5-series aluminum alloy sheets, their preparation methods and applications
By employing single-stage homogenization and precise cold rolling annealing processes, the contradiction between surface quality and mechanical properties in the process of achieving high strength and ultra-thinness of 5-series aluminum alloy sheets has been resolved. This has resulted in a high-strength, excellent formability, and texture-free anodized surface, thereby reducing production costs.
Patent Information
- Application Number
- CN202611449689.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-10
AI Technical Summary
Existing 5-series aluminum alloy sheets have difficulty balancing high plasticity and surface quality after anodizing during the process of achieving high strength and ultra-thinness, especially issues such as material texture defects and uneven gloss. Traditional processes are lengthy and costly.
By employing single-stage homogenization treatment, controlling the cold rolling reduction rate, and low-temperature annealing processes, combined with precise composition design, the uniformity of the internal temperature field and the stability of the microstructure of the ingot are achieved through grain refinement and control of the distribution of second-phase particles.
It achieves a synergistic balance of high strength, excellent formability and superior surface quality. The material is free of material marks and has high gloss after anodizing, which reduces production costs and energy consumption.
Smart Images

Figure CN123063642A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum alloys, and more specifically, to a 5-series aluminum alloy sheet, its preparation method, and its application. Background Technology
[0002] Currently, the requirements for casing materials in 3C electronic products (such as smartphones, tablets, and wearable devices) are becoming increasingly stringent. Aluminum alloys, with their excellent specific strength, good thermal conductivity, ease of processing, and unique metallic texture, have become the mainstream material for manufacturing casings of high-end 3C products. Among the many aluminum alloy series, 5-series aluminum alloys (i.e., 5xxx series aluminum alloys), due to their copper-free composition, excellent corrosion resistance, good weldability, and moderate strength, are widely used in structures requiring high corrosion resistance. However, as product design evolves towards "thinner, stronger, and more aesthetically pleasing," traditional 5-series aluminum alloys, especially high-magnesium-content alloys such as 5H59, have gradually revealed a series of technical bottlenecks that urgently need to be addressed during application, particularly the significant contradiction between achieving high strength and ultra-thinness and balancing the surface quality of anodized aluminum.
[0003] Firstly, high magnesium content is a key element in improving the strength of 5-series aluminum alloys, but increased magnesium content also leads to a deterioration in material processing performance. In traditional hot and cold rolling processes, high-magnesium aluminum alloys are prone to work hardening, resulting in decreased plasticity. To obtain ultra-thin sheets (e.g., less than 1.0 mm thick), multiple cold rolling and intermediate annealing processes are necessary. However, existing production processes often struggle to maintain high strength while ensuring sufficient cold-forming capacity of the sheet material.
[0004] Secondly, anodizing is a key post-treatment process for improving the appearance and corrosion resistance of 5-series aluminum alloys. However, traditional high-magnesium 5-series aluminum alloys are prone to developing "texture lines" defects on the surface after anodizing. Texture lines appear as faintly visible linear marks on the surface of the sheet, severely damaging the smoothness and specular reflection effect of the oxide film, leading to increased color difference and uneven gloss. The formation of these texture lines is closely related to the distribution of second-phase particles (such as Fe-containing phases and Al3Mg2 phases) in the alloy. When the Fe-containing phase is large or unevenly distributed, these second-phase particles will preferentially dissolve or hinder the uniform growth of the oxide film during anodizing, forming microscopic pits or protrusions, which in turn cause diffuse reflection of light, resulting in visual texture lines. Furthermore, if the Al3Mg2 phase precipitates continuously along the grain boundaries in a network pattern, it will not only weaken the grain boundary bonding force, leading to bending and cracking, but also generate surface roughness due to vigorous dissolution during oxidation, further exacerbating appearance defects.
[0005] Furthermore, the industry typically employs multi-stage homogenization heat treatment (such as two-stage or three-stage heating) to eliminate segregation in ingots and promote the dissolution of the second phase. However, this traditional process is lengthy, energy-intensive, and time-consuming. Moreover, for ultra-thin high-magnesium alloys, the complex temperature control curves make it difficult to ensure absolute uniformity of the internal temperature field of the ingot, easily leading to localized overheating or insufficient remelting. On the other hand, to improve surface quality, it is often necessary to sacrifice strength by reducing magnesium content or increasing impurity elements, or to control precipitated phases through extremely complex cold rolling reduction strategies. However, this increases the uncontrollability of production costs and makes it difficult to achieve a synergistic balance between mechanical properties and anode surface quality.
[0006] Therefore, how to provide an ultra-thin 5-series aluminum alloy sheet for anodizing that can take into account both high mechanical properties and high surface quality after anodizing is one of the technical problems that need to be solved in this field. Summary of the Invention
[0007] The main objective of this invention is to provide a 5-series aluminum alloy sheet, its preparation method, and its application, in order to solve the problems of the lengthy preparation process of 5-series aluminum alloy sheets in the prior art, and the difficulty in achieving both high mechanical properties and high surface quality after anodizing.
[0008] To achieve the above objectives, a first aspect of the present invention provides a method for preparing a 5-series aluminum alloy sheet, comprising: step S1, preparing raw materials according to the composition of the 5-series aluminum alloy sheet; the composition of the 5-series aluminum alloy sheet, by weight percentage, includes 0~0.08wt.% Si, 0~0.15wt.% Fe, 0~0.10wt.% Cu, 0~0.10wt.% Mn, 5.00wt.%~6.00wt.% Mg, 0~0.05wt.% Cr, 0~0.05wt.% Zn, 0~0.03wt.% Ti, with the balance being Al and unavoidable impurity elements; step S2, the raw materials are subjected to casting treatment to obtain... Step S3: The alloy ingot undergoes a single-stage homogenization treatment to obtain a homogenized ingot. The heating rate of the single-stage homogenization treatment is <70℃ / h, the holding temperature is 500℃~520℃, and the holding time is 2h~6h. Step S4: The homogenized ingot undergoes hot rolling to obtain a first plate. The first plate undergoes a first cold rolling treatment to obtain a second plate. The second plate undergoes intermediate annealing to obtain a third plate. Step S5: The third plate undergoes a second cold rolling treatment to obtain a fourth plate. The fourth plate undergoes finished product annealing to obtain a 5-series aluminum alloy plate. The total reduction rate of the second cold rolling treatment is <50%. The holding temperature of the finished product annealing treatment is 70℃~120℃, and the holding time is 2h~4h.
[0009] Further, in step S3, the heating rate of the single-stage homogenization treatment is 40 DEG C / h-60 DEG C / h; and / or, in step S5, the total reduction of the second cold rolling treatment is 30%-40%, and the holding temperature of the finished product annealing treatment is 80 DEG C-100 DEG C.
[0010] Further, the thickness of the alloy ingot is 400mm-600mm; the thickness of the first plate is 3.5mm-5mm; the thickness of the second plate is 0.7mm-0.9mm; and the thickness of the fourth plate is 0.5mm-0.8mm.
[0011] Further, in step S2, the casting treatment is semi-continuous casting, and the casting temperature of the semi-continuous casting is 695 DEG C-715 DEG C, and the casting speed is 43mm / min-53mm / min; the crystallizer of the semi-continuous casting is cooled by a circulating cooling water system, wherein the cooling water flow is 135m 3 / h-147m 3 / h, and the cooling water temperature entering the crystallizer is ≤28 DEG C.
[0012] Further, in step S4, the opening rolling temperature of the hot rolling treatment is 480 DEG C-500 DEG C, the final rolling temperature is 280 DEG C-320 DEG C, and the rolling pass is 17-19 passes.
[0013] Further, in step S4, the total reduction of the first cold rolling treatment is 74%-86%.
[0014] Still further, in step S4, the heating rate of the intermediate annealing treatment is >2 DEG C / s, the holding temperature is 380±10 DEG C, and the holding time is 2s-10s; and / or, the cooling mode of the intermediate annealing treatment is water cooling.
[0015] The second aspect of the present application provides a 5-series aluminum alloy plate, which is prepared by the preparation method of the 5-series aluminum alloy plate.
[0016] Further, the tensile strength of the 5-series aluminum alloy plate is >360MPa, the yield strength is >280MPa, and the elongation is >10%; and / or, the 5-series aluminum alloy plate is subjected to 180 DEG bending without cracking; and / or, the 5-series aluminum alloy plate is subjected to anodic oxidation to obtain a 5-series aluminum alloy anodized plate, and the glossiness of the 5-series aluminum alloy anodized plate is 10Gu-20Gu, and the color difference is <0.25.
[0017] The third aspect of the present application provides an application of the 5-series aluminum alloy plate as a structural material and / or surface material in the field of computers, communications and consumer electronics, wherein the 5-series aluminum alloy plate is subjected to anodic oxidation to obtain a 5-series aluminum alloy anodized plate, and the 5-series aluminum alloy anodized plate is used as a structural material and / or surface material.
[0018] By controlling the heating rate and holding conditions of the single-stage homogenization treatment, limiting the total reduction rate of the second cold rolling treatment to control the trace precipitation of the dispersed phase, and controlling the conditions of the finished product annealing treatment to stabilize the microstructure, the technical solution of the present application achieves the purposes of simplifying the heat treatment process, reducing the production cost and improving the production efficiency, while realizing the synergistic balance of the mechanical properties of the material and the quality of the anode surface, thereby obtaining the 5-series aluminum alloy plate with high mechanical strength, no decay of mechanical properties during storage, no cracking in 180° bending, and uniform surface color, high gloss, low color difference, and no material line defects after anodic oxidation treatment. BRIEF DESCRIPTION OF DRAWINGS
[0019] The accompanying drawings, which form a part of the present application, are intended to provide further understanding of the present application and are incorporated herein for explanation by way of the exemplary embodiments of the present application and the illustrations thereof. The present application is not limited by the accompanying drawings.
[0020] Figure 1 A scanning electron microscope (SEM) characterization result graph of the cast ingot after the homogenization treatment of step (3) of the embodiment 1 of the present application;
[0021] Figure 2 A SEM characterization graph of the 5-series aluminum alloy plate provided by the embodiment 1 of the present application, wherein the morphology of the Al3Mg2 dispersed phase is shown;
[0022] Figure 3 A SEM characterization graph of the 5-series aluminum alloy plate provided by the embodiment 2 of the present application, wherein the morphology of the Fe-containing second phase compound is shown;
[0023] Figure 4 A SEM characterization graph of the plate provided by the comparative example 1 of the present application, wherein the morphology of the Fe-containing second phase compound is shown;
[0024] Figure 5 A SEM characterization graph of the plate provided by the comparative example 2 of the present application, wherein the morphology of the Al3Mg2 dispersed phase is shown. DETAILED DESCRIPTION
[0025] It should be noted that the embodiments in the present application and the features in the embodiments can be combined with each other without conflict. The present application will be described in detail below with reference to the embodiments.
[0026] As described in the background, the prior art lacks a 5-series aluminum alloy plate capable of simultaneously satisfying high-strength ultra-thin, stable storage performance, and anode oxidation surface without material line defects and a preparation method thereof. The existing process either cannot balance high strength and good formability, or the surface quality after anode oxidation is not up to standard, and the production cost is relatively high. In order to solve the above technical problems, the first aspect of the present application provides a preparation method of a 5-series aluminum alloy plate, comprising: step S1, preparing raw materials according to the composition of the 5-series aluminum alloy plate; the composition of the 5-series aluminum alloy plate includes 0~0.08wt.% of Si, 0~0.15wt.% of Fe, 0~0.10wt.% of Cu, 0~0.10wt.% of Mn, 5.00wt.%~6.00wt.% of Mg, 0~0.05wt.% of Cr, 0~0.05wt.% of Zn, 0~0.03wt.% of Ti, the balance is Al and inevitable impurity elements; step S2, the raw materials are treated by casting to obtain an alloy ingot; step S3, the alloy ingot is treated by single-stage homogenization to obtain a homogenized ingot; the heating rate of single-stage homogenization is <70℃ / h, the holding temperature is 500℃~520℃, and the holding time is 2h~6h; step S4, the homogenized ingot is treated by hot rolling to obtain a first plate; the first plate is treated by first cold rolling to obtain a second plate; the second plate is treated by intermediate annealing to obtain a third plate; step S5, the third plate is treated by second cold rolling to obtain a fourth plate; the fourth plate is treated by finished product annealing to obtain a 5-series aluminum alloy plate; the total reduction rate of the second cold rolling is <50%; the holding temperature of the finished product annealing is 70℃~120℃, and the holding time is 2h~4h.
[0027] The above preparation method provided by the present application solves the contradiction that the 5-series high-magnesium aluminum alloy is difficult to balance in terms of "high strength, corrosion resistance, easy processing, and excellent surface quality" by strictly controlling the high-magnesium content and the upper limit of trace elements in the alloy composition, and combining with subsequent heat treatment and deformation process.
[0028] Firstly, in the component formula of the 5-series aluminum alloy plate provided by the application, the Mg content is limited to 5.00wt.%-6.00wt.%, which is the basis for achieving high strength, and a high magnesium content provides a large amount of solid solution strengthening elements. At the same time, the impurities and alloying elements such as Si≤0.08%, Fe≤0.15%, Mn≤0.10%, Cu≤0.10% are strictly limited, especially the content of Fe and Mn, the core mechanism of which is to inhibit the formation of coarse needle-shaped or block-shaped Fe-containing phases (such as Al3FeSi, etc.) and coarse intermetallic compounds (such as Al6(Fe, Mn)). High content of Fe and Mn will lead to the coarsening of the second phase particles, and in the anodic oxidation process, due to the difference in electrochemical activity, micro concave pits will be formed around the second phase, thereby causing the macroscopic visible gloss reduction and "material lines" and other defects. By limiting these elements, the second phase particles are ensured to be small and dispersed, laying a microstructure foundation for obtaining a high-gloss, defect-free anodized surface. Ti as a grain refiner helps to obtain small casting grains, so that the second phase particles are more uniformly distributed.
[0029] In view of the problems of long process and high energy consumption of the traditional multi-stage homogenization process, in the subsequent homogenization process, a single-stage slow heating homogenization heat treatment process is adopted, and the segmented temperature control mode is abandoned. By controlling the slow heating rate, the internal temperature field of the ingot is uniformly and synchronously raised, providing sufficient kinetic conditions for atomic diffusion of the primary magnesium-containing phase, promoting the full decomposition of the coarse primary Al3Mg2 phase in the ingot during the heating stage, and completely dissolving into the α-Al matrix, thereby preventing the occurrence of overburning defects in the subsequent high-temperature heat treatment process. Compared with the traditional two-stage homogenization process, the present application eliminates the low-temperature homogenization heat treatment, reduces the continuous energy consumption and equipment occupation time of the heat treatment furnace, improves the overall production efficiency of the ingot pretreatment, and adapts to the large-scale continuous industrial production of ultra-thin high-magnesium anode aluminum material. Of course, at the same time, the above-mentioned single-stage homogenization treatment is not just a simple reduction of the traditional multi-stage process, but a process design based on kinetic control, which realizes a technical effect superior to or equivalent to multi-stage homogenization through precise parameter setting. Especially, the above-mentioned single-stage homogenization treatment process does not exist in isolation, but is closely matched with the subsequent hot rolling, cold rolling and annealing processes. Since the single-stage homogenization ensures the high uniformity of the composition and the absence of overburning structure in the ingot, the deformation resistance during subsequent hot rolling is more uniform, reducing the risk of surface cracking; at the same time, the uniform matrix provides an ideal initial state for the recovery and recrystallization after cold rolling. Especially when cooperating with "second cold rolling reduction rate <50%" and "low-temperature finished product annealing", the uniform matrix helps the Al3Mg2 phase to form a dispersed, small and point-shaped precipitate at the grain boundary, rather than a network distribution along the grain boundary. This not only ensures high mechanical strength and excellent bending performance of the material, but more importantly, avoids the "material line" defects during anodic oxidation.
[0030] Regarding the issue of surface defects and the inability to simultaneously achieve high strength and a uniform, aesthetically pleasing anodized appearance after anodizing of the aforementioned materials, this invention addresses this problem by precisely matching the secondary cold rolling reduction with the final annealing process, thereby achieving controllable, trace precipitation of the dispersed Al3Mg2 phase. If the reduction rate is too high, the dislocation density will be too high, easily leading to a large, continuous precipitation (network distribution) of the Al3Mg2 phase along grain boundaries during subsequent annealing. This network precipitate will dissolve violently during anodizing, forming grooves, disrupting the continuity of the oxide film, and resulting in a decrease in surface defects and gloss. Simultaneously, the uneven precipitation of the Al3Mg2 phase between the surface and core layers of the sheet can cause cracking during bending. This scheme limits the total reduction rate of the second cold rolling to <50%, controls the residual dislocation density and lattice distortion energy in the matrix, so that during the subsequent annealing of the finished product, the Al3Mg2 phase tends to precipitate in a dispersed, dotted, and discontinuous form at the grain boundaries, effectively reducing the generation of material marks and the decrease in gloss. At the same time, the precipitation of the surface and core layers of the plate is uniform, and it does not crack when bent.
[0031] In summary, the preparation method provided by this invention achieves the following effects:
[0032] Firstly, high strength and stability: high Mg content results in high solid solution content and higher strength; at the same time, due to low-temperature annealing, the material has strong resistance to aging softening and performance fluctuations during long-term storage.
[0033] Secondly, excellent formability: The Al3Mg2 phase is uniformly precipitated in the surface and core layers of the board, so that the resulting board does not crack when bent at 180°.
[0034] Thirdly, excellent surface quality: Due to proper control of impurities such as Fe / Mn, and the dispersed precipitation of Al3Mg2 phase rather than its network distribution along grain boundaries, the oxide film grows uniformly during anodizing, with fewer corrosion pits and reduced roughness at the interface between the oxide film and the aluminum substrate, thus achieving a high-quality surface with uniform color, high gloss, and no material defects.
[0035] In practical applications, for example, the composition of the above-mentioned 5-series aluminum alloy sheet by weight percentage includes 0.06wt.%~0.08wt.% Si, 0.10wt.%~0.12wt.% Fe, 0.01wt.%~0.02wt.% Cu, 0.02wt.%~0.06wt.% Mn, 5.5wt.%~5.9wt.% Mg, 0.01wt.%~0.03wt.% Cr, 0.01wt.%~0.03wt.% Ti, with the balance being Al and unavoidable impurity elements.
[0036] In step S3, the heating rate of the single-stage homogenization treatment is further preferably 40℃ / h to 60℃ / h. This preferred heating rate, while ensuring that the primary magnesium-containing phase is fully dissolved into the aluminum matrix, further promotes a more uniform rise in the internal temperature field of the ingot, providing more sufficient kinetic time for atomic diffusion, thereby more thoroughly eliminating component segregation, improving matrix purity, and obtaining 5-series aluminum alloy sheets with higher overall performance. In step S5, the total reduction rate of the second cold rolling treatment is further preferably 30% to 40%, and the holding temperature of the finished product annealing treatment is 80℃ to 100℃. The above-mentioned preferred reduction rate retains sufficient dislocation density and deformation energy as a driving force for subsequent precipitation, and can more effectively reduce dislocation entanglement and grain boundary distortion caused by excessive reduction rate; combined with the finished product annealing temperature of 80℃ to 100℃, it can more effectively promote the formation of appropriate amount and fine dispersed precipitation of Al3Mg2 phase at the grain boundary, thereby significantly improving the bending toughness of the sheet and the surface quality after anodizing.
[0037] Regarding the deformation process in the above preparation method, preferably: the thickness of the alloy ingot is 400mm~600mm; the thickness of the first plate is 3.5mm~5mm; the thickness of the second plate is 0.7mm~0.9mm; and the thickness of the fourth plate is 0.5mm~0.8mm. In this preferred embodiment, the thickness range from the ingot to the finished plate is further optimized to match the aforementioned process parameters, enabling the obtained ultrathin plate to maintain better ductility and surface quality after anodizing while possessing high strength.
[0038] In step S2, to optimize the initial solidification structure of the obtained alloy ingot, thereby obtaining fine casting grains and reducing the degree of initial segregation, and further reducing the burden on homogenization treatment, the casting process is preferably semi-continuous casting. The casting temperature of semi-continuous casting is 695℃~715℃, and the casting speed is 43mm / min~53mm / min. The crystallizer of semi-continuous casting is cooled by a circulating cooling water system, wherein the cooling water flow rate is 135m³ / min. 3 / h~147m 3 The cooling water temperature entering the crystallizer is ≤28℃. Furthermore, after casting, the width of the resulting alloy ingot is preferably 1200mm~1400mm, and the length is preferably 5000mm~7000mm, in order to improve the thermal uniformity inside the ingot and thus obtain more consistent performance.
[0039] In step S4, the preferred hot rolling temperature is 480℃~500℃, the preferred final rolling temperature is 280℃~320℃, and the preferred number of rolling passes is 17~19. This provides a better foundation for obtaining fine second-phase compounds and grains, and also helps to reduce uneven deformation and surface defects during the rolling process, further improving the surface quality and thickness accuracy of the sheet.
[0040] In step S4, to form a more uniform deformed structure and further reduce stress concentration, thereby obtaining finer and more uniform recrystallized grains in subsequent annealing, the total reduction rate of the first cold rolling process is preferably 74% to 86%. Furthermore, for the first and second cold rolling processes, the rolling speeds are preferably independently 100 m / min to 400 m / min (more preferably, the rolling speed of the first cold rolling process is 100 m / min to 200 m / min, and the rolling speed of the second cold rolling process is 200 m / min to 400 m / min). These preferred rolling speeds help reduce vibration and defects during rolling, and also better maintain the dimensional stability of the sheet during cold rolling, thereby further improving the surface quality of the resulting sheet after anodizing.
[0041] Furthermore, to more significantly eliminate work hardening, restore plasticity, and optimize the final grain size, in step S4, the heating rate of the intermediate annealing treatment is preferably >2℃ / s (exemplarily, 3℃ / s~5℃ / s), the holding temperature is 380±10℃, and the holding time is 2s~10s. Preferably, water cooling is used for the above intermediate annealing treatment, which can more effectively prevent the precipitation of Al3Mg2 phase during cooling, further improving the uniformity of the final obtained sheet material.
[0042] A second aspect of the present invention provides a 5-series aluminum alloy sheet, which is prepared by the above-described method for preparing 5-series aluminum alloy sheets. Thanks to the precise composition design and specific thermomechanical processing techniques described above, the resulting 5-series aluminum alloy sheet exhibits superior performance, effectively balancing high mechanical properties with high surface quality after anodizing.
[0043] Further, preferably: the average grain size of the 5-series aluminum alloy sheet is 10μm~30μm; the metallographic structure of the 5-series aluminum alloy sheet includes an aluminum matrix and Fe-containing phases and Al3Mg2 phases dispersed in the aluminum matrix, wherein the average size of the Fe-containing phase is ≤1.5μm; based on the total area of the metallographic structure of the 5-series aluminum alloy sheet as 100%, the area ratio of the Fe-containing phase is ≤0.5%, and the area ratio of the Al3Mg2 phase is ≤3.0%. Smaller grains can significantly improve the yield strength of the material through the Hall-Petch mechanism. It also improves the isotropy of the material and enhances the crack resistance during 180° bending. Controlling the average size and area ratio of the Fe-containing phase avoids damage to the continuity of the matrix. During the anodizing process, these fine second phases do not cause significant differences in electrochemical corrosion, thus effectively eliminating micro-pits formed by second-phase compounds, fundamentally suppressing surface defects and ensuring surface smoothness. Controlling the area ratio of the Al3Mg2 phase reduces the severe dissolution of the Al3Mg2 phase during anodizing, lowers the interface roughness of anodizing, and thus maintains a high-gloss surface with low color difference and a high-quality appearance.
[0044] It should be noted that due to the complex structural changes and crystal formation during the preparation process, and the limitations of the alloy material field and existing testing and characterization methods, it is difficult to comprehensively and quantitatively characterize the more specific microstructure and metallographic features of the obtained 5-series aluminum alloy sheet. However, the performance test results have already shown that the 5-series aluminum alloy sheet obtained by this invention has higher mechanical properties and exhibits better surface quality after anodizing. Specifically, in several preferred embodiments, the tensile strength of the aforementioned 5-series aluminum alloy sheet is >360MPa (more preferably 360MPa~380MPa), the yield strength is >280MPa (more preferably 285MPa~300MPa), and the elongation is >10% (more preferably 11%~14%); and / or, the aforementioned 5-series aluminum alloy sheet is bent at 180° without cracking; and / or, the 5-series aluminum alloy sheet is anodized to obtain a 5-series aluminum alloy anodized sheet, the gloss of the 5-series aluminum alloy anodized sheet is 10Gu~20Gu (more preferably 13Gu~16Gu), and the color difference is <0.25 (more preferably 0.20~0.22).
[0045] A third aspect of this invention provides an application of the aforementioned 5-series aluminum alloy sheet as a structural material and / or surface material in the fields of computers, communications, and consumer electronics. The 5-series aluminum alloy sheet is anodized to obtain an anodized 5-series aluminum alloy sheet, which is then used as a structural material and / or surface material. As a structural material, the aforementioned 5-series aluminum alloy sheet provided by this invention exhibits superior mechanical properties, enabling it to withstand the mechanical stresses experienced by 3C products during use. Furthermore, a 180° bending test demonstrates its ease of processing and forming, meeting the dual requirements of lightweight design and high strength. As a surface material, the 5-series aluminum alloy sheet, after anodizing, possesses a high gloss, low color difference, and a surface free of material defects, allowing it to replace traditional materials and achieve lightweight iteration and aesthetic upgrades for products. Moreover, the specific steps and conditions during the anodizing process are not limited; methods commonly used in the art can be employed.
[0046] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.
[0047] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.
[0048] Example 1
[0049] A method for preparing 5-series aluminum alloy sheet:
[0050] The alloy composition of this embodiment is as follows: Si = 0.06 wt.%; Fe = 0.10 wt.%; Cu = 0.02 wt.%; Mn = 0.06 wt.%; Mg = 5.85 wt.%; Cr = 0.02 wt.%; Ti = 0.02 wt.%; and the balance being Al and unavoidable impurities. The preparation method includes the following steps:
[0051] (1) First, prepare the raw materials according to the above ingredients.
[0052] (2) Semi-continuous casting: The resulting ingot dimensions are 500mm×1200mm×7000mm (thickness×width×length), with a casting temperature of 705℃, a casting speed of 45mm / min, and a crystallizer cooling water flow rate of 141m³. 3 / h, cooling water temperature 26℃.
[0053] (3) Homogenization treatment: After the ingot is cut off, the upper and lower surfaces are milled by 15mm, the heating rate is 40℃ / h, the homogenization temperature is 520℃, and the holding time is 3h.
[0054] (4-1) Hot rolling: initial rolling temperature 500℃, hot roughing 19 passes, final rolling temperature 320℃, final rolling thickness 4.0mm.
[0055] (4-2) First cold rolling: The plate is cold rolled to 0.9 mm at a rolling speed of 150 m / min, with a total reduction rate of 77.5%.
[0056] (4-3) After the first cold rolling, intermediate annealing is carried out at a temperature of 380℃, a heating rate of 3℃ / s, and a holding time of 10s. After annealing, water cooling treatment is used.
[0057] (5-1) Second cold rolling: A finished plate with a thickness of 0.6 mm was produced at a rolling speed of 300 m / min, with a total reduction rate of 33.33%.
[0058] (5-2) Finished product annealing: The finished product annealing temperature is 80℃ and the holding time is 2h.
[0059] Thus, 5-series aluminum alloy sheets were obtained.
[0060] In the above process, the homogenized ingot obtained in step (3) was characterized by SEM, and the results are shown in [the table below]. Figure 1 .Depend on Figure 1 As can be seen, by using the above homogenization process, the primary AlMg phase has been completely dissolved back into the matrix, and no overheating phenomenon was found. This indicates that slow heating can fully dissolve the AlMg phase back into the matrix, thereby replacing low-temperature homogenization and achieving the goal of cost reduction and efficiency improvement.
[0061] The final 5-series aluminum alloy sheet was characterized by SEM, and the results are shown in the figure. Figure 2 . Figure 2 The morphology of the Al3Mg2 dispersed phase is also shown. It can be seen that a small amount of Al3Mg2 phase precipitates in the finished board, distributed in a dotted pattern, accounting for approximately 1.06% of the total area.
[0062] Meanwhile, the aluminum alloy sheet and strip prepared using the above process have a tensile strength of 370 MPa, a yield strength of 290 MPa, an elongation of 13%, do not crack when bent at 180°, do not degrade in performance over long-term storage, and after anodizing, have a gloss of 15 Gu, a color difference of 0.22, and no material texture defects, meeting the technical requirements for appearance of 3C products. The above performance characterization results are shown in Table 1.
[0063] Example 2
[0064] A method for preparing 5-series aluminum alloy sheet:
[0065] The alloy composition of this embodiment is as follows: Si = 0.08 wt.%; Fe = 0.12 wt.%; Cu = 0.01 wt.%; Mn = 0.02 wt.%; Mg = 5.66 wt.%; Cr = 0.02 wt.%; Ti = 0.02 wt.%; and the balance being Al and unavoidable impurities. The preparation method includes the following steps:
[0066] (1) First, prepare the raw materials according to the above ingredients.
[0067] (2) Semi-continuous casting: The resulting ingot dimensions are 500mm×1200mm×7000mm (thickness×width×length), with a casting temperature of 701℃, a casting speed of 46mm / min, and a crystallizer cooling water flow rate of 145m³ / min. 3 / h, cooling water temperature 26℃.
[0068] (3) Homogenization treatment: After the ingot is cut off, the upper and lower surfaces are milled by 15mm, the heating rate is 50℃ / h, the homogenization temperature is 500℃, and the holding time is 3h.
[0069] (4-1) Hot rolling: initial rolling temperature 500℃, hot roughing 19 passes, final rolling temperature 310℃, final rolling thickness 3.0mm.
[0070] (4-2) First cold rolling: The plate is cold rolled to 0.8 mm at a rolling speed of 150 m / min, with a total reduction rate of 73.33%.
[0071] (4-3) After the first cold rolling, intermediate annealing is carried out at a temperature of 380℃, a heating rate of 3℃ / s, and a holding time of 10s. After annealing, water cooling treatment is used.
[0072] (5-1) Second cold rolling: A finished sheet with a thickness of 0.5 mm was produced at a rolling speed of 350 m / min, with a total reduction rate of 37.5%.
[0073] (5-2) Finished product annealing: The finished product annealing temperature is 100℃ and the holding time is 2h.
[0074] Thus, 5-series aluminum alloy sheets were obtained.
[0075] The final 5-series aluminum alloy sheet was characterized by SEM, and the results are shown in the figure. Figure 3 . Figure 3 The morphology of the Fe-containing second-phase compound is also shown. The finished plate has a small number of second-phase compounds with small size. Statistically, the area of the Fe-containing phase accounts for about 0.25%, and the average size is about 1.28 μm.
[0076] Meanwhile, the aluminum alloy sheet and strip prepared using the above process have a tensile strength of 368 MPa, a yield strength of 288 MPa, an elongation of 14%, do not crack when bent at 180°, do not degrade in performance over long-term storage, and after anodizing, have a gloss of 14 Gu, a color difference of 0.22, and no material texture defects, meeting the technical requirements for appearance of 3C products. The above performance characterization results are shown in Table 1.
[0077] Example 3
[0078] The only difference between this embodiment and embodiment 1 is that the heating rate of the homogenization process in step (3) is changed to 65℃ / h.
[0079] Example 4
[0080] The only difference between this embodiment and embodiment 1 is that the heating rate of the homogenization process in step (3) is changed to 30℃ / h.
[0081] Example 5
[0082] The only difference between this embodiment and Embodiment 1 is that in step (5-1), the total reduction rate of the second cold rolling is changed to 20%, thereby obtaining a sheet with a thickness of 0.72 mm; at the same time, the holding temperature for the final annealing of the finished product is changed to 70°C; the remaining preparation steps are consistent with Embodiment 1.
[0083] Example 6
[0084] The only difference between this embodiment and Embodiment 2 is that, while keeping the final sheet thickness unchanged, the thickness of the sheet obtained by the first cold rolling is changed to 0.9 mm. At this time, the total reduction rate of the first cold rolling is 70%, and the total reduction rate of the second cold rolling is 44.4%. At the same time, the holding temperature for the final annealing of the finished product is changed to 120°C. The remaining preparation steps are consistent with Embodiment 2.
[0085] Example 7
[0086] The only difference between this embodiment and Embodiment 1 is that the thickness values of the sheet metal obtained in each step of the deformation process are different. Specifically:
[0087] In step (2), an ingot with a thickness of 300 mm is obtained;
[0088] In step (4-1), a hot-rolled sheet with a thickness of 2.8 mm is obtained;
[0089] In step (4-2), a sheet material with a thickness of 1.2 mm after the first cold rolling is obtained;
[0090] In step (5-1), a second cold-rolled sheet with a thickness of 0.66 mm is obtained (with a reduction rate of 45%).
[0091] Example 8
[0092] The only difference between this embodiment and Embodiment 1 is that the thickness values of the sheet metal obtained in each step of the deformation process are different. Specifically:
[0093] In step (2), an ingot with a thickness of 700 mm is obtained;
[0094] In step (4-1), a hot-rolled sheet with a thickness of 2.5 mm is obtained;
[0095] In step (4-2), a sheet material with a thickness of 1.0 mm after the first cold rolling is obtained;
[0096] In step (5-1), a second cold-rolled sheet with a thickness of 0.55 mm is obtained (with a reduction rate of 45%).
[0097] Comparative Example 1
[0098] The only difference between this comparative example and Example 1 is that the Mn content in the alloy composition is increased to 0.20 wt.%, while the content of other components and subsequent preparation steps remain the same as in Example 1.
[0099] Figure 4 The image shows a scanning electron microscope (SEM) image of the second phase morphology of the finished product plate obtained in Comparative Example 1. It can be seen that the second phase in the finished product plate is relatively coarse, with some particles appearing as large lumps. Statistical analysis shows that the area containing the Fe phase accounts for approximately 0.65%, and the average size of the Fe phase is 1.56 μm. It is speculated that increasing the Mn content coarsens the Fe-containing compounds, and during the anodizing process, these compounds are easily incorporated into the oxide film, thus affecting the light reflection of the film and forming texture lines.
[0100] Furthermore, the aluminum alloy sheet and strip produced by this process has a tensile strength of 375 MPa, a yield strength of 290 MPa, an elongation of 12%, does not crack when bent at 180°, and its performance does not degrade after 3 months of storage. After anodizing, the gloss is 11 Gu, the color difference is 0.28, and there are material texture defects, which do not meet the technical requirements for appearance of 3C products. The above performance characterization results are shown in Table 1.
[0101] Comparative Example 2
[0102] The only difference between this comparative example and Example 1 is that, while keeping the final sheet thickness unchanged, the thickness of the sheet obtained by the first cold rolling is changed to 1.5 mm. At this time, the total reduction rate of the first cold rolling is 62.5%, and the total reduction rate of the second cold rolling is 60%. At the same time, the holding temperature for the final annealing of the finished product is changed to 210°C. The remaining preparation steps are consistent with those of Example 1.
[0103] Figure 5The image shows the morphology of the Al3Mg2 dispersed phase in the finished plate prepared using the process in Comparative Example 2. It can be seen that the Al3Mg2 dispersed phase precipitates continuously along the grain boundaries in a network distribution. Subsequently, during the anodic process, the Al3Mg2 dispersed phase dissolves violently, forming pits. The undulating structure of the interface disrupts the continuity and smoothness of the oxide film, enhances multi-directional light scattering, weakens specular reflection, and consequently reduces gloss. Furthermore, the precipitation of the dispersed phase exacerbates grain banding, thus intensifying material defects.
[0104] Furthermore, the aluminum alloy sheet and strip produced by this process has a tensile strength of 380 MPa, a yield strength of 294 MPa, an elongation of 12%, cracking upon 180° bending, and no performance degradation during long-term storage. After anodizing, the gloss is 8.6 Gu, the color difference is 0.35, and there are material texture defects, which do not meet the technical requirements for appearance of 3C products. The above performance characterization results are shown in Table 1.
[0105] Comparative Example 3
[0106] The only difference between this comparative example and Example 1 is that, while keeping the final thickness of the sheet unchanged, the thickness of the sheet obtained by the first cold rolling is changed to 1.5 mm. At this time, the total reduction rate of the first cold rolling is 62.5%, and the total reduction rate of the second cold rolling is 60%.
[0107] Comparative Example 4
[0108] The only difference between this comparative example and Example 1 is that the heating rate of the homogenization process in step (3) is changed to 70°C / h.
[0109] Comparative Example 5
[0110] The only difference between this comparative example and Example 1 is that the heat preservation temperature for homogenization in step (3) is changed to 450°C and the heat preservation time is changed to 8h.
[0111] Comparative Example 6
[0112] The only difference between this comparative example and Example 1 is that the heat preservation temperature for homogenization in step (3) is changed to 550°C and the heat preservation time is changed to 1h.
[0113] Comparative Example 7
[0114] The only difference between this comparative example and Example 1 is that the holding temperature for the annealing treatment of the finished product in step (5-2) is changed to 60°C and the holding time is changed to 5h.
[0115] Comparative Example 8
[0116] The only difference between this comparative example and Example 1 is that the holding temperature for the annealing treatment of the finished product in step (5-2) is changed to 130°C and the holding time is changed to 1 hour.
[0117] Test methods
[0118] Tensile strength, yield strength, and elongation: tested according to GB228.1-2021. For these three mechanical properties, higher test values indicate better mechanical properties of the sample. However, for the aluminum alloy sheet involved in this invention, it is considered to meet the usage requirements when its tensile strength is higher than 360 MPa, yield strength is higher than 280 MPa, and elongation is higher than 10%.
[0119] Cracking after 180° bend: A universal testing machine and a support roller bending fixture were used to perform a 180° 0T bend test on the test sample. The pressure head was continuously applied until the two wings of the sample were completely in contact, and the outer side of the bend was checked for cracks.
[0120] Anodizing treatment: The aluminum alloy sheets obtained in the above embodiments and comparative examples were subjected to anodizing treatment. The specific operation and experimental conditions were as follows: anodizing was carried out in a 180g / L sulfuric acid solution at 20℃, with a voltage of 12.5V and a time controlled at 30~40min, and anodized samples corresponding to each embodiment and comparative example were obtained. Subsequently, the gloss of each anodized sample was tested using a Rhopoint Novo-Gloss haze meter; the color difference of each anodized sample was tested using a YS3060 high-precision spectrophotometer; and the surface texture defects were observed visually under oblique strong light from a flashlight in a dark room.
[0121] The test results are shown in Table 1.
[0122] Table 1
[0123]
[0124] As can be seen from the above description, the embodiments of the present invention achieve the following by controlling the heating rate and holding conditions of the single-stage homogenization treatment, limiting the total reduction rate of the second cold rolling treatment to regulate the trace precipitation of the dispersed phase, and controlling the conditions of the finished product annealing treatment to stabilize the microstructure. This simplifies the heat treatment process, reduces production costs and improves production efficiency, and achieves a synergistic balance between the mechanical properties of the material and the surface quality of the anode. As a result, 5-series aluminum alloy sheets with high mechanical strength, no decrease in mechanical properties during storage, no cracking when bent at 180°, and uniform surface color, high gloss, low color difference and no material texture defects after anodizing treatment.
[0125] In each comparative example:
[0126] Comparing Comparative Example 1 with the various embodiments, it can be seen that the gloss, color difference, and anodized surface quality of the sample obtained in Comparative Example 1 deteriorated (gloss decreased from 15 Gu to 11 Gu, color difference increased from 0.22 to 0.28, and material texture defects appeared). This shows that controlling the Mn content ≤ 0.10 wt.% is crucial for suppressing the coarsening of the Fe-containing phase and ensuring the quality of the anodized surface. Excessive Mn content will promote the formation of coarse Fe-containing second-phase compounds and affect the light reflection performance of the oxide film.
[0127] Comparing Comparative Example 2 with the various embodiments, it can be seen that the 180° bending performance, gloss, color difference, and anodized surface quality of the sample obtained in Comparative Example 2 are significantly worse (bending cracks, gloss decreased from 15Gu to 8.6Gu, color difference increased from 0.22 to 0.35, and material texture defects appeared). This indicates that the second cold rolling total reduction rate and the finished product annealing temperature are too high, which may cause a large amount of continuous network precipitation of Al3Mg2 phase along the grain boundaries. During anodizing, it dissolves violently to form pits and material textures. At the same time, the Al3Mg2 phase will precipitate unevenly in the surface and core layers of the plate, thus causing bending cracks.
[0128] Comparing Comparative Example 3 with each embodiment, it can be seen that the elongation and 180° bending performance of the sample obtained in Comparative Example 3 deteriorated significantly (the elongation decreased from 13% to 8%, and the bending cracked). This shows that an excessively large total reduction in the second cold rolling (such as 60%) will lead to an excessively high matrix dislocation density and severe work hardening. Even without high-temperature annealing, the material will still lose sufficient cold forming ability due to excessive residual stress.
[0129] Comparing Comparative Example 4 with the various embodiments, it can be seen that the tensile strength and yield strength of the sample obtained in Comparative Example 4 deteriorated (tensile strength decreased from 370 MPa to 358 MPa, and yield strength decreased from 290 MPa to 278 MPa). This indicates that when the homogenization heating rate is too high (≥70℃ / h), the atomic diffusion time is insufficient, the primary Al3Mg2 phase in the ingot is not fully dissolved, and the component segregation is not completely eliminated, resulting in a significant decrease in the mechanical properties of the material after subsequent processing.
[0130] Comparing Comparative Example 5 with each embodiment, it can be seen that the gloss, color difference and anodized surface quality of the sample obtained in Comparative Example 5 deteriorated (gloss decreased from 15Gu to 9Gu, color difference increased from 0.22 to 0.26, and material texture defects appeared). This shows that when the homogenization heat preservation temperature is too low (such as 450℃), even if the heat preservation time is extended, the coarse primary Fe-containing phase cannot be dissolved and re-dissolved. The residual coarse second phase causes surface defects during the anodizing process.
[0131] Comparing Comparative Example 6 with the various embodiments, it can be seen that the gloss, color difference and anodized surface quality of the sample obtained in Comparative Example 6 deteriorated significantly (gloss decreased from 15Gu to 8Gu, color difference increased from 0.22 to 0.27, and material texture defects appeared). This indicates that when the homogenization heat preservation temperature is too high (e.g., 550℃) and the heat preservation time is insufficient (e.g., 1h), the ingot grains will grow abnormally, resulting in a decrease in the quality of the anodized surface.
[0132] Comparing Comparative Example 7 with the various embodiments, it can be seen that the tensile strength and yield strength of the sample obtained in Comparative Example 7 deteriorated (tensile strength decreased from 370MPa to 357MPa, and yield strength decreased from 290MPa to 275MPa). This indicates that when the annealing temperature of the finished product is held for a long time (such as 5h), the recovery process of the material is relatively complex, resulting in the material's mechanical properties not meeting the standards.
[0133] Comparing Comparative Example 8 with the various embodiments, it can be seen that the gloss, color difference, and anodized surface quality of the sample obtained in Comparative Example 8 deteriorated (gloss decreased from 15 Gu to 9 Gu, color difference increased from 0.22 to 0.26, and material texture defects appeared). This indicates that excessively high annealing temperature (such as 130℃) will cause a large amount of Al3Mg2 phase to precipitate at the grain boundaries, and it will dissolve violently during anodizing to form pits, resulting in a decrease in surface properties and the generation of material texture.
[0134] In various embodiments:
[0135] Comparing Examples 3 and 4 with Example 1, it can be seen that by optimizing the heating rate of the homogenization treatment in step (3), it is possible to further promote a more uniform rise in the internal temperature field of the ingot, while ensuring that the initial magnesium-containing phase is fully dissolved back into the aluminum matrix, thus providing more sufficient kinetic time for atomic diffusion, thereby more thoroughly eliminating component segregation, improving matrix purity, and obtaining 5-series aluminum alloy plates with higher comprehensive performance.
[0136] Comparing Examples 5 and 6 with Example 1, it can be seen that by optimizing the total reduction rate of the second cold rolling and the holding temperature of the final annealing, it is possible to more effectively promote the formation of a suitable amount of fine dispersed precipitation of Al3Mg2 phase at the grain boundaries, thereby significantly improving the bending toughness of the plate and the surface quality after anodizing.
[0137] Comparing Examples 7 and 8 with Example 1, it can be seen that by optimizing the thickness range of each step, it is possible to better match the process parameters defined by the present invention, so that the obtained ultra-thin sheet can maintain better ductility and surface quality after anodizing while possessing high strength.
[0138] It should be noted that the terms "first," "second," etc., used in the specification and claims of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such terms can be used interchangeably where appropriate so that the embodiments of this application described herein can be implemented, for example, in a sequence other than those described herein.
[0139] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing 5-series aluminum alloy sheet, characterized in that, include: Step S1: Prepare raw materials according to the composition of the 5-series aluminum alloy sheet; The composition of the 5-series aluminum alloy sheet by weight percentage includes 0~0.08wt.% Si, 0~0.15wt.% Fe, 0~0.10wt.% Cu, 0~0.10wt.% Mn, 5.00wt.%~6.00wt.% Mg, 0~0.05wt.% Cr, 0~0.05wt.% Zn, 0~0.03wt.% Ti, with the balance being Al and unavoidable impurity elements; Step S2: The raw material is cast to obtain an alloy ingot; Step S3: The alloy ingot undergoes a single-stage homogenization treatment to obtain a homogenized ingot; the heating rate of the single-stage homogenization treatment is <70℃ / h, the holding temperature is 500℃~520℃, and the holding time is 2h~6h. Step S4: The homogenized ingot is hot-rolled to obtain a first plate; the first plate is cold-rolled to obtain a second plate; the second plate is annealed in the middle to obtain a third plate. Step S5: The third sheet is subjected to a second cold rolling process to obtain a fourth sheet; the fourth sheet is subjected to a finished product annealing process to obtain the 5-series aluminum alloy sheet; the total reduction rate of the second cold rolling process is <50%; the heat preservation temperature of the finished product annealing process is 70℃~120℃, and the heat preservation time is 2h~4h.
2. The method for preparing 5-series aluminum alloy sheet according to claim 1, characterized in that, In step S3, the heating rate of the single-stage homogenization treatment is 40℃ / h~60℃ / h; and / or, In step S5, the total reduction rate of the second cold rolling process is 30%~40%, and the holding temperature of the finished product annealing process is 80℃~100℃.
3. The method for preparing 5-series aluminum alloy sheet according to claim 1 or 2, characterized in that, The thickness of the alloy ingot is 400mm~600mm; The thickness of the first plate is 3.5mm to 5mm; The thickness of the second plate is 0.7mm~0.9mm; The thickness of the fourth plate is 0.5mm to 0.8mm.
4. The method for preparing 5-series aluminum alloy sheet according to any one of claims 1 to 3, characterized in that, In step S2, the casting process is semi-continuous casting, and the casting temperature is 695℃~715℃, and the casting speed is 43mm / min~53mm / min; the crystallizer of the semi-continuous casting is cooled by a circulating cooling water system, wherein the cooling water flow rate is 135m³ / min. 3 / h~147m 3 / h, the cooling water temperature entering the crystallizer is ≤28℃.
5. The method for preparing 5-series aluminum alloy sheet according to any one of claims 1 to 4, characterized in that, In step S4, the initial rolling temperature of the hot rolling process is 480℃~500℃, the final rolling temperature is 280℃~320℃, and the number of rolling passes is 17~19.
6. The method for preparing 5-series aluminum alloy sheet according to any one of claims 1 to 5, characterized in that, In step S4, the total reduction rate of the first cold rolling process is 74% to 86%.
7. The method for preparing 5-series aluminum alloy sheet according to any one of claims 1 to 6, characterized in that, In step S4, the heating rate of the intermediate annealing treatment is >2℃ / s, the holding temperature is 380±10℃, and the holding time is 2s~10s; and / or, the cooling method of the intermediate annealing treatment is water cooling.
8. A 5-series aluminum alloy sheet, characterized in that, The 5-series aluminum alloy sheet is prepared by the method for preparing 5-series aluminum alloy sheet according to any one of claims 1 to 7.
9. The 5-series aluminum alloy sheet according to claim 8, characterized in that, The 5-series aluminum alloy sheet has a tensile strength > 360 MPa, a yield strength > 280 MPa, and an elongation > 10%; and / or, the 5-series aluminum alloy sheet does not crack when bent at 180°; and / or, the 5-series aluminum alloy sheet is anodized to obtain an anodized 5-series aluminum alloy sheet, wherein the gloss of the anodized 5-series aluminum alloy sheet is 10 Gu~20 Gu, and the color difference is < 0.
25.
10. The application of the 5-series aluminum alloy sheet as described in claim 8 or 9 as a structural material and / or surface material in the fields of computers, communications, and consumer electronics products, characterized in that, The 5-series aluminum alloy sheet is anodized to obtain anodized 5-series aluminum alloy sheet, which is then used as the structural material and / or the surface material.