum hydroxide intermediate; the content of hydrolyzable alkoxy groups is 0.085 mmol / g.

[0057] Take 300g of boron nitride, add 6000mL of 3mol / L sodium hydroxide solution, treat at 80℃ for 12h, wash with water until neutral, and then dry. After further drying, the aluminum hydroxide intermediate and boron nitride together introduce 0.72g of water. Based on the predetermined total water molar amount being 0.80 times the molar amount of hydrolyzable alkoxy groups, the predetermined total water amount is 1.22g, and the added water amount is 0.50g. After mixing the solids, add 0.50g of water via atomization over 10min, continue mixing at 40℃ for 20min, and then dry.

[0058] The extracted Si of the obtained composite flame retardant is 39 μg / g, and the D90 is 29.4 μm. The corresponding thermally conductive potting compound has a viscosity of 38.1 Pa·s at 25℃, a thermal conductivity of 1.72 W / (m·K), a 7-day delamination rate of 1.6%, a limiting oxygen index of 31.2%, and a vertical burning rating of V-0 for a 3.2 mm sample.

[0059] Example 5

[0060] Except for the process parameters explicitly listed below, the conditions in Example 5 are the same as those in Example 1.

[0061] Take 1000g of aluminum hydroxide, 3.0% vinyltrimethoxysilane (by mass of aluminum hydroxide), 80g of anhydrous isopropanol, 0.10g of glacial acetic acid, and 4.92g of water. Add water to the treatment solution at a molar ratio of approximately 0.45:1 for alkoxy groups, and react at 65℃ for 35 min. Wash the reactants three times with anhydrous acetone and dry under vacuum at 70℃ for 1 h. Weigh 1000g of the obtained aluminum hydroxide intermediate; the content of hydrolyzable alkoxy groups is 0.245 mmol / g.

[0062] Take 300g of boron nitride, add 6000mL of 5mol / L sodium hydroxide solution, treat at 95℃ for 24h, wash with water until neutral, and then dry. The aluminum hydroxide intermediate and boron nitride together introduce 1.10g of water. Based on the predetermined total water molar ratio of 1.00:1 to the molar amount of hydrolyzable alkoxy groups, the predetermined total water amount is 4.41g, and the added water amount is 3.31g. After mixing the solids, add the 3.31g water via atomization over 30min, continue mixing at 70℃ for 60min, and then dry.

[0063] The extracted Si of the obtained composite flame retardant is 37 μg / g, and the D90 is 31.2 μm. The corresponding thermally conductive potting compound has a viscosity of 40.3 Pa·s at 25℃, a thermal conductivity of 1.76 W / (m·K), a 7-day delamination rate of 1.8%, a limiting oxygen index of 31.6%, and a vertical burning rating of V-0 for a 3.2 mm sample.

[0064] Comparative Example 1 Take 20g of vinyltrimethoxysilane and 80g of anhydrous isopropanol, add 8.0g of water, adjust the pH to 4.5 with glacial acetic acid, and stir at 25°C for 60min to obtain a pre-hydrolyzed solution. Add 1000g of pre-dried aluminum hydroxide and 300g of boron nitride that has been hydroxylated and dried using the same method as in Example 1, mix at 250r / min, and react at 60°C for 30min. Wash the reactants three times with anhydrous acetone, with the mass ratio of anhydrous acetone to solid material being 2:1 for each wash. After solid-liquid separation, vacuum dry at 60°C for 2h.

[0065] The obtained composite flame retardant has an extractable Si of 71 μg / g and a D90 of 41.6 μm; the corresponding thermally conductive potting compound has a viscosity of 48.7 Pa·s at 25℃, a thermal conductivity of 1.49 W / (m·K), a 7-day delamination rate of 3.4%, a limiting oxygen index of 31.2%, and a vertical burning rating of V-0.

[0066] Comparative Example 2 Take 1000g of pre-dried aluminum hydroxide and 300g of boron nitride that has been hydroxylated and dried using the same method as in Example 1, and mix them solidly at 200 rpm for 20 min. Prepare a treatment solution containing 20g of vinyltrimethoxysilane, 80g of anhydrous isopropanol, 2.20g of water, and 0.10g of glacial acetic acid. Add the mixed powder to the solution within 10 min, mix at 250 rpm, and react at 60°C for 30 min. Wash the reactants three times with anhydrous acetone, each time at a mass ratio of 2:1 between anhydrous acetone and solids. After solid-liquid separation, vacuum dry at 60°C for 2 h.

[0067] The obtained composite flame retardant has an extractable Si of 63 μg / g and a D90 of 38.7 μm; the corresponding thermally conductive potting compound has a viscosity of 45.5 Pa·s at 25℃, a thermal conductivity of 1.55 W / (m·K), a 7-day delamination rate of 2.9%, a limiting oxygen index of 31.4%, and a vertical burning rating of V-0.

[0068] Comparative Example 3 The surface reaction of aluminum hydroxide with vinyltrimethoxysilane was carried out according to Example 1, omitting anhydrous acetone washing, and directly vacuum dried at 60°C for 2 hours. 1000 g of the resulting treated powder was weighed, with a hydrolyzable alkoxy content of 0.185 mmol / g and a water content of 0.10 wt%. 300 g of boron nitride, treated in the same manner as in Example 1, with a water content of 0.12 wt%, was added. Based on a predetermined total water molar ratio of 0.90:1 to the hydrolyzable alkoxy molar ratio, the predetermined total water amount was 3.00 g, with 1.36 g of water introduced by the two solids, and 1.64 g of additional water added. The mixing, water supply, and drying conditions for the remaining solids were the same as in Example 1.

[0069] The obtained composite flame retardant has an extractable Si of 358 μg / g and a D90 of 50.4 μm; the corresponding thermally conductive potting compound has a viscosity of 58.6 Pa·s at 25℃, a thermal conductivity of 1.37 W / (m·K), a 7-day delamination rate of 5.6%, a limiting oxygen index of 31.3%, and a vertical burning rating of V-0.

[0070] Comparative Example 4 The washed and dried aluminum hydroxide intermediate was prepared according to Example 1. 1000g of the intermediate was weighed, and the hydrolyzable alkoxy content was 0.160 mmol / g, and the water content was 0.10 wt%. The total water content was controlled according to the predetermined total water content of 2.59g determined in Example 1, and the 0.36g of water introduced by the subsequent addition of 300g of boron nitride was included in the water content, so the total added water content was 1.23g.

[0071] First, 1.23g of water was atomized into 1000g of aluminum hydroxide intermediate within 15min, and the mixture was continued at 50℃ for 30min. Then, 300g of boron nitride that had been hydroxylated and dried in the same way as in Example 1 was added, and the mixture was mixed solid at 200r / min for 20min. Finally, the mixture was vacuum dried at 80℃ for 3h.

[0072] The extracted Si of the obtained composite flame retardant is 46 μg / g, and the D90 is 44.1 μm. The corresponding thermally conductive potting compound has a viscosity of 51.2 Pa·s at 25℃, a thermal conductivity of 1.41 W / (m·K), a 7-day delamination rate of 4.1%, a limiting oxygen index of 31.4%, and a vertical burning rating of V-0.

[0073] Comparative Example 5 The aluminum hydroxide surface reaction, washing, drying, boron nitride treatment, and solid mixing were carried out according to Example 1. The difference was that the total amount of water was calculated based on the molar amount of methoxy groups contained in the initial vinyltrimethoxysilane. 20g of vinyltrimethoxysilane contains approximately 0.405mol of methoxy groups, and calculated at 0.90 times, the total amount of water is approximately 6.56g. The aluminum hydroxide intermediate and boron nitride together introduce 1.36g of water, therefore the amount of water added is 5.20g. The method of adding the water and the subsequent mixing and drying conditions are the same as in Example 1.

[0074] The extracted Si of the obtained composite flame retardant is 44 μg / g, and the D90 is 55.6 μm. The corresponding thermally conductive potting compound has a viscosity of 62.1 Pa·s at 25℃, a thermal conductivity of 1.32 W / (m·K), a 7-day delamination rate of 6.0%, a limiting oxygen index of 31.1%, and a vertical burning rating of V-0.

[0075] Comparative Example 6 The treatment was carried out according to Example 1, except that the water introduced by the aluminum hydroxide intermediate and boron nitride was not deducted when calculating the amount of water added. 2.59 g of water was directly added at a ratio of 0.90 mol water / mol hydrolyzable alkoxy group; an additional 1.36 g of water was introduced by the two solid materials, resulting in a total water volume approximately 1.37 times the molar amount of the hydrolyzable alkoxy group. All other conditions were the same as in Example 1.

[0076] The obtained composite flame retardant has an extractable Si of 42 μg / g and a D90 of 30.2 μm; the corresponding thermally conductive potting compound has a viscosity of 39.2 Pa·s at 25℃, a thermal conductivity of 1.71 W / (m·K), a 7-day delamination rate of 1.5%, a limiting oxygen index of 31.5%, and a vertical burning rating of V-0.

[0077] Comparative Example 7 The treatment was carried out according to Example 1, with 1000g of aluminum hydroxide intermediate and 100g of boron nitride. The water content of the aluminum hydroxide intermediate was 0.10wt%, and the water content of the boron nitride was 0.12wt%, with a total water content of 1.12g from the two solids; the planned total water content remained 2.59g, and the added water content was 1.47g. All other conditions were the same as in Example 1.

[0078] The obtained composite flame retardant has an extractable Si of 34 μg / g and a D90 of 20.8 μm; the corresponding thermally conductive potting compound has a viscosity of 29.7 Pa·s at 25℃, a thermal conductivity of 1.34 W / (m·K), a 7-day delamination rate of 0.9%, a limiting oxygen index of 33.0%, and a vertical burning rating of V-0.

[0079] Comparative Example 8 Following the treatment in Example 1, the amount of aluminum hydroxide intermediate was 1000g, and the amount of boron nitride was adjusted to 500g. The water content of the aluminum hydroxide intermediate was 0.10wt%, and the water content of the boron nitride was 0.12wt%, with a total water content introduced by the two solids of 1.60g; the predetermined total water content remained 2.59g, and the amount of added water was 0.99g. All other conditions were the same as in Example 1.

[0080] The obtained composite flame retardant has an extractable Si of 35 μg / g and a D90 of 39.8 μm; the corresponding thermally conductive potting compound has a viscosity of 65.4 Pa·s at 25℃, a thermal conductivity of 1.93 W / (m·K), a 7-day delamination rate of 4.6%, a limiting oxygen index of 29.7%, and a vertical burning rating of V-1.

[0081] Test Results Summary Table 1: Test results of composite powders in each embodiment and comparative example.

[0082]

[0083] Table 2: Application performance of thermally conductive potting compounds in various examples and comparative examples.

[0084]

[0085] Results Analysis Example 1 and Comparative Example 1 used the same main raw materials. Comparative Example 1 used silane pre-hydrolysis followed by co-treatment with aluminum hydroxide and boron nitride, while Example 1 used aluminum hydroxide for silane surface reaction and washing, followed by the addition of boron nitride. Compared to Comparative Example 1, the D90 of Example 1 decreased from 41.6 μm to 26.8 μm, the viscosity of the thermally conductive potting compound at 25°C decreased from 48.7 Pa·s to 35.6 Pa·s, the 7-day delamination rate decreased from 3.4% to 1.0%, and the thermal conductivity increased from 1.49 W / (m·K) to 1.80 W / (m·K).

[0086] It should be noted that pH 4.5 in Comparative Example 1 is the process condition in its silane pre-hydrolysis treatment route. Example 1 and Comparative Example 1 are used to compare the differences in results obtained from the above different treatment routes, rather than to evaluate the single parameter pH.

[0087] The main difference between Example 1 and Comparative Example 2 is whether the two fillers are present simultaneously during silane surface treatment. In Comparative Example 2, aluminum hydroxide and boron nitride were mixed first and then uniformly treated with silane. Its D90, viscosity, and delamination rate were all higher than those of Example 1, while its thermal conductivity was lower than that of Example 1.

[0088] The difference between Example 1 and Comparative Example 3 is whether or not washing was performed after the reaction on the aluminum hydroxide surface. Without washing, the extractable Si increased from 34 μg / g to 358 μg / g, D90 increased from 26.8 μm to 50.4 μm, and the viscosity and delamination rate of the thermally conductive potting compound increased significantly. This indicates that washing before the addition of boron nitride affects the subsequent powder dispersion and adhesive application performance.

[0089] Example 1 and Comparative Example 4 mainly exchanged the order of boron nitride addition and water introduction, with both examples containing 1.23 g of water. Comparative Example 4 introduced water first and then added boron nitride, resulting in a D90 of 44.1 μm, a thermally conductive potting compound viscosity of 51.2 Pa·s, a delamination rate of 4.1%, and a thermal conductivity of 1.41 W / (m·K), all of which are significantly different from Example 1. This indicates that the order of the two process steps affects the final powder and adhesive properties.

[0090] The difference between Example 1 and Comparative Example 5 lies in the calculation basis of the predetermined total water amount. Example 1 was calculated based on the actual measured hydrolyzable alkoxy groups in the aluminum hydroxide intermediate after washing and drying, while Comparative Example 5 was calculated based on the methoxy groups contained in the initial silane feed amount; water introduced by the powder was deducted from both groups. In Comparative Example 5, after increasing the added water amount to 5.20 g, D90, viscosity, and stratification rate significantly increased, while the thermal conductivity decreased.

[0091] The difference between Example 1 and Comparative Example 6 lies in whether the water introduced by the two solid materials is included in the predetermined total water volume. In Comparative Example 6, 2.59g of water is added directly at a 0.90 equivalent, resulting in an actual total water volume of approximately 1.37 equivalents. In Example 1, after deducting the water introduced by the powder, 1.23g of water is added, further reducing its D90, viscosity, and stratification rate.

[0092] Examples 2, 1, and 3, using boron nitride to aluminum hydroxide intermediate mass ratios of 25:100, 30:100, and 35:100 respectively, all achieved a V-0 vertical combustion rating and maintained good overall performance in terms of thermal conductivity, viscosity, and stratification. In Comparative Example 7, reducing the mass ratio to 10:100 significantly decreased the thermal conductivity; in Comparative Example 8, increasing the ratio to 50:100 improved the thermal conductivity, but significantly increased the system viscosity and stratification rate, and lowered the vertical combustion rating to V-1.

[0093] The above results indicate that by organizing the reaction of aluminum hydroxide on the silane surface, washing, addition of boron nitride, solid mixing, and subsequent water treatment in a specific order, and by controlling the amount of water introduced by the hydrolyzable alkoxy groups of the intermediate and the solids, a composite flame retardant suitable for high-filling applications of thermally conductive potting compounds can be obtained.

[0094] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0095] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing a flame retardant for thermally conductive potting compound, characterized in that: Aluminum hydroxide was reacted with a hydrolyzable silane coupling agent on the surface. The reactants were washed, separated from solids and liquids and dried to obtain an aluminum hydroxide intermediate containing hydrolyzable alkoxy groups. Quantitative analysis of hydrolyzable alkoxy groups in the washed and dried aluminum hydroxide intermediate; Boron nitride flakes with hydroxyl groups on their surface were mixed with aluminum hydroxide intermediate in a solid mixture at a mass ratio of 25:100 to 35:

100. The water content of the aluminum hydroxide intermediate and boron nitride was measured before solid mixing. After the solids are mixed, water is introduced and mixing continues. During the mixing process, hydrolysis of hydrolyzable alkoxy groups and condensation of silanols occur. The reactants were dried to obtain a composite flame retardant for thermally conductive potting compound.

2. The method for preparing a flame retardant for thermally conductive potting compound according to claim 1, characterized in that: The hydrolyzable silane coupling agent is an organosilane coupling agent containing a trialkoxysilane group. The amount of hydrolyzable silane coupling agent used is 1.0% to 3.0% of the mass of aluminum hydroxide.

3. The method for preparing a flame retardant for thermally conductive potting compound according to claim 1, characterized in that: The reactants after the surface reaction were washed 2 to 3 times with anhydrous acetone, and the mass ratio of anhydrous acetone to solid material used in each wash was 1:1 to 3:

1. After solid-liquid separation, the mixture was vacuum dried at 50 to 70°C for 1 to 3 hours.

4. The method for preparing a flame retardant for thermally conductive potting compound according to claim 1, characterized in that: The content of hydrolyzable alkoxy groups is 0.08–0.25 mmol / g.

5. The method for preparing a flame retardant for thermally conductive potting compound according to claim 4, characterized in that: The hydrolyzable alkoxy groups were quantified using alcohol exchange and gas chromatography.

6. The method for preparing a flame retardant for thermally conductive potting compound according to claim 1, characterized in that: Boron nitride was added to a 3-5 mol / L sodium hydroxide solution and treated at 80-95℃ for 12-24 h. After washing with water until neutral, the solution was dried.

7. The method for preparing a flame retardant for thermally conductive potting compound according to claim 1, characterized in that: The surface reaction temperature is 55–65°C, the reaction time is 25–35 min, and the ratio of the molar amount of water added to the treatment solution used in the surface reaction to the molar amount of alkoxy groups contained in the hydrolyzable silane coupling agent is 0.15:1–0.45:

1.

8. The method for preparing a flame retardant for thermally conductive potting compound according to claim 4, characterized in that: The total molar amount of water introduced by the two solid materials is determined based on the water content of the aluminum hydroxide intermediate and boron nitride. The total molar amount of water introduced by the two solid materials is lower than the predetermined total molar amount of water. The predetermined total molar amount of water is 0.8 to 1.0 times the molar amount of hydrolyzable alkoxy groups. The amount of water added is determined according to the difference between the predetermined total molar amount of water and the total molar amount of water introduced by the two solid materials.

9. The method for preparing a flame retardant for thermally conductive potting compound according to claim 8, characterized in that: Add water via atomization over 10–30 minutes, and continue mixing at 40–70°C for 20–60 minutes after water addition is complete.

10. The method for preparing a flame retardant for a thermally conductive potting compound according to claim 2, characterized in that: The hydrolyzable silane coupling agent is vinyltrimethoxysilane.

Citation Information

Patent Citations

  • Silicon rubber with excellent electric arc resistant performance and preparation method thereof

    CN102585506A

  • Composite heat-conducting filler, preparation method thereof, heat-conducting silicone rubber, preparation method thereof and application of heat-conducting silicone rubber

    CN119570115B