A method and product for preventing cracking of large-section alloy steel through bainitic pretreatment.
By using intermittent rapid cooling and bainitic transformation treatment, the cracking problem in the pretreatment process of large-size mold steel was solved, achieving uniform microstructure and improved performance, simplifying the process flow and reducing energy consumption.
Patent Information
- Application Number
- CN202611481313.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies have problems with surface corner cracking or internal micro-cracks in the pretreatment of large-size mold steel. In particular, the cooling rate of the core of large-section forging billets is difficult to control precisely, which makes it easy for structural stress and thermal stress to cause cracking. Moreover, the process window is extremely narrow and the scrap rate is high.
An intermittent rapid cooling method was adopted to control the surface temperature of the large-section alloy steel workpiece to always be higher than the martensitic transformation start temperature. When the cooling ended, the surface temperature returned to below the upper limit temperature of the bainitic transformation zone. Isothermal heat preservation was carried out in the bainitic transformation temperature range to obtain the initial microstructure with bainite as the matrix.
It effectively reduces the structural stress caused by martensitic transformation, avoids the risk of cracking, achieves uniformity and stability of the microstructure, simplifies the subsequent spheroidizing annealing process, and improves the machinability and mechanical properties of the product.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of heat treatment processing technology for mold steel, and in particular to a method and product for preventing cracking bainitic pretreatment of large-section alloy steel. Background Technology
[0002] In the production of large-size mold steel, forged billets typically require preliminary annealing after forging to reduce hardness and facilitate machining. However, these billets often exhibit defects such as uneven intragranular carbide structure, continuous precipitation of network carbides along grain boundaries, and severe compositional segregation. To obtain a uniformly dispersed granular carbide structure to meet the requirements of high-end equipment manufacturing, pretreatment is usually performed before spheroidizing annealing.
[0003] Existing technologies generally employ a pretreatment process of "high-temperature normalizing + rapid cooling," which involves heating the forging billet to above the Acm temperature to austenitize it and then rapidly cooling it to obtain a martensitic structure, thereby suppressing the precipitation of network carbides. However, for large-section forging billets with a slab thickness greater than 400mm or a round billet diameter greater than 500mm, this process has significant drawbacks: Because the cooling rate of the core of a large-section forging billet is difficult to control precisely, the temperature difference between the surface and the core can easily exceed 200°C, generating huge structural and thermal stresses, which can cause surface corner cracks or internal microcracks. At the same time, in order to ensure that the core fully obtains martensite and significantly increases the cooling intensity, the risk of deformation and cracking will be further aggravated, resulting in an extremely narrow process window and a high scrap rate.
[0004] Therefore, there is an urgent need to develop a pretreatment method that can effectively eliminate structural inhomogeneities such as network carbides and fundamentally avoid the risk of cracking during the pretreatment process of large-size forging billets. Summary of the Invention
[0005] Based on the above analysis, the present invention aims to provide a method and product for anti-cracking bainitic pretreatment of large-section alloy steel, in order to solve at least one of the problems of network carbide precipitation, surface edge cracking or internal microcracks in existing large-size mold steel.
[0006] On the one hand, the present invention provides a method for preventing cracking bainitic pretreatment of large cross-section alloy steel, comprising the following steps: Step S1: Perform austenitizing treatment on the forged large-section alloy steel workpiece to obtain a high-temperature austenitic structure; Step S2: The austenitized large-section alloy steel workpiece is subjected to intermittent rapid cooling. During the cooling process, the surface temperature of the large-section alloy steel workpiece is controlled to always be higher than the martensitic transformation start temperature, and the surface temperature return is lower than the upper limit temperature of the bainitic transformation zone at the end of cooling, so that the core of the large-section alloy steel workpiece is cooled to below the pearlite transformation start temperature. Step S3: Place the cooled large-section alloy steel workpiece in the bainite transformation temperature range for isothermal heat preservation, so that the supercooled austenite completes the bainite transformation and obtains the initial bainite structure.
[0007] Furthermore, the large-section alloy steel workpiece is a large-size die steel forging billet with a slab thickness greater than 400mm or a round billet diameter greater than 500mm; the material of the large-size die steel forging billet is selected from any one of 4Cr5MoSiV1, 4Cr5MoSiV, 4Cr5Mo2SiV or 4Cr5Mo3SiV.
[0008] Furthermore, the intermittent rapid cooling in step S2 includes: alternating between water quenching and intermittent reheating, controlling the single water quenching time, so that the surface temperature of the large cross-section alloy steel workpiece fluctuates above the martensitic transformation initiation temperature, while simultaneously cooling the core of the large cross-section alloy steel workpiece to below the pearlitic transformation initiation temperature.
[0009] Further, preferably, the single water quenching cooling time is 4 min to 12 min; the number of alternating water quenching cooling and intermittent reheating is 5 to 10 times; the total liquid cooling time is 30 min to 120 min; so that the core of the large cross-section alloy steel workpiece is cooled to below 600°C, and the surface reheating temperature is below 450°C at the end of cooling.
[0010] Furthermore, the bainite transformation temperature range in step S3 is 325℃~420℃; the isothermal holding time is 8h~15h.
[0011] Further, the austenitizing treatment of the large-section alloy steel workpiece in step S1 includes: heating the large-section alloy steel workpiece to 800℃ at a heating rate of no more than 70℃ / h and holding it at that temperature for 2h~5h; continuing to heat it to the high-temperature austenitizing range at a heating rate of no more than 50℃ / h and holding it at that temperature; the high-temperature austenitizing range is Ac3+(50~100)℃, and the holding time is calculated based on 1.5min / mm × the effective thickness of the large-section alloy steel workpiece.
[0012] Furthermore, the initial bainitic microstructure obtained in step S3 is a microstructure with bainitic matrix and dispersed undissolved carbides.
[0013] Furthermore, after step S3, the process also includes: directly performing isothermal spheroidizing annealing on the large-section alloy steel workpiece.
[0014] On the other hand, the present invention also provides a large-section alloy steel product, wherein the large-section alloy steel product is pretreated by the anti-cracking bainitic pretreatment method for large-section alloy steel as described above.
[0015] Furthermore, the large-section alloy steel product has a network carbide grade ≤1, a core microstructure grade of AS2~AS4, a cross-sectional hardness range of 195HB~210HB, and an unnotched impact toughness greater than 300J.
[0016] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects: 1. The anti-cracking bainitic pretreatment method for large-section alloy steel provided by the present invention reduces the occurrence of surface martensite phase transformation by controlling the surface temperature of the workpiece to always be higher than the martensite transformation start temperature (Ms point) during intermittent rapid cooling. This greatly reduces the structural stress caused by the inconsistency between the volume expansion of martensite transformation and the shrinkage of austenite in the core, and solves the problem of easy cracking of large-section forging billets during rapid cooling to suppress carbide precipitation.
[0017] 2. In this invention, the surface temperature rises below the upper limit of the bainite transformation zone at the end of cooling, ensuring that the workpiece has avoided the carbide precipitation sensitive zone and is in a suitable bainite transformation initiation state before entering the isothermal stage. Combined with the subsequent isothermal holding in the bainite transformation temperature range, the supercooled austenite is fully transformed into a low-stress initial structure with bainite as the matrix, achieving both microstructure control and crack prevention, and providing an ideal microstructure basis for subsequent spheroidizing annealing.
[0018] 3. Intermittent rapid cooling alternates between water quenching and intermittent reheating, causing the workpiece surface temperature to fluctuate above the martensitic transformation initiation temperature. This ensures a sufficient cooling rate to suppress the precipitation of carbides along grain boundaries in the core, while the intermittent reheating releases accumulated thermal stress, further reducing the risk of cracking.
[0019] 4. During the bainitic transformation, carbides are dispersed and precipitated in the matrix, forming a microstructure with bainitic matrix and dispersed undissolved carbides. These dispersed carbides can be directly used as the nucleation substrate for spheroidizing in the subsequent spheroidizing annealing process. Compared with the processing path of carbon supersaturation solid solution in the martensitic route, which requires tempering to precipitate before spheroidizing, the pretreated workpiece of this invention has low internal stress and can directly enter the isothermal spheroidizing annealing process. The spheroidizing efficiency is higher and the carbide particle size distribution is more uniform, which improves the machinability and mechanical properties of the final product. At the same time, it simplifies the process flow and reduces energy consumption and production cycle.
[0020] 5. The large-section alloy steel products obtained by using the pretreatment method of this invention and combining it with subsequent spheroidizing annealing have a network carbide grade ≤1, a core microstructure grade of AS2~AS4, a cross-sectional hardness range of 195HB~210HB, and an unnotched impact toughness greater than 300J, thus achieving a comprehensive improvement in the hardness, toughness, and microstructure uniformity of the large-section alloy steel products.
[0021] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objectives and other advantages of this invention can be realized and obtained through the specific points highlighted in the description. Detailed Implementation
[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of the embodiments, and are not intended to limit the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Furthermore, unless otherwise specified, the raw materials mentioned below are all commercially available products; and the process steps or preparation methods not mentioned in detail are all process steps or preparation methods known to those skilled in the art.
[0023] For Cr-Mo-Si-V series hot work die steels such as 4Cr5MoSiV1, 4Cr5MoSiV, 4Cr5Mo2SiV, and 4Cr5Mo3SiV, there is a common defect in the microstructure after forging: network carbides are continuously precipitated along the grain boundaries. Before subsequent spheroidizing annealing, pretreatment is required to eliminate the network carbides and obtain a suitable initial microstructure.
[0024] The commonly used process route in existing technologies, which involves "high-temperature normalizing + rapid cooling," involves heating the forged billet to above its austenitizing temperature and then rapidly cooling it. This rapid cooling rate suppresses the re-precipitation of carbides along grain boundaries, ultimately resulting in a martensitic structure. Martensite has a low transformation temperature, and with a sufficiently fast cooling rate, it can reliably suppress the precipitation of proeutectoid carbides, thereby eliminating network carbides.
[0025] However, martensitic transformation is a diffusionless shear transformation, accompanied by approximately 4% volume expansion. In the processing of large cross-section workpieces, this generates greater structural stress, which, combined with the thermal stress resulting from a temperature difference between the surface and core exceeding 200°C, can easily lead to workpiece cracking. Furthermore, since carbon in martensite is in a supersaturated solid solution state, it requires tempering to precipitate carbides before undergoing a spheroidization process. This spheroidization path is longer, and controlling the uniformity of the microstructure is more difficult.
[0026] For large-size die steel forgings with a slab thickness greater than 400mm or a round billet diameter greater than 500mm, this contradiction is particularly prominent: to ensure that the core also obtains martensite, the cooling intensity must be greatly increased, but the greater the cooling intensity, the higher the risk of cracking, and the extremely narrow the process window.
[0027] The present invention selects bainite as the target pretreatment microstructure based on the following considerations: 1. Bainite transformation is a semi-diffusion phase transformation. Its volume change is much smaller than that of martensite transformation. Moreover, the isothermal transformation takes place at a constant temperature. The entire cross section completes the transformation under the same thermodynamic conditions, and the residual stress level is also greatly reduced.
[0028] 2. During the bainitic transformation, carbides are dispersed and precipitated in the matrix, forming a microstructure with lower bainite as the matrix and dispersed undissolved carbides. These dispersed carbides can be directly used as the nucleation substrate for spheroidizing in the subsequent spheroidizing annealing process, which is beneficial for obtaining a uniform and fine spheroidized carbide microstructure. In addition, the lower bainitic microstructure has low internal stress, and can directly enter the spheroidizing annealing process after pretreatment, without the need for tempering to eliminate quenching stress as required by the martensitic route. This simplifies the process and reduces energy consumption.
[0029] Compared with the prior art, the present invention provides a method for preventing cracking of large-section alloy steel through bainitic pretreatment, which includes the following steps: Step S1: Perform austenitizing treatment on the forged large-section alloy steel workpiece to obtain a high-temperature austenitic structure; Step S2: The austenitized large-section alloy steel workpiece is subjected to intermittent rapid cooling. During the cooling process, the surface temperature of the large-section alloy steel workpiece is controlled to always be higher than the martensitic transformation start temperature, and the surface temperature return is lower than the upper limit temperature of the bainitic transformation zone at the end of cooling, so that the core of the large-section alloy steel workpiece is cooled to below the pearlite transformation start temperature. Step S3: Place the cooled large-section alloy steel workpiece in the bainite transformation temperature range for isothermal heat preservation, so that the supercooled austenite completes the bainite transformation and obtains the initial bainite structure.
[0030] Step S2 is a key step in the synergistic achievement of crack prevention and microstructure control in this invention. Maintaining the surface temperature consistently above the Ms point aims to reduce the martensitic transformation on the surface, thereby eliminating the microstructure stress caused by the inconsistency between the volume expansion of martensite during transformation and the contraction of austenite in the core, thus reducing the risk of cracking at its source. The intermittent nature of the "intermittent rapid cooling" allows the core heat to provide "self-tempering" temperature compensation to the surface, dynamically maintaining the temperature difference between the surface and core within a certain range. When the surface temperature returns to below the upper limit of the bainite transformation zone at the end of cooling, it prevents unexpected pearlite or coarse bainite transformations during the high-temperature period, ensuring that the workpiece avoids the carbide precipitation sensitive zone and is in a suitable bainite transformation initiation state before entering the isothermal stage. Combined with the isothermal holding in the bainite transformation temperature range in step S3, the supercooled austenite is fully transformed into a low-stress initial microstructure with bainite as the matrix, achieving a balance between microstructure control and crack prevention, providing an ideal microstructure basis for subsequent spheroidizing annealing.
[0031] In this invention, "large cross section" specifically refers to workpiece specifications with a slab thickness greater than 400mm or a round billet diameter greater than 500mm. Such specifications have an extremely high risk of cracking due to the long heat conduction path and large temperature difference between the surface and the core. "Return temperature" refers to the physical phenomenon that the surface temperature of a workpiece rises due to the conduction of internally accumulated heat to the outside during the intermittent cooling water-air cooling stage.
[0032] Specifically, in step S1, the large-section alloy steel workpiece after forging is subjected to austenitization treatment. A segmented heating strategy is adopted, that is, the workpiece is first heated to 800℃ at a heating rate of no more than 70℃ / h and held for 2h~5h. For example, the heating rate can be 60℃ / h, 65℃ / h, 67℃ / h, or 70℃ / h, and the holding time can be 2h, 3h, 4h, or 5h.
[0033] Then, continue heating at a rate not exceeding 50℃ / h to the high-temperature austenitizing range and hold at that temperature. This high-temperature austenitizing range is Ac3 + (50~100)℃. For example, the heating rate can be 30℃ / h, 40℃ / h, 45℃ / h, 48℃ / h, or 50℃ / h, and the target temperature can be Ac3 + 60℃, Ac3 + 80℃, or Ac3 + 90℃. The holding time is calculated at 1.5min / mm × the effective thickness of the workpiece.
[0034] The principle behind the segmented heating strategy is as follows: The first stage, involving prolonged holding at 800℃, aims to homogenize the temperature of the workpiece's surface and core, eliminate residual forging stress, and preheat the matrix to prevent microcracks caused by thermal shock during subsequent high-temperature heating. The second stage, involving slow heating to a specific range above Ac3, ensures sufficient dissolution of carbides and elimination of network carbides while preventing excessive austenite grain growth. The linear relationship between holding time and effective thickness ensures complete austenitization of the core of large-section workpieces, providing a precondition for uniform composition during subsequent cooling transformation.
[0035] According to some embodiments of the present invention, in step S2, the austenitized workpiece is subjected to intermittent rapid cooling. During the cooling process, the surface temperature of the workpiece is controlled to always be higher than the martensitic transformation start temperature (Ms point), and the surface temperature return is lower than the upper limit temperature of the bainitic transformation zone at the end of the cooling process, so that the core of the workpiece is cooled to below the pearlite transformation start temperature. This is a key step in the present invention to achieve the synergistic effect of crack prevention and microstructure regulation.
[0036] Specifically, intermittent rapid cooling is achieved by alternating between water quenching and intermittent reheating. The duration of each water quenching cycle is controlled to keep the workpiece surface temperature above the martensitic transformation initiation temperature while simultaneously cooling the workpiece core below the pearlitic transformation initiation temperature. In this process, the duration of a single water quenching cycle is 4 to 12 minutes, for example: 4 minutes, 8 minutes, 12 minutes; the number of alternating water quenching and reheating cycles is 5 to 10 times, for example: 5 times, 7 times, 9 times, 10 times; the total liquid cooling time is 30 to 120 minutes, for example: 30 minutes, 60 minutes, 90 minutes, 120 minutes; the workpiece core is cooled to below 600°C, and the surface reheating temperature is below 450°C at the end of cooling.
[0037] The single water quenching time of 4 to 12 minutes is determined based on the heat capacity and heat transfer coefficient of the large cross-section workpiece. If it is less than 4 minutes, it cannot provide sufficient cooling rate to suppress the precipitation of proeutectoid carbides along the grain boundaries; if it exceeds 12 minutes, the surface cold storage is too large, and even if the temperature is returned to the surface after water quenching, it is difficult to maintain it above the Ms point, which can easily induce martensitic transformation. The purpose of intermittent reheating is to use the heat in the core to perform "self-tempering" temperature compensation on the surface, so that the temperature difference of the core is dynamically maintained within a safe range.
[0038] The surface temperature is kept below 450°C at the end of cooling to ensure that the workpiece has completely avoided the pearlite transformation zone (the pearlite transformation initiation temperature is usually 600°C~650°C) before entering the next process. This prevents unexpected pearlite or coarse bainite transformation during the high-temperature stay and also prepares for the temperature transition to the bainite isothermal zone.
[0039] Taking typical steel grades to which this invention is applicable as examples, the key phase transformation temperature reference values for each steel grade are as follows: 4Cr5MoSiV1: Ac3 is approximately 940℃~950℃, corresponding to an austenitizing temperature range of approximately 990℃~1050℃; Ms point is approximately 300℃~330℃ (the measured value in the embodiment of this invention is 325℃); the upper limit temperature of the bainite transformation region is approximately 400℃~450℃; the pearlite transformation initiation temperature is approximately 600℃~650℃.
[0040] 4Cr5MoSiV: Ac3 is approximately 910℃~920℃, corresponding to an austenitizing temperature range of approximately 960℃~1020℃; Ms point is approximately 310℃~340℃; the upper limit temperature of the bainite transformation zone is approximately 400℃~450℃; and the pearlite transformation initiation temperature is approximately 600℃~650℃.
[0041] 4Cr5Mo2SiV: Ac3 is approximately 900℃~910℃, corresponding to an austenitizing temperature range of approximately 950℃~1010℃; Ms point is approximately 300℃~330℃; the upper limit temperature of the bainite transformation zone is approximately 400℃~450℃; and the pearlite transformation initiation temperature is approximately 600℃~650℃.
[0042] 4Cr5Mo3SiV: Ac3 is approximately 820℃~880℃, corresponding to an austenitizing temperature range of approximately 870℃~930℃; Ms point is approximately 280℃~310℃; the upper limit temperature of the bainite transformation region is approximately 450℃~500℃; and the pearlite transformation initiation temperature is approximately 600℃~650℃.
[0043] The phase transformation temperatures mentioned above are reference ranges for each steel grade under typical compositions. Actual values are affected by the specific composition ratios. Those skilled in the art can determine the actual material composition by using the expansion method or TTT chart.
[0044] According to some embodiments of the present invention, in step S3, the cooled workpiece is placed in the bainite transformation temperature range for isothermal heat preservation, so that the supercooled austenite completes the bainite transformation and obtains the initial bainite structure.
[0045] Specifically, the bainitic transformation temperature range is 325℃~420℃, for example: 325℃, 350℃, 380℃, 400℃, 420℃; the isothermal holding time is 8h~15h, for example: 8h, 10h, 12h, 14h, 15h.
[0046] It should be noted that the upper limit temperature of the bainite transformation zone for the steel to which this invention is applicable is approximately 400 ℃ ~ 450 ℃. The actual isothermal temperature should be controlled in its lower limit region (350–420 ℃) to promote the formation of lower bainite and inhibit the formation of upper bainite or martensite. The specific selection of this temperature range can be further adjusted according to the specific steel grade. The purpose is to strictly limit it above the Ms point and below the upper limit temperature of the bainite transformation, in order to promote the formation of lower bainite rather than lamellar bainite or martensite.
[0047] Lower bainite consists of a ferrite matrix and a dispersed carbide second phase. This microstructure exhibits low internal stress and good toughness reserves. Furthermore, the dispersed fine carbides act as nucleation sites for spheroidized carbide precipitation during subsequent spheroidizing annealing, significantly shortening the spheroidizing cycle and improving carbide dispersion. An isothermal holding time of at least 8 hours ensures that the transformation of supercooled austenite reaches over 95%, preventing the formation of a large amount of retained martensite upon cooling to room temperature due to incomplete transformation. An isothermal holding time of no more than 15 hours balances production efficiency with the need to prevent excessive carbide coarsening. The final initial bainitic microstructure is characterized by a lower bainite matrix with dispersed undissolved carbides.
[0048] After completing the above pretreatment, the workpiece can be directly subjected to isothermal spheroidizing annealing. Since the lower bainite structure obtained by pretreatment has extremely low internal stress and ideal carbide distribution, the workpiece can be directly put into the furnace for spheroidizing treatment without intermediate tempering or slow cooling buffer. This not only greatly shortens the production process, but also avoids the energy consumption and oxidation loss caused by multiple heating and cooling.
[0049] Taking a typical steel grade to which this invention applies as an example, the common process conditions for isothermal spheroidizing annealing are as follows: the workpiece is heated to above Ac1 (e.g., 850℃~880℃) and held for 10h~20h to fully austenitize the microstructure and retain undissolved carbides as spheroidizing nuclei; then the temperature is lowered to below Ar1 (e.g., 720℃~760℃) and isothermally held for 15h~30h to decompose the austenite into ferrite and spheroidized carbides at subcritical temperatures; finally, the furnace is cooled to below 500℃ and then air-cooled after removal from the furnace.
[0050] Among them, the Ac1 of 4Cr5MoSiV1 is about 830℃~860℃, and the Ar1 is about 730℃~760℃; the Ac1 and Ar1 of other steels in the same series are similar. Those skilled in the art can determine the specific parameters by means of TTT diagram based on the actual material composition.
[0051] It should be noted that the anti-cracking bainitic pretreatment method of the present invention targets the post-forging microstructure, and its technical contribution is concentrated in the pretreatment process itself. For Cr-Mo-Si-V series hot work die steels, the forging process and the initial annealing process after forging (the main purpose of which is to reduce hardness in order to remove the billet at the riser and to prevent post-forging cooling cracking) have little impact on the microstructure and properties of subsequent pretreatment and the final spheroidizing annealed product under normal conditions.
[0052] Unless severe coarse-grained or mixed-grained problems occur during forging, variations in conventional forging parameters (such as forging temperature, forging ratio, and final forging temperature) and preliminary annealing parameters (such as annealing temperature and holding time) will not substantially affect the quality of the bainitic microstructure obtained after pretreatment according to this invention, as well as the carbide morphology, distribution, and mechanical properties of the final spheroidized annealed product. In other words, the core technical effects of this invention—eliminating network carbides, obtaining a uniform and fine initial bainitic microstructure, and preventing cracking—mainly depend on the process control of the three core steps in the pretreatment process: austenitization, intermittent rapid cooling, and isothermal transformation of bainite, rather than upstream conventional processes.
[0053] This feature gives the invention good process adaptability and production stability. Under normal forging and preliminary annealing conditions, it can ensure a stable and reliable pretreatment effect without special adjustments to the upstream process.
[0054] To more clearly describe the present invention, the following embodiments and comparative examples are provided for further illustration.
[0055] Example 1 This embodiment uses a large-size hot work die steel round billet made of 4Cr5MoSiV1 material as the processing object, with a cross-sectional diameter of 890mm.
[0056] S1. The forged and annealed workpiece is placed in a heat treatment furnace and heated to 800℃ at a heating rate of 70℃ / h and held for 5h. Then, the temperature is increased to 1030℃ at a heating rate of 50℃ / h and held for 22.5h to completely austenitize the core of the workpiece and eliminate network carbides.
[0057] S2. Intermittent rapid cooling is achieved by alternating water quenching and intermittent reheating. The single water quenching time is 12 minutes, the number of alternations is 10, and the surface reheating temperature is 390°C at the end of cooling. The core of the workpiece is cooled to below the pearlite transformation initiation temperature.
[0058] S3. The workpiece is held isothermally at 400℃ for 14 hours to obtain an initial microstructure with bainite as the matrix. After the isothermal transformation, the workpiece is directly subjected to isothermal spheroidizing annealing.
[0059] Example 2 This embodiment uses a large-size hot work die steel square billet made of 4Cr5MoSiV material, with a cross-sectional thickness of 780mm. Compared to the round billet in Example 1, the square billet dissipates heat faster at its corners and exhibits more significant stress concentration, requiring higher precision in process control.
[0060] S1. The forged and annealed workpiece is placed in a heat treatment furnace and heated to 800℃ at a heating rate of 70℃ / h and held for 4h; then the temperature is increased to 1030℃ at a heating rate of 50℃ / h and held for 20h to completely austenitize the core of the workpiece and eliminate network carbides.
[0061] S2. Intermittent rapid cooling is achieved by alternating water quenching and intermittent reheating. The single water quenching time is 10 minutes, and the number of alternations is 9. The surface reheating temperature is 375°C at the end of cooling. The single water quenching time is slightly shorter than that in Example 1 to prevent local overcooling at the corners of the billet below the Ms point.
[0062] S3. Place the workpiece in the bainitic transformation temperature range of 390℃ and hold it isothermally for 11.5 hours. After isothermal treatment, proceed directly to isothermal spheroidizing annealing.
[0063] Example 3 This embodiment uses a large-size hot work die steel billet made of 4Cr5Mo2SiV material as the processing object, with a cross-sectional thickness of 500mm, which is close to the smaller end of the applicable scope of this invention. Since the heat capacity of the 500mm cross-section is significantly smaller than that of the 890mm round billet in Example 1 and the 780mm square billet in Example 2, the heat conduction path from the core to the outside is shorter, requiring higher precision in controlling the intermittent cooling parameters.
[0064] S1. The forged and annealed workpiece is placed in a heat treatment furnace and heated to 800℃ at a heating rate of 70℃ / h and held for 5h. Then, the temperature is increased to 1030℃ at a heating rate of 50℃ / h and held for 12.5h to completely austenitize the core of the workpiece and eliminate network carbides.
[0065] S2. Intermittent rapid cooling is achieved by alternating water quenching and intermittent reheating. The single water quenching time is 6 minutes, and the number of alternations is 6. The surface reheating temperature is 380°C at the end of cooling. The single water quenching time and the number of alternations are both reduced compared to Example 1 to prevent the surface layer from dropping below the Ms point due to excessive cold storage.
[0066] S3. Place the workpiece in the bainitic transformation temperature range of 410℃ and hold it isothermally for 12 hours. After isothermal treatment, directly perform isothermal spheroidizing annealing.
[0067] Comparative Example 1 Comparative Example 1 involved processing a 780mm 4Cr5MoSiV square billet, identical to that in Example 2. The post-forging pretreatment steps included: S1. The forged and annealed workpiece is placed in a heat treatment furnace and heated to 800℃ at a heating rate of 70℃ / h and held for 4h; then the temperature is increased to 1030℃ at a heating rate of 50℃ / h and held for 20h to completely austenitize the core of the workpiece and eliminate network carbides.
[0068] S2. The surface temperature is rapidly cooled to 370°C by a single water immersion in water for 15 minutes. However, the surface temperature rises to 650°C during the subsequent transfer into the furnace in air.
[0069] S3. Place the workpiece in a 390℃ furnace and keep it at that temperature for 11.5 hours. After the holding time is completed, proceed directly with isothermal spheroidizing annealing.
[0070] Comparative Example 2 Comparative Example 2 involved machining a 4Cr5MoSiV1 round billet (890 mm) identical to that of Example 1, with the following post-forging pretreatment steps: S1. The forged and annealed workpiece is placed in a heat treatment furnace and heated to 800℃ at a heating rate of 70℃ / h and held for 5h. Then, the temperature is increased to 1030℃ at a heating rate of 50℃ / h and held for 22.5h to completely austenitize the core of the workpiece and eliminate network carbides.
[0071] S2. Intermittent rapid cooling is achieved by alternating water quenching and intermittent reheating. The single water quenching time is 12 minutes, but the number of alternations is reduced to 7 times compared to Example 1. The surface reheating temperature is 500°C at the end of cooling.
[0072] S3. Place the workpiece in a 400℃ furnace and keep it at that temperature for 14 hours. After the holding time is completed, perform isothermal spheroidizing annealing directly.
[0073] Comparative Example 3 Comparative Example 3 involved processing a 500mm 4Cr5Mo2SiV square billet, identical to that in Example 3. The post-forging pretreatment steps included: S1. The forged and annealed workpiece is placed in a heat treatment furnace and heated to 800℃ at a heating rate of 70℃ / h and held for 3h. Then, the temperature is increased to 1020℃ at a heating rate of 50℃ / h and held for 12.5h to completely austenitize the core of the workpiece and eliminate network carbides.
[0074] S2. Intermittent rapid cooling is achieved by alternating water quenching and intermittent reheating. The single water quenching time is 6 minutes, the number of alternations is 6, and the surface reheating temperature is 380℃ at the end of cooling.
[0075] S3. Place the workpiece in a treatment furnace at 410℃ and keep it at that temperature for 5 hours. After the temperature is maintained, perform isothermal spheroidizing annealing directly.
[0076] Comparative Example 4 Comparative Example 4 involved processing a 500mm 4Cr5Mo2SiV square billet, identical to that in Example 3. The post-forging pretreatment steps included: S1. The forged and annealed workpiece is placed in a heat treatment furnace and heated directly from room temperature to 1020℃ at a rate of 70℃ / h and held for 12.5h.
[0077] S2. Intermittent rapid cooling is achieved by alternating water quenching and intermittent reheating. The single water quenching time is 6 minutes, the number of alternations is 6, and the surface reheating temperature is 380℃ at the end of cooling.
[0078] S3. Place the workpiece in a treatment furnace at 410℃ and keep it at that temperature for 12 hours. After the temperature is maintained, perform isothermal spheroidizing annealing directly.
[0079] Comparative Example 5 Comparative Example 5 involved processing a 500mm 4Cr5Mo2SiV square billet, identical to that in Example 3. The post-forging pretreatment steps included: S1. The forged and annealed workpiece is placed in a heat treatment furnace and heated to 800℃ at a heating rate of 70℃ / h and held for 3h. Then, the temperature is increased to 1020℃ at a heating rate of 50℃ / h and held for 12.5h to completely austenitize the core of the workpiece and eliminate network carbides.
[0080] S2. Intermittent rapid cooling is achieved by alternating water quenching and intermittent reheating. The single water quenching time is extended to 15 minutes, and the number of alternations is 6. This causes the surface temperature of the workpiece to drop to 210°C after reheating, which is far below the Ms point (approximately 325°C) of this steel grade.
[0081] S3. Place the workpiece in a treatment furnace at 410℃ and keep it at that temperature for 12 hours. After the temperature is maintained, perform isothermal spheroidizing annealing directly.
[0082] Performance testing The above-described embodiments and comparative examples were subjected to performance tests, mainly including cracking, network carbides, core microstructure grade, cross-sectional hardness, and unnotched impact toughness. The standards used for each test item are as follows: (1) Cracking condition: Visual inspection of the surface and corners of the pretreated workpiece, and magnetic particle testing (according to GB / T 15822.1-2024 standard) to detect surface and near-surface microcracks.
[0083] (2) Network carbide grade: Take a sample from the cross section of the workpiece, and after grinding and polishing and etching with 4% nitric acid alcohol solution, observe the distribution morphology of carbides along the grain boundaries using an optical microscope, and evaluate the grade by referring to the rating chart in GB / T 1299 standard.
[0084] (3) Core microstructure grade: Samples are taken from the core of the workpiece, and after grinding, polishing and etching, the matrix structure morphology is observed using an optical microscope. The microstructure grade is evaluated according to the AS (Annealed Structure) rating standard.
[0085] (4) Cross-sectional hardness: The Brinell hardness test is performed on the cross-section of the workpiece according to GB / T 231.1 standard. The test load is 3000 kgf, the indenter diameter is 10 mm, and the range value is measured at multiple points along the cross-section.
[0086] (5) Unnotched impact toughness: Cut an unnotched standard specimen from the workpiece and conduct a room temperature impact test according to GB / T 229 standard, and record the impact absorption energy.
[0087] The test results are shown in Table 1.
[0088] Table 1 Performance test results of each embodiment and comparative example
[0089] Combining Examples 1-3 and Comparative Examples 1-5 and referring to Table 1, it can be seen that Examples 1-3, within the process parameters defined by this invention, all achieved comprehensive performance indicators such as no cracking, network carbide grade ≤1, core microstructure grade AS2~AS4, cross-sectional hardness 195HB~210HB, and unnotched impact toughness greater than 300J. This verifies the universality of the technical solution of this invention in different steel grades (4Cr5MoSiV1, 4Cr5MoSiV, 4Cr5Mo2SiV), different cross-sectional shapes (round billet, square billet), and different specifications (500mm~890mm).
[0090] In Comparative Example 1, a single cooling process was used. Although the surface was cooled to 370°C, the surface temperature rebound (650°C) at the end of cooling exceeded the upper limit of the bainite transformation zone (450°C). The workpiece remained in the high-temperature range for too long, re-entering the rapid precipitation temperature range of proeutectoid carbides. This caused the carbon elements already dissolved in the matrix to precipitate again along the grain boundaries, forming a continuous network of carbides. Ultimately, this resulted in the carbide grade in the workpiece deteriorating to level 3 and the microstructure grade decreasing to AS16. This result demonstrates the decisive role of the present invention's limitation of "the surface temperature rebound below the upper limit of the bainite transformation zone at the end of cooling" in suppressing secondary carbide precipitation.
[0091] In Comparative Example 2, insufficient cooling intensity led to excessively high surface temperature (500℃). The cooling rate in the core of the large-section workpiece failed to effectively avoid the pearlite transformation zone, resulting in an unexpected pearlite or coarse bainite transformation in the core. The network carbide grade reached level 3, the microstructure grade was AS15, and the impact toughness was as low as 260J. This result confirms that sufficient cooling depth is a prerequisite for ensuring a qualified core microstructure.
[0092] In Comparative Example 3, the isothermal holding time for bainite (5 h) was lower than the 8 h lower limit specified in this invention. The bainite transformation was insufficient, and a large amount of untransformed retained austenite continuously accumulated carbon during the isothermal stage. During subsequent cooling to room temperature, this carbon-rich austenite partially transformed into brittle martensite and precipitated carbides at grain boundaries, forming a network distribution. Ultimately, this resulted in a network carbide grade of 3 and a microstructure grade of AS15. This result highlights the crucial role of sufficient isothermal time in ensuring adequate bainite transformation and preventing carbide segregation induced by retained austenite.
[0093] In Comparative Example 4, the 800℃ preheating and holding stage was eliminated, and a single-stage rapid heating method was adopted. The temperature difference between the surface and core of the large cross-section workpiece instantly exceeded the thermal stress yield limit of the material, inducing microcracks at stress concentration points such as corners, which then expanded into macro-cracks (4 arc-shaped cracks with a depth of 3cm) during subsequent quenching and cooling, reducing material utilization by 5%. This result demonstrates the fundamental role of segmented preheating in eliminating thermal shock and preventing cracking.
[0094] In Comparative Example 5, the excessively long single water quenching time caused the surface temperature to drop below the Ms point in the early cooling stage (1-2 water quenches). The surface layer underwent significant martensitic transformation accompanied by volume expansion. However, due to the hysteresis effect of heat conduction in the 500mm cross-section, the core temperature remained far above the Ms point. This asynchronous transformation between the surface and core resulted in substantial structural stress, leading to numerous cracks on the surface and edges of the final slab. Some cracks exceeded 8cm in depth, rendering the workpiece unusable. This counterexample demonstrates that in this invention, "maintaining the surface temperature consistently above the martensitic transformation initiation temperature" is the bottom line for preventing cracking.
[0095] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preventing cracking and pretreating bainitic deposits in large-section alloy steel, characterized in that, Includes the following steps: Step S1: Perform austenitizing treatment on the forged large-section alloy steel workpiece to obtain a high-temperature austenitic structure; Step S2: The austenitized large-section alloy steel workpiece is subjected to intermittent rapid cooling. During the cooling process, the surface temperature of the large-section alloy steel workpiece is controlled to always be higher than the martensitic transformation start temperature, and the surface temperature return is lower than the upper limit temperature of the bainitic transformation zone at the end of cooling, so that the core of the large-section alloy steel workpiece is cooled to below the pearlite transformation start temperature. Step S3: Place the cooled large-section alloy steel workpiece in the bainite transformation temperature range for isothermal heat preservation, so that the supercooled austenite completes the bainite transformation and obtains the initial bainite structure.
2. The method for preventing cracking of large-section alloy steel by bainitic pretreatment according to claim 1, characterized in that, The large-section alloy steel workpiece is a large-size die steel forging billet with a slab thickness greater than 400mm or a round billet diameter greater than 500mm; the material of the large-size die steel forging billet is selected from any one of 4Cr5MoSiV1, 4Cr5MoSiV, 4Cr5Mo2SiV or 4Cr5Mo3SiV.
3. The method for preventing cracking of large-section alloy steel through bainitic pretreatment according to claim 1, characterized in that, The intermittent rapid cooling in step S2 includes: By alternating water quenching and intermittent reheating, and controlling the single water quenching time, the surface temperature of the large-section alloy steel workpiece fluctuates above the martensitic transformation initiation temperature, while the core of the large-section alloy steel workpiece is cooled to below the pearlitic transformation initiation temperature.
4. The method for preventing cracking of large-section alloy steel by bainitic pretreatment according to claim 3, characterized in that, The single water quenching cooling time is 4 min to 12 min, and the number of alternating water quenching and intermittent reheating is 5 to 10 times, with a total liquid cooling time of 30 min to 120 min; so that the core of the large cross-section alloy steel workpiece is cooled to below 600℃, and the surface reheating temperature is below 450℃ at the end of cooling.
5. The method for preventing cracking of large-section alloy steel through bainitic pretreatment according to claim 1, characterized in that, The bainite transformation temperature range in step S3 is 325℃~420℃; the isothermal holding time is 8h~15h.
6. The method for preventing cracking of large-section alloy steel through bainitic pretreatment according to claim 1, characterized in that, The austenitizing treatment of the large-section alloy steel workpiece in step S1 includes: The large-section alloy steel workpiece is heated to 800℃ at a heating rate of no more than 70℃ / h and held at that temperature for 2h~5h. Continue heating at a rate not exceeding 50℃ / h to the high-temperature austenitizing range and hold at that temperature; The high-temperature austenitizing range is Ac3+(50~100)℃, and the holding time is calculated as 1.5min / mm × the effective thickness of the large cross-section alloy steel workpiece.
7. The method for anti-cracking bainitic pretreatment of large-section alloy steel according to any one of claims 1 to 6, characterized in that, The initial bainitic microstructure obtained in step S3 is a microstructure with bainitic matrix and dispersed undissolved carbides.
8. The method for anti-cracking bainitic pretreatment of large-section alloy steel according to any one of claims 1 to 6, characterized in that, After step S3, the process also includes: directly performing isothermal spheroidizing annealing on the large cross-section alloy steel workpiece.
9. A large-section alloy steel product, characterized in that, The large-section alloy steel product is pretreated using the anti-cracking bainitic pretreatment method for large-section alloy steel as described in any one of claims 1 to 8.
10. The large-section alloy steel product according to claim 9, characterized in that, The large-section alloy steel product has a network carbide grade ≤1, a core microstructure grade of AS2~AS4, a cross-sectional hardness range of 195HB~210HB, and an unnotched impact toughness greater than 300J.