An Al-Mg-Si alloy sheet, its preparation method and application

By combining ingot heating and homogenization treatment in the production of Al-Mg-Si alloy plates, using hot rough rolling with large reduction and cold rolling with large processing rate, and combining Mn and Cr dispersed phase pinning of grain boundaries and solid solution pre-aging treatment, the problems of redundancy and high energy consumption caused by independent homogenization and intermediate annealing are solved, and the preparation of plates with uniform structure and good isotropy is achieved, thus improving the stamping forming performance.

CN123063699APending Publication Date: 2026-11-10GUANGXI NANNAN ALUMINUM PROCESSING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611587010.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-14
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the existing Al-Mg-Si alloy sheet production process, the independent homogenization annealing and cold rolling intermediate annealing processes are lengthy and energy-intensive. Moreover, it is difficult to obtain sheets with uniform microstructure and good isotropy without eliminating these processes, which affects the stamping performance.

Method used

By combining ingot heating and homogenization treatment, using hot rough rolling with large reduction and cold rolling with large processing rate, combined with Mn and Cr dispersed phase pinning of grain boundaries and solution pre-aging treatment, the independent homogenization and intermediate annealing are eliminated, so that ingot homogenization and heating can be completed at the same time, and cold rolling can be performed directly after hot rolling, retaining deformation energy storage until the solution stage.

Benefits of technology

To obtain sheet metal with low cube texture volume fraction, high proportion of randomly oriented grains, fine grains and plastic strain ratio anisotropy Δr≤0.10, to meet the stringent requirements of automotive four doors and two covers and outer panels, shorten the process flow and reduce energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063699A_ABST
    Figure CN123063699A_ABST
Patent Text Reader

Abstract

This invention discloses an Al-Mg-Si alloy sheet, its preparation method, and its applications, belonging to the field of aluminum alloy material technology. The method includes melting and casting, ingot machining, heating, hot rolling, cold rolling, solution quenching, and pre-aging. After machining, the ingot is not subjected to independent homogenization annealing; instead, it is directly heated so that homogenization and heating are completed in the same process. Hot rough rolling uses a large reduction, and the hot finish rolling temperature is 360-420℃, followed by natural air cooling to below 60℃. Cold rolling is performed directly with a single-pass processing rate of 40-52%, without intermediate annealing before or between passes. Solution quenching and pre-aging are performed on the continuous annealing line. This invention shortens the process, reduces energy consumption, and yields a sheet with a cube texture ≤8%, random orientation grains ≥50%, grain size ≤23μm, and Δr ≤0.10, exhibiting excellent isotropy, making it suitable for automotive body panels.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aluminum alloy material technology, specifically relating to an Al-Mg-Si alloy sheet, its preparation method, and its application. Background Technology

[0002] Al-Mg-Si alloys (6xxx series aluminum alloys) possess high specific strength, good stamping formability, excellent corrosion resistance, and high recycling value, making them the preferred material for lightweight automotive components, especially for sheet metal parts used in the four doors, two hoods, and body panels of new energy vehicles. The plastic strain ratio anisotropy Δr is a key indicator for measuring the isotropy of sheet metal; excessively large Δr will directly lead to issues such as earing, uneven wall thickness, and poor forming consistency during stamping.

[0003] The properties of Al-Mg-Si alloy sheets are significantly affected by texture and the second phase, which in turn depend primarily on processes such as heating, hot rolling, cold rolling, and heat treatment. Traditional production processes typically require homogenization annealing of the ingots and control of the pass rate and rolling temperature during rolling. Additionally, intermediate annealing is introduced during the cold rolling stage to reduce material anisotropy. A typical process flow is: melting and casting → ingot homogenization heat treatment → ingot milling → ingot heating → hot rolling (single pass reduction generally not exceeding 40 mm) → cold rolling (single pass reduction generally not exceeding 40%) → intermediate annealing → cold rolling → solution quenching → pre-aging treatment → T4P state coil.

[0004] The process has the following shortcomings: First, the homogenization annealing is separated from the subsequent heating process, requiring the ingot to undergo an independent heat treatment cycle of "homogenization—cooling—machining—reheating," which is lengthy and energy-intensive. Second, although homogenization can eliminate dendrite segregation, prolonged high-temperature holding can cause the second phase to coarsen and spheroidize, and the solute distribution to tend towards equilibrium. This leads to a decrease in dislocation multiplication and energy storage capacity during subsequent hot rolling deformation, as well as insufficient recrystallization driving force, which is not conducive to obtaining a fine, uniform, and randomly oriented recrystallized structure. Third, the reduction in hot rolling and cold rolling passes is relatively small, resulting in insufficient utilization of deformation energy storage and difficulty in fully breaking down the cast dendrites and second-phase network through large deformation. Fourth, although intermediate annealing can weaken the deformation texture to some extent, its recovery and recrystallization process may promote the preferential nucleation and growth of cube-oriented grains, thereby increasing the cube texture ratio and promoting grain coarsening.

[0005] In the prior art, CN118957367A discloses a 6000 series aluminum alloy material for automotive body panels and its efficient and low-carbon preparation method. This method involves hot-rolling a cast alloy ingot directly after homogenization heat treatment without cooling, followed by self-annealing at room temperature. The hot-rolled strip coil is then directly cold-rolled without intermediate annealing, and finally, a T4P state sheet is obtained through solution quenching and pre-aging treatment. This method eliminates intermediate annealing during cold rolling and omits the cooling and reheating steps after homogenization, thus shortening the process to some extent. However, although the pre-hot working process is directly connected to hot rolling, it does not employ high-reduction hot rough rolling. Furthermore, the self-annealing at room temperature after hot rolling releases the deformation energy accumulated during hot rolling before cold rolling, failing to retain the stored energy for recrystallization nucleation in the subsequent solution stage. Additionally, this method does not effectively control the cube texture ratio, the proportion of randomly oriented grains, and the anisotropy Δr of the plastic strain ratio.

[0006] Therefore, how to compensate for the homogenization and texture weakening functions of the above two processes by coordinating the process parameters of heating, hot rolling, cold rolling and heat treatment without independent homogenization annealing and cold rolling intermediate annealing, and obtain Al-Mg-Si alloy plates with uniform structure and good isotropy, while shortening the process flow and reducing energy consumption, has become an urgent technical problem to be solved in this field. Summary of the Invention

[0007] In view of the above, it is necessary to provide an Al-Mg-Si alloy plate, its preparation method and application, so as to obtain a plate with low cube texture, high random orientation, fine grain and Δr≤0.10 without eliminating independent homogenization and intermediate annealing.

[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0009] A method for preparing Al-Mg-Si alloy sheet includes melting and casting, ingot machining, ingot heating, hot rolling, cold rolling, solution quenching, and pre-aging treatment. Ingot machining includes head and tail trimming and milling. After machining, no independent homogenization annealing is performed; instead, the ingot is directly heated at a temperature of 520-580℃ for 5-30 hours, ensuring homogenization and heating are completed in the same process. Hot rolling includes hot roughing and hot finishing. The hot roughing is performed in multiple passes to roll the ingot to a sheet thickness of 20-40 mm, with each pass reducing the thickness by 45-55 mm. Hot finishing rolling involves rolling the sheet material into coils 5-10 mm thick through multiple passes, with a final rolling temperature of 360-420℃. After hot rolling, the coils are naturally air-cooled to below 60℃. The cold rolling process involves directly cold-rolling the naturally air-cooled coils to 0.7-1.2 mm thick using a single-pass processing rate of 40-52%. No intermediate annealing is performed before or between cold rolling passes. Solution quenching and pre-aging treatments are then performed sequentially on a continuous annealing line. The solution quenching temperature is 520-580℃, the pre-aging temperature is 200-300℃, and the strip running speed is 30-50 m / min.

[0010] In this invention, the chemical composition of the ingot, by mass percentage, is as follows: Si: 0.4-1.4%, Fe: ≤0.5%, Cu: ≤0.5%, Mn: 0.05-0.3%, Mg: 0.35-0.8%, Cr: 0.01-0.05%, Zn: ≤0.3%, Ti: ≤0.3%, with the balance being aluminum and unavoidable impurities; each unavoidable impurity element is <0.05%, and the total amount of unavoidable impurity elements is <0.10%; wherein, Si, Cu, Mn, Fe, and Ti are added in the form of Al-20Si, Al-50Cu, Al-10Mn, Al-10Fe, and Al-6Ti master alloys, respectively, and Mg is added in the form of pure magnesium; the mass ratio of Mg to Si in the ingot is 0.4-1.1; and Mn and Cr form dispersed phases pinning grain boundaries during hot rolling and solution treatment to inhibit grain growth.

[0011] In this invention, the ingot is further heated at a temperature of 570-580°C and held for 5-10 hours.

[0012] In this invention, the reduction in each pass of the hot roughing is 48-55 mm, and the final rolling temperature of the hot finishing is 380-420℃.

[0013] In this invention, the cold rolling process is further described as three passes, with a total cold rolling processing rate of 80-90% and a single pass processing rate of 40-52%; preferably, the single pass processing rate is 45-50%.

[0014] In this invention, the solution quenching temperature is 520-560℃, the pre-aging temperature is 220-280℃, and the strip running speed is 40-50m / min.

[0015] The present invention also proposes a method for preparing the Al-Mg-Si alloy sheet, wherein the Al-Mg-Si alloy sheet has a cube texture volume fraction ≤8%, a random orientation grain volume fraction ≥50%, an average grain size ≤23μm, and a plastic strain ratio anisotropy Δr ≤0.10; preferably, the cube texture volume fraction ≤7.5%, the random orientation grain volume fraction ≥52%, the average grain size ≤22.5μm, and Δr ≤0.09; wherein the texture volume fraction and the average grain size are analyzed and characterized by scanning electron microscopy electron backscatter diffraction (EBSD) technique, and Δr is determined according to GB / T 5027.

[0016] In this invention, the ingot heating is 570-580℃ and held for 5-10 hours; the reduction in each pass of the hot rough rolling is 48-55 mm; the final rolling temperature of the hot finish rolling is 400-420℃; the solution quenching temperature is 520-560℃; the pre-aging temperature is 220-280℃; and the strip running speed is 40-50 m / min.

[0017] The present invention also proposes an Al-Mg-Si alloy sheet, which is prepared by the method described above, wherein the Al-Mg-Si alloy sheet has a cube texture volume fraction ≤8%, a random orientation grain volume fraction ≥50%, an average grain size ≤23μm, and a plastic strain ratio anisotropy Δr ≤0.10; wherein the texture volume fraction and the average grain size are characterized by scanning electron microscopy electron backscatter diffraction (EBSD) technique, and Δr is determined according to GB / T 5027.

[0018] The present invention also proposes the application of the Al-Mg-Si alloy sheet in the preparation of outer panels for automobile four doors and two covers or automobile body panels.

[0019] Compared with the prior art, the present invention has at least the following beneficial effects.

[0020] 1. Under the premise of eliminating independent homogenization annealing and cold rolling intermediate annealing, the Al-Mg-Si alloy sheet obtained by this invention has a cube texture volume fraction of 6.44%-7.39%, a random orientation grain volume fraction of 52.67%-60.11%, an average grain size of 20.46-22.56 μm, and a plastic strain ratio anisotropy Δr of 0.07-0.10. In contrast, the corresponding values ​​of Comparative Examples 1-10, which did not adopt the process synergy scheme of this invention, are 8.63%-14.29%, 31.12%-48.26%, 22.18-38.45 μm, and 0.12-0.20, respectively. Among them, Comparative Examples 1-6 still retain the intermediate annealing of cold rolling (Comparative Examples 4-6 also retain an independent homogenization treatment), with a cube texture of 12.34%-13.88% and Δr of 0.12-0.16; although Comparative Examples 7-9 also canceled the independent homogenization and intermediate annealing, their Δr is still as high as 0.18-0.20 because the key process parameters deviate from the scope of this invention. It can be seen that the technical effect of this invention does not stem from the simplification of the process itself, but from the coordinated control of the parameters of each process. This invention achieves both a short process and high isotropy. Δr≤0.10 means that the tendency to form ears is small, the wall thickness distribution is uniform, and the forming consistency is good during sheet metal stamping, which can meet the stringent requirements of automotive four doors and two hoods and outer panels for body panels.

[0021] 2. This invention achieves "deformation homogenization" instead of "diffusion homogenization" by combining ingot heating and homogenization with large reduction in hot rough rolling. Ingot heating (520-580℃, held for 5-30 hours) completes homogenization and heating simultaneously, avoiding the problems of pre-equilibration of the as-cast microstructure, pre-coarsening and spheroidizing of the second phase in independent homogenization treatment, and the re-precipitation of the second phase during subsequent cooling and difficulty in full dissolution during reheating. This allows the ingot to directly enter the hot rolling process without pre-equilibration, thus enabling it to invest in and maintain higher deformation energy during subsequent large reduction deformation. At the same time, the large reduction of 45-55mm in each pass of hot rough rolling allows strain to penetrate to the core of the ingot, further investing in high deformation energy and fully breaking down the as-cast dendrites and second-phase network, which is beneficial for obtaining a fine, uniform, and randomly oriented recrystallized microstructure in the subsequent solution treatment stage. Compared to Comparative Examples 1-3, Comparative Examples 4-6 added an independent homogenization treatment of 560℃×10h and the subsequent cooling-machining-reheating cycle (the heating regime was then adjusted to 560℃×3h). With the other process parameters remaining the same, Δr increased from 0.12-0.14 to 0.15-0.16, demonstrating that independent homogenization in the process system of this invention is not only useless but also harmful. The elimination of independent homogenization in this invention is not a simple omission of a process but an active process design based on the aforementioned reverse principle. In particular, the preferred "high-temperature short-time" heating scheme of this invention (570-580℃ holding time for 5-10h, corresponding to Examples 4 and 5) achieves optimal overall performance despite a significantly shorter holding time compared to 30h in Example 1—Example 5 has a low Δr of 0.07 and a high random orientation grain ratio of 60.11%, achieving a balance between energy saving and performance improvement.

[0022] 3. This invention controls the hot finishing rolling temperature between 360-420℃, a window with bidirectional criticality. At the lower limit, Comparative Example 7 only reduced the finishing rolling temperature to 310℃. Although the grain size was as fine as 22.18μm, the cube texture was as high as 13.91%, random orientation was only 37.27%, and Δr reached 0.18, indicating that when the finishing rolling temperature was too low, dynamic recrystallization was insufficient and a large amount of deformation texture remained. At the upper limit, Comparative Example 10 only increased the finishing rolling temperature to 430℃. Its cube texture was as high as 15.10%, random orientation was only 32.57%, the grain size coarsened to 36.15μm, and Δr reached 0.18, indicating that when the finishing rolling temperature was above 420℃, the cube-oriented grains gained orientation growth advantage, the grain boundary mobility increased, leading to an increase in cube texture, a decrease in random orientation, grain coarsening, and an increase in Δr. The temperature range of 360-420℃ falls at the lower edge of the dynamic recrystallization temperature range. This range provides sufficient thermal activation to complete recrystallization and eliminate deformation texture, while the low grain boundary mobility inhibits selective growth of cube-oriented grains. Simultaneously, it retains the pinning effect of fine, dispersed grains relative to the grain boundaries, exhibiting significant selectivity. It is noteworthy that the average grain size of Comparative Example 7 (22.18 μm) is even finer than the 22.56 μm of Example 4 of this invention, yet its Δr is as high as 0.18, while that of Example 4 is only 0.08. This fully demonstrates that the technical value of this invention does not stem from the conventional goal of "refining grains" itself, but rather from the precise control of texture and anisotropy.

[0023] 4. This invention employs an energy-retaining recrystallization path, replacing the textural weakening of intermediate annealing with a one-time release of energy stored during cold rolling. After hot rolling, the coil is naturally air-cooled to below 60°C before direct cold rolling. The low temperature suppresses dynamic recovery and retains deformation energy storage. Combined with a processing rate of 40-52%, this forms high-density dislocation cells and shear bands, providing efficient nucleation sites for recrystallization. The deformation energy is accumulated and released all at once during the solid solution stage, with a nucleation rate far exceeding the grain growth rate, directly resulting in fine and randomly oriented recrystallized grains. In contrast, conventional intermediate annealing or self-annealing releases the stored energy earlier, and the cube-oriented subgrains preferentially nucleate and grow, thus increasing the cube texture ratio (the cube texture in Comparative Examples 1-3 is as high as 12.34%-13.88%), further demonstrating the unconventional nature of this invention's technical approach.

[0024] 5. This invention ensures the stability of fine-grained microstructure and properties through the synergistic effect of Mn and Cr dispersed phase pinning of grain boundaries and solution pre-aging. The 0.05%-0.3% Mn and 0.01%-0.05% Cr in the ingot form fine dispersed phases during hot rolling and solution treatment, effectively pinning grain boundaries and inhibiting recrystallization grain growth. After the second phase is sufficiently broken down and refined through hot rolling with high reduction and cold rolling with high processing rates, it can be fully solution-treated under mild conditions of 520-580℃ and 30-50 m / min. Pre-aging (200-300℃) controls the size and density of Mg-Si atomic clusters, enabling the sheet to exhibit both good stamping formability and bake-hardening response in the T4P state. Comparative Example 8, by simply increasing the solution and pre-aging temperatures to 590℃ and 360℃ respectively, resulted in grain coarsening to 38.45 μm and Δr reaching 0.19, confirming the necessity of the aforementioned parameter synergy. Furthermore, the results of Comparative Example 9 further reveal the multi-factor effect of Δr: its cube texture is 8.63%, and the proportion of randomly oriented grains is 48.26%. The texture level is the best among the comparative examples and is close to that of the embodiment of the present invention. However, due to the reduction of only 30 mm in each pass of hot rough rolling, the cast dendrites and second-phase network are not sufficiently broken, the grains are coarsened to 32.28 μm, and the microstructure uniformity is poor. As a result, its Δr is as high as 0.20, which is the worst among the comparative examples. This shows that Δr is jointly governed by texture and grain size / microstructure uniformity. Simply optimizing the texture is not enough to obtain a low Δr. The large reduction in hot rough rolling is also an indispensable process step to achieve a low Δr.

[0025] 6. In summary, the results of the comparative examples further demonstrate that the process parameters of the present invention are not independent preferred values, and any deviation of any parameter alone cannot achieve Δr ≤ 0.10: Comparative Example 7 only reduced the final rolling temperature to 310℃, and Δr was 0.18; Comparative Example 10 only increased the final rolling temperature to 430℃, and Δr was 0.18; Comparative Example 9 only reduced the reduction of each pass of hot roughing to 30mm, and Δr was 0.20; Comparative Example 8 only increased the solution treatment and pre-aging temperatures to 590℃ and 360℃, and Δr was 0.19; Comparative Examples 1-3, with a route of low reduction, low final rolling, low processing rate combined with intermediate annealing, had Δr of 0.12-0.14; Comparative Examples 4-6, with the addition of independent homogenization on this route, actually increased Δr to 0.15-0.16. As can be seen, the technical effect of this invention is a synergistic system composed of heating regime, large reduction in hot rough rolling, final rolling temperature in hot finish rolling, large processing rate in cold rolling, and solution pre-aging parameters. Among these, the large reduction provides an alternative means of deformation homogenization to eliminate independent homogenization and lays the organizational foundation for energy release; while the lower final rolling temperature suppresses the selective growth of cube texture, it must rely on the high energy storage provided by the large reduction to complete sufficient dynamic recrystallization (Comparative Example 7 shows that lowering this temperature alone leads to incomplete recrystallization and performance degradation); and the large processing rate and direct cold rolling below 60°C retain deformation energy storage until the solution stage, replacing the texture weakening function of intermediate annealing. These parameters work together to determine the final texture composition and anisotropy level; any parameter deviating from the scope of this invention alone cannot simultaneously achieve cube texture suppression, random orientation enhancement, and grain refinement, resulting in an increase in Δr. This effect of multi-parameter synergistic control is difficult to achieve by simply changing a single process parameter. Attached Figure Description

[0026] Figure 1 These are EBSD images of the T4P-state Al-Mg-Si alloy plates prepared in Example 1 and Comparative Example 1 of this invention, wherein... Figure 1 (a) is an EBSD image of the T4P state Al-Mg-Si alloy plate prepared in Example 1 of the present invention; Figure 1 (b) is an EBSD image of the T4P state Al-Mg-Si alloy plate prepared in Comparative Example 1.

[0027] Figure 2 The pole figures and inverse pole figures are shown for the T4P state Al-Mg-Si alloy plates prepared in Example 1 and Comparative Example 1 of this invention, wherein... Figure 2 (a) is the pole figure and inverse pole figure of the T4P state Al-Mg-Si alloy plate prepared in Example 1 of the present invention; Figure 2 (b) are the pole diagram and inverse pole diagram of the T4P state Al-Mg-Si alloy plate prepared in Comparative Example 1. Detailed Implementation

[0028] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0029] I. Testing Methods

[0030] 1. Texture testing

[0031] Texture characterization was performed using a ZEISS EVO MA10 scanning electron microscope equipped with an electron backscatter diffraction (EBSD) probe. A 10×10 mm sample was taken from each of the aluminum alloy rolls used in the examples and comparative examples. These samples were mechanically polished sequentially with 1200#, 1500#, and 3000# sandpaper, followed by electropolishing at room temperature using a 5% HClO4 (perchloric acid) + 95% C2H5OH solution at 20 V for 10 s. Finally, EBSD was used for orientation imaging to analyze the RD-ND planes of the samples, obtaining the texture type, volume fraction of each texture component, and average grain size. Grain boundaries were defined as those with an orientation difference greater than 15°, and the average grain size was calculated accordingly.

[0032] 2. Mechanical property testing

[0033] After the aluminum alloy coils of each embodiment and comparative example were heat-treated and then left to stand at room temperature for 7 days, samples were taken for performance testing. According to GB / T 5027-2007, the plastic strain ratios r0, r2, r3, r4, and r5 at 15% engineering strain, at angles of 0°, 45°, and 90° to the rolling direction, were measured respectively. 45 r 90 And according to Δr=(r0+r 90 -2r 45 ) / 2 Calculate the anisotropy of the plastic strain ratio Δr.

[0034] 3. Definition of processing rate

[0035] The single-pass processing rate of the present invention is calculated as (entrance thickness of the pass - exit thickness) / entrance thickness × 100%.

[0036] The total cold rolling processing rate described in this invention is calculated as (cold rolling inlet thickness - final outlet thickness) / inlet thickness × 100%.

[0037] II. Implementation Examples

[0038] Example 1

[0039] This embodiment provides a method for preparing Al-Mg-Si alloy plates, including the following steps:

[0040] (1) Smelting and casting: Aluminum ingots and Al-20Si, Al-50Cu, Al-10Mn, Al-10Fe, and Al-6Ti master alloys are smelted in a smelting furnace, and after degassing and slag removal, they are cast to obtain ingots. The chemical composition of the ingots is as follows: Si: 0.450%, Fe: 0.125%, Cu: 0.121%, Mn: 0.118%, Mg: 0.434%, Cr: 0.018%, Zn: 0.015%, Ti: 0.022%, with the balance being aluminum and unavoidable impurity elements. Each unavoidable impurity element is <0.05%, and the total amount of unavoidable impurity elements is <0.10%. Mg is added in the form of pure magnesium.

[0041] (2) Milling the ingot: The ingot produced by melting and casting is cut at the head and tail and milled to obtain an ingot with a length of 7500mm and a thickness of 520mm. The present invention can be implemented in the range of 400-600mm in ingot thickness.

[0042] (3) Ingot heating: The milled ingot is heated at 520℃ and held for 30 hours so that the homogenization and heating of the ingot are completed in the same process, without separate homogenization annealing.

[0043] (4) Hot rolling: The heated ingot is taken out of the furnace and subjected to hot rough rolling. After 10 passes (to avoid the problem of bite difficulty caused by excessive reduction in the early stage, the reduction of the first 7 passes is set to 45mm, and the reduction of the last 3 passes is set to 55mm, with a total reduction of 480mm and an average reduction of about 48mm per pass), the ingot is rolled into a plate with a thickness of 40mm. Then, hot finish rolling is carried out, and the plate is rolled into a coil with a thickness of 9mm after 4 passes. The final rolling temperature of hot finish rolling is 360℃. After hot rolling, the coil is naturally air-cooled to below 60℃.

[0044] (5) Cold rolling: The coil material that has been naturally air-cooled to below 60°C is directly cold rolled to 1.2mm in 9-5-2.5-1.2 rolling passes. The processing rates of each pass are 44.4%, 50%, and 52%, respectively, and the total cold rolling processing rate is 86.7%. No intermediate annealing is performed before cold rolling or between cold rolling passes.

[0045] (6) Solution quenching and pre-aging treatment: The rolled coils were subjected to solution quenching and pre-aging treatment sequentially on a continuous annealing line. The solution temperature was 580℃, and the coils were cooled with water after solution treatment. The pre-aging temperature was 300℃. The strip running speed was 30m / min during both solution quenching and pre-aging treatment. After pre-aging, the coils were naturally cooled to room temperature to obtain T4P state Al-Mg-Si alloy plates.

[0046] Example 2

[0047] This embodiment provides a method for preparing Al-Mg-Si alloy plates, including the following steps:

[0048] (1) Smelting and casting: The chemical composition of the ingot is as follows (mass percentage of elements): Si: 0.711%, Fe: 0.236%, Cu: 0.241%, Mn: 0.206%, Mg: 0.623%, Cr: 0.011%, Zn: 0.018%, Ti: 0.031%, with the balance being aluminum and unavoidable impurity elements. Each unavoidable impurity element is <0.05%, and the total amount of unavoidable impurity elements is <0.10%. Mg is added in the form of pure magnesium.

[0049] (2) Milling the surface of the ingot: Same as in Example 1, to obtain an ingot with a length of 7500mm and a thickness of 520mm.

[0050] (3) Ingot heating: Heating is carried out at 540℃ for 25 hours, so that the homogenization of the ingot is completed in the same process as the heating, without separate homogenization annealing.

[0051] (4) Hot rolling: The hot roughing roll is rolled into a 35mm thick plate through 10 passes (to avoid the problem of bite difficulty caused by excessive reduction in the early stage, the reduction of the first 3 passes is set to 45mm, and the reduction of the last 7 passes is set to 50mm, with a total reduction of 485mm and an average reduction of about 48.5mm per pass). The hot finishing roll is rolled into an 8mm thick coil through multiple passes, with a final rolling temperature of 380℃. After hot rolling, the plate is naturally air-cooled to below 60℃.

[0052] (5) Cold rolling: The material is directly cold rolled to 1.1 mm in 8-4.5-2.2-1.1 rolling passes. The processing rates of each pass are 43.8%, 51.1% and 50%, respectively, and the total cold rolling processing rate is 86.25%. No intermediate annealing is performed before cold rolling or between cold rolling passes.

[0053] (6) Solution quenching and pre-aging treatment: Solution temperature 560℃, pre-aging temperature 280℃, strip running speed 35m / min. The rest is the same as in Example 1.

[0054] Example 3

[0055] This embodiment provides a method for preparing Al-Mg-Si alloy plates, including the following steps:

[0056] (1) Smelting and casting: The chemical composition of the ingot is as follows (mass percentage of elements): Si: 0.958%, Fe: 0.327%, Cu: 0.279%, Mn: 0.288%, Mg: 0.715%, Cr: 0.025%, Zn: 0.022%, Ti: 0.029%, with the balance being aluminum and unavoidable impurity elements. Each unavoidable impurity element is <0.05%, and the total amount of unavoidable impurity elements is <0.10%. Mg is added in the form of pure magnesium.

[0057] (2) Milling the surface of the ingot: Same as in Example 1.

[0058] (3) Ingot heating: Heating is carried out at 560℃ for 20 hours, so that the homogenization of the ingot is completed in the same process as the heating, without separate homogenization annealing.

[0059] (4) Hot rolling: The hot roughing roll is rolled into a 30mm thick plate through 10 passes (to avoid the problem of bite difficulty caused by excessive reduction in the early stage, the reduction of the first 4 passes is set to 45mm, the reduction of the 5th and 6th passes is set to 55mm, and the reduction of the last 4 passes is set to 50mm, with a total reduction of 490mm and an average reduction of about 49mm per pass). The hot finishing roll is rolled into a 7mm thick coil through multiple passes, with a final rolling temperature of 400℃. After hot rolling, the plate is naturally air-cooled to below 60℃.

[0060] (5) Cold rolling: The material is directly cold rolled to 1 mm in 7-4-2-1 rolling passes. The processing rates of each pass are 42.9%, 50%, and 50%, respectively, and the total cold rolling processing rate is 85.7%. No intermediate annealing is performed before cold rolling or between cold rolling passes.

[0061] (6) Solution quenching and pre-aging treatment: Solution temperature 550℃, pre-aging temperature 260℃, strip running speed 40m / min. The rest is the same as in Example 1.

[0062] Example 4

[0063] This embodiment provides a method for preparing Al-Mg-Si alloy plates, including the following steps:

[0064] (1) Smelting and casting: The chemical composition of the ingot is as follows (mass percentage of elements): Si: 1.132%, Fe: 0.306%, Cu: 0.311%, Mn: 0.184%, Mg: 0.765%, Cr: 0.036%, Zn: 0.029%, Ti: 0.021%, with the balance being aluminum and unavoidable impurity elements. Each unavoidable impurity element is <0.05%, and the total amount of unavoidable impurity elements is <0.10%. Mg is added in the form of pure magnesium.

[0065] (2) Milling the surface of the ingot: Same as in Example 1.

[0066] (3) Ingot heating: Heating is carried out at 570℃ for 10 hours, so that the homogenization of the ingot is completed in the same process as the heating, without separate homogenization annealing.

[0067] (4) Hot rolling: The hot roughing roll is rolled in 10 passes (to avoid the problem of bite difficulty caused by excessive reduction in the early stage, the reduction of the first 4 passes is set to 46 mm, the reduction of the 5th and 6th passes is set to 55 mm, and the reduction of the last 4 passes is set to 50 mm, with a total reduction of 494 mm and an average reduction of about 49.4 mm per pass) to roll the ingot to a plate with a thickness of 26 mm; the hot finishing roll is rolled in multiple passes to roll the plate to a coil with a thickness of 6 mm, with a final rolling temperature of 410℃. After hot rolling, the plate is naturally air-cooled to below 60℃.

[0068] (5) Cold rolling: The material is directly cold rolled to 0.8 mm in 6-3-1.5-0.8 rolling passes. The processing rates of each pass are 50%, 50%, and 46.7%, respectively, and the total cold rolling processing rate is 86.7%. No intermediate annealing is performed before cold rolling or between cold rolling passes.

[0069] (6) Solution quenching and pre-aging treatment: Solution temperature 540℃, pre-aging temperature 240℃, strip running speed 45m / min. The rest is the same as in Example 1.

[0070] Example 5

[0071] This embodiment provides a method for preparing Al-Mg-Si alloy plates, including the following steps:

[0072] (1) Smelting and casting: The chemical composition of the ingot is as follows (mass percentage of elements): Si: 1.379%, Fe: 0.256%, Cu: 0.218%, Mn: 0.172%, Mg: 0.625%, Cr: 0.024%, Zn: 0.018%, Ti: 0.015%, with the balance being aluminum and unavoidable impurity elements. Each unavoidable impurity element is <0.05%, and the total amount of unavoidable impurity elements is <0.10%. Mg is added in the form of pure magnesium.

[0073] (2) Milling the surface of the ingot: Same as in Example 1.

[0074] (3) Ingot heating: Heating is carried out at 580℃ for 5 hours, so that the homogenization of the ingot is completed in the same process as the heating, without separate homogenization annealing.

[0075] (4) Hot rolling: The hot roughing roll is rolled into a 22mm thick plate through 10 passes (to avoid the problem of bite difficulty caused by excessive reduction in the early stage, the reduction of the first 4 passes is set to 47mm, the reduction of the 5th and 6th passes is set to 55mm, and the reduction of the last 4 passes is set to 50mm, with a total reduction of 498mm and an average reduction of about 49.8mm per pass). The hot finishing roll is rolled into a 5mm thick coil through multiple passes, with a final rolling temperature of 420℃. After hot rolling, the plate is naturally air-cooled to below 60℃.

[0076] (5) Cold rolling: The material is directly cold rolled to 0.7 mm in 5-2.6-1.3-0.7 rolling passes. The processing rates of each pass are 48%, 50% and 46.2% respectively, and the total cold rolling processing rate is 86%. No intermediate annealing is performed before cold rolling or between cold rolling passes.

[0077] (6) Solution quenching and pre-aging treatment: Solution temperature 520℃, pre-aging temperature 220℃, strip running speed 50m / min. The rest is the same as in Example 1.

[0078] III. Comparative Example

[0079] Comparative Example 1

[0080] The difference from Example 1 is as follows: the ingot is rolled to 40mm through multiple hot roughing passes (each pass reducing by 32mm), and the final hot finishing temperature is 350℃; after the coil cools to below 60℃, it is rolled into a 3.5mm coil through 9-7.5-5.1-3.5 rolling passes, and then the coil is subjected to intermediate annealing on a continuous annealing line at a speed of 15m / min and an annealing temperature of 400℃; after annealing, it is rolled into a 1.2mm coil through 3.5-2.5-1.7-1.2 rolling passes. The remaining processes are the same as in Example 1.

[0081] Comparative Example 2

[0082] The difference from Example 1 is as follows: The ingot is rolled to 35mm using multiple hot roughing passes (each pass reduction controlled at 35mm), resulting in a 7mm thick coil after hot rolling. The final hot finishing temperature is 300℃. After cooling to below 60℃, the coil is rolled to 3.5mm thickness using 7-5.1-3.5 rolling passes, followed by intermediate annealing at 15m / min and 400℃. After annealing, it is rolled to 1.0mm thickness using 3.5-2.4-1.6-1.0 rolling passes. The remaining processes are the same as in Example 1.

[0083] Comparative Example 3

[0084] The difference from Example 1 is as follows: The ingot is rolled to 30mm using multiple hot roughing passes (each pass reduction controlled at 38mm), resulting in a 5mm thick coil after hot rolling. The final hot finishing temperature is 250℃. After cooling to below 60℃, the coil is rolled to 3.5mm thickness using 5-3.5 rolling passes, followed by intermediate annealing at 15m / min and 400℃. After annealing, it is rolled to 0.8mm thickness using 3.5-2.2-1.3-0.8 rolling passes. The remaining processes are the same as in Example 1.

[0085] Comparative Example 4

[0086] The difference from Example 1 is as follows: After casting, the ingot is first subjected to homogenization treatment at 560℃ for 10 hours. After cooling, the ingot is trimmed at both ends and milled. Then, the ingot is heated to 560℃ and held for 3 hours before being rolled. The ingot is then rolled to 40mm in multiple passes (each pass has a reduction of 32mm), and the hot finish rolling temperature is 350℃. After the coil cools to below 60℃, it is rolled into a 3.5mm coil with 9-7.5-5.1-3.5 rolling passes. Then, it undergoes intermediate annealing at a speed of 15m / min and a temperature of 400℃. After annealing, it is rolled into a 1.2mm coil with 3.5-2.5-1.7-1.2 rolling passes. The remaining processes are the same as in Example 1.

[0087] Comparative Example 5

[0088] The difference from Example 1 is as follows: After casting, the ingot is first subjected to a homogenization treatment at 560℃ for 10 hours. After cooling, the ingot is trimmed at both ends and milled. Then, the ingot is heated to 560℃ and held for 3 hours before being rolled. The ingot is then rolled to 35mm using multiple hot roughing passes (each pass reduction controlled at 35mm). The resulting coil thickness is 7mm, and the final hot finishing temperature is 300℃. After cooling to below 60℃, the coil is rolled to 3.5mm using 7-5.1-3.5 rolling passes. Intermediate annealing is then performed at 15m / min and 400℃. After annealing, the coil is rolled to 1.0mm using 3.5-2.4-1.6-1.0 rolling passes. The remaining processes are the same as in Example 1.

[0089] Comparative Example 6

[0090] The difference from Example 1 is as follows: After casting, the ingot is first subjected to homogenization treatment at 560℃ for 10 hours. After cooling, the ingot is trimmed and milled. Then, the ingot is heated to 560℃ and held for 3 hours before being rolled. Hot roughing is performed through multiple passes (each pass reduction controlled at 38mm) to roll the ingot to 30mm. The thickness of the rolled coil is 5mm, and the final hot finishing temperature is 250℃. After cooling to below 60℃, the coil is rolled into a 3.5mm coil with 5-3.5 rolling passes. Intermediate annealing is then performed at a speed of 15m / min and a temperature of 400℃. After annealing, it is rolled into a 0.8mm coil with 3.5-2.2-1.3-0.8 rolling passes. The remaining processes are the same as in Example 1.

[0091] Comparative Example 7

[0092] The difference from Example 1 is that the hot finishing rolling temperature is 310°C, while the remaining processes are the same as in Example 1.

[0093] Comparative Example 8

[0094] The difference from Example 1 is that the solution quenching and pre-aging treatment temperatures are 590℃ and 360℃, respectively, and the speed is 30m / min. The remaining procedures are the same as in Example 1.

[0095] Comparative Example 9

[0096] The difference from Example 1 is that the ingot is rolled to 40mm by multiple passes of hot rough rolling (each pass has a reduction of 30mm), and the remaining processes are the same as in Example 1.

[0097] Comparative Example 10

[0098] The difference from Example 1 is that the hot finishing rolling temperature is 430°C, while the remaining processes are the same as in Example 1.

[0099] IV. Performance Test Results

[0100] The texture and mechanical properties of the T4P state aluminum alloy sheets prepared in Examples 1-5 and Comparative Examples 1-10 were tested, and the results are shown in Table 1.

[0101] Table 1. Microstructure and anisotropic property test results of Examples 1-5 and Comparative Examples 1-10

[0102]

[0103] As shown in Table 1, the cube texture volume fraction of Examples 1-5 was 6.44-7.39%, the random orientation grain volume fraction was 52.67-60.11%, the average grain size was 20.46-22.56 μm, and the Δr was 0.07-0.10; while the corresponding values ​​for Comparative Examples 1-10 were 8.63-15.10%, 31.12-48.26%, 22.18-38.45 μm, and 0.12-0.20, respectively. The performance of Examples 1-5 was significantly better than that of Comparative Examples 1-10.

[0104] Furthermore, Comparative Examples 4-6, compared to Comparative Examples 1-3, added an independent homogenization process of 560℃×10h and a subsequent cooling-machining-reheating cycle (the subsequent heating regime was adjusted accordingly to 560℃×3h), while the other process parameters remained the same. The results showed that Δr increased from 0.12-0.14 in Comparative Examples 1-3 to 0.15-0.16 in Comparative Examples 4-6. This indicates that even with a conventional process route of small reduction, low final rolling temperature, small processing rate combined with intermediate annealing, adding an independent homogenization process and a complete thermal cycle still cannot improve, or even worsens, the anisotropy of the sheet material. The mechanism is that homogenization causes the second phase to coarsen and spheroidize, and the solute distribution to tend towards equilibrium, leading to a decrease in dislocation proliferation and energy storage capacity during subsequent hot rolling deformation, and insufficient recrystallization driving force. Therefore, the present invention's elimination of independent homogenization and adoption of integrated homogenization-heating is not a simple omission of a process, but rather an active process design based on the above principles.

[0105] Comparative Examples 7-10 represent examples where only a single parameter was changed: Comparative Example 7 reduced the hot finishing rolling temperature to 310℃, resulting in an average grain size as small as 22.18μm, but with a cube texture as high as 13.91%, random orientation as low as 37.27%, and Δr as high as 0.18; Comparative Example 9 reduced the reduction in each pass of hot roughing rolling to 30mm, resulting in grain coarsening to 32.28μm and Δr as high as 0.20; Comparative Example 8 increased the solution treatment and pre-aging temperatures to 590℃ and 360℃, respectively, resulting in grain coarsening to 38.45μm and Δr as high as 0.19; Comparative Example 10 increased the finishing rolling temperature to 430℃, resulting in a cube texture as high as 15.10%, grain coarsening to 36.15μm, and Δr as high as 0.18. Both excessively low and excessively high finishing rolling temperatures lead to deterioration of microstructure and properties, and the 360-420℃ window has a bidirectional criticality. Therefore, the technical effect of this invention does not stem from the conventional goal of "refining grains" (the grains in Comparative Example 7 are even finer than in some embodiments, but the anisotropy is significantly worsened), but rather from the texture control resulting from the synergistic effect of various parameters including high-reduction hot roughing, low-temperature final rolling, high-processing-rate cold rolling, and solution pre-aging. If any parameter deviates from the scope of this invention, a sheet material with Δr ≤ 0.10 cannot be obtained.

[0106] V. Analysis of Attached Figures

[0107] The invention will now be further analyzed with reference to the accompanying drawings.

[0108] Figure 1 (a) is a photograph of the grain structure of the T4P state aluminum alloy sheet prepared in Example 1. Figure 1 (b) A photograph of the grain structure of the T4P state aluminum alloy sheet prepared in Comparative Example 1. As can be seen from the comparison, the grain size of Example 1 is significantly smaller than that of Comparative Example 1, and the grain distribution is more uniform. This is consistent with the data in Table 1, which shows an average grain size of 20.46 μm for Example 1 and an average grain size of 34.62 μm for Comparative Example 1.

[0109] Figure 2 (a) is the pole figure and inverse pole figure of the T4P state aluminum alloy sheet prepared in Example 1. Figure 2 (b) Pole diagrams and inverse pole diagrams of the T4P state aluminum alloy sheet prepared in Comparative Example 1. Figure 2 (a) As can be seen from the pole figure, the pole density distribution of each major texture component in Example 1 is relatively diffuse, and no highly concentrated pole density region appears; Figure 2 (b) The pole figure shows a significantly more concentrated pole density region in Comparative Example 1, indicating a stronger preference orientation. Combined with the inverse pole figure analysis, Figure 2 In (a), the maximum pole density of the inverse pole figure IPF is 3.10. Figure 2 (b) shows that the maximum IPF density of the inverse pole figure is 4.17. The lower the maximum IPF density, the more random the grain orientation and the weaker the preferred orientation in the material. Therefore, the plate prepared in Example 1 has a weaker preferred orientation and a higher proportion of randomly oriented grains than Comparative Example 1. This is completely consistent with the results in Table 1, which shows that Example 1 has a cube texture of 7.26% and a random orientation of 52.67%, while Comparative Example 1 has a cube texture of 13.88% and a random orientation of 34.26%.

[0110] The above-mentioned figure analysis further proves that the present invention effectively controls the texture type and grain structure of Al-Mg-Si alloy by integrating homogenization and heating, large reduction in hot rough rolling, low-temperature final rolling in hot finish rolling, direct air cooling after hot rolling, large processing rate in cold rolling without intermediate annealing, and the synergistic combination of solution treatment and pre-aging, thereby obtaining fine and uniform grains and excellent isotropy.

[0111] In summary, the Al-Mg-Si alloy sheets prepared in Examples 1-5 of this invention have a cube texture volume fraction ≤8%, a random orientation grain volume fraction ≥50%, an average grain size ≤23μm, and a plastic strain ratio anisotropy Δr ≤0.10. They possess both fine and uniform grain structure and excellent isotropy, meeting the requirements for high formability and high isotropy for automotive four-door hoods and body panels. Comparative Examples 1-9, due to the absence of the process synergy scheme of this invention, exhibit significantly inferior cube texture ratio, random orientation grain ratio, grain size, and Δr compared to the examples. The results of Comparative Examples 4-6 further demonstrate that adding independent homogenization treatment actually worsens Δr. Comparative Example 10, by simply increasing the final rolling temperature to 430°C, achieved a cube texture of 15.10%, a random orientation of only 32.57%, grain coarsening to 36.15 μm, and a Δr of 0.18, further verifying the criticality of the upper limit of the final rolling temperature. Together with Comparative Example 7 (final rolling at 310°C, Δr of 0.18), it demonstrates that the 360-420°C window has bidirectional selectivity. Furthermore, this invention significantly shortens the process and reduces energy consumption by eliminating the separate homogenization heat treatment process and its cooling-reheating cycle, as well as the intermediate annealing process during cold rolling.

[0112] The above embodiments are only used to illustrate the present invention, and their descriptions are relatively specific and detailed, but they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make several modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention.

Claims

1. A method for preparing Al-Mg-Si alloy sheet, comprising melting and casting, ingot machining, ingot heating, hot rolling, cold rolling, solution quenching, and pre-aging treatment, characterized in that: The ingot machining includes cutting the head and tail and milling the surface. After machining, the ingot is not subjected to independent homogenization annealing, but is directly heated. The ingot heating temperature is 520-580℃ and the holding time is 5-30h, so that the ingot homogenization and heating are completed in the same process. The hot rolling process includes hot roughing and hot finishing. The hot roughing process rolls the ingot into a sheet with a thickness of 20-40 mm through multiple passes, with a reduction of 45-55 mm in each pass. The hot finishing process rolls the sheet into a coil with a thickness of 5-10 mm through multiple passes, and the final rolling temperature of the hot finishing process is 360-420℃. After hot rolling, the coil is naturally air-cooled to below 60℃. The cold rolling process is as follows: the coil material that has been naturally air-cooled to below 60°C is directly cold-rolled to 0.7-1.2mm at a single-pass processing rate of 40-52%, without intermediate annealing before cold rolling or between cold rolling passes; Solution quenching and pre-aging treatment are performed sequentially on a continuous annealing line. The solution quenching temperature is 520-580℃, the pre-aging temperature is 200-300℃, and the strip running speed is 30-50m / min.

2. The method for preparing Al-Mg-Si alloy sheet according to claim 1, characterized in that, The chemical composition of the ingot, by mass percentage, is as follows: Si: 0.4-1.4%, Fe: ≤0.5%, Cu: ≤0.5%, Mn: 0.05-0.3%, Mg: 0.35-0.8%, Cr: 0.01-0.05%, Zn: ≤0.3%, Ti: ≤0.3%, with the balance being aluminum and unavoidable impurities; each unavoidable impurity element is <0.05%, and the total amount of unavoidable impurity elements is <0.10%; wherein, Si, Cu, Mn, Fe, and Ti are added in the form of Al-20Si, Al-50Cu, Al-10Mn, Al-10Fe, and Al-6Ti master alloys, respectively, and Mg is added in the form of pure magnesium; the mass ratio of Mg to Si in the ingot is 0.4-1.1; and Mn and Cr form dispersed phases pinning grain boundaries during hot rolling and solution treatment to inhibit grain growth.

3. The method for preparing Al-Mg-Si alloy sheet according to claim 1, characterized in that, The ingot is heated to a temperature of 570-580℃ and held for 5-10 hours.

4. The method for preparing Al-Mg-Si alloy sheet according to claim 1, characterized in that, The reduction in each pass of the hot roughing rolling is 48-55 mm, and the final rolling temperature of the hot finishing rolling is 380-420℃.

5. The method for preparing Al-Mg-Si alloy sheet according to claim 1, characterized in that, The cold rolling process consists of 3 passes, with a total cold rolling processing rate of 80-90% and a single pass processing rate of 40-52%.

6. The method for preparing Al-Mg-Si alloy sheet according to claim 1, characterized in that, The solution quenching temperature is 520-560℃, the pre-aging temperature is 220-280℃, and the strip running speed is 40-50m / min.

7. The method for preparing Al-Mg-Si alloy sheet according to any one of claims 1-6, characterized in that, The resulting Al-Mg-Si alloy sheet has a cube texture volume fraction ≤8%, a random orientation grain volume fraction ≥50%, an average grain size ≤23μm, and a plastic strain ratio anisotropy Δr ≤0.

10.

8. The method for preparing Al-Mg-Si alloy sheet according to claim 1, characterized in that, The ingot is heated to 570-580℃ and held for 5-10 hours. The reduction in each pass of the hot roughing rolling is 48-55 mm. The final rolling temperature of the hot finishing rolling is 400-420℃. The solution quenching temperature is 520-560℃. The pre-aging temperature is 220-280℃. The strip running speed is 40-50 m / min.

9. An Al-Mg-Si alloy sheet, characterized in that, The Al-Mg-Si alloy plate is prepared by the method described in any one of claims 1-8, and the Al-Mg-Si alloy plate has a cube texture volume fraction ≤8%, a random orientation grain volume fraction ≥50%, an average grain size ≤23μm, and a plastic strain ratio anisotropy Δr ≤0.

10.