Process for producing high strength and toughness rail with rare earth Y
By using rare earth element Y and specific metallurgical treatment and rolling processes, the problem of premature peeling cracks in rails has been solved, enabling the production of high-strength, high-toughness rails, extending their service life and reducing inclusion content.
Patent Information
- Application Number
- CN202611226410.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-13
- Publication Date
- 2026-11-10
AI Technical Summary
Existing rails are prone to premature spalling cracks during service, which affects train operation safety, and current technology is unable to effectively improve the strength and toughness of rails to reduce such failures.
By employing rare earth Y element smelting and specific rolling processes, and by controlling chemical composition and process parameters, including converter smelting, LF refining, VD treatment and continuous casting processes, combined with the addition of rare earth wire and rolling cooling control, the microstructure of the rail is refined, thereby improving its strength and toughness.
The produced rails possess excellent strength, hardness, and toughness, reducing the formation of early peeling cracks, extending service life, and reducing inclusion content through rare earth purification, thereby improving the overall performance of the rails.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallurgical materials technology, and in particular relates to a production process for high-strength and high-toughness steel rails with rare earth element Y. Background Technology
[0002] During their service life on railway tracks, rails typically experience major failure modes such as wear and spalling. Premature spalling, in particular, can lead to severe damage like spalling and fragmentation, impacting train safety. One way to reduce spalling cracks from a material mechanical property perspective is to increase the material's yield strength, thereby enhancing its resistance to deformation. Therefore, by designing a rational chemical composition and fully utilizing the characteristics of the rolling process, based on the chemical composition and manufacturing processes required by material standards, the strength and toughness of rails can be maximized. This has significant production and economic implications for reducing early-stage spalling cracks in rails.
[0003] Rare earth elements are an important resource in my country, and their effects on materials have been extensively studied both domestically and internationally. Adding trace amounts of rare earth elements can influence the microstructure and mechanical properties of steel. Baogang possesses abundant rare earth resources and has previously utilized rare earth elements in its domestic rail production to purify steel and microalloy it, developing steel products in multiple fields with significant results. This patent provides a production process for adding γ-rare earth elements to improve the strength of export rails. This has significant production and economic implications for fully enhancing the service performance of export rails, leveraging Baogang's rare earth rail advantages, and building the Baogang rare earth rail brand. Summary of the Invention
[0004] The purpose of this invention is to provide a production process for high-strength and high-toughness steel rails by adding rare earth element Y. By adding rare earth element Y, steel rails with good strength and toughness matching are smelted and rolled. The process has unique production efficiency, is energy-saving and environmentally friendly, and has good economic benefits. It is suitable for large-scale production and has good promotion value.
[0005] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:
[0006] This invention discloses a production process for high-strength and high-toughness steel rails incorporating rare earth element Y, comprising:
[0007] The steel rail smelting process is as follows: molten iron → converter smelting → LF refining → VD → continuous casting. Converter smelting employs aluminum-free deoxidation and alloying, with normal argon blowing throughout the refining process. LF refining uses medium-basicity, strongly reducing slag to treat the molten steel, with a deep vacuum time of 15-20 minutes / min; a deep vacuum degree of 7-9 kPa and a soft blowing time of 18-22 minutes / min; the temperature after VD is 1536-1546 °C. Rare earth wire is added at the VD station, and before addition, the [O] content in the steel is measured, with [O] ≤ 10 ppm. During continuous casting, the superheat is controlled between 15-30 °C, and the casting speed is between 0.6 m / min and 0.7 m / min.
[0008] Rail rolling process: Continuous casting billet—sawing—heating—BD1 rolling—BD2 rolling—CCS universal mill continuous rolling—sawing—cooling—head and tail trimming—straightening—inspection—packaging—weighing—warehousing; the billet preheating temperature is no more than 800℃; the heating temperature is 1200℃, and the heating time is no less than 3 hours; the furnace exit temperature is no less than 1100℃, the rolling temperature is 1080℃~1160℃, and the final rolling temperature is 900~950℃; during the cooling process after final rolling, the rail spacing is ≥350mm; compared with the original rolling process, the final rolling temperature is reduced, and rare earth elements are used to refine the steel grains; the cooling interval after rolling is increased to enhance the temperature drop rate of the rail after rolling and refine the internal microstructure.
[0009] The chemical composition of the rail by mass percentage is as follows: C 0.70~0.78%; Si 0.35~0.55%; Mn 0.80~1.20%; P≤0.025%; S≤0.025%; Cr≤0.3%; V+Nb≤0.25%; RE alloy; rare earth Y alloy with 30% rare earth content, added in an amount of 0.003~0.015%; the remainder is Fe and impurities, with a total mass fraction of 100%.
[0010] Furthermore, the mechanical properties of the hot-rolled rails meet the following requirements: tensile strength ≥1080MPa, elongation ≥10%, impact toughness at -40℃ ≥20J, and rail tread hardness ≥330HB.
[0011] Furthermore, the chemical composition of the rail by mass percentage is as follows: C 0.75%; Si 0.43%; Mn 0.98%; P 0.018%; S 0.007%; Cr 0.28%; V 0.13%; Nb 0.04%; Y addition 0.0006%; the remainder is Fe and impurities, with a total mass fraction of 100%.
[0012] Furthermore, the chemical composition of the rail by mass percentage is as follows: C 0.73%; Si 0.50%; Mn 1.00%; P 0.015%; S 0.004%; Cr 0.25%; V 0.2%; Nb 0.03%; Y addition 0.0098%; the remainder is Fe and impurities, with a total mass fraction of 100%.
[0013] Furthermore, the chemical composition of the rail by mass percentage is as follows: C 0.70%; Si 0.52%; Mn 0.98%; P 0.017%; S 0.009%; Cr 0.26%; V 0.16%; Nb 0.04%; Y addition 0.012%; the remainder is Fe and impurities, with a total mass fraction of 100%.
[0014] Furthermore, the mechanical properties of the hot-rolled rails meet the following requirements: tensile strength 1118-1156 MPa, elongation 13-13.5%.
[0015] Furthermore, the impact toughness at -40℃ is ≥20.2-21.8J, and the hardness of the rail tread is 337-340HB.
[0016] The main alloying elements Si, Mn, and Cr added to this material are intended to improve the strength of the rail and ensure a suitable heat treatment temperature for the phase transformation. The C content in this steel is designed to have a high solid solubility with Fe, resulting in solid solution strengthening and improved strength and hardness. Considering the material's toughness and elongation, the C content is set at the upper-middle limit. Mn expands the austenite phase region, increasing the stability of the supercooled austenite and significantly improving the hardenability of the steel. Si reduces the austenite-ferrite transformation rate, improving the steel's strength, elasticity, and tempering resistance. However, considering the weldability of the rail, the Si content should not be too high, as Si has poor thermal conductivity, which is detrimental to rail welding. The main role of Nb and V in the steel is to inhibit grain growth by precipitating fine niobium carbonitrides and vanadium nitrides, thereby refining the austenite grains and simultaneously improving the steel's strength, hardness, and toughness. In addition, the added RE element is a rare earth Y alloy. Basic theoretical research on rare earths has proven that rare earths have the function of controlling the morphology of sulfides during the smelting process, forming rare earth sulfur oxides and reducing the formation of other metal sulfur compounds. This new sulfur compound does not deform or is very small during the rolling process, which refines the grains in the steel. Combined with rolling process control, it hinders grain coarsening and growth, refines the interlamellar spacing of micro-pearl, and improves the toughness of the material after cooling.
[0017] Compared with the prior art, the beneficial technical effects of the present invention are as follows:
[0018] The rail steel of this invention has good strength, hardness and mechanical properties. Rails produced from it meet technical requirements and have improved impact toughness, which plays an important role in reducing and minimizing the formation of early peeling cracks. In addition, the A-level inclusions and C-level inclusions in the steel are reduced, which fully utilizes the purification and modification effects of rare earth elements on steel inclusions and improves the service life of the rails. Detailed Implementation
[0019] A process for producing high-strength and high-toughness steel rails by incorporating rare earth element Y includes:
[0020] The steel rail smelting process is as follows: molten iron → converter smelting → LF refining → VD → continuous casting. Converter smelting employs aluminum-free deoxidation alloying, with normal argon blowing throughout the refining process. LF refining uses medium-basicity, strongly reducing slag to treat the molten steel, with a deep vacuum time of 15-20 minutes / min; a deep vacuum degree of 7-9 kPa and a soft blowing time of 18-22 minutes / min; the temperature after VD is 1536-1546 °C. Rare earth wire is added at the VD station, and before addition, the [O] content in the steel is measured, with [O] ≤ 10 ppm. During continuous casting, the superheat is controlled between 15-30 °C, and the casting speed is between 0.6 m / min and 0.7 m / min.
[0021] Table 1 Comparison of different components during implementation (wt.%)
[0022] Example C Si Mn Cr Nb V Y P S Example 1 0.75 0.43 0.98 0.28 0.04 0.13 0.0038 0.018 0.007 Example 2 0.73 0.5 1 0.25 0.03 0.2 0.0069 0.015 0.004 Example 3 0.7 0.52 0.98 0.26 0.04 0.16 0.0081 0.017 0.009 Comparative Example 0.73 0.47 1.02 0.27 - - - 0.016 0.003
[0023] The rail rolling process is as follows: continuous casting of square billet—sawing—heating—BD1 rolling—BD2 rolling—CCS universal mill continuous rolling—sawing—cooling—head and tail trimming—straightening—inspection—packaging—weighing—warehousing; the temperature of the preheating section of the square billet is not greater than 800℃; the heating temperature is 1200℃, and the heating time is not less than 3 hours; the furnace exit temperature is not lower than 1100℃, the rolling temperature is 1080℃~1160℃, and the final rolling temperature is 900~950℃; during the cooling process after final rolling, the rail spacing is ≥350mm; compared with the original rolling process, the final rolling temperature is reduced, and rare earth elements are used to refine the steel grains; the cooling interval after rolling is increased to enhance the temperature drop rate of the rail after rolling and refine the internal microstructure.
[0024] Properties of rolled steel samples: Tensile test specimens had a diameter d0 = 12.5 mm and a gauge length Lo = 5do. Tread hardness was measured by randomly sampling the rail, with a specimen length of 250 mm. 0.5 mm of the rail head was ground off at five test points. Brinell hardness tests were performed, and the average value was calculated. The test temperature was 20℃ ± 5℃. The experimental results are shown in Table 2. Inclusions were inspected according to method A, and the results are shown in Table 3.
[0025] Table 2 Mechanical properties of each example
[0026] Example Tensile strength σb (MPa) Elongation δ (%) Brinell hardness (HB) Impact toughness (-40℃) / J Example 1 1118 13.0 337 21.2 Example 2 1123 13.5 338 20.2 Example 3 1156 13.0 340 21.8 Comparative Example 1085 12.5 331 15,8
[0027] Table 3. Inclusions in each example
[0028] Example Category A Category B Category C Category D Example 1 1.0 1.0 1.0 1.0 Example 2 0.5 0.5 1.0 0.5 Example 3 0.5 0.5 1.0 0.5 Comparative Example 1.5 1.0 1.5 1.0
[0029] As can be seen from Tables 2 and 3, each example has good strength, hardness and mechanical properties. The rails produced from them meet the technical requirements and the impact toughness is improved, which plays an important role in reducing and minimizing the formation of early peeling cracks. In addition, the A-level inclusions in the steel are reduced and the C-level inclusions are reduced, which fully demonstrates the purification and modification effect of rare earth on steel inclusions and improves the service life of the rails.
[0030] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A production process for high-strength and high-toughness steel rails incorporating rare earth element Y, characterized in that, include: The steel rail smelting process is as follows: molten iron → converter smelting → LF refining → VD → continuous casting; converter smelting adopts aluminum-free deoxidation alloying, and the whole process is carried out with normal argon blowing according to the refining process; LF uses medium basicity and strong reducing refining slag to treat molten steel, with a deep vacuum time of 15~20 min; deep vacuum degree of 7~9 kPa and soft blowing time of 18~22 min; VD temperature of 1536~1546℃; rare earth wire is added at the VD station, and the O content in the steel is measured before addition, with O ≤10ppm; in continuous casting production, the superheat is controlled between 15~30℃, and the casting speed is between 0.6m / min and 0.7m / min; Rail rolling process: Continuous casting billet—sawing—heating—BD1 rolling—BD2 rolling—CCS universal mill continuous rolling—sawing—cooling—head and tail trimming—straightening—inspection—packaging—weighing—warehousing; the billet preheating temperature is no more than 800℃; the heating temperature is 1200℃, and the heating time is no less than 3 hours; the furnace exit temperature is no less than 1100℃, the rolling temperature is 1080℃~1160℃, and the final rolling temperature is 900~950℃; during the cooling process after final rolling, the rail spacing is ≥350mm; compared with the original rolling process, the final rolling temperature is reduced, and rare earth elements are used to refine the steel grains; the cooling interval after rolling is increased to enhance the temperature drop rate of the rail after rolling and refine the internal microstructure. The chemical composition of the rail by mass percentage is as follows: C 0.70~0.78%; Si 0.35~0.55%; Mn 0.80~1.20%; P≤0.025%; S≤0.025%; Cr≤0.3%; V+Nb≤0.25%; RE alloy; rare earth Y alloy with 30% rare earth content, added in an amount of 0.003~0.015%; the remainder is Fe and impurities, with a total mass fraction of 100%.
2. The high-strength and high-toughness rail production process with added rare earth element Y according to claim 1, characterized in that, The mechanical properties of the hot-rolled rails meet the following requirements: tensile strength ≥1080MPa, elongation ≥10%, impact toughness at -40℃ ≥20J, and rail tread hardness ≥330HB.
3. The production process for high-strength and high-toughness steel rails with added rare earth element Y according to claim 1, characterized in that, The chemical composition of the rail by mass percentage is as follows: C 0.75%; Si 0.43%; Mn 0.98%; P 0.018%; S 0.007%; Cr 0.28%; V 0.13%; Nb 0.04%; Y added 0.006%; the remainder is Fe and impurities, with a total mass fraction of 100%.
4. The production process for high-strength and high-toughness steel rails with added rare earth element Y according to claim 1, characterized in that, The chemical composition of the rail by mass percentage is as follows: C 0.73%; Si 0.50%; Mn 1.00%; P 0.015%; S 0.004%; Cr 0.25%; V 0.2%; Nb 0.03%; Y 0.0098%; the remainder is Fe and impurities, with a total mass fraction of 100%.
5. The production process for high-strength and high-toughness steel rails with added rare earth element Y according to claim 1, characterized in that, The chemical composition of the rail by mass percentage is as follows: C 0.70%; Si 0.52%; Mn 0.98%; P 0.017%; S 0.009%; Cr 0.26%; V 0.16%; Nb 0.04%; Y 0.012%; the remainder is Fe and impurities, with a total mass fraction of 100%.
6. The production process for high-strength and high-toughness steel rails with added rare earth element Y according to claim 1, characterized in that, The mechanical properties of the hot-rolled rails meet the following requirements: tensile strength 1118-1156MPa, elongation 13-13.5%.
7. The production process for high-strength and high-toughness steel rails with added rare earth element Y according to claim 6, characterized in that, Impact toughness at -40℃ ≥20.2-21.8J, rail tread hardness 337-340HB.