A Sn-containing martensitic steel, a method for manufacturing the same, a method for welding using the same, and an automobile

By introducing trace amounts of boron into martensitic steel to achieve grain boundary chemical reconstruction, the embrittlement problem caused by Sn grain boundary segregation was solved, resulting in high strength, high toughness, and efficient welding, which is suitable for automobile manufacturing.

CN123063684APending Publication Date: 2026-11-10UNIV OF SCI & TECH BEIJING
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202611430384.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies have failed to effectively solve the embrittlement problem caused by Sn grain boundary segregation in Sn-containing martensitic steel during resistance spot welding, and the welding efficiency is low, which cannot meet the needs of lightweight and efficient automobile production.

Method used

By introducing trace amounts of boron (B) into martensitic steel to perform grain boundary chemical reconstruction, the strong grain boundary segregation driving force of B is used to replace Sn, forming a B-rich and Sn-poor amorphous/disordered interface layer, which suppresses Sn grain boundary segregation. Combined with appropriate welding thermal cycling parameters, the chemical reconstruction of grain boundaries during ultrafast cooling is achieved.

Benefits of technology

It significantly improves the strength and toughness of resistance spot welded joints of Sn-containing martensitic steel, while taking into account efficient welding performance, thus meeting the requirements of automotive lightweighting and efficient production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063684A_ABST
    Figure CN123063684A_ABST
Patent Text Reader

Abstract

The application provides a Sn-containing martensitic steel, a preparation method thereof, a welding method using the same and an automobile, and relates to the technical field of metallurgy. The Sn-containing martensitic steel is composed of the following components: 0.15-0.25% of carbon, 1.5-1.7% of silicon, 1.9-2.2% of manganese, 0.02-0.15% of tin, 15-50 ppm of boron, and the balance of iron and inevitable impurities, with the total mass being 100%. The preparation method of the Sn-containing martensitic steel comprises the following steps: vacuum induction smelting raw materials to obtain molten steel and pouring to obtain a steel ingot; performing first heat treatment, forging, homogenization treatment, rolling, first water quenching, second heat treatment and second water quenching on the steel ingot to obtain the Sn-containing martensitic steel. The Sn-containing martensitic steel provided by the application not only conforms to the application trend of 'high strength and thin specification' of martensitic steel for the light weight of automobiles, but also solves the problem of welding embrittlement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of metallurgical technology, and in particular to a Sn-containing martensitic steel, a method for preparing the same, a method for welding the same, and an automobile. Background Technology

[0002] With the urgent need for "green and low-carbon" and "circular economy" steel in the automotive industry, the smelting of recycled high-strength steel from scrap steel resources such as steel from dismantled end-of-life vehicles has become a mainstream trend. However, scrap steel inevitably carries residual elements such as Cu, Sn, and Sb. Among these, Sn, due to its low oxidation potential, cannot be removed by oxidation slag in conventional steelmaking processes and has a strong tendency for grain boundary segregation. Therefore, in advanced high-strength steel for automobiles, the Sn content gradually increases with the use of scrap steel.

[0003] The performance of resistance spot welded joints in automotive steel determines vehicle body safety. In the field of advanced high-strength steel resistance spot welding, to improve the cross tensile strength (CTS) performance of spot welded joints, broaden the welding process window, and suppress spatter, the most readily available technologies in the industry currently focus on optimizing external welding thermo-mechanical process parameters, adjusting electrode structure, and controlling heat input for different initial microstructures (martensite + ferrite / bainite + martensite + retained austenite / multiphase steel). These technologies significantly reduce production efficiency in actual welding processes. Furthermore, existing technologies do not consider the increase in Sn content due to scrap steel recycling, and even more importantly, they do not address the fundamental issue of Sn grain boundary segregation under ultra-fast cooling leading to deterioration of spot welded joint performance. Representative solutions mainly include the following three categories: (1) Multi-segment spot welding process (using bainitic high-strength steel as the base material, refer to patent document CN 120133680A) 180 Patent document CN 120133680 A discloses a method for improving the CTS performance of bainitic high-strength steel. The initial microstructure of the base material is 70%~90% bainite + 5%~10% martensite + 2%~8% retained austenite. The composition system only restricts P ≤ 0.009% and S ≤ 0.009%, without considering the presence and harmful effects of the residual element Sn. This method employs a three-stage spot welding process. First stage (preheating): Welding time 200~230ms, current 2.5~3.5kA, cooling 100~200ms, used to eliminate surface gaps; Second stage (main welding): welding time 400~520ms, current 7.0~12.0kA, cooling 500~800ms, to promote the growth of the weld nugget; Third stage (tempering): welding time 200~300ms, current 3.5~6.5kA, to improve the structural stress.

[0004] The use of chromium-zirconium-copper spherical electrodes (end face diameter 6.0~8.0mm) is based on the core logic of eliminating shrinkage cavities and segregation in bainitic steel HAZ by extending the cooling time and increasing the welding time. This addresses the issues of tempering softening and structural stress in bainitic structures, rather than grain boundary embrittlement.

[0005] (2) Variable pressure dual-pulse / multi-pulse scheme (using phosphorus-coated zinc-aluminum-magnesium steel and 980MPa zinc-coated multiphase steel as base materials, refer to patent documents CN 116944645 A and CN 119304330 A) Patent document CN 116944645 A addresses a variable pressure dual-pulse process for phosphorus-added high-strength zinc-plated aluminum-magnesium steel sheets (substrate grade HC220YD+ZM, multiphase / deep-drawing microstructure). The process involves pre-pressing (200~300ms, 1.5~2.5kN) → first current (I1=0.5~0.6I2, 100~200ms) → cooling (20~40ms) → second current (I2=I_F-0.2kA, 200~320ms) → holding pressure (20~40ms), and is accompanied by a self-made Cr-Zr-Cu electrode cap (145° truncated cone angle). Its technical problems are attributed to zinc layer volatilization, poor soldering, and solder joint depressions. The base material composition focuses on P, Al, and Ti microalloying, completely neglecting the risk of grain boundary segregation due to residual elements such as Sn.

[0006] Patent document CN 119304330 A addresses the issue of interface failure in 980MPa grade galvanized multiphase steel (CP980+Z, ferrite / bainite multiphase) by employing a solution of ultra-high preheating current (20~25kA, 10~20ms) + multiple pulses (double / triple / quadruple pulses, adjusted according to plate thickness) + long pulse interval (450~750ms). Its initial microstructure is not entirely martensite, and it also attributes embrittlement to zinc layer interference and incomplete bonding of melt nuclei, without addressing the non-equilibrium segregation mechanism of Sn at the original austenite grain boundary (PAGB).

[0007] (3) Three-stage gradual current increase scheme (using 1200MPa grade high-strength galvanized steel as the base material, refer to patent document CN119589081 A) Patent document CN 119589081 A describes a three-stage spot welding method for galvanized high-strength steel (initial microstructure containing martensite / ferrite) with a yield strength ≥900MPa and tensile strength ≥1200MPa: the first stage involves a gradual increase in A2.8~3.8kA, the second stage involves a gradual increase in A4.5~5.2kA to 5.0~11.0kA, and the third stage involves a gradual increase in A4.5~5.5kA to 3.0~5.0kA, combined with specific cooling times (60~100ms, 20~40ms, 0~20ms) and pressure (3.5~4.5kN). This scheme improves the spatter limit current by controlling the overall heat input to regulate the growth rate of the melt nucleus and plastic ring. The design of the base material composition focuses on Mo, Cr, and Nb alloying (C 0.105~0.135%, Si 0.25~0.35%, etc.), and still lists Sn, P, S, etc. as "unavoidable impurities of 0.008~0.020%" and limits them to the upper limit. It does not realize the reality that Sn (0.03~0.08wt%) in recycled steel must exist and needs to be actively controlled at the grain boundary scale.

[0008] The base material composition systems of the aforementioned existing technologies are all geared towards conventionally smelted high-purity / low residual element high-strength steels (bainitic, multiphase, galvanized high-strength steel), and have never taken "regenerated martensitic steel containing 0.03~0.08wt% Sn" as a specific target. Its initial microstructure is mostly bainitic, ferrite-martensite multiphase or hot-formed martensite mixed microstructure. The technical solutions are all limited to external thermo-mechanical parameter repair (current, time, pressure, electrode), and do not solve the problem at the microscale of grain boundary chemical reconstruction (such as B-mediated Sn substitution), resulting in poor CTS performance of spot welded joints of Sn-containing martensitic steel. Summary of the Invention

[0009] The purpose of this application is to provide a Sn-containing martensitic steel, a method for preparing the same, a method for welding the same, and an automobile, in order to solve the above-mentioned problems.

[0010] To achieve the above objectives, this application adopts the following technical solution: A Sn-containing martensitic steel, calculated by total mass, consists of the following components: Carbon 0.15~0.25%, silicon 1.5~1.7%, manganese 1.9~2.2%, tin 0.02~0.15%, boron 15~50 ppm, balance iron and unavoidable impurities.

[0011] Preferably, the boron content is 20-40 ppm and the tin content is 0.03-0.08%.

[0012] This application also provides a method for preparing the Sn-containing martensitic steel described above, comprising: The raw materials are vacuum induction melted to obtain molten steel, which is then cast into steel ingots. The steel ingot is subjected to a first heat treatment, forging, homogenization treatment, rolling, first water quenching, second heat treatment, and second water quenching to obtain the Sn-containing martensitic steel.

[0013] Preferably, the temperature of the first heat treatment is 1150~1250℃ and the time is 1.5-3h.

[0014] Preferably, the homogenization treatment is performed at a temperature of 1150~1250℃ for 40-60 minutes.

[0015] Preferably, the method for preparing Sn-containing martensitic steel satisfies one or more of the following conditions: (1) The thickness of the rolled plate is 1.5-2.5 mm; (2) The final rolling temperature is not lower than 950℃; (3) The temperature of the second heat treatment is 850-950℃ and the time is 20-40min.

[0016] This application also provides a method for welding using the aforementioned Sn-containing martensitic steel, comprising: Weld the two pieces of material to be welded together; The heat input energy density of the welding is 80~180 J / mm². 3 Cooling rate not less than 10 3 K / s.

[0017] Preferably, the welding is resistance spot welding, the current of the resistance spot welding is 8-12kA, the time is 300-400ms, the electrode pressure is 3.0-5.5kN, and the cooling method is natural cooling or circulating water cooling, the water temperature of the circulating water cooling is 15-25℃, and the flow rate is 3-8L / min; the material of the spherical electrode of the resistance spot welding is chromium zirconium copper, and the electrode end face diameter is 6-8mm.

[0018] Preferably, the welding is laser welding, wherein the laser welding power is 1.5-3.0kW, the defocusing amount is +2-+5mm, the pulse time is 10-50ms, and the cooling rate is 10. 4 -10 5 K / s; Alternatively, the welding may be electron beam welding or high-frequency induction welding.

[0019] This application also provides an automobile whose raw material includes the Sn-containing martensitic steel described above; or, Its raw materials include materials obtained by the aforementioned method for preparing Sn-containing martensitic steel.

[0020] Compared with the prior art, the beneficial effects of this application include: The Sn-containing martensitic steel provided in this application achieves fundamental improvement through "boron (B) microalloying to reconstruct the grain boundary chemical composition": Targeted composition: For martensitic steel containing Sn (0.03~0.08 wt%), 20~40 ppm of trace B is introduced to competitively replace Sn by utilizing the stronger grain boundary segregation driving force of B (there is no synergistic regulation of B and Sn in the existing technology). Lightweight adaptability: It works directly on ultra-high strength martensitic steel systems without relying on the "thick-gauge reinforcement" of bainitic / multiphase steel, perfectly matching the characteristic of martensitic steel to "maintain high strength under thin gauge", thus maximizing the lightweight effect; Mechanism differences: By inhibiting the segregation of Sn at the original austenitic grain boundaries through the segregation of B at the original austenitic grain boundaries, the composition of the original austenitic grain boundaries is reconstructed. Efficiency and compatibility: Without relying on the "ultra-long cooling interval" (such as 500~800 ms) common in existing technologies, it can actively reconstruct grain boundary chemistry within the conventional welding cycle and complete grain boundary strengthening, eliminating Sn-induced intergranular embrittlement at the atomic scale, thus balancing performance and efficiency.

[0021] In summary, existing technologies suffer from inherent defects such as unsuitability of the base material system (avoiding Sn), targeted misalignment of the initial microstructure (bainite / multiphase vs. martensite, ignoring the advantages of thin-gauge high strength), lack of microscopic mechanisms, and low process efficiency, making them unable to solve the grain boundary embrittlement problem of Sn-containing ultra-high-strength martensitic steel under ultra-fast cooling. This application proposes for the first time a grain boundary chemical reconstruction scheme based on boron microalloying, filling the gap in existing technologies. This approach not only aligns with the trend of "high strength, thin gauge" application of martensitic steel in automotive lightweighting but also solves the welding embrittlement problem. Attached Figure Description

[0022] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments will be briefly described below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation on the scope of this application.

[0023] Figure 1 This is a schematic diagram of the welding sample from Example 1; Figure 2 Photographs of the tensile testing machines used in the examples and comparative examples; Figure 3 The cross-shaped tensile load curves are for Example 1 and Comparative Example 1. Figure 4 This is a cross-shaped tensile fracture morphology diagram of Example 1; Figure 5 This is the atomic probe chromatography spectrum of Comparative Example 1; Figure 6 This is the atomic probe chromatography spectrum of Example 1. Detailed Implementation

[0024] To better illustrate the technical solution provided in this application, the technical solution will be described in its entirety before the embodiments, as follows: A Sn-containing martensitic steel, calculated by total mass, consists of the following components: Carbon 0.15~0.25% (can be 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25% or any value between 0.15% and 0.25%), silicon 1.5~1.7% (can be 1.5%, 1.6%, 1.7% or any value between 1.5% and 1.7%), manganese 1.9~2.2% (can be 1.9%, 2.0%, 2.1%, 2.2%). 2% or any value between 1.9% and 2.2%, tin 0.02% to 0.15% (can be 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15% or any value between 0.02% and 0.15%), boron 20% to 40% (can be 20%, 30%, 40% or any value between 20% and 40%), balance iron and unavoidable impurities.

[0025] To further explain this application, the technical issues are described in more detail: Based on the technical solutions disclosed in patent documents CN 120133680 A, CN 116944645 A, CN 119304330 A, CN 119589081 A, CN 120572112 A, CN 119260126 A, etc., the existing technology has the following objective shortcomings in solving the problem of spot welding of high-strength steel, which cannot be overcome by its own means: (1) The composition system of the base material does not involve Sn-containing martensitic steel, and the problem of grain boundary segregation of residual element Sn is not recognized. The following patents all design the base material composition for conventional steelmaking and do not consider the residual element Sn as an object requiring active control. For example: CN 120133680 A (Bainitic steel) and CN 119589081 A (1200MPa grade galvanized steel) only generally specify P≤0.009% and S≤0.009%, without mentioning the control of Sn content or the effect of Sn on grain boundary embrittlement; Although CN 116944645 A (phosphorus-plated zinc-aluminum-magnesium steel) focuses on the element P, its technical problems are attributed to "high phosphorus content leading to poor welding and surface depressions", without involving the intergranular embrittlement mechanism related to Sn; The composition design of CN 119304330 A (980MPa galvanized multiphase steel) and CN 120572112 A (hot stamping steel) completely failed to consider the reality that Sn will inevitably accumulate in recycled steel, nor did it propose a solution to reconstruct grain boundary chemistry through microalloying (such as B).

[0026] The above schemes all treat Sn as an "unavoidable impurity" and impose an upper limit on it, rather than designing a specific composition system for martensitic steel containing 0.03~0.08wt% Sn. As a result, they cannot fundamentally suppress grain boundary weakening when facing ultra-high strength steel containing Sn.

[0027] (2) Targeted misalignment of initial microstructure: targeting bainitic / multiphase steel instead of ultra-high-strength martensitic steel, thus missing the potential for lightweighting. The initial microstructure of the base material in existing technologies differs fundamentally from that of this invention, making them unsuitable for meeting the core requirements of automotive lightweighting. CN 120133680 A specifies that its base material is bainitic high-strength steel with "70%~90% bainite + 5%~10% martensite + 2%~8% retained austenite"; CN 119304330 A refers to 980MPa grade galvanized multiphase steel (CP980+Z), and CN 116944645 A refers to phosphorus-added high-strength galvanized aluminum-magnesium steel sheet (HC220YD+ZM), both of which are multiphase or deep-drawing structures; Even for CN 119589081 A (1200MPa grade) and CN 120572112 A (hot stamping steel), which involve ultra-high strength steel, the technical solutions are not specifically optimized for the Sn segregation behavior of the fully martensitic structure under ultra-fast cooling.

[0028] Existing solutions often adopt the approach of "trading low strength and large thickness for safety" (e.g., the strength of bainitic steel is usually below 1200MPa), without utilizing the characteristic of martensitic steel that "can maintain ultra-high strength even with thin dimensions". This means that existing technologies cannot fully realize the potential of martensitic steel in terms of thinning and weight reduction, which does not conform to the development trend of automotive lightweighting that emphasizes both high strength and thin dimensions of materials.

[0029] (3) The technical attribution is limited to macroscopic process optimization and does not touch on the mechanism of grain boundary chemical reconstruction. Existing technological improvements have all remained at the level of adjusting external thermo-mechanical parameters, failing to recognize that Sn grain boundary segregation is the microscopic root cause of intergranular embrittlement. CN 120133680 A attributes the improvement of CTS to "eliminating shrinkage defects, promoting melt nugget growth, and reducing structural stress"; CN 119304330 A attributes the interface failure to "zinc layer interference" and solves it by "dissipating the zinc layer with ultra-large preheating current"; CN 116944645 A attributes the poor solder joint to "phosphorus causing surface depressions" and improves it through "variable pressure double pulse"; CN 119589081 A attributes the narrow spot welding window to "high alloy element content" and alleviates it by "three-stage slow current control of weld nugget growth rate".

[0030] None of the above solutions mentioned the mechanism of "Sn segregation at grain boundaries leading to intergranular embrittlement," nor did they propose a technical approach to achieve chemical reconstruction of grain boundaries through competitive segregation of trace amounts of B. As a result, they could not fundamentally eliminate the grain boundary weakening problem in Sn-containing martensitic steel.

[0031] (4) Welding efficiency is limited by conservative processes and is difficult to adapt to high-speed cycles. To compensate for the unresolved embrittlement problem, existing technologies generally adopt a conservative strategy of extending the welding cycle, which objectively reduces production efficiency. The second-stage welding time of CN 120133680 A reaches 400~520 ms, and the cooling time is even longer, reaching 500~800 ms; CN 119304330 A has a multi-pulse interval time of 450~750 ms (board thickness <1.5mm) or 650~750 ms (board thickness ≥1.5mm). The second stage of welding in CN 119589081 A takes 300-420 ms and emphasizes that "controlling the growth rate of the weld nugget diameter requires long cooling".

[0032] This "time-for-quality" approach results in a single-point welding cycle that far exceeds the conventional cycle time for automotive body-in-white welding (which typically requires a single-point cycle of <1 second), making it difficult to meet the high-efficiency production requirements of modern automobile manufacturing.

[0033] (5) The unresolved contradiction between "high strength" and "high toughness" restricts the improvement of safety. While existing technologies can improve joint strength to some extent, they cannot solve the inherent brittleness problem of ultra-high strength steel. For example, the background technology in CN 120572112 A mentions that hot-stamped steel tends to fail via "interfacial fracture," resulting in "fatigue testing and energy absorption of weld joints failing to meet standards." Due to the lack of grain boundary control methods, existing technologies cannot improve energy absorption and fatigue resistance by enhancing grain boundary toughness while ensuring ultra-high strength (e.g., above 1200 MPa), thus limiting the application of martensitic steel in automotive safety structural components.

[0034] In an optional embodiment, the boron content is 20-40 ppm and the tin content is 0.03-0.08%.

[0035] This application also provides a method for preparing the Sn-containing martensitic steel described above, comprising: The raw materials are vacuum induction melted to obtain molten steel, which is then cast into steel ingots. The steel ingot is subjected to a first heat treatment, forging, homogenization treatment, rolling, first water quenching, second heat treatment, and second water quenching to obtain the Sn-containing martensitic steel.

[0036] In an optional embodiment, the temperature of the first heat treatment is 1150-1250℃ (which can be any value between 1150℃, 1200℃, 1250℃) and the time is 1.5-3h (which can be any value between 1.5h, 2h, 2.5h, 3h).

[0037] In an optional embodiment, the homogenization treatment is performed at a temperature of 1150-1250°C (which can be any value between 1150°C, 1200°C, 1250°C or 1150-1250°C) and for a time of 40-60 min (which can be any value between 40 min, 50 min, 60 min or 40-60 min).

[0038] In an optional embodiment, the method for preparing Sn-containing martensitic steel satisfies one or more of the following conditions: (1) The thickness of the rolled plate is 1.5-2.5 mm (it can be any value between 1.5 mm, 2 mm, 1.5 mm or 1.5-2.5 mm). (2) The final rolling temperature is not lower than 950℃; (3) The temperature of the second heat treatment is 850-950℃ (which can be any value between 850℃, 900℃, 950℃ or 850-950℃), and the time is 40-60min (which can be any value between 40min, 50min, 60min or 40-60min).

[0039] First heat treatment (pre-forging heating): The steel ingot is heated to 1150~1250 ℃ (typically 1200 ℃) and held for 1.5~3 h (typically 2 h). Its purpose is to fully austenitize the as-cast structure, dissolve the coarse carbides and alloy phases precipitated during casting, provide a uniform plastic matrix for subsequent forging deformation, and reduce compositional segregation, laying the foundation for the uniform distribution of microalloying elements such as B and Sn in subsequent processes.

[0040] Forging: The steel ingot, after the first heat treatment, undergoes multiple forging processes. The purpose is to break up the coarse dendritic structure in the cast state, weld the internal pores, significantly improve the density of the steel, and promote subsequent recrystallization through energy storage in plastic deformation, ensuring a good balance of strength and toughness in the final product.

[0041] Homogenization treatment: Hold at 1150~1250 ℃ (typical value 1200 ℃) for 40~60 min (typical value 50 min). This process is particularly critical for Sn-containing steel: on the one hand, it further eliminates microsegregation after forging and prevents Sn from pre-aggregating at grain boundaries; on the other hand, the high-temperature holding promotes the full solid dissolution of microalloying element B into the matrix, avoiding the formation of insoluble BN or Fe2B inclusions.

[0042] Rolling: The homogenized slab is subjected to multiple hot rolling passes, with the final rolling temperature controlled at no less than 900~950 ℃ (typically no less than 950 ℃), ultimately rolling into a thin plate with a thickness of 1.5~2.5 mm (typically 2 mm). Its purpose is to further refine the austenite grains. By controlling the rolling temperature and deformation, the dislocation density and substructure of the final microstructure are regulated, while avoiding excessively high final rolling temperatures that lead to coarse grains, or excessively low temperatures that cause work hardening cracking.

[0043] First water quenching: Water quenching is performed immediately after rolling. The purpose is to rapidly freeze the high-temperature austenitic structure, suppress the transformation of proeutectoid ferrite or pearlite, and directly obtain a full martensite (or martensite + a small amount of retained austenite) structure, ensuring that the initial structure of the base material is the ultra-high strength martensite matrix required by this invention.

[0044] Second heat treatment (tempering before tempering and quenching): The steel plate after the first water quenching is reheated to 850~950 ℃ (typically 900 ℃) and held for 20~40 min (typically 30 min). The purpose of this process is to temper the martensite, eliminate internal stress, and adjust the toughness of the matrix.

[0045] Second water quenching: After the second heat treatment holding is completed, water quenching is performed again. The purpose is to quench the microstructure again into tempered martensite or full martensite, fix the optimized grain boundary chemical composition and microstructure after the second heat treatment, and finally obtain Sn-containing martensitic steel base material with both ultra-high strength and good plasticity, providing an ideal microstructure and compositional basis for grain boundary chemical reconstruction in the subsequent resistance spot welding process.

[0046] This application also provides a method for welding using the aforementioned Sn-containing martensitic steel, comprising: Weld the two pieces of material to be welded together; The heat input energy density of the welding is 80~180 J / mm². 3 (can be 80 J / mm)3 100 J / mm 3 120 J / mm 3 140 J / mm 3 160 J / mm 3 180 J / mm 3 Or 80-180 J / mm 3 (any value between), cooling rate not less than 10 3 K / s.

[0047] Ultra-fast cooling (≥10) in resistance spot welding (or laser welding) 3 During the thermal cycling process (K / s), the stronger grain boundary segregation driving force of B atoms replaces the Sn atoms that have already segregated on PAGB (original austenite grain boundary); at the same time, during the rapid solidification of FZ (fusion zone), a B-rich and Sn-poor amorphous / disordered interface layer is formed, forcing Sn to undergo spatial separation.

[0048] In one optional embodiment, the welding is resistance spot welding, and the resistance spot welding current is 8-12kA (it can be 8kA, 9kA, 10kA, etc.). The resistance welding electrode is made of chromium zirconium copper, with a contact angle of 3.0-5.5 kN. The electrode pressure is 3.0-5.5 kN. The cooling method is natural cooling or circulating water cooling. The circulating water temperature is 15-25℃. The flow rate is 3-8 L / min. The material of the spherical electrode for resistance spot welding is chromium zirconium copper, and the electrode end face diameter is 6-8 mm. Dynamic electrode pressure is introduced during the welding process. For example, high pressure (4~5.5 kN) is applied at peak current to break the oxide film, and the pressure is reduced (3~3.5 kN) during the cooling stage to reduce restraint stress. Combined with grain boundary reconstruction of B, this further prevents crystallization cracks.

[0049] In an optional embodiment, the welding is laser welding, wherein the laser welding power is 1.5-3.0kW, the defocus brightness is +2-+5mm, the pulse time is 10-50ms, and the cooling rate is 10. 4 -10 5 K / s; Alternatively, the welding may be electron beam welding or high-frequency induction welding.

[0050] It should be noted that, in addition to natural cooling, welding cooling can be achieved by high-pressure gas jet cooling (such as helium or nitrogen, pressure 0.5~1.0 MPa) or gas mist cooling, in order to precisely control the cooling curve and ensure that excessive Sn segregation is suppressed before B segregation is completed.

[0051] Those skilled in the art will understand that, regardless of whether it is resistance heating, light energy, electronic kinetic energy, or electromagnetic induction heating, as long as the heat input energy density is controlled within 80~180 J / mm² during the actual welding process... 3 Within the range, and ensure that the melt core and heat-affected zone are at least 10 3 Cooling at a rate of K / s can activate the segregation inhibition effect of boron atoms on tin atoms during ultrafast cooling, thereby improving joint performance. Therefore, all welding methods that meet the above-mentioned thermal cycling characteristics fall within the protection scope of this invention.

[0052] This application also provides an automobile whose raw material includes the Sn-containing martensitic steel described above; or, Its raw materials include materials obtained by the aforementioned method for preparing Sn-containing martensitic steel.

[0053] The implementation schemes of this application will be described in detail below with reference to specific embodiments. However, those skilled in the art will understand that the following embodiments are only for illustrating this application and should not be regarded as limiting the scope of this application. Unless otherwise specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments used without specified manufacturers are all conventional products that can be purchased commercially.

[0054] Example 1 This embodiment provides a Sn-containing martensitic steel with the following composition (wt%): C 0.21%, Si 1.60%, Mn 2.07%, Sn 0.05%, B 27 ppm (precisely added), with the balance being Fe and unavoidable impurities.

[0055] The preparation method of the above-mentioned Sn-containing martensitic steel is as follows: The raw materials are vacuum induction melted to obtain molten steel, which is then cast into steel ingots. The steel ingot was heated to 1200 ℃ and held for 2 hours before forging. The forged steel was cut into small slabs, homogenized at 1200 ℃ for 50 minutes, and then rolled in five passes. The slabs were rolled into 2 mm thick plates with a final rolling temperature of not less than 950 ℃, and immediately water-quenched after rolling. Finally, the plates were reheated to 900 ℃, held for 30 minutes, and water-quenched again. Before resistance spot welding, the oxide scale on the surface of the hot-rolled plates was removed, reducing the plate thickness from 2 mm to 1.5 mm, and the surface was cleaned to remove oil and impurities.

[0056] Resistance spot welding: The recommended sample size for welding is 30×100 mm, such as... Figure 1 As shown. A spherical electrode made of chromium-zirconium copper was selected, with an electrode end diameter of 6.0 mm. This electrode selection is consistent with the electrode specifications in CN 120133680 A and CN 116944645 A. Two samples were vertically overlapped and placed between the upper and lower electrodes, and welded using a medium-frequency inverter DC resistance spot welder. The key process parameters were set as follows: welding current 10kA, welding time 360ms, electrode pressure 4kN, cooling method using circulating water with a water temperature controlled at 20±5℃ and a flow rate of 3 L / min, and a post-weld pressure holding time of 360ms.

[0057] After the above processing, the cross tensile properties were tested using a tensile testing machine at a speed of 5 mm / min. Figure 2 As shown. The cross tensile test continued until the sample completely fractured, and the fracture surface exhibited typical rock-like intergranular brittleness characteristics.

[0058] Cross tensile test results: Peak load approximately 8000 N, joint energy absorption approximately 72 J, such as Figure 3 As shown, the fracture morphology completely transforms from intergranular brittle fracture to dimple ductile fracture, as... Figure 4 As shown, this invention represents the first time that a fundamental performance breakthrough has been achieved in a tin-containing martensitic steel system through grain boundary chemical reconstruction, without any degradation.

[0059] Analysis: Under the exact same Sn content, preparation process and welding parameters, the joint performance underwent a qualitative leap simply by adding a trace amount of 27 ppm of B.

[0060] Example 2 This embodiment provides a Sn-containing martensitic steel with the following composition (wt%): C 0.20%, Si 1.59%, Mn 2.08%, Sn 0.05%, B 26 ppm (precisely added), with the balance being Fe and unavoidable impurities.

[0061] The preparation method of the above-mentioned Sn-containing martensitic steel is as follows: The raw materials are vacuum induction melted to obtain molten steel, which is then cast into steel ingots. The steel ingot is heated to 1200 ℃ and held for 1.5 hours before forging. The forged steel is cut into small slabs, homogenized at 1200 ℃ for 50 minutes, and then rolled in five passes to produce a 2 mm thick sheet. The final rolling temperature is not lower than 950 ℃, and the sheet is immediately water-quenched after rolling. Finally, the sheet is reheated to 900 ℃, held for 30 minutes, and water-quenched again. Before resistance spot welding, the oxide scale on the surface of the hot-rolled sheet is removed, the sheet thickness is reduced from 2 mm to 1.5 mm, and the surface is cleaned to remove oil and impurities.

[0062] Resistance spot welding: The recommended sample size for welding is 30×100 mm. A spherical electrode made of chromium-zirconium copper is selected, with an electrode end diameter of 6.0 mm. This electrode selection is consistent with the electrode specifications in CN 120133680 A and CN 116944645 A. Two samples are vertically overlapped and placed between the upper and lower electrodes, and welding is performed using a medium-frequency inverter DC resistance spot welder. The key process parameters are set as follows: welding current 10kA, welding time 360ms, electrode pressure 4kN, cooling method using circulating water with a water temperature controlled at 20±5℃ and a flow rate of 3 L / min, and a post-weld pressure holding time of 360ms.

[0063] After the above processing, the cross tensile properties were tested using a tensile testing machine at a speed of 5 mm / min. The cross tensile test continued until the sample completely fractured, and the fracture surface exhibited typical rock-like intergranular brittleness characteristics.

[0064] Cross tensile test results: peak load approximately 8100 N, joint energy absorption approximately 72 J. The fracture morphology completely transformed from intergranular brittle fracture to dimple ductile fracture. This invention represents the first time that a fundamental performance breakthrough has been achieved in a tin-containing martensitic steel system through grain boundary chemical reconstruction, without any degradation.

[0065] Analysis: With identical Sn and B contents and welding parameters, only the holding time of the first heat treatment was changed, and the joint performance did not change significantly.

[0066] Example 3 This embodiment provides a Sn-containing martensitic steel with the following composition (wt%): C 0.19%, Si 1.57%, Mn 2.00%, Sn 0.05%, B 16 ppm (precisely added), with the balance being Fe and unavoidable impurities.

[0067] The preparation method of the above-mentioned Sn-containing martensitic steel is as follows: The raw materials are vacuum induction melted to obtain molten steel, which is then cast into steel ingots. The steel ingot was heated to 1200 ℃ and held for 2 hours before forging. The forged steel was cut into small slabs, homogenized at 1200 ℃ for 50 minutes, and then rolled in five passes. The slabs were rolled into 2 mm thick plates with a final rolling temperature of not less than 950 ℃, and immediately water-quenched after rolling. Finally, the plates were reheated to 900 ℃, held for 30 minutes, and water-quenched again. Before resistance spot welding, the oxide scale on the surface of the hot-rolled plates was removed, reducing the plate thickness from 2 mm to 1.5 mm, and the surface was cleaned to remove oil and impurities.

[0068] Resistance spot welding: The recommended sample size for welding is 30×100 mm. A spherical electrode made of chromium-zirconium copper is selected, with an electrode end diameter of 6.0 mm. This electrode selection is consistent with the electrode specifications in CN 120133680 A and CN 116944645 A. Two samples are vertically overlapped and placed between the upper and lower electrodes, and welding is performed using a medium-frequency inverter DC resistance spot welder. The key process parameters are: welding current 10kA, welding time 360ms, electrode pressure 4.5kN, cooling method using circulating water with a water temperature controlled at 20±5℃ and a flow rate of 3L / min, and a post-weld pressure holding time of 360ms.

[0069] After the above processing, the cross tensile properties were tested using a tensile testing machine at a speed of 5 mm / min. The cross tensile test continued until the sample completely fractured, and the fracture surface exhibited typical rock-like intergranular brittleness characteristics.

[0070] Cross tensile test results: peak load approximately 7600 N, joint energy absorption approximately 66 J. The fracture morphology completely transformed from intergranular brittle fracture to dimple ductile fracture. This invention represents the first time that a fundamental performance breakthrough has been achieved in a tin-containing martensitic steel system through grain boundary chemical reconstruction, without any degradation.

[0071] Analysis: With identical Sn and B contents and preparation processes, only the welding pressure was changed, and the joint performance did not change significantly.

[0072] Comparative Example 1 Unlike Example 1, B is not added; instead, iron is used.

[0073] Cross tensile test results: peak load was approximately 5400 N, a decrease of approximately 36% compared to Example 1; joint energy absorption was approximately 21 J.

[0074] Analysis: Under identical preparation processes and welding parameters, the addition of only 0.05 wt% Sn without the addition of B resulted in catastrophic degradation of the joint performance. This directly demonstrates that the addition of trace amounts of B can eliminate Sn-induced embrittlement through grain boundary competitive segregation.

[0075] Comparative Example 2 Unlike Example 1, no B was added, and the Sn content was 0.11%.

[0076] Cross tensile test results: peak load 4500 N, joint energy absorption approximately 14 J.

[0077] Analysis: Under the same preparation process and welding parameters, the performance of spot welded joints gradually deteriorates with the increase of Sn content.

[0078] Comparative Example 3 Unlike Example 1, B and Sn are not added; instead, iron is used.

[0079] Cross tensile test results: peak load 8500 N, joint energy absorption approximately 105 J.

[0080] Analysis: Since the base material does not contain Sn, there is no Sn grain boundary segregation problem. Even without adding Bo, the welded joint still maintains good plasticity and toughness. This proves that in the absence of Sn, the spot weld embrittlement problem of Sn-containing martensitic steel does not exist at all, which conversely confirms that Sn is the root cause of embrittlement.

[0081] Comparative Example 4 Unlike Example 1, the content of B is 12 ppm.

[0082] Cross tensile test results: peak load 6200N, joint energy absorption approximately 38 J.

[0083] Analysis: Under the same preparation process and welding parameters, the reduction of B content led to a significant decrease in the performance of the spot weld joint, but it was still slightly higher than that of Comparative Example 1, proving that the addition of B still has a regulatory effect.

[0084] Grain boundary segregation characterization: The implementation mechanism of the technical solution of this invention is the essence that distinguishes it from existing technologies. Atomic probe chromatography (APT) quantitative data show that there is significant Sn grain boundary segregation in the B-free steel (Comparative Example 1), with an excess of 2.26 ± 0.081 atoms nm. -2 ,like Figure 5 As shown. After the microalloying treatment with B according to the present invention (Example 1), the excess amount of B at the grain boundaries reaches 3.52 ± 0.15 atoms nm. -2 Meanwhile, the excess Sn at the grain boundaries decreased to 0.048 ± 0.056 atoms nm. -2 Approaching zero segregation level, such as Figure 6As shown. The corresponding macroscopic properties are a cross tensile load ≥8000 N, energy absorption ≥70 J, and the fracture mode completely changes from intergranular to dimple plasticity. Existing technologies such as CN 120133680 A only eliminate shrinkage cavities and segregation by extending the cooling time, and CN 116944645 A only solves cold solder joints by varying the pressure, neither of which involves the aforementioned atomic-scale grain boundary chemical reconstruction process.

[0085] Compared with existing technologies, this invention not only achieves a breakthrough improvement in macroscopic mechanical properties, but also solves the problem of grain boundary embrittlement of Sn-containing martensitic steel under ultrafast cooling conditions at the microscopic mechanism level.

[0086] First, this invention elevates Sn from an "impurity" to a "controllable target" by introducing trace amounts of boron (B). Utilizing the competitive relationship between B and Sn in grain boundary segregation, it fundamentally improves the grain boundary chemical environment. Existing technologies (such as CN 120133680A and CN 119589081A) do not consider the Sn enrichment problem caused by scrap steel recycling, nor do they recognize that Sn atoms segregate towards the original austenite grain boundaries during the ultrafast cooling process of resistance spot welding, leading to a sharp decrease in grain boundary binding energy. This invention, based on the principle of "competitive segregation," utilizes the stronger grain boundary adsorption capacity of B atoms to thermodynamically preemptively occupy active grain boundary sites. This targeted improvement in composition design directly brings about a qualitative change in grain boundary composition: according to quantitative analysis of atomic probe chromatography (APT) data, after implementing this invention, the excess boron at the grain boundaries reaches 3.52 ± 0.15 atoms nm. -2 Meanwhile, the excess Sn at the grain boundaries is suppressed to 0.048 ± 0.056 atoms nm. -2 The Sn atoms are at extremely low levels. This means that Sn atoms are effectively "squeezed out" of the grain boundaries, eliminating the material basis for intergranular embrittlement at its source. In contrast, existing technologies, lacking such grain boundary chemical control methods, cannot change the enrichment state of Sn atoms at the grain boundaries in Sn-containing steel, even with concessions in process parameters (such as significantly extending the cooling time).

[0087] Secondly, based on the aforementioned mechanism of microscopic grain boundary reconstruction, this invention achieves unexpected technical effects in macroscopic cross tensile (CTS) performance. Existing technologies, such as CN 120133680 A, can improve the CTS performance of bainitic steel to 12.27 kN using a three-stage spot welding process, but the microstructure of the base material is fundamentally different from the fully martensitic steel of this invention, and it does not face the challenge of Sn segregation. In contrast, this invention, when facing the more difficult-to-weld material system of Sn-containing martensitic steel, increases the peak cross tensile load from approximately 5400 N in the non-B-containing control sample to over 8000 N through boron-mediated grain boundary strengthening, an increase of approximately 40%. More significantly, the joint energy absorption jumps from approximately 20 J to approximately 70 J, an increase of approximately 250%. While existing technologies (such as CN 119304330 A) eliminate zinc layer interference through ultra-large preheating current, they only address the interface contact problem and do not address the essence of grain boundary bonding. This invention significantly improves the intrinsic bonding strength of grain boundaries through chemical reconstruction, enabling the joint to absorb more energy and undergo plastic deformation when subjected to tensile loads, rather than suddenly breaking in a brittle state.

[0088] Third, this invention achieves a fundamental shift in the fracture mode, a key indicator for measuring the toughness of welded joints. In conventional welded joints without boron (B) control samples and existing technologies, due to the grain boundary segregation of Sn, the fracture surface typically exhibits a typical "candy-like" intergranular brittle characteristic, indicating that cracks propagate along the grain boundaries, resulting in extremely poor joint reliability. However, this invention successfully implements the competitive substitution of Sn by B, completely transforming the fracture morphology into dimple ductile fracture. The mechanism of this transformation lies in the purification of grain boundaries by the introduction of B. This shift in fracture mode directly demonstrates the effectiveness of this invention in solving the Sn embrittlement problem and provides a solid guarantee of reliability for the application of Sn-containing martensitic steel in automotive safety structural components. No existing technology has achieved such a thorough shift in fracture mode without relying on complex heat treatment or expensive alloying.

[0089] Finally, this invention perfectly balances performance improvement with production efficiency, overcoming the inherent drawback of prior art's "trading time for quality." Existing technologies (such as CN 120133680 A) require cooling times of 500-800 ms to alleviate unresolved grain boundary embrittlement; CN 119304330 A uses pulse intervals of 450-750 ms. These long-cycle processes significantly reduce production efficiency, making it difficult to meet the high-speed cycle requirements of 60-80 weld points per minute in modern automotive manufacturing. This invention, however, is different. Since grain boundary reconstruction is spontaneously completed through atomic diffusion during ultrafast cooling, it does not rely on lengthy thermal cycles. Therefore, this invention can complete high-quality welding in conventional or even shorter welding times. This "high efficiency and high quality" characteristic makes this invention not only technologically advanced but also highly valuable for industrial application, perfectly meeting the dual demands of high-performance materials and high-efficiency manufacturing in automotive lightweighting.

[0090] In summary, this invention solves the grain boundary embrittlement problem of Sn-containing martensitic steel at the atomic scale through the technical solution of "trace B composition design + ultrafast cooling grain boundary reconstruction". It has achieved significant results in multiple dimensions such as cross tensile load, energy absorption, fracture mode and production efficiency, which are superior to the existing technology. Moreover, there is a strict causal relationship between these effects, which is in line with the basic principles of materials science and welding technology.

[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.

Claims

1. A Sn-containing martensitic steel, characterized in that, Based on a total mass of 100%, it consists of the following components: Carbon 0.15~0.25%, silicon 1.5~1.7%, manganese 1.9~2.2%, tin 0.02~0.15%, boron 15~50 ppm, balance iron and unavoidable impurities.

2. The Sn-containing martensitic steel according to claim 1, characterized in that, The boron content is 20-40 ppm, and the tin content is 0.03-0.08%.

3. A method for preparing Sn-containing martensitic steel according to claim 1 or 2, characterized in that, include: The raw materials are vacuum induction melted to obtain molten steel, which is then cast into steel ingots. The steel ingot is subjected to a first heat treatment, forging, homogenization treatment, rolling, first water quenching, second heat treatment, and second water quenching to obtain the Sn-containing martensitic steel.

4. The method for preparing Sn-containing martensitic steel according to claim 3, characterized in that, The temperature of the first heat treatment is 1150-1250℃, and the time is 1.5-3h.

5. The method for preparing Sn-containing martensitic steel according to claim 3, characterized in that, The homogenization process is carried out at a temperature of 1150-1250℃ for 40-60 minutes.

6. The method for preparing Sn-containing martensitic steel according to any one of claims 3-5, characterized in that, One or more of the following conditions must be met: (1) The thickness of the rolled plate is 1.5-2.5 mm; (2) The final rolling temperature is not lower than 950℃; (3) The temperature of the second heat treatment is 850-950℃ and the time is 40-60min.

7. A method for welding Sn-containing martensitic steel according to claim 1 or 2, characterized in that, include: Weld the two pieces of material to be welded together; The heat input energy density of the welding is 80~180 J / mm². 3 Cooling rate not less than 10 3 K / s.

8. The method according to claim 7, characterized in that, The welding is resistance spot welding, with a current of 8-12kA, a time of 300-400ms, an electrode pressure of 3.0-5.5kN, and a cooling method of natural cooling or circulating water cooling. The circulating water cooling water temperature is 15-25℃, and the flow rate is 3-8L / min. The spherical electrode of the resistance spot welding is made of chromium zirconium copper, and the electrode end face diameter is 6-8mm.

9. The method according to claim 7, characterized in that, The welding is laser welding, with a power of 1.5-3.0kW, a defocusing amount of +2-+5mm, a pulse time of 10-50ms, and a cooling rate of 10. 4 -10 5 K / s; Alternatively, the welding may be electron beam welding or high-frequency induction welding.

10. A car, characterized in that, Its raw materials include the Sn-containing martensitic steel as described in claim 1 or 2; or, The raw materials include those prepared by the method for preparing Sn-containing martensitic steel as described in any one of claims 3-6.

Citation Information

Patent Citations

  • Phosphorus-added high-strength zinc-aluminum-magnesium-plated steel plate spot welding process

    CN116944645A

  • Method for improving welding spot quality of resistance spot welding of three-layer board

    CN119260126A

  • Method for solving interface failure of resistance spot-welded joint of 980MPa-grade galvanized complex-phase steel plate

    CN119304330A

  • Method for lifting 1200 MPa-grade high-strength galvanized steel spot welding window

    CN119589081A

  • Bainite-based high-strength steel and CTS performance improving method thereof

    CN120133680A