A high-impact carbon fiber sizing agent, its preparation method and application
A high-impact carbon fiber sizing agent was prepared by compounding polyethersulfone epoxy resin and polyetherimide, which solved the problems of insufficient toughness and poor emulsion stability in the existing technology, and improved the impact resistance and interfacial bonding strength of the composite material, making it suitable for aerospace and automotive lightweighting applications.
Patent Information
- Application Number
- CN202611367263.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-10
AI Technical Summary
Existing carbon fiber sizing agents have insufficient toughness and poor emulsification stability, resulting in poor impact resistance of composite materials, which makes it difficult to meet the needs of high-end equipment.
A water-based emulsion sizing agent is prepared by using polyethersulfone epoxy resin as the main material, compounded with polyetherimide resin, and combined with specific emulsifiers and co-emulsifiers through a mild preparation process, forming a uniform and stable sizing agent.
It significantly improves the impact resistance and fracture toughness of carbon fiber composites, enhances interfacial bonding strength, meets the material requirements of lightweight aerospace and automotive fields, and the preparation process is environmentally friendly and cost-controllable.
Smart Images

Figure CN123064014A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of carbon fiber material surface treatment technology, and more specifically, to a high-impact carbon fiber sizing agent, its preparation method, and its application. Background Technology
[0002] Carbon fiber, with its superior properties such as high strength, high modulus, low density, and high temperature resistance, has become a core reinforcement in high-end composite materials for aerospace, transportation, and new energy fields. However, carbon fiber has a smooth surface, strong chemical inertness, low surface energy, and its monofilaments are brittle and prone to static electricity. During production, weaving, and subsequent compounding processes, problems such as poor bundle cohesion, excessive fibrous strands, and poor wettability with the resin matrix can easily occur, severely affecting the interfacial bonding strength and overall mechanical properties of the composite material. Sizing is an effective means to solve these problems. By coating the carbon fiber surface with a uniform polymer film, static electricity can be reduced, fibers can be protected, bundle cohesion can be improved, and compatibility with the matrix resin can be enhanced, thereby strengthening the interfacial bonding and fully leveraging the reinforcing effect of carbon fiber.
[0003] Currently, carbon fiber sizing agents are mainly classified into epoxy, polyurethane, and polyamide types. Among them, epoxy sizing agents are the most widely used due to their good compatibility with traditional epoxy resins and strong adhesion. However, their inherent weakness in toughness leads to poor impact resistance in composite materials, making it difficult to meet the impact and fracture resistance requirements of high-end equipment. Although polyethersulfone resin has excellent heat resistance, chemical corrosion resistance, and toughness, its interaction with the carbon fiber surface is weak, and its emulsion stability is poor, making it difficult to prepare uniformly dispersed and storage-stable emulsion-type sizing agents.
[0004] In existing technologies, solution-type sizing agents have been prepared by sulfonating and modifying polyethersulfone to improve interfacial adhesion. However, these methods suffer from problems such as environmental pollution from organic solvents and high costs, and do not involve toughening modification with compounded resins. Other methods utilize bisphenol A-type epoxy resin-based emulsion sizing agents, which improve interfacial properties by introducing nano-SiO2 compounded emulsifiers. However, these still rely primarily on epoxy resin, resulting in insufficient toughness and limited improvement in impact resistance. Therefore, this invention aims to provide an environmentally friendly water-based emulsion sizing agent that combines good emulsification stability and excellent impact resistance, using polyethersulfone epoxy resin as the main component and compounded with polyetherimide for synergistic modification. Summary of the Invention
[0005] To address the problems of insufficient toughness, poor emulsification stability, unsatisfactory impact resistance of composite materials, and lack of novelty of single resin systems in existing carbon fiber sizing agents, the present invention aims to provide a high-impact carbon fiber sizing agent, its preparation method, and its application. By using polyethersulfone epoxy resin as the main material and compounding it with polyetherimide (PEI) resin for synergistic modification, the impact resistance and fracture toughness of carbon fiber composite materials are significantly improved.
[0006] This invention is implemented as follows: In a first aspect, the present invention provides a high-impact carbon fiber sizing agent, wherein the sizing agent is a water-based emulsion, comprising the following components by mass percentage: 30%-50% main resin, 3%-8% emulsifier, 1%-3% co-emulsifier, and the balance being deionized water; wherein the main resin is composed of polyethersulfone epoxy resin and polyetherimide, and the mass ratio of the polyethersulfone epoxy resin to the polyetherimide is (8-9):(1-2).
[0007] In an optional embodiment, the polyethersulfone epoxy resin is an epoxy-terminated polyethersulfone resin with an epoxy value of 0.15-0.30 eq / 100g and a number-average molecular weight of 2000-5000.
[0008] In an optional embodiment, the polyetherimide has a number-average molecular weight of 2500-5000 and a glass transition temperature ≥210°C.
[0009] In an optional embodiment, the emulsifier includes a nonionic emulsifier and anionic emulsifier, and the mass ratio of the nonionic emulsifier to the anionic emulsifier is (2-3):1; And / or, the nonionic emulsifier is at least one of alkylphenol polyoxyethylene ether or castor oil polyoxyethylene ether; And / or, the anionic emulsifier is at least one of sodium dodecylbenzenesulfonate or sodium nonylphenol polyoxyethylene ether sulfate.
[0010] In an optional embodiment, the co-emulsifier is at least one of ethylene glycol monobutyl ether or propylene glycol methyl ether.
[0011] Secondly, the present invention provides a method for preparing a high-impact carbon fiber sizing agent as described in any of the foregoing embodiments, comprising the following steps: After mixing polyethersulfone epoxy resin and polyetherimide, the mixture is heated and stirred. After the first stirring, the two are thoroughly mixed. After cooling, the main resin blend is obtained. Mix the emulsifier and co-emulsifier, add some deionized water and stir until homogeneous to obtain an emulsion; The main resin blend is added to the emulsion, and an emulsification reaction is carried out by a second stirring to obtain a preliminary emulsion. The preliminary emulsion is first dispersed, and the remaining deionized water is added for a second dispersion. After filtration, the sizing agent is obtained.
[0012] In an optional embodiment, the first stirring includes the following steps: heating to 60°C-80°C at a rate of 2°C / min-3°C / min, and stirring at a speed of 300r / min-500r / min for 1h-2h; And / or, the second stirring speed is 800 r / min-1200 r / min, the temperature is 15℃-30℃, and the time is 30 min-60 min; And / or, the rotation speed of the first dispersion is 2000 r / min-3000 r / min, the time is 20 min-40 min, and the temperature is ≤40℃; And / or, the second dispersion is performed at a rotation speed of 2000 r / min-3000 r / min, for a time of 10 min-20 min, and at a temperature of ≤40℃; And / or, the filter screen used for filtration is 100-200 mesh.
[0013] Thirdly, the present invention provides a carbon fiber composite material, which is formed by composite molding of carbon fiber and resin matrix. Before composite molding, the carbon fiber is first sized by a high impact-resistant carbon fiber sizing agent as described in any of the foregoing embodiments, and then dried and cured in stages. The sizing amount on the surface of the carbon fiber is 1.0%-1.5% of the carbon fiber mass.
[0014] In an optional embodiment, the sizing agent temperature is 25℃-35℃ and the carbon fiber feeding speed is 600 m / min-650 m / min during the sizing process; the segmented drying process is as follows: drying at 100℃-130℃ for 5s-10s, followed by drying at 150℃-200℃ for 10s-20s.
[0015] In an optional embodiment, the resin matrix is polyethersulfone resin or polyimide resin; the molding temperature is 280℃-320℃, the pressure is 10MPa-20MPa, and the heat and pressure holding time is 10min-20min.
[0016] The present invention has the following beneficial effects: (1) This invention innovatively combines polyethersulfone epoxy resin with polyetherimide, which effectively improves the weak bonding force between single polyethersulfone resin and carbon fiber through their synergistic effect. At the same time, it is combined with a compound emulsifier and a co-emulsifier, and combined with a specific preparation process, the resulting water-based emulsion sizing agent is evenly dispersed, and there is no layering or precipitation after being stored at room temperature and sealed for more than 6 months. Moreover, there is no evaporation of organic solvents, which is environmentally friendly. In addition, the preparation method of this invention does not require complicated equipment, the reaction conditions are mild, the operation is simple, and all raw materials used are industrially mass-produced products, so the cost is controllable and suitable for large-scale production and application.
[0017] (2) The polyethersulfone epoxy resin in the sizing agent proposed in this invention provides good adhesion and basic toughness, while the compounded polyetherimide further enhances the interfacial bonding ability and fracture toughness. The synergistic effect of the two enables the sized carbon fiber and the resin matrix to form a strong interfacial bond, which can effectively transfer and disperse impact loads, inhibit crack propagation, and avoid brittle fracture. According to the test, the carbon fiber composite material prepared by the sizing agent of this invention has an impact strength that is more than 45% higher than that of traditional epoxy sizing agents and more than 25% higher than that of single polyethersulfone sizing agents. The fracture toughness is more than 30% higher than that of single polyethersulfone sizing agents, and the flexural strength is also significantly improved. It can meet the requirements of aerospace, automotive lightweighting and other fields for the impact resistance and fracture resistance of materials. Attached Figure Description
[0018] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0019] Figure 1 This is a scanning electron microscope image of the fibers after sizing with the sizing agent in the embodiments of this application; Figure 2 This is a schematic diagram of the interface bonding of carbon fiber composite materials in the embodiments of this application. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0021] The following is a detailed description of the high impact-resistant carbon fiber sizing agent proposed in this invention, its preparation method, and its application.
[0022] In a first aspect, the present invention provides a high-impact carbon fiber sizing agent, wherein the sizing agent is a water-based emulsion and comprises the following components by mass percentage: 30%-50% main resin, 3%-8% emulsifier, 1%-3% co-emulsifier, and the balance being deionized water; The main resin is composed of polyethersulfone epoxy resin and polyetherimide, and the mass ratio of the polyethersulfone epoxy resin to the polyetherimide is (8-9):(1-2), for example, but not limited to 8:1, 8:2, 9:1 or 9:2, etc.
[0023] In some preferred embodiments, the polyethersulfone epoxy resin is an epoxy-terminated polyethersulfone resin with an epoxy value of 0.15-0.30 eq / 100g, such as 0.015 eq / 100g, 0.20 eq / 100g, 0.25 eq / 100g, or 0.30 eq / 100g; and a number-average molecular weight of 2000-5000, such as 2000, 3000, 4000, or 5000. It is a pale yellow transparent liquid at room temperature, possessing both the high toughness of polyethersulfone and the high adhesion of epoxy resin. It can form strong physical adsorption and chemical interaction with the carbon fiber surface, while providing a good emulsification basis for the sizing agent.
[0024] In some embodiments of this application, the number average molecular weight of the polyetherimide is 2500-5000, for example, it can be 2500, 3000, 3500, 4000, 4500 or 5000, and the glass transition temperature (Tg) is ≥210℃.
[0025] In this application, polyetherimide is selected as the compounding resin. Firstly, it exhibits excellent compatibility with polyethersulfone epoxy resin, forming a stable blend system that achieves uniform dispersion without the need for additional compatibilizers, thus solving the technical problem of easy delamination in blends of different resins. Secondly, the imide groups in the polyetherimide molecule can form strong interactions with the hydroxyl and carboxyl groups on the carbon fiber surface. Simultaneously, its excellent toughness further enhances the fracture resistance of the sizing agent, creating a synergistic "bonding-toughening" effect with the polyethersulfone epoxy resin. This significantly improves the impact resistance and interfacial bonding strength of the carbon fiber composite material, distinguishing it from existing single polyethersulfone or epoxy sizing agents and other compounding systems. Furthermore, the heat resistance of polyetherimide further optimizes the high-temperature stability of the sizing agent, preventing degradation of the sizing layer during subsequent high-temperature molding of the carbon fiber after sizing, ensuring the overall stability of the composite material's performance—an advantage difficult to achieve with existing compounding systems.
[0026] Furthermore, the emulsifier in this application includes a nonionic emulsifier and anionic emulsifier, and the mass ratio of the nonionic emulsifier to the anionic emulsifier is (2-3):1, for example, it can be 2:1, 2.5:1 or 3:1, etc.; preferably, the nonionic emulsifier is at least one of alkylphenol polyoxyethylene ether (OP-10) or castor oil polyoxyethylene ether (EL-40); preferably, the anionic emulsifier is at least one of sodium dodecylbenzenesulfonate (SDBS) or sodium nonylphenol polyoxyethylene ether sulfate (NPES).
[0027] In this process, the anionic emulsifier adsorbs at the oil-water interface, imparting a negative charge to the emulsion droplets and inhibiting droplet aggregation through electrostatic repulsion. The nonionic emulsifier further enhances the repulsive force between droplets through the steric hindrance effect of the polyoxyethylene chain segments, while simultaneously regulating the wettability of the emulsion on the carbon fiber surface. The combination of the two emulsifiers forms a dual stabilizing mechanism of "electrostatic repulsion + steric hindrance," ensuring that the emulsion remains uniformly dispersed during long-term storage, preventing aggregation or sedimentation, and reducing the impact of small-molecule emulsifier residues on the composite material's properties.
[0028] In some preferred embodiments, the co-emulsifier is at least one of ethylene glycol monobutyl ether or propylene glycol methyl ether; its function is to reduce the interfacial tension between oil and water, help improve the dispersion uniformity and storage stability of the emulsion, and prevent the sizing agent from stratifying or settling during storage.
[0029] Secondly, the present invention provides a method for preparing a high-impact carbon fiber sizing agent as described in any of the foregoing embodiments, comprising the following steps: S1. After mixing polyethersulfone epoxy resin and polyetherimide, heat and stir. After the first stirring, the two are fully mixed until a uniform and transparent blended resin system is formed. After cooling, the main resin blend is obtained.
[0030] Specifically, the first stirring includes the following steps: heating to 60℃-80℃ at 2℃ / min-3℃ / min to avoid excessively rapid heating that could lead to resin degradation or uneven mixing; and then stirring at 300r / min-500r / min for 1h-2h.
[0031] S2. Mix the nonionic emulsifier, anionic emulsifier and co-emulsifier, add some deionized water and stir evenly to obtain an emulsion; S3. Add the main resin blend from step S1 to the emulsion from step S2, and carry out the emulsification reaction by stirring for the second time to obtain the preliminary emulsion.
[0032] In some preferred embodiments, the second stirring speed is 800 r / min-1200 r / min, for example, it can be 800 r / min, 900 r / min, 1000 r / min, 1100 r / min or 1200 r / min, etc.; the temperature is 15℃-30℃, and the time is 30min-60min, for example, it can be 30min, 40min, 50min or 60min, etc. S4. The preliminary emulsion is dispersed for the first time, and the remaining deionized water is added for the second dispersion. The mixture is then filtered through a 100-200 mesh filter to remove impurities and unemulsified resin particles, thus obtaining the sizing agent. It is then sealed and stored in a cool, ventilated place.
[0033] In some preferred embodiments, the rotation speed of the first dispersion is 2000 r / min-3000 r / min, for example, 2000 r / min, 2500 r / min or 3000 r / min; the time is 20 min-40 min, for example, 20 min, 25 min, 30 min, 35 min or 40 min; the temperature is ≤40℃ during the high-speed dispersion process to prevent emulsifier failure or emulsion separation; The second dispersion time is 10-20 minutes, for example, it can be 10 minutes, 15 minutes or 20 minutes, etc.
[0034] Thirdly, the present invention provides a carbon fiber composite material, which is formed by composite molding of carbon fiber and resin matrix, wherein the carbon fiber is first sized by a high impact-resistant carbon fiber sizing agent as described in any of the foregoing embodiments before composite molding.
[0035] Specifically, it includes the following steps: (1) Sizing treatment: The carbon fiber is sized by immersion in a sizing tank. The temperature of the sizing agent is 25℃-35℃, the carbon fiber feeding speed is 600 m / min-650 m / min, and the sizing amount is controlled to be 1.0%-1.5% of the carbon fiber mass. It should be noted that the "sizing amount" mentioned in this application refers to the amount of sizing agent adhering to the surface of carbon fiber, that is, the percentage of the dry matter mass of the sizing agent adhering to the surface of carbon fiber after sizing treatment, relative to the mass of the carbon fiber itself.
[0036] For example, the temperature of the sizing agent can be, for example, 25°C, 27°C, 29°C, 31°C, 33°C, or 35°C; the wire feed speed can be, for example, 600 m / min, 610 m / min, 620 m / min, 630 m / min, 640 m / min, or 650 m / min; and the sizing amount can be, for example, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, or 1.5% of the carbon fiber mass.
[0037] (2) Drying and curing: The sized carbon fiber is sent into a drying oven and dried in stages. The first stage of drying is at a temperature of 100℃-130℃ and a drying time of 5s-10s. This is used to remove moisture and emulsifier from the sizing agent and avoid rapid evaporation of moisture, which can cause bubbles or pinholes in the sizing layer. The second stage of drying is at a temperature of 150℃-200℃ and a drying time of 10s-20s. This promotes the resin molecular chains to spread and interpenetrate on the surface of the carbon fiber, forming a continuous, dense sizing layer that is firmly bonded to the fiber surface. (3) Preparation of composite materials: The dried and cured sized carbon fiber is combined with the resin matrix and then molded to prepare carbon fiber composite material. The molding temperature is 280℃-320℃, the molding pressure is 10MPa-20MPa, the heat and pressure holding time is 10min-20min, and the material is demolded after cooling to room temperature to ensure that the internal structure of the composite material is dense and the interface is well bonded, thus obtaining the finished product.
[0038] Furthermore, the resin matrix is a thermoplastic resin, preferably one of polyethersulfone resin and polyimide resin, which has good compatibility with the main resin of the sizing agent. The polyethersulfone epoxy resin in the main resin provides good adhesion and toughness, and the compounded polyetherimide (PEI) resin further enhances toughness and interfacial bonding ability. The two work synergistically to form a strong interfacial bond between the sized carbon fiber and the resin matrix, effectively transferring impact load. At the same time, the addition of polyetherimide can significantly improve the fracture toughness of the composite material, avoid brittle fracture when the material is impacted, and further improve the interfacial bonding quality and impact resistance of the composite material.
[0039] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0040] Example 1 This embodiment provides a high-impact carbon fiber sizing agent, which comprises the following components by mass percentage: main resin: 35%, which is a compound of epoxy-terminated polyethersulfone resin (epoxy value 0.20 eq / 100g, number average molecular weight 3000) and polyetherimide (PEI, number average molecular weight 3500, Tg=220℃) in a mass ratio of 8.5:1.5; Emulsifier: 5%, composed of alkylphenol polyoxyethylene ether (OP-10) and sodium dodecylbenzene sulfonate (SDBS) in a mass ratio of 2.5:1; Co-emulsifier: 2%, which is ethylene glycol monobutyl ether; Deionized water: 58%.
[0041] Its preparation method includes the following steps: S1. Add epoxy-terminated polyethersulfone resin and polyetherimide (PEI) to the reactor in proportion, heat to 70°C at a rate of 2.5°C / min, stir at 400 r / min, keep warm and stir for 1.5 h to form a uniform and transparent blended resin system, and cool to room temperature for later use. S2. Mix OP-10, SDBS and ethylene glycol monobutyl ether in a certain proportion, add 20% deionized water, stir evenly to obtain an emulsion; S3. Slowly add the main resin blend to the emulsion, control the stirring speed to 1000 r / min, and stir at room temperature for 45 min to form a preliminary emulsion. S4. Transfer the preliminary emulsion to a high-speed disperser, control the speed at 2500 r / min, disperse for 30 min, then add the remaining deionized water and continue to disperse for 15 min to obtain a uniform and stable water-based emulsion. S5. After filtration through a 150-mesh filter to remove impurities, the finished sizing agent is obtained.
[0042] Example 2 This embodiment provides a high-impact carbon fiber sizing agent, which comprises the following components by weight percentage: Main resin: 30%, which is a mixture of epoxy-terminated polyethersulfone liquid resin (epoxy value 0.15eq / 100g, number average molecular weight 2000) and polyetherimide (PEI, number average molecular weight 2500, Tg=210℃) in a mass ratio of 8:2. Emulsifier: 3%, composed of castor oil polyoxyethylene ether (EL-40) and nonylphenol polyoxyethylene ether sodium sulfate (NPES) in a mass ratio of 2:1; Co-emulsifier: 1%, propylene glycol methyl ether; Deionized water: 66%.
[0043] The preparation method differs from Example 1 only in the following steps: in step S1, the temperature is raised to 60°C, the stirring speed is 300 r / min, and the temperature is maintained for 2 h; in step S3, the stirring speed is 800 r / min, and the stirring is carried out for 60 min; in step S4, the high-speed dispersion speed is 2000 r / min, and the dispersion is carried out for 40 min.
[0044] Example 3 This embodiment provides a high-impact carbon fiber sizing agent, which comprises the following components by weight percentage: Main resin: 50%, which is a mixture of epoxy-terminated polyethersulfone liquid resin (epoxy value 0.30 eq / 100g, number average molecular weight 5000) and polyetherimide (PEI, number average molecular weight 5000, Tg=230℃) in a mass ratio of 9:1. Emulsifier: 8%, composed of OP-10, EL-40 and SDBS in a mass ratio of 1.5:1:1; Co-emulsifier: 3%, which is a mixture of ethylene glycol monobutyl ether and propylene glycol methyl ether in a mass ratio of 1:1; Deionized water: 39%.
[0045] The preparation method differs from Example 1 only in the following steps: Step S1: heat to 80°C, stir at 500 r / min, and keep warm for 1 h; Step S3: stir at 1200 r / min for 30 min; Step S4: disperse at 3000 r / min for 20 min.
[0046] Comparative Example 1 This comparative example provides a sizing agent and its preparation method, which differs from Example 1 only in that: a single-terminated epoxy polyethersulfone liquid resin is used as the main resin, and no polyetherimide (PEI) compound resin is added.
[0047] Comparative Example 2 This comparative example provides a sizing agent and its preparation method, which differs from Example 1 only in that: bisphenol A type epoxy resin (E51) is used as the main resin, and polyethersulfone epoxy liquid resin and polyetherimide (PEI) are not added.
[0048] Comparative Example 3 This comparative example provides a sizing agent and its preparation method, which differs from Example 1 only in that the mass ratio of terminal epoxy polyethersulfone resin to polyetherimide (PEI) in the main resin is 5:5.
[0049] Experimental Example 1 The sizing agents prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to storage stability tests. The results are shown in Table 1. The storage stability was evaluated by the following method: each sizing agent was sealed and stored in a cool and ventilated place (temperature 5℃-35℃). The state of the emulsion was observed regularly, and the time when layering, precipitation or gelation occurred was recorded to visually reflect the storage performance of the sizing agent.
[0050] The sizing agents prepared in Examples 1-3 and Comparative Examples 1-3 were used to prepare carbon fiber composite materials, including the following steps: Sizing treatment: Polyacrylonitrile-based carbon fibers are passed through a sizing tank containing various sizing agents. The temperature of the sizing agents is controlled at 30±1℃, the fiber feeding speed is 600m / min, and the sizing amount is controlled at 1.2% of the carbon fiber mass. Drying and curing: The sized carbon fiber is sent into a drying oven. The first section is dried at 130℃ for 10 seconds, and the second section is dried at 200℃ for 10 seconds. Composite material preparation: The sized carbon fiber is combined with the polyethersulfone resin matrix, the molding temperature is 300℃, the pressure is 15MPa, the heat and pressure are held for 15min, and the carbon fiber composite material is obtained by cooling and demolding.
[0051] The carbon fiber composites prepared in each group were tested for impact strength, flexural strength and fracture toughness. The results are shown in Table 1.
[0052] Impact strength was tested according to GB / T 1451-2005 "Test Method for Impact Properties of Carbon Fiber Reinforced Plastics"; flexural strength was tested according to GB / T 1449-2005 "Test Method for Flexural Properties of Carbon Fiber Reinforced Plastics"; and fracture toughness was tested according to ASTM D5045 standard. The mechanical property data in Table 1 are the arithmetic mean of three parallel tests under the same test conditions to ensure the reliability and repeatability of the data.
[0053] Table 1. Performance Test Results
[0054] Figure 1 and Figure 2 The images shown are scanning electron microscope (SEM) images of the carbon fiber surface and the composite material interface after sizing agent treatment in Example 1. Figure 1 As can be seen, the coating on the fiber surface is uniform, continuous, and dense, without agglomerates or exposed areas, indicating that the sizing agent has good spreadability and film-forming properties on the fiber surface. Figure 2 It is evident that a significant amount of matrix resin adheres to the surface of the carbon fiber, and no obvious interfacial gaps or large-area debonding defects are observed between the fiber and the resin matrix, indicating that the matrix resin has adequately wetted the surface of the carbon fiber.
[0055] Based on the test results in Table 1, the sizing agents prepared in Examples 1-3 of this invention showed no stratification or precipitation after being stored at room temperature and sealed for 6-8 months, while Comparative Example 1 (single polyethersulfone epoxy resin) showed slight stratification after 4 months, indicating that the introduction of polyetherimide effectively improved the long-term storage stability of the emulsion. In terms of mechanical properties, the carbon fiber composites prepared in Examples 1-3 had impact strengths of 185 kJ / m², 172 kJ / m², and 198 kJ / m², respectively; flexural strengths of 1680 MPa, 1590 MPa, and 1750 MPa, respectively; and fracture toughnesses of 8.2 kJ / m², 7.8 kJ / m², and 8.6 kJ / m², respectively. These were significantly better than those of Comparative Example 1 (impact strength 148 kJ / m², flexural strength 1520 MPa, fracture toughness 6.9 kJ / m²) and Comparative Example 2 (impact strength 128 kJ / m², flexural strength 1600 MPa, fracture toughness 6.5 kJ / m²). The impact strength of Comparative Example 3 (154 kJ / m²) was significantly lower. 2 ), bending strength (1540 MPa) and fracture toughness (7.1 kJ / m), 2Although superior to Comparative Examples 1 and 2, indicating that the introduction of PEI does indeed help improve the toughness of the composite material, the high PEI ratio (5:5) led to decreased system compatibility, resulting in significant stratification and precipitation after only 3 months. Its storage stability was the worst among all groups, suggesting that there is an optimal range for PEI addition; excessive addition can disrupt the homogeneous structure of the emulsion and accelerate stratification. The above data fully demonstrate that the compounding of polyethersulfone epoxy resin and polyetherimide produced a significant synergistic toughening effect, comprehensively improving the impact strength, flexural strength, and fracture toughness of the composite material. While Comparative Example 1 showed acceptable flexural strength, its impact strength and fracture toughness were significantly lower than the example, verifying the key role of PEI in improving impact resistance. Comparative Example 2 had the lowest impact strength among all groups, indicating that the inherent defect of insufficient toughness in traditional epoxy sizing agents makes it difficult to meet the requirements of high impact resistance. Although Comparative Example 3 improved mechanical properties, its overall performance was still inferior to the example due to the stability issues of the emulsion. In summary, this invention, through the synergistic compounding of polyethersulfone epoxy resin and polyetherimide, simultaneously solves the technical problems of poor emulsion stability and insufficient impact resistance of composite materials in the prior art, and has significant industrial application value.
[0056] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A high-impact carbon fiber sizing agent, characterized in that, The sizing agent is a water-based emulsion, comprising the following components by mass percentage: 30%-50% main resin, 3%-8% emulsifier, 1%-3% co-emulsifier, and the balance being deionized water; wherein the main resin is composed of polyethersulfone epoxy resin and polyetherimide, and the mass ratio of the polyethersulfone epoxy resin to the polyetherimide is (8-9):(1-2).
2. The high impact-resistant carbon fiber sizing agent according to claim 1, characterized in that, The polyethersulfone epoxy resin is an epoxy-terminated polyethersulfone resin with an epoxy value of 0.15-0.30 eq / 100g and a number-average molecular weight of 2000-5000.
3. The high-impact carbon fiber sizing agent according to claim 1, characterized in that, The polyetherimide has a number-average molecular weight of 2500-5000 and a glass transition temperature ≥210℃.
4. The high impact-resistant carbon fiber sizing agent according to claim 1, characterized in that, The emulsifier includes nonionic emulsifier and anionic emulsifier, and the mass ratio of the nonionic emulsifier to the anionic emulsifier is (2-3):1; And / or, the nonionic emulsifier is at least one of alkylphenol polyoxyethylene ether or castor oil polyoxyethylene ether; And / or, the anionic emulsifier is at least one of sodium dodecylbenzenesulfonate or sodium nonylphenol polyoxyethylene ether sulfate.
5. The high impact-resistant carbon fiber sizing agent according to claim 1, characterized in that, The co-emulsifier is at least one of ethylene glycol monobutyl ether or propylene glycol methyl ether.
6. A method for preparing a high-impact carbon fiber sizing agent as described in any one of claims 1-4, characterized in that, Includes the following steps: After mixing polyethersulfone epoxy resin and polyetherimide, the mixture is heated and stirred. After the first stirring, the two are thoroughly mixed. After cooling, the main resin blend is obtained. Mix the emulsifier and co-emulsifier, add some deionized water and stir until homogeneous to obtain an emulsion; The main resin blend is added to the emulsion, and an emulsification reaction is carried out by a second stirring to obtain a preliminary emulsion. The preliminary emulsion is first dispersed, and the remaining deionized water is added for a second dispersion. After filtration, the sizing agent is obtained.
7. The preparation method according to claim 6, characterized in that, The first stirring includes the following steps: Increase the temperature to 60℃-80℃ at a rate of 2℃ / min-3℃ / min, and stir at a speed of 300r / min-500r / min for 1h-2h; And / or, the second stirring speed is 800 r / min-1200 r / min, the temperature is 15℃-30℃, and the time is 30 min-60 min; And / or, the rotation speed of the first dispersion is 2000 r / min-3000 r / min, the time is 20 min-40 min, and the temperature is ≤40℃; And / or, the second dispersion is performed at a rotation speed of 2000 r / min-3000 r / min for 10 min-20 min, and at a temperature of ≤40℃; And / or, the filter screen used for filtration is 100-200 mesh.
8. A carbon fiber composite material, characterized in that, The carbon fiber composite material is formed by composite molding of carbon fiber and resin matrix. Before composite molding, the carbon fiber is first coated with a high impact-resistant carbon fiber sizing agent as described in any one of claims 1-5, and then dried and cured in stages. The amount of sizing on the surface of the carbon fiber is 1.0%-1.5% of the carbon fiber mass.
9. A carbon fiber composite material according to claim 8, characterized in that, In the sizing process, the sizing agent temperature is 25℃-35℃, and the carbon fiber feeding speed is 600 m / min-650 m / min; the segmented drying process is as follows: drying at 100℃-130℃ for 5s-10s, and then drying at 150℃-200℃ for 10s-20s.
10. A carbon fiber composite material according to claim 8, characterized in that, The resin matrix is polyethersulfone resin or polyimide resin; the molding temperature is 280℃-320℃, the pressure is 10MPa-20MPa, and the heat and pressure holding time is 10min-20min.