A method for selective chemical silver plating in semi-etched grooves of copper-clad ceramic substrates

By combining full-surface chemical silver plating with ultraviolet laser engraving, the problems of printing difficulties and insufficient precision in silver plating of the groove area of ​​copper-clad ceramic substrates have been solved. This has achieved precise matching between the silver plating layer and the chip welding area, improved packaging yield and plating adhesion, simplified the process flow, and reduced production costs.

CN123063757APending Publication Date: 2026-11-10江苏富乐华功率半导体研究院有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611309131.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the existing technology, the silver plating method in the groove area of ​​copper-clad ceramic substrate has problems such as printing difficulties, residual pollution, and insufficient precision, resulting in low packaging yield, high production cost, and complex process.

Method used

After full-surface chemical silver plating, ultraviolet laser engraving is used to remove the silver plating layer in non-soldering areas. By combining optimized chemical silver plating solution composition and laser parameters, selective removal of the silver plating layer is achieved.

Benefits of technology

It achieves precise matching between the silver plating layer and the chip welding area, avoids ink residue and chemical corrosion, simplifies the process, improves packaging yield and plating adhesion, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063757A_ABST
    Figure CN123063757A_ABST
Patent Text Reader

Abstract

This invention discloses a selective chemical silver plating method for semi-etched grooves in copper-clad ceramic substrates, relating to the field of copper-clad ceramic substrate technology. Unlike traditional methods that first mask non-soldering areas before chemical silver plating, this invention first forms a full-coverage silver plating layer within the groove, then selectively removes the silver plating layer from non-soldering areas using laser. This ensures that the retained core silver plating area precisely corresponds to the chip soldering area, avoiding the residual contamination problems associated with traditional screen printing ink masking methods. The silver plating layer adhesion is more stable and reliable. The ultraviolet laser positioning is precise, the heat conduction range is small, and the edges of the silver plating layer are neat. Simultaneously, it eliminates multiple processes such as printing ink, exposure and development, and ink removal cleaning, simplifying the production process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of copper-clad ceramic substrate technology, specifically a method for selective chemical silver plating in the semi-etched grooves of copper-clad ceramic substrates. Background Technology

[0002] Copper-clad ceramic substrates, due to their excellent thermal conductivity, insulation, and mechanical strength, have become the core packaging material for high-end electronic devices such as power modules for new energy vehicles and power amplifiers for 5G base stations. In semi-etched trench embedded packaging chip projects, a chemical silver plating layer of the same size as the chip welding area needs to be prepared in the groove formed by the semi-etching of the copper layer on the substrate to ensure a strong weld and smooth electrical signal transmission.

[0003] In existing technologies, silver plating methods for the grooved areas of copper-clad ceramic substrates are mainly divided into full-area chemical silver plating and partial chemical silver plating. Full-area chemical silver plating is simple, but excess silver plating areas can lead to stress concentration, solder overflow, chip slippage, and increased production costs during chip soldering. Partial chemical silver plating first covers the non-silver-plated areas with blocking ink, and then performs selective silver plating through chemical ink removal. However, the depth of the semi-etched groove is usually 150~300μm. The three-dimensional structure formed by the groove wall and bottom makes it easy for ink to seep into the groove wall gaps during printing due to capillary action, forming residues that are difficult to completely remove during subsequent ink removal, affecting the adhesion of the plating layer. At the same time, it is difficult to fill the groove with printed ink, the exposure energy for full-area filling is difficult to control, the precision of selective silver plating is insufficient, the silver plating area cannot be precisely matched with the chip soldering area, and the packaging yield is less than 90%. Moreover, the existing partial silver plating process relies on multiple processes such as wet film printing, exposure and development, which is complex and prone to chemical contamination, further restricting the reliability of the product.

[0004] Therefore, in order to overcome the problems of printing difficulties, residual pollution, and insufficient precision in the selective silver plating of semi-etched grooves using the existing barrier ink method, a selective chemical silver plating method based on ultraviolet laser engraving is developed to achieve precise matching between the silver plating area in the groove and the chip welding area, which is of great significance for improving the plating quality and packaging yield. Summary of the Invention

[0005] The purpose of this invention is to provide a selective chemical silver plating method in the semi-etched grooves of copper-clad ceramic substrates to solve the problems mentioned in the prior art.

[0006] To achieve the above objectives, the present invention provides the following technical solution: A method for selective chemical silver plating in a semi-etched groove on a copper-clad ceramic substrate, the method comprising the following steps: S1: Perform semi-etching on the copper-clad ceramic substrate to form embedded grooves, then degrease, micro-etch, acid pickling, washing, and drying to obtain the copper-clad ceramic substrate with the embedded grooves completed. S2: Take the copper-clad ceramic substrate after the embedded groove is completed, pre-immerse it, silver-plat it, clean and dry it to form a silver plating layer in the groove and on the surface of the substrate, and obtain a copper-clad ceramic substrate with a chemical silver plating layer. S3: Based on the preset size of the chip welding area, use ultraviolet laser to carve the chemical silver plating layer in the groove, remove the silver plating layer in the non-welding area in the groove, and obtain a copper-clad ceramic substrate with selective silver plating layer. S4: Take a copper-clad ceramic substrate with a selective silver plating layer, clean it, and dry it to obtain a copper-clad ceramic substrate with selective silver plating in the semi-etched groove.

[0007] In a more optimized manner, in S2, the pre-impregnation solution used includes the following components, by volume: 15-20% component 1, 4-8% component 2, 0.5-1.0% nitric acid, and 1000-2000 ppm Cu. 2+ Component 1 includes the following components, by concentration: 30-50 mL / L ammonia, 10-20 g / L glucose, 2-5 g / L sodium hydroxide, 1-3 g / L imidazole, and the remainder is pure water; Component 2 includes the following components, by concentration: 50-100 g / L potassium sodium tartrate, 15-25 g / L hydrazine sulfate, and the remainder is pure water.

[0008] In a more optimized manner, in S2, the chemical silver plating agent used for silver plating includes the following components, by volume: 2-4% of agent A, 20-30% of agent B, 4-6% of agent C, 0.5-1.0% nitric acid, and 3000-5000 ppm Cu. 2+ The remainder is pure water; Agent A includes the following components, by concentration: 27~32 g / L silver nitrate, 2~6 g / L tartaric acid, 10~15 mL / L ethanol, with the remainder being pure water; Agent B includes the following components, by concentration: 30~50 mL / L ammonia, 10~20 g / L glucose, 2~5 g / L sodium hydroxide, 1~3 g / L imidazole, with the remainder being pure water; Agent C includes the following components, by concentration: 50~100 g / L potassium sodium tartrate, 15~25 g / L hydrazine sulfate, with the remainder being pure water.

[0009] In a more optimized manner, in S1, the etching solution used for the semi-etching process includes the following components, by concentration: 1.7~2.1 mol / L hydrochloric acid, 130~170 g / L Cu. 2+ The rest is pure water.

[0010] In a more optimized manner, in S2, the thickness of the electroless silver plating layer is 1~3μm; in S3, the engraving depth is 1.2~3.5μm.

[0011] In a more optimized configuration, the parameters for ultraviolet laser engraving in S3 are: wavelength of 355nm, power of 10~30W, engraving speed of 50~200mm / s, and spot diameter of 10~50μm.

[0012] In a more optimized manner, in S2, the pre-immersion temperature is 35~45℃, the circulation rate of the pre-immersion solution is 30~70L / min, the silver plating temperature is 53~57℃, and the circulation rate of the silver plating solution is 30~70L / min.

[0013] In a more optimized manner, in S1, the micro-etching solution used includes the following components by volume: 35-45% 98% sulfuric acid, 3-5% 30% hydrogen peroxide, 10-12% polyethylene glycol, and the remainder is pure water; the micro-etching treatment time is 60-120s; the acid used for pickling is an aqueous solution containing 30-50mL / L sulfuric acid, and the treatment time is 30-90s.

[0014] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention first performs full-surface chemical silver plating within the groove, then uses ultraviolet laser to selectively remove the silver plating layer from non-soldering areas, retaining only the core silver plating area corresponding to the chip soldering area. Compared to traditional selective silver plating methods that first shield non-soldering areas before silver plating, this method allows for uniform deposition of the plating solution without being restricted by the groove structure during full-surface silver plating. It avoids residual contamination caused by shielding materials seeping into gaps, ensuring the stable adhesion between the silver plating layer and the copper substrate.

[0015] 2. This invention employs ultraviolet laser to selectively remove the silver plating layer. The short wavelength of the ultraviolet laser, after focusing, allows for a spot diameter on the order of micrometers, enabling precise control of the laser beam's trajectory and position on the silver plating surface. Simultaneously, the extremely short laser interaction time minimizes the heat transfer to the surrounding area, preventing thermal impact on the plating layer around the engraved area. Therefore, the retained silver plating area precisely matches the chip bonding surface, avoiding dimensional deviations caused by insufficient masking precision in traditional processes.

[0016] 3. Silver has a much higher absorption rate in the ultraviolet band than copper. During laser treatment, the energy is mainly absorbed by the silver plating layer and vaporized and peeled off. By the time the energy reaches the copper surface, it is insufficient to cause melting or oxidation of the copper substrate. This physical removal method does not require the use of chemical agents, avoiding corrosion of the tank walls by chemical agents, and resulting in a clean edge to the silver plating layer. At the same time, it eliminates multiple processes such as printing ink, exposure and development, and ink removal and cleaning, simplifying the process, shortening the production cycle, and correspondingly reducing production costs. Attached Figure Description

[0017] Figure 1This is a topographic image of the copper-clad ceramic substrate after the embedded groove in Example 1 has been completed; Figure 2 This is a morphology diagram of the chemical silver plating layer on the copper-clad ceramic substrate in Example 1; Figure 3 This is a topographic image of the chemical silver plating region in the groove area of ​​the copper-clad ceramic substrate with selective silver plating in Example 1. Detailed Implementation

[0018] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0019] It should be noted that the following quantities are by volume, and there are no special restrictions on the manufacturers of the raw materials involved in this invention. Exemplary examples include: in the following embodiments and comparative examples, the Si3N4 ceramic substrate has a copper layer thickness of 0.4 mm; the remaining raw materials are commercially available analytical grade or industrial grade reagents.

[0020] Example 1: A method for selective chemical silver plating in the semi-etched grooves of a copper-clad ceramic substrate, comprising the following steps: S1: A 7mm × 7mm × 0.17mm groove was prepared on the surface of a Si3N4 ceramic substrate using chemical etching. The substrate was etched at an etching temperature of 50℃ to a depth of 0.3mm. The conveyor speed in the etching section was 0.75m / min. The etching solution contained 1.9mol / L hydrochloric acid and 150g / L Cu. 2+ The aqueous solution has a conductivity of 35 S / m and a specific gravity of 1.29. First, remove the oil stains on the substrate surface, then immerse it in the micro-etching solution for 90s. The micro-etching solution is an aqueous solution containing 40% 98% sulfuric acid, 4% 30% hydrogen peroxide, and 11% polyethylene glycol. Finally, immerse it in a 40 mL / L sulfuric acid solution for 60s to remove the residual oxides after micro-etching. Rinse it with deionized water and blow it dry to obtain the copper-clad ceramic substrate with the embedded groove completed. S2: First, immerse the copper-clad ceramic substrate with the embedded groove completed in a pre-immersion solution at 38℃ and a circulation rate of 50L / min for 5 minutes. Then, transfer it to a chemical silver plating solution at 55℃ and a circulation rate of 50L / min for 15 minutes to form a uniform silver plating layer with a thickness of 2μm. Clean and dry, rinse three times with deionized water for 2 minutes each time, and dry in a 70℃ oven for 25 minutes to obtain a copper-clad ceramic substrate with a chemical silver plating layer. The preparation method of the pre-immersion solution is as follows: take 17 volumes of an aqueous solution containing 40mL / L ammonia, 15g / L glucose, 3g / L sodium hydroxide, and 2g / L imidazole; 6 volumes of an aqueous solution containing 75g / L potassium sodium tartrate and 20g / L hydrazine sulfate; 0.7 volumes of nitric acid; and 1500ppm Cu 2+ The remainder is pure water; mix thoroughly to obtain the pre-immersion solution. The preparation method for the chemical silver plating solution is as follows: Take 3 volumes of an aqueous solution containing 30 g / L silver nitrate, 4 g / L tartaric acid, and 12 mL / L ethanol; 25 volumes of an aqueous solution containing 40 mL / L ammonia, 15 g / L glucose, 3 g / L sodium hydroxide, and 2 g / L imidazole; 5 volumes of an aqueous solution containing 75 g / L potassium sodium tartrate and 20 g / L hydrazine sulfate; 0.8 volumes of nitric acid; and 4000 ppm Cu 2+ The remainder is pure water. After mixing evenly, a chemical silver plating solution is obtained. S3: Fix the copper-clad ceramic substrate with chemical silver plating on the worktable of the laser engraving machine. Set the laser parameters as follows: laser wavelength 355nm, power 20W, engraving speed 100mm / s, spot diameter 30μm, and engraving depth 2.5μm. Based on the chip welding area size, which is 4.8mm×4.8mm, draw a closed-loop engraving path and perform closed-loop engraving along the periphery of the silver plating layer in the groove. Remove the non-target silver plating layer with an edge width of 1.0mm. Start the engraving program to complete the selective removal operation and obtain the copper-clad ceramic substrate with selective silver plating. S4: Place the copper-clad ceramic substrate with selective silver plating into a 40kHz ultrasonic cleaner, clean it with deionized water for 8 minutes to remove the silver powder residue generated during engraving, and dry it in a 75℃ oven for 25 minutes to obtain a copper-clad ceramic substrate with selective silver plating in the semi-etched grooves.

[0021] Example 2: A method for selective chemical silver plating in the semi-etched grooves of a copper-clad ceramic substrate, comprising the following steps: S1: A 7mm × 7mm × 0.17mm groove was prepared on the surface of a Si3N4 ceramic substrate using chemical etching. The substrate was etched at an etching temperature of 48℃ to a depth of 0.3mm. The conveyor speed in the etching section was 0.75m / min. The etching solution contained 1.7mol / L hydrochloric acid and 130g / L Cu. 2+The aqueous solution has a conductivity of 15 S / m and a specific gravity of 1.28. First, remove the oil stains on the substrate surface, then immerse it in the micro-etching solution for 90 seconds. The micro-etching solution is an aqueous solution containing 35% 98% sulfuric acid, 3% 30% hydrogen peroxide, and 10% polyethylene glycol. Finally, immerse it in a 40 mL / L sulfuric acid solution for 60 seconds to remove the residual oxides after micro-etching. Rinse it with deionized water and blow it dry to obtain the copper-clad ceramic substrate with the embedded groove completed. S2: First, immerse the copper-clad ceramic substrate with the embedded groove completed in a pre-immersion solution at 35℃ and a circulation rate of 30L / min for 5 minutes. Then, transfer it to a chemical silver plating solution at 53℃ and a circulation rate of 30L / min for 12 minutes to form a uniform silver plating layer with a thickness of 1.5μm. Clean and dry, rinse three times with deionized water for 2 minutes each time, and dry in a 70℃ oven for 25 minutes to obtain a copper-clad ceramic substrate with a chemical silver plating layer. The preparation method of the pre-immersion solution is as follows: take 15 volumes of an aqueous solution containing 30mL / L ammonia, 10g / L glucose, 2g / L sodium hydroxide, and 1g / L imidazole; 4 volumes of an aqueous solution containing 50g / L potassium sodium tartrate and 15g / L hydrazine sulfate; 0.5 volumes of nitric acid; and 1000ppm Cu 2+ The remainder is pure water; mix thoroughly to obtain the pre-immersion solution. The preparation method for the chemical silver plating solution is as follows: Take 2 volumes of an aqueous solution containing 27 g / L silver nitrate, 2 g / L tartaric acid, and 10 mL / L ethanol; 20 volumes of an aqueous solution containing 30 mL / L ammonia, 10 g / L glucose, 2 g / L sodium hydroxide, and 1 g / L imidazole; 4 volumes of an aqueous solution containing 50 g / L potassium sodium tartrate and 15 g / L hydrazine sulfate; 0.5 volumes of nitric acid; and 3000 ppm Cu 2+ The remainder is pure water. After mixing evenly, a chemical silver plating solution is obtained. S3: Fix the copper-clad ceramic substrate with chemical silver plating on the worktable of the laser engraving machine. Set the laser parameters as follows: laser wavelength 355nm, power 10W, engraving speed 50mm / s, spot diameter 10μm, and engraving depth 1.2μm. Based on the chip welding area size, which is 4.8mm×4.8mm, draw a closed-loop engraving path and perform closed-loop engraving along the periphery of the silver plating layer in the groove. Remove the non-target silver plating layer with an edge width of 1.0mm. Start the engraving program to complete the selective removal operation and obtain the copper-clad ceramic substrate with selective silver plating. S4: Place the copper-clad ceramic substrate with selective silver plating into a 40kHz ultrasonic cleaner, clean it with deionized water for 8 minutes to remove the silver powder residue generated during engraving, and dry it in a 75℃ oven for 25 minutes to obtain a copper-clad ceramic substrate with selective silver plating in the semi-etched grooves.

[0022] Example 3: A selective chemical silver plating method for semi-etched grooves in copper-clad ceramic substrates, comprising the following steps: S1: A 7mm × 7mm × 0.17mm groove was prepared on the surface of a Si3N4 ceramic substrate using chemical etching. The substrate was etched at an etching temperature of 52℃ to a depth of 0.3mm. The conveyor speed in the etching section was 0.75m / min. The etching solution contained 2.1mol / L hydrochloric acid and 170g / L Cu. 2+ The aqueous solution has a conductivity of 60 S / m and a specific gravity of 1.30. First, remove the oil stains on the substrate surface, then immerse it in the micro-etching solution for 90 seconds. The micro-etching solution is an aqueous solution containing 45% 98% sulfuric acid, 5% 30% hydrogen peroxide, and 12% polyethylene glycol. Finally, immerse it in a 40 mL / L sulfuric acid solution for 60 seconds to remove the oxides remaining after micro-etching. Rinse it with deionized water and blow it dry to obtain the copper-clad ceramic substrate with the embedded groove completed. S2: First, immerse the copper-clad ceramic substrate with the embedded groove completed in a pre-immersion solution at 45℃ and a circulation rate of 70L / min for 5 minutes. Then, transfer it to a chemical silver plating solution at 57℃ and a circulation rate of 70L / min for 18 minutes to form a uniform silver plating layer with a thickness of 3μm. Clean and dry, rinse three times with deionized water for 2 minutes each time, and dry in a 70℃ oven for 25 minutes to obtain a copper-clad ceramic substrate with a chemical silver plating layer. The preparation method of the pre-immersion solution is as follows: Take 20 volumes of an aqueous solution containing 50mL / L ammonia, 20g / L glucose, 5g / L sodium hydroxide, and 3g / L imidazole; 8 volumes of an aqueous solution containing 100g / L potassium sodium tartrate and 25g / L hydrazine sulfate; 1 volume of nitric acid; and 2000ppm Cu 2+ The remainder is pure water; mix thoroughly to obtain the pre-impregnation solution. The preparation method for the chemical silver plating solution is as follows: Take 4 volumes of an aqueous solution containing 32 g / L silver nitrate, 6 g / L tartaric acid, and 15 mL / L ethanol; 30 volumes of an aqueous solution containing 50 mL / L ammonia, 20 g / L glucose, 5 g / L sodium hydroxide, and 3 g / L imidazole; 6 volumes of an aqueous solution containing 100 g / L potassium sodium tartrate and 25 g / L hydrazine sulfate; 1 volume of nitric acid; and 5000 ppm Cu 2+ The remainder is pure water. After mixing evenly, a chemical silver plating solution is obtained. S3: Fix the copper-clad ceramic substrate with chemical silver plating on the worktable of the laser engraving machine. Set the laser parameters as follows: laser wavelength 355nm, power 30W, engraving speed 200mm / s, spot diameter 50μm, and engraving depth 3.5μm. Based on the chip welding area size, which is 4.8mm×4.8mm, draw a closed-loop engraving path and perform closed-loop engraving along the periphery of the silver plating layer in the groove. Remove the non-target silver plating layer with an edge width of 1.0mm. Start the engraving program to complete the selective removal operation and obtain the copper-clad ceramic substrate with selective silver plating. S4: Place the copper-clad ceramic substrate with selective silver plating into a 40kHz ultrasonic cleaner, clean it with deionized water for 8 minutes to remove the silver powder residue generated during engraving, and dry it in a 75℃ oven for 25 minutes to obtain a copper-clad ceramic substrate with selective silver plating in the semi-etched grooves.

[0023] Comparative Example 1: Selective silver plating was performed in the semi-etched grooves using a photosensitive ink exposure and development method. The rest of the procedure was the same as in Example 1. The specific operation is as follows: S1: A 7mm × 7mm × 0.17mm groove was prepared on the surface of a Si3N4 ceramic substrate using chemical etching. The substrate was etched at an etching temperature of 50℃ to a depth of 0.3mm. The conveyor speed in the etching section was 0.75m / min. The etching solution contained 1.9mol / L hydrochloric acid and 150g / L Cu. 2+ The aqueous solution has a conductivity of 35 S / m and a specific gravity of 1.29. First, remove the oil stains on the substrate surface, then immerse it in the micro-etching solution for 90s. The micro-etching solution is an aqueous solution containing 40% 98% sulfuric acid, 4% 30% hydrogen peroxide, and 11% polyethylene glycol. Finally, immerse it in a 40 mL / L sulfuric acid solution for 60s to remove the residual oxides after micro-etching. Rinse it with deionized water and blow it dry to obtain the copper-clad ceramic substrate with the embedded groove completed. S2: Photosensitive ink is coated in the groove and on the substrate surface using wet film printing. The ink thickness is flush with the copper layer surface. The copper-clad ceramic substrate coated with ink is placed in an 80℃ oven for 15 minutes, exposed, and developed. The ink in the chip soldering area is dissolved and removed to expose the copper surface, resulting in the copper-clad ceramic substrate after development opening. S3: First, immerse the copper-clad ceramic substrate after development and opening in a pre-immersion solution at 38℃ and a circulation rate of 50L / min for 5 minutes. Then, transfer it to a chemical silver plating solution at 55℃ and a circulation rate of 50L / min for 15 minutes to form a uniform silver plating layer with a thickness of 2μm. Clean and dry, rinse three times with deionized water for 2 minutes each time, and dry in a 70℃ oven for 25 minutes to obtain a copper-clad ceramic substrate with a chemical silver plating layer. The preparation method of the pre-immersion solution is as follows: take 17 volumes of an aqueous solution containing 40mL / L ammonia, 15g / L glucose, 3g / L sodium hydroxide, and 2g / L imidazole; 6 volumes of an aqueous solution containing 75g / L potassium sodium tartrate and 20g / L hydrazine sulfate; 0.7 volumes of nitric acid; and 1500ppm Cu 2+ The remainder is pure water; mix thoroughly to obtain the pre-immersion solution. The preparation method for the chemical silver plating solution is as follows: Take 3 volumes of an aqueous solution containing 30 g / L silver nitrate, 4 g / L tartaric acid, and 12 mL / L ethanol; 25 volumes of an aqueous solution containing 40 mL / L ammonia, 15 g / L glucose, 3 g / L sodium hydroxide, and 2 g / L imidazole; 5 volumes of an aqueous solution containing 75 g / L potassium sodium tartrate and 20 g / L hydrazine sulfate; 0.8 volumes of nitric acid; and 4000 ppm Cu 2+ The remainder is pure water. After mixing evenly, a chemical silver plating solution is obtained. S4: At 50°C, a copper-clad ceramic substrate with a chemical silver plating layer is immersed in a 3wt% sodium hydroxide aqueous solution for 3 minutes to remove the ink protective layer, then cleaned with deionized water, and dried in a 75°C oven for 25 minutes to obtain a copper-clad ceramic substrate with selective silver plating in the semi-etched grooves.

[0024] Comparative Example 2: The ultraviolet laser engraving power was too high, resulting in excessive engraving depth. The rest of the process was the same as in Example 1. The specific operation is as follows: S1: A 7mm × 7mm × 0.17mm groove was prepared on the surface of a Si3N4 ceramic substrate using chemical etching. The substrate was etched at an etching temperature of 50℃ to a depth of 0.3mm. The conveyor speed in the etching section was 0.75m / min. The etching solution contained 1.9mol / L hydrochloric acid and 150g / L Cu. 2+ The aqueous solution has a conductivity of 35 S / m and a specific gravity of 1.29. First, remove the oil stains on the substrate surface, then immerse it in the micro-etching solution for 90s. The micro-etching solution is an aqueous solution containing 40% 98% sulfuric acid, 4% 30% hydrogen peroxide, and 11% polyethylene glycol. Finally, immerse it in a 40 mL / L sulfuric acid solution for 60s to remove the residual oxides after micro-etching. Rinse it with deionized water and blow it dry to obtain the copper-clad ceramic substrate with the embedded groove completed. S2: First, immerse the copper-clad ceramic substrate with the embedded groove completed in a pre-immersion solution at 38℃ and a circulation rate of 50L / min for 5 minutes. Then, transfer it to a chemical silver plating solution at 55℃ and a circulation rate of 50L / min for 15 minutes to form a uniform silver plating layer with a thickness of 2μm. Clean and dry, rinse three times with deionized water for 2 minutes each time, and dry in a 70℃ oven for 25 minutes to obtain a copper-clad ceramic substrate with a chemical silver plating layer. The preparation method of the pre-immersion solution is as follows: take 17 volumes of an aqueous solution containing 40mL / L ammonia, 15g / L glucose, 3g / L sodium hydroxide, and 2g / L imidazole; 6 volumes of an aqueous solution containing 75g / L potassium sodium tartrate and 20g / L hydrazine sulfate; 0.7 volumes of nitric acid; and 1500ppm Cu 2+ The remainder is pure water; mix thoroughly to obtain the pre-immersion solution. The preparation method for the chemical silver plating solution is as follows: Take 3 volumes of an aqueous solution containing 30 g / L silver nitrate, 4 g / L tartaric acid, and 12 mL / L ethanol; 25 volumes of an aqueous solution containing 40 mL / L ammonia, 15 g / L glucose, 3 g / L sodium hydroxide, and 2 g / L imidazole; 5 volumes of an aqueous solution containing 75 g / L potassium sodium tartrate and 20 g / L hydrazine sulfate; 0.8 volumes of nitric acid; and 4000 ppm Cu 2+ The remainder is pure water. After mixing evenly, a chemical silver plating solution is obtained. S3: Fix the copper-clad ceramic substrate with chemical silver plating on the worktable of the laser engraving machine. Set the laser parameters as follows: laser wavelength 355nm, power 40W, engraving speed 250mm / s, spot diameter 5μm, and engraving depth 4.5μm. Based on the chip welding area size, which is 4.8mm×4.8mm, draw a closed-loop engraving path and perform closed-loop engraving along the periphery of the silver plating layer in the groove. Remove the non-target silver plating layer with an edge width of 1.0mm. Start the engraving program to complete the selective removal operation and obtain the copper-clad ceramic substrate with selective silver plating. S4: Place the copper-clad ceramic substrate with selective silver plating into a 40kHz ultrasonic cleaner, clean it with deionized water for 8 minutes to remove the silver powder residue generated during engraving, and dry it in a 75℃ oven for 25 minutes to obtain a copper-clad ceramic substrate with selective silver plating in the semi-etched grooves.

[0025] Comparative Example 3: The ultraviolet laser engraving power was too low, and the engraving depth was too shallow. The rest was the same as in Example 1. The specific operation is as follows: S1: A 7mm × 7mm × 0.17mm groove was prepared on the surface of a Si3N4 ceramic substrate using chemical etching. The substrate was etched at an etching temperature of 50℃ to a depth of 0.3mm. The conveyor speed in the etching section was 0.75m / min. The etching solution contained 1.9mol / L hydrochloric acid and 150g / L Cu. 2+The aqueous solution has a conductivity of 35 S / m and a specific gravity of 1.29. First, remove the oil stains on the substrate surface, then immerse it in the micro-etching solution for 90s. The micro-etching solution is an aqueous solution containing 40% 98% sulfuric acid, 4% 30% hydrogen peroxide, and 11% polyethylene glycol. Finally, immerse it in a 40 mL / L sulfuric acid solution for 60s to remove the residual oxides after micro-etching. Rinse it with deionized water and blow it dry to obtain the copper-clad ceramic substrate with the embedded groove completed. S2: First, immerse the copper-clad ceramic substrate with the embedded groove completed in a pre-immersion solution at 38℃ and a circulation rate of 50L / min for 5 minutes. Then, transfer it to a chemical silver plating solution at 55℃ and a circulation rate of 50L / min for 15 minutes to form a uniform silver plating layer with a thickness of 2μm. Clean and dry, rinse three times with deionized water for 2 minutes each time, and dry in a 70℃ oven for 25 minutes to obtain a copper-clad ceramic substrate with a chemical silver plating layer. The preparation method of the pre-immersion solution is as follows: take 17 volumes of an aqueous solution containing 40mL / L ammonia, 15g / L glucose, 3g / L sodium hydroxide, and 2g / L imidazole; 6 volumes of an aqueous solution containing 75g / L potassium sodium tartrate and 20g / L hydrazine sulfate; 0.7 volumes of nitric acid; and 1500ppm Cu 2+ The remainder is pure water; mix thoroughly to obtain the pre-immersion solution. The preparation method for the chemical silver plating solution is as follows: Take 3 volumes of an aqueous solution containing 30 g / L silver nitrate, 4 g / L tartaric acid, and 12 mL / L ethanol; 25 volumes of an aqueous solution containing 40 mL / L ammonia, 15 g / L glucose, 3 g / L sodium hydroxide, and 2 g / L imidazole; 5 volumes of an aqueous solution containing 75 g / L potassium sodium tartrate and 20 g / L hydrazine sulfate; 0.8 volumes of nitric acid; and 4000 ppm Cu 2+ The remainder is pure water. After mixing evenly, a chemical silver plating solution is obtained. S3: Fix the copper-clad ceramic substrate with chemical silver plating on the worktable of the laser engraving machine. Set the laser parameters as follows: laser wavelength 355nm, power 5W, engraving speed 30mm / s, spot diameter 80μm, and engraving depth 0.8μm. Based on the chip welding area size, which is 4.8mm×4.8mm, draw a closed-loop engraving path and perform closed-loop engraving along the periphery of the silver plating layer in the groove. Remove the non-target silver plating layer with an edge width of 1.0mm. Start the engraving program to complete the selective removal operation and obtain the copper-clad ceramic substrate with selective silver plating. S4: Place the copper-clad ceramic substrate with selective silver plating into a 40kHz ultrasonic cleaner, clean it with deionized water for 8 minutes to remove the silver powder residue generated during engraving, and dry it in a 75℃ oven for 25 minutes to obtain a copper-clad ceramic substrate with selective silver plating in the semi-etched grooves.

[0026] Performance Testing: Copper-clad ceramic substrates with selective silver plating in the semi-etched grooves obtained in the examples and comparative examples were used. The length and width dimensions of the core silver plating area were measured using an optical microscope. Five different locations were selected for each sample, and the average value was calculated. The deviation between the measured dimensions and the preset chip soldering area size (4.8mm × 4.8mm) was calculated, and the absolute value of the deviation was taken as the silver plating area size deviation. Referring to ASTM B571-23, the tape peeling method was used for testing. The tape was tightly adhered to the silver plating surface, and a rubber roller was used to roll it back and forth three times to ensure full contact between the tape and the plating layer. After standing for 1 minute, the tape was quickly pulled up in a direction perpendicular to the plating surface. The surface of the tape was observed for any plating material peeling off, peeling, or blistering. This was done according to ASTM standards. B571 standard grading: Grade 5: No peeling or flaking of the plating, excellent adhesion; Grade 4: Slight peeling of the plating, but the area is less than 5%, good adhesion; Grade 3: Peeling area of ​​the plating is between 5% and 15%, average adhesion; Grade 2 and below: Large-area peeling of the plating, unacceptable adhesion. After soldering the chip to the silver-plated area, it was subjected to a thermal cycling test of -40℃ to 125℃ for 1000 cycles. In each cycle, -40℃ and 125℃ were maintained for 30 minutes each, and the temperature transition time did not exceed 5 minutes. After the cycle, the solder joints were checked for cracking or cold solder joints. 1000 substrates from each example and comparative example were taken and chip soldered and packaged on the same packaging production line under the same process conditions. After packaging, the number of qualified products was counted, and the percentage of qualified products to the total number of tests was calculated as an evaluation index of production yield. The results are shown in Table 1 below. Table 1

[0027] Conclusion: As shown in the table above, the selective chemical silver plating method for the semi-etched grooves of the copper-clad ceramic substrate of the present invention has the following significant innovations and beneficial effects: As can be seen from Examples 1-3 and Comparative Example 1, the dimensional deviation of the silver-plated area in Examples 1-3 was controlled within ≤±50μm, the coating adhesion reached the ASTM B571 Level 5 standard, and the solder joints after thermal cycling showed no cracking or poor soldering, with a packaging yield greater than 96%. However, when Comparative Example 1 used the photosensitive ink exposure and development method, ink residue was present, the coating adhesion was only the ASTM B571 Level 4 standard, the dimensional deviation of the silver-plated area was ±180μm, the solder joints showed slight cracking after thermal cycling, the packaging yield was 89.3%, and the process was more complicated, adding exposure and development steps, resulting in high process complexity and a long production cycle.

[0028] As shown in Examples 1-3 and Comparative Examples 2-3, in Comparative Example 2, when the laser power was too high and the engraving was too deep, although the dimensional deviation of the silver plating area could be controlled within ≤±70μm, the plating adhesion dropped to ASTM B571 Level 3 standard, and the solder joints showed poor soldering after thermal cycling, resulting in a packaging yield of only 87.9%. In Comparative Example 3, when the laser power was too low and the engraving was too shallow, the plating adhesion was at ASTM B571 Level 4 standard, the dimensional deviation of the silver plating area exceeded ±200μm, and the packaging yield was only 84.6%. This indicates that when the laser energy is insufficient, the silver plating layer in the non-welding area cannot be completely vaporized and removed, and there is still residual silver plating layer in the engraved area. At the same time, when the laser power is too high and the engraving is too deep, the laser energy density is too high, and the remaining energy after penetrating the silver plating layer exceeds the damage threshold of the copper substrate, resulting in obvious melting and oxidation damage to the copper substrate. Therefore, reasonably controlling the laser power and engraving depth is crucial for protecting the copper substrate and ensuring the welding quality of the product.

[0029] In summary, this invention first performs full-surface chemical silver plating on the grooves of the copper-clad ceramic substrate, followed by ultraviolet laser engraving, effectively avoiding ink residue issues and improving plating adhesion. The precise positioning of the ultraviolet laser ensures a high-precision correspondence between the silver plating area and the chip welding area; simultaneously, by rationally controlling the laser parameters, the silver plating layer is completely removed while avoiding damage to the copper substrate, ensuring the welding quality of the product. Furthermore, this invention eliminates multiple processes such as wet film printing, exposure and development, and ink removal cleaning, simplifying the process and correspondingly reducing production costs.

[0030] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.

Claims

1. A method for selective chemical silver plating in a semi-etched groove on a copper-clad ceramic substrate, characterized in that: The selective chemical silver plating method includes the following steps: S1: Perform semi-etching on the copper-clad ceramic substrate to form embedded grooves, then degrease, micro-etch, acid pickling, washing, and drying to obtain the copper-clad ceramic substrate with the embedded grooves completed. S2: Take the copper-clad ceramic substrate after the embedded groove is completed, pre-immerse it, silver-plat it, clean and dry it to form a silver plating layer in the groove and on the surface of the substrate, and obtain a copper-clad ceramic substrate with a chemical silver plating layer. S3: Based on the preset size of the chip welding area, use ultraviolet laser to carve the chemical silver plating layer in the groove, remove the silver plating layer in the non-welding area in the groove, and obtain a copper-clad ceramic substrate with selective silver plating layer. S4: Take a copper-clad ceramic substrate with a selective silver plating layer, clean it, and dry it to obtain a copper-clad ceramic substrate with selective silver plating in the semi-etched groove.

2. The selective chemical silver plating method for semi-etched grooves in copper-clad ceramic substrates according to claim 1, characterized in that: In S2, the pre-impregnation solution used includes the following components, by volume: 15-20% component 1, 4-8% component 2, 0.5-1.0% nitric acid, and 1000-2000 ppm Cu. 2+ Component 1 includes the following components, by concentration: 30-50 mL / L ammonia, 10-20 g / L glucose, 2-5 g / L sodium hydroxide, 1-3 g / L imidazole, and the remainder is pure water; Component 2 includes the following components, by concentration: 50-100 g / L potassium sodium tartrate, 15-25 g / L hydrazine sulfate, and the remainder is pure water.

3. The selective chemical silver plating method for semi-etched grooves in copper-clad ceramic substrates according to claim 1, characterized in that: In S2, the chemical silver plating agent used includes the following components, by volume: 2-4% Agent A, 20-30% Agent B, 4-6% Agent C, 0.5-1.0% nitric acid, and 3000-5000 ppm Cu. 2+ The remainder is pure water; Agent A includes the following components, by concentration: 27~32 g / L silver nitrate, 2~6 g / L tartaric acid, 10~15 mL / L ethanol, with the remainder being pure water; Agent B includes the following components, by concentration: 30~50 mL / L ammonia, 10~20 g / L glucose, 2~5 g / L sodium hydroxide, 1~3 g / L imidazole, with the remainder being pure water; Agent C includes the following components, by concentration: 50~100 g / L potassium sodium tartrate, 15~25 g / L hydrazine sulfate, with the remainder being pure water.

4. The selective chemical silver plating method for semi-etched grooves in copper-clad ceramic substrates according to claim 1, characterized in that: In S1, the etching solution used in the semi-etching process includes the following components, by concentration: 1.7~2.1 mol / L hydrochloric acid, 130~170 g / L Cu. 2+ The rest is pure water.

5. The selective chemical silver plating method for semi-etched grooves in copper-clad ceramic substrates according to claim 1, characterized in that: In S2, the thickness of the electroless silver plating layer is 1~3μm; in S3, the engraving depth is 1.2~3.5μm.

6. The selective chemical silver plating method for semi-etched grooves in copper-clad ceramic substrates according to claim 1, characterized in that: In S3, the parameters for ultraviolet laser engraving are: wavelength of 355nm, power of 10~30W, engraving speed of 50~200mm / s, and spot diameter of 10~50μm.

7. The selective chemical silver plating method for semi-etched grooves in copper-clad ceramic substrates according to claim 1, characterized in that: In S2, the pre-immersion temperature is 35~45℃, and the circulation rate of the pre-immersion solution is 30~70L / min; the silver plating temperature is 53~57℃, and the circulation rate of the silver plating solution is 30~70L / min.

8. The selective chemical silver plating method for semi-etched grooves in copper-clad ceramic substrates according to claim 1, characterized in that: In S1, the micro-etching solution used includes the following components by volume: 35-45% 98% sulfuric acid, 3-5% 30% hydrogen peroxide, 10-12% polyethylene glycol, and the remainder is pure water; the micro-etching treatment time is 60-120s; the acid used for pickling is an aqueous solution containing 30-50mL / L sulfuric acid, and the treatment time is 30-90s.