An air-preheated lifting kiln and its atmosphere conditioning and rapid cooling method
By laying multiple layers of staggered refractory bricks and airflow channels on the furnace door of the lifting kiln, combined with valve control, the problems of gray spots on ceramic products and long cooling cycles caused by poor atmosphere were solved, achieving rapid cooling and efficient utilization.
Patent Information
- Application Number
- CN202611228513.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-13
- Publication Date
- 2026-11-10
AI Technical Summary
Existing lifting kilns suffer from poor atmosphere due to sealing issues, resulting in gray spots on ceramic products, long cooling cycles, and low kiln utilization.
Multiple layers of staggered refractory bricks are laid on the steel structure of the furnace door to form a stepped labyrinth seal structure. Air inlet holes and airflow channels are opened on it. Combined with valve control, air preheating and atmosphere conditioning are achieved. Through staged atmosphere conditioning and cooling methods, the stability of the atmosphere inside the furnace and rapid cooling are ensured.
It effectively prevents gray spots on ceramic products, shortens the cooling time from 6 days to 3 days, and improves kiln utilization and production efficiency.
Smart Images

Figure CN123065236A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of ceramic sintering technology, specifically relating to an air-preheated lifting kiln and its atmosphere regulation and rapid cooling method. Background Technology
[0002] Lift-type kilns are core thermal equipment in the field of advanced ceramic material preparation, especially suitable for the sintering of high-performance alumina ceramics, electronic ceramics, and structural ceramics. Compared with traditional pusher kilns and roller kilns, lift-type kilns have outstanding advantages such as flexible and adjustable furnace volume, strong controllability of temperature field distribution, and freely programmable sintering curves. Therefore, they occupy an irreplaceable position in the production of large-size ceramic parts, irregularly shaped structural parts, and precision ceramic products with stringent requirements for temperature uniformity.
[0003] The basic structure of existing lifting kilns typically includes the outer furnace shell, inner furnace lining, furnace door, furnace chamber, refractory insulation layer, electric heating elements, and temperature control system. A multi-layered stepped labyrinth seal structure is commonly used between the furnace door and the furnace body. This design aims to improve the sealing performance of the furnace chamber, reduce the escape of high-temperature furnace gases, thereby ensuring the uniformity and stability of the temperature field inside the furnace, reducing heat loss, and improving the sintering consistency of the products.
[0004] Meanwhile, during the binder removal stage of ceramic sintering, organic binders, dispersants, and other additives in the green body decompose at high temperatures, producing exhaust gases containing hydrocarbons, carbon monoxide, carbon dioxide, and water vapor. To meet environmental emission requirements, existing technologies typically channel these exhaust gases through flue gas ducts into a flue gas incinerator for secondary combustion treatment, thereby achieving the full decomposition of harmful components and meeting emission standards.
[0005] While the aforementioned technical solutions have addressed the sealing and exhaust gas treatment issues to some extent, they have also introduced new technical challenges. On one hand, the highly sealed furnace structure results in extremely poor atmospheric flow within the furnace. Gaseous products generated during the decomposition of organic matter in the binder removal stage cannot be promptly discharged, easily leading to the formation of a localized reducing or carbon-enriched atmosphere inside the furnace. Under these unfavorable atmospheric conditions, during the high-temperature sintering process of alumina ceramics, carbon residues react with impurity ions in the material, causing appearance defects such as gray spots and uneven coloring inside the finished product, severely impacting the product's appearance quality and commercial value.
[0006] On the other hand, due to the excellent overall sealing of the furnace body, heat cannot be rapidly released through natural convection or forced ventilation during the cooling stage after sintering, resulting in an extremely slow cooling rate. Taking a typical furnace with effective dimensions of 2400×800mm as an example, it often takes up to 6 days to cool naturally from the highest sintering temperature to the temperature ready for opening. This long cooling period not only significantly reduces the furnace's equipment turnover rate and production efficiency but also increases the energy consumption cost per batch of products, thus restricting the release of production capacity for large-scale production.
[0007] To address the aforementioned issues, some existing technologies attempt to improve atmosphere control and cooling efficiency by opening closable ventilation openings on the top or side walls of the furnace. However, the direct entry of cold air into the high-temperature furnace can cause severe thermal shock to the refractory materials, heating elements, and products being sintered, potentially leading to serious consequences such as refractory lining peeling, accelerated oxidation of heating wires, and even product cracking, thus shortening the equipment's service life and affecting the yield. Summary of the Invention
[0008] The purpose of this invention is to overcome the above-mentioned problems and provide a solution to the technical problems of gray spots on ceramic products caused by poor atmosphere in existing sealed lifting kilns, as well as long cooling cycles and low kiln utilization.
[0009] To achieve the above objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides an air preheating type lifting kiln, including a kiln body and a lifting kiln door disposed at the bottom of the kiln body, the kiln body having a furnace chamber inside, and a flue gas outlet communicating with the furnace chamber on the kiln body; The lifting furnace door includes a furnace door steel structure and multiple layers of refractory bricks laid on the furnace door steel structure. The multiple layers of refractory bricks are laid in a vertical direction and adjacent layers of refractory bricks are staggered in the horizontal direction. The furnace door steel structure has multiple air inlet holes that penetrate the furnace door steel structure, and a valve is installed at each air inlet hole; the refractory brick layer has multiple airflow channels, the number of air inlet holes and airflow channels are the same and correspond one-to-one, one end of each airflow channel is an air inlet port and the other end is an air outlet port, the air inlet port is connected to the corresponding air inlet hole, and the air outlet port is located on the side surface of the refractory brick layer facing the furnace. In the stacking direction of the refractory brick layers, the airflow channels extend in a bent shape.
[0010] A further improvement of the present invention is that the refractory brick layer includes a first refractory brick layer, a second refractory brick layer, a third refractory brick layer, a fourth refractory brick layer and a fifth refractory brick layer laid sequentially from bottom to top, and the adjacent refractory brick layers are staggered and stacked in the horizontal direction.
[0011] A further improvement of the present invention is that the airflow channel is formed by connecting refractory bricks with first through holes and semi-circular grooves in each refractory brick layer. The first through hole penetrates the center of the refractory brick along the thickness direction. The semi-circular groove is opened on the upper surface of the refractory brick. One end of the semi-circular groove is connected to the first through hole, and the other end of the semi-circular groove extends to the side of the refractory brick.
[0012] A further improvement of the present invention is that the first through hole of the refractory brick in the same layer is connected to the semi-circular groove; in two adjacent layers of refractory brick, the side end of the semi-circular groove of the lower layer of refractory brick is vertically opposite to and connected to the first through hole of the upper layer of refractory brick; the opening direction of the semi-circular groove faces the center side of the furnace.
[0013] A further improvement of the present invention is that the plurality of air inlet holes are staggered on the upper surface of the furnace door steel structure, and the spacing between two adjacent air inlet holes is equal to the width of a single refractory brick; the refractory bricks are laid in the first refractory brick layer at positions corresponding to each air inlet hole, and the first through hole of the refractory brick is coaxially aligned with the corresponding air inlet hole.
[0014] A further improvement of the present invention is that the valve is a manual regulating valve or an electric regulating valve, and the valve is installed on the lower surface of the furnace door steel structure and covers the opening of the air inlet hole.
[0015] Secondly, the present invention also provides an atmosphere conditioning and cooling method for an air preheating type lifting kiln, wherein the air preheating type lifting kiln further includes a flue gas pipe, one end of the flue gas pipe is connected to the exhaust port, and the other end of the flue gas pipe is connected to the kiln body; The method includes the following steps: Degreasing stage: The furnace temperature is raised from room temperature to the first temperature. During this stage, the valve is fully open, and the combustion heating function and exhaust function of the furnace body are activated simultaneously. Medium-temperature sintering stage: After the furnace temperature reaches the first temperature, it continues to rise to the second temperature. During this stage, the combustion heating function and exhaust function of the furnace body are turned off, and the valve is switched to a half-open state. High-temperature sintering stage: After the furnace temperature reaches the second temperature, the temperature continues to rise to the highest sintering temperature and is held at that temperature. During this stage, the valve is switched to the fully closed state, and the combustion heating function and exhaust function of the furnace body are kept off. Natural cooling stage: Heating is stopped, and the furnace temperature is allowed to drop naturally from the highest sintering temperature to the third temperature. During this stage, the valves remain fully closed, and the combustion heating function and exhaust function of the furnace body remain closed. First controllable cooling stage: After the furnace temperature drops to the third temperature, it continues to cool down to the fourth temperature. During this stage, the valve is switched to a half-open state, and the combustion heating function and exhaust function of the furnace body are kept closed. The second controllable cooling stage: After the furnace temperature drops to the fourth temperature, it continues to cool down to the fifth temperature. In this stage, the valve is switched to the fully open state, the exhaust function of the furnace body is turned on, and its combustion heating function is turned off.
[0016] A further improvement of the present invention is that the first temperature is 700~900℃, the second temperature is 1200~1350℃, the highest sintering temperature is 1550~1650℃, the third temperature is 1100~1250℃, the fourth temperature is 700~900℃, and the fifth temperature is 250~400℃.
[0017] A further improvement of the present invention is that, during the glue discharge stage, the exhaust gas generated in the furnace enters the furnace body through the exhaust port and flue gas pipe, and is discharged after being heated by combustion in the furnace body.
[0018] A further improvement of the present invention is that, in the second controllable cooling stage, after the valve is fully opened, air enters the airflow channel through the air inlet hole, is preheated by the airflow channel, flows from bottom to top through the furnace, and then enters the furnace body through the exhaust port and flue gas pipe, and is discharged by the exhaust function of the furnace body.
[0019] Compared with the prior art, the present invention has the following beneficial effects: This invention provides an air-preheated lifting kiln. By installing a lifting kiln door at the bottom of the kiln body and laying multiple layers of staggered refractory bricks on the steel structure of the kiln door, a stepped labyrinth seal structure is formed between the kiln door and the kiln opening. This ensures the kiln's long-lasting seal during the sintering process and effectively prevents the escape of high-temperature furnace gases. Multiple air inlets penetrating the kiln door steel structure are provided with valves. These are matched with airflow channels in the refractory brick layers, each corresponding to one of the air inlets. Each airflow channel has an air inlet at one end, connected to the corresponding air inlet, and an air outlet at the other end, located on the side of the refractory brick layer facing the furnace. These channels extend in a bent shape along the stacking direction of the refractory brick layers, allowing outside air to be indirectly preheated by the refractory brick layer of the kiln door before entering the furnace. This avoids cold air directly entering and causing cold shock to the furnace refractory materials, heating elements, and products to be sintered, thus protecting the internal components of the kiln and extending the equipment's service life. Meanwhile, multiple independent airflow channels, combined with valve on / off control, allow the kiln to flexibly adjust the amount of air entering the furnace according to process requirements, thereby achieving on-demand adjustment of the oxidation atmosphere inside the furnace. The structure is simple and easy to implement.
[0020] Furthermore, the refractory brick layer comprises a first to a fifth refractory brick layer laid sequentially from bottom to top, with adjacent layers horizontally staggered. The airflow channel is formed by the corresponding interconnection of refractory bricks with first through holes and semi-circular grooves in each refractory brick layer. The first through hole penetrates the center of the refractory brick along its thickness direction, and the semi-circular groove is opened on the upper surface of the refractory brick with one end connected to the first through hole and the other end extending to the side of the refractory brick. This causes the airflow channel to form an extended path with multiple bends and turns in the stacking direction, which prolongs the residence time of air inside the furnace door, significantly improves the heat exchange efficiency between air and the refractory brick layer, and ensures that the cold air is fully preheated before reaching the furnace.
[0021] Furthermore, the first through hole and the semi-circular groove of the same layer of refractory bricks are interconnected. The end of the side of the semi-circular groove of the lower layer of refractory bricks in the vertical direction is opposite to and connected to the first through hole of the upper layer of refractory bricks. The opening of the semi-circular groove faces the center of the furnace. This allows the grooves and through holes of each layer of refractory bricks to be connected alternately to form a continuous airflow channel. No additional pipes are required, which simplifies the construction difficulty of the furnace door and reduces the manufacturing cost.
[0022] Furthermore, multiple air inlet holes are staggered on the upper surface of the furnace door steel structure, and the spacing between adjacent air inlet holes is equal to the width of a single refractory brick. Refractory bricks are laid in the first refractory brick layer at positions corresponding to each air inlet hole, with their first holes coaxially aligned with the air inlet holes. This ensures that the air inlet port of each airflow channel is precisely connected to the corresponding air inlet hole, avoiding channel blockage caused by positional offset during the laying process, and ensuring the uniformity of air intake in each airflow channel.
[0023] This invention also provides an atmosphere regulation and cooling method for an air-preheated lifting kiln. During the binder removal stage, the valves are fully opened while the kiln's combustion heating and exhaust functions are simultaneously activated, allowing for ample air circulation within the furnace. Hydrocarbons and CO generated during ceramic binder removal are introduced into the kiln through exhaust ports and flue gas pipes for combustion heating before being discharged. Simultaneously, preheated fresh air enters the furnace, effectively preventing the retention of organic decomposition products within the kiln, which could lead to gray spots on the ceramic products and ensure product appearance quality. During the medium-temperature sintering stage, the kiln's combustion heating and exhaust functions are closed, and the valves are switched to a semi-open state to maintain a weakly oxidizing atmosphere within the kiln, avoiding the adverse effects of excessive air on the sintering process. During the high-temperature sintering stage, the valves are fully closed, and the kiln's combustion heating and exhaust functions remain shut off, ensuring a completely sealed furnace and guaranteeing a stable temperature field required for high-temperature sintering, ensuring sufficient densification of the ceramics. During the natural cooling stage, heating is stopped, the valves remain fully closed, and the kiln's combustion heating and exhaust functions remain shut off. After natural cooling, preheated air is introduced through the half-open valve of the first controllable cooling stage to promote cooling, and the fully open valve of the second controllable cooling stage is used to activate the furnace exhaust function and shut down its combustion heating function for forced exhaust. The air, which has been preheated through the airflow channel of the furnace door, flows from bottom to top through the furnace chamber, and then enters the furnace body through the flue gas outlet and flue gas pipe and is discharged by the exhaust function. This achieves forced convection heat exchange of the hot air in the furnace. Under the premise of ensuring equipment safety, the cooling time is shortened from the original 6 days to 3 days, which significantly improves the turnover rate and production efficiency of the kiln. Attached Figure Description
[0024] The accompanying drawings described herein are for illustrative purposes only and are not intended to limit the scope of the invention in any way. Furthermore, the shapes and proportions of the components in the drawings are merely illustrative to aid in understanding the invention and do not specifically limit the shapes and proportions of the components of the invention.
[0025] Figure 1 This is a schematic diagram of the overall structure of the air preheating type lifting kiln of the present invention; Figure 2 This is a schematic diagram of the refractory brick layer structure; Figure 3 This is a top view of the refractory brick layer; Figure 4 This is a schematic diagram of the airflow channel structure; Figure 5 A schematic diagram of the structure of the first through hole and the semi-circular groove in a refractory brick; Figure 6 A schematic diagram of the air inlet port structure on the first layer of refractory bricks; Figure 7 This is a schematic diagram of the air outlet structure on the fifth layer of refractory bricks.
[0026] The components are: 1. Furnace body; 2. Lifting furnace door; 3. Furnace chamber; 4. Smoke outlet; 5. Refractory brick layer; 51. First refractory brick layer; 52. Second refractory brick layer; 53. Third refractory brick layer; 54. Fourth refractory brick layer; 55. Fifth refractory brick layer; 6. Airflow channel; 61. Air inlet port; 62. Air outlet port; 7. Refractory brick; 71. First through hole; 72. Semi-circular groove. Detailed Implementation
[0027] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The components of the embodiments of the present invention described and shown in the accompanying drawings can generally be arranged and designed in various different configurations.
[0028] Therefore, the following detailed description of the embodiments of the invention provided in the accompanying drawings is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the invention without inventive effort are within the scope of protection of the invention.
[0029] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.
[0030] In the description of the embodiments of the present invention, it should be noted that if terms such as "upper," "lower," "horizontal," or "inner" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship commonly used when the product of the invention is in use, they are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of the present invention. Furthermore, terms such as "first" and "second" are only used to distinguish descriptions and should not be construed as indicating or implying relative importance.
[0031] Furthermore, the use of the term "horizontal" does not imply that the component must be absolutely horizontal, but rather that it can be slightly tilted. For example, "horizontal" simply means that its direction is more horizontal than "vertical," and does not mean that the structure must be completely horizontal, but can be slightly tilted.
[0032] In the description of the embodiments of the present invention, it should also be noted that, unless otherwise explicitly specified and limited, the terms "set," "install," "connect," and "link" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in the present invention according to the specific circumstances.
[0033] The present invention will now be described in further detail with reference to the accompanying drawings: This invention provides an air-preheated lifting kiln, comprising a furnace body 1 and a lifting furnace door 2 located at the bottom of the furnace body 1. The furnace body 1 has a furnace chamber 3 inside, and a flue gas outlet 4 communicating with the furnace chamber 3 is provided on the furnace body 1. The lifting furnace door 2 includes a furnace door steel structure and multiple layers of refractory bricks 5 laid on the furnace door steel structure. The multiple layers of refractory bricks 5 are stacked vertically, and adjacent layers of refractory bricks 5 are staggered in the horizontal direction. When the lifting system drives the lifting furnace door 2 to the closed position, the multiple layers of refractory bricks 5 extend into the lower opening of the furnace chamber 3. The lower opening of the furnace chamber 3 is provided with a trapezoidal sealing surface that matches the stepped staggered structure of the refractory bricks 5. The refractory bricks 5 and the trapezoidal sealing surface below the furnace chamber 3 are completely corresponding and interlocked in the vertical direction, forming a complete stepped labyrinth sealing structure, thereby achieving a sealed fit between the lifting furnace door 2 and the furnace body 1.
[0034] As a specific embodiment, taking the effective size of the furnace chamber 3 as 2400×800mm as an example, the size of the bottom steel structure of the furnace door is 2800×1200mm, and the depth is 50mm. The size of the refractory bricks 7 used to lay the furnace door 2 is 200×100×50mm. The furnace door steel structure is provided with multiple air inlet holes that penetrate the furnace door steel structure. For example, six φ25mm through holes are drilled in a staggered manner on the bottom steel structure of the furnace door. A valve is installed at each air inlet hole, which serves as a switch valve for air to enter the furnace chamber 3. The multi-layer refractory brick layer 5 is provided with multiple airflow channels 6. The number of air inlet holes and airflow channels 6 are the same and correspond one-to-one. One end of each airflow channel 6 is an air inlet port 61, and the other end is an air outlet port 62. The air inlet port 61 is connected to the corresponding air inlet hole, and the air outlet port 62 is located on the side surface of the multi-layer refractory brick layer 5 facing the furnace chamber 3. In the stacking direction of the multi-layer refractory brick layer 5, the airflow channel 6 extends in a bent shape.
[0035] The multi-layered refractory brick layer 5 includes a first refractory brick layer 51, a second refractory brick layer 52, a third refractory brick layer 53, a fourth refractory brick layer 54, and a fifth refractory brick layer 55 laid sequentially from bottom to top, with adjacent refractory brick layers 5 staggered in the horizontal direction. The airflow channel 6 is formed by connecting refractory bricks 7 layer by layer in each refractory brick layer 5. The refractory brick 7 is a perforated refractory brick, with a first through hole 71 of φ25mm drilled at its center, and a semi-circular groove 72 of φ25mm drilled from the center to the side of its upper surface. One end of the semi-circular groove 72 is connected to the first through hole 71, and the other end of the semi-circular groove 72 extends to the side of the refractory brick 7. During installation, the first refractory brick layer 51 is embedded within the furnace door steel structure, with perforated refractory bricks 7 aligned with the air inlet holes. The semi-circular grooves 72 of the perforated refractory bricks 7 serve as part of the air passage, with their openings facing the center of the furnace 3. The second refractory brick layer 52 is laid in a staggered manner, with perforated refractory bricks 7 placed where semi-circular grooves 72 are located, again with the openings of the semi-circular grooves 72 facing the center of the furnace 3. This process is repeated for the third, fourth, and fifth refractory brick layers 53, until the entire furnace door 2 refractory brick installation is complete. It should be noted that, except for the perforated refractory bricks 7 placed in specific locations, all other locations are covered with ordinary, non-perforated refractory bricks.
[0036] In the specific structure, the first through hole 71 and the semi-circular groove 72 of the same layer of refractory bricks 7 are interconnected; in the two adjacent layers of refractory bricks 5, the side end of the semi-circular groove 72 of the lower layer of refractory bricks 7 is vertically aligned with and connected to the first through hole 71 of the upper layer of refractory bricks 7; the opening of the semi-circular groove 72 faces the center of the furnace 3. Thus, each airflow channel 6 starts from the first refractory brick layer 51 and ascends to the furnace 3 in a stepped manner. That is, after the outside air enters the airflow channel 6 through the air inlet hole at the bottom of the furnace door 2, it flows upward layer by layer along a tortuous path, and finally enters the furnace 3 at the air outlet port 62 of the fifth refractory brick layer 55. Multiple air inlet holes are staggered on the upper surface of the furnace door steel structure, and the distance between two adjacent air inlet holes is equal to the width of a single refractory brick 7. Refractory bricks 7 are laid in the first refractory brick layer 51 at positions corresponding to each air inlet hole, and the first through hole 71 of the refractory brick 7 is coaxially aligned with the corresponding air inlet hole. The valve is a manual or electric regulating valve, installed on the lower surface of the furnace door steel structure and covering the opening of the air inlet hole. Through the above-mentioned stepped, bent channel design, external cold air is preheated by the refractory bricks 7 at the furnace bottom before entering the furnace chamber 3, effectively preventing cold air from directly entering and causing cold shock to the refractory material, heating elements, and products in the furnace chamber 3, leading to cracking or reduced service life.
[0037] This invention also provides an atmosphere conditioning and cooling method for an air-preheated lifting kiln, wherein the air-preheated lifting kiln further includes a flue gas duct, one end of which is connected to the exhaust port 4, and the other end of which is connected to the furnace body 1. The exhaust gas in the furnace chamber 3 is introduced into the furnace body 1 for treatment via the exhaust port 4 and the flue gas duct. Taking A-95 alumina ceramic sintering as an example, the method specifically includes the following steps: Debinding stage: The furnace temperature is raised from room temperature to a first temperature, which is 700~900℃ (preferably 800℃). During this stage, the valves are fully open, and the air inlet valve at the bottom of the furnace door 2 and the combustion heating and exhaust functions of the furnace body 1 are opened simultaneously. This ensures that the exhaust gas (mainly containing various hydrocarbons, CO, CO2 and water vapor, etc.) generated during the ceramic sintering debinding stage enters the furnace body 1 through the exhaust port 4 and the flue gas pipe, is fully decomposed and discharged after combustion heating in the furnace body 1. At the same time, fresh air enters the airflow channel 6 through the air inlet, and after preheating, enters the furnace chamber 3, ensuring sufficient air circulation in the furnace so that the decomposition products of organic matter are discharged in time, avoiding the appearance of gray spots in the ceramic body.
[0038] Medium-temperature sintering stage: After the furnace temperature reaches the first temperature, it continues to rise to the second temperature, which is 1200~1350℃ (preferably 1300℃). During this stage, the combustion heating function and exhaust function of the furnace body 1 are turned off, and the valve is switched to a half-open state. High-temperature sintering stage: After the furnace temperature reaches the second temperature, it continues to rise to the highest sintering temperature and holds at that temperature, which is 1550~1650℃ (preferably 1600℃). During this stage, the valve is switched to a fully closed state, the air inlet valve at the bottom of the furnace door 2 is closed, and ceramic sintering is completed according to the set sintering curve. The combustion heating function and exhaust function of the furnace body 1 remain closed.
[0039] Natural cooling stage: Heating is stopped, allowing the furnace temperature to naturally decrease from the highest sintering temperature to a third temperature, which is 1100~1250℃ (preferably 1200℃). During this stage, the valve remains fully closed, and the combustion heating and exhaust functions of the furnace body 1 remain off, achieving natural cooling of the kiln. First controllable cooling stage: After the furnace temperature drops to the third temperature, it continues to cool to a fourth temperature, which is 700~900℃ (preferably 800℃). During this stage, the valve is switched to a half-open state, and cold air enters the airflow channel 6 through the air inlet hole. After being preheated through the stepped channel, it reaches the interior of the furnace chamber 3, promoting kiln cooling. The combustion heating and exhaust functions of the furnace body 1 remain off. The second controllable cooling stage: After the furnace temperature drops to the fourth temperature, it continues to cool down to the fifth temperature, which is 250~400℃ (preferably 300℃). In this stage, the valves are switched to the fully open state, the air inlet valve at the bottom of the furnace door 2 is opened, and the exhaust function of the furnace body 1 is turned on while its combustion heating function is turned off. That is, the exhaust function of the furnace body 1 is turned on but the combustion heating function is not turned on, and the hot air in the furnace is forcibly exhausted. After the valves are fully open, the air enters the airflow channel 6 through the air inlet, is preheated by the airflow channel 6, flows from bottom to top through the furnace chamber 3, and then enters the furnace body 1 through the flue gas outlet 4 and the flue gas pipe, and is discharged by the exhaust function of the furnace body 1. The combination of the entry of hot air from the bottom and the forced exhaust from the top achieves rapid cooling of the kiln.
[0040] Alumina ceramic products sintered in the above manner are free of gray spots, and the overall kiln cooling time is shortened from the original 6 days to 3 days, significantly improving kiln utilization. This invention, through improvements to the kiln structure and the combination of staged atmosphere regulation and cooling methods, simply and easily solves the problem of gray spots during ceramic sintering, while also greatly improving equipment turnover efficiency.
[0041] Many embodiments and applications beyond the examples provided will be apparent to those skilled in the art upon reading the foregoing description. Therefore, the scope of this teaching should not be determined by reference to the foregoing description, but rather by reference to the foregoing claims and the full scope of their equivalents. For purposes of completeness, all articles and references, including patent applications and publications, are incorporated herein by reference. The omission of any aspect of the subject matter disclosed herein in the foregoing claims is not intended as a waiver of that subject matter, nor should it be construed as an indication that the applicant has not considered that subject matter as part of the disclosed inventive subject matter.
[0042] The above content provides a further detailed description of the present invention. It should not be construed that the specific embodiments of the present invention are limited to this. For those skilled in the art, several simple deductions or substitutions can be made without departing from the concept of the present invention, and all such deductions or substitutions should be considered to fall within the scope of protection of the present invention as defined by the submitted claims.
Claims
1. An air-preheated lifting kiln, characterized in that, It includes a furnace body (1) and a liftable furnace door (2) located at the bottom of the furnace body (1). The furnace body (1) has a furnace chamber (3) inside and a flue gas outlet (4) connected to the furnace chamber (3) is provided on the furnace body (1). The lifting furnace door (2) includes a furnace door steel structure and a multi-layer refractory brick layer (5) laid on the furnace door steel structure. The multi-layer refractory brick layer (5) is laid in a vertical direction and adjacent refractory brick layers (5) are staggered in the horizontal direction. The furnace door steel structure is provided with multiple air inlet holes that penetrate the furnace door steel structure, and a valve is installed at each air inlet hole; the refractory brick layer (5) is provided with multiple airflow channels (6), the number of air inlet holes and airflow channels (6) are the same and correspond one-to-one, one end of each airflow channel (6) is an air inlet port (61) and the other end is an air outlet port (62), the air inlet port (61) is connected to the corresponding air inlet hole, and the air outlet port (62) is located on the side surface of the refractory brick layer (5) facing the furnace (3); In the stacking direction of the refractory brick layer (5), the airflow channel (6) extends in a bent shape.
2. The air-preheated lifting kiln according to claim 1, characterized in that, The refractory brick layer (5) includes a first refractory brick layer (51), a second refractory brick layer (52), a third refractory brick layer (53), a fourth refractory brick layer (54) and a fifth refractory brick layer (55) laid sequentially from bottom to top, with adjacent refractory brick layers (5) being staggered and stacked in the horizontal direction.
3. The air-preheated lifting kiln according to claim 2, characterized in that, The airflow channel (6) is formed by connecting the refractory bricks (7) with first through holes (71) and semi-circular grooves (72) in each refractory brick layer (5) layer by layer. The first through hole (71) penetrates the center of the refractory brick (7) along the thickness direction. The semi-circular groove (72) is opened on the upper surface of the refractory brick (7). One end of the semi-circular groove (72) is connected to the first through hole (71), and the other end of the semi-circular groove (72) extends to the side of the refractory brick (7).
4. The air-preheated lifting kiln according to claim 3, characterized in that, The first through hole (71) of the refractory brick (7) in the same layer is connected to the semi-circular groove (72); in the two adjacent layers of refractory bricks (5), the side end of the semi-circular groove (72) of the lower layer of refractory brick (7) is vertically opposite to and connected to the first through hole (71) of the upper layer of refractory brick (7); the opening direction of the semi-circular groove (72) is towards the center side of the furnace (3).
5. The air-preheated lifting kiln according to claim 3, characterized in that, Multiple air inlet holes are staggered on the upper surface of the furnace door steel structure, and the distance between two adjacent air inlet holes is equal to the width of a single refractory brick (7); the refractory brick (7) is laid in the first refractory brick layer (51) at the position corresponding to each air inlet hole, and the first through hole (71) of the refractory brick (7) is coaxially aligned with the corresponding air inlet hole.
6. The air-preheated lifting kiln according to claim 1, characterized in that, The valve is a manual regulating valve or an electric regulating valve, and the valve is installed on the lower surface of the furnace door steel structure and covers the opening of the air inlet hole.
7. A method for atmosphere conditioning and cooling of an air-preheated lifting kiln as described in any one of claims 1 to 6, characterized in that, The air preheating type lifting kiln also includes a flue gas duct, one end of which is connected to the flue gas outlet (4), and the other end of which is connected to the furnace body (1). The method includes the following steps: Degreasing stage: The furnace temperature is raised from room temperature to the first temperature. During this stage, the valve is fully open, and the combustion heating function and exhaust function of the furnace body (1) are turned on at the same time. Medium-temperature sintering stage: When the furnace temperature reaches the first temperature, it continues to rise to the second temperature. During this stage, the combustion heating function and exhaust function of the furnace body (1) are turned off, and the valve is switched to a half-open state. High-temperature sintering stage: After the furnace temperature reaches the second temperature, the temperature continues to rise to the highest sintering temperature and is held. During this stage, the valve is switched to the fully closed state, and the combustion heating function and exhaust function of the furnace body (1) are kept closed. Natural cooling stage: heating is stopped, and the furnace temperature is allowed to drop naturally from the highest sintering temperature to the third temperature. During this stage, the valves are kept fully closed, and the combustion heating function and exhaust function of the furnace body (1) are kept off. First controllable cooling stage: When the furnace temperature drops to the third temperature, it continues to cool down to the fourth temperature. During this stage, the valve is switched to a half-open state, and the combustion heating function and exhaust function of the furnace body (1) are kept closed. Second controllable cooling stage: When the furnace temperature drops to the fourth temperature, continue to cool down to the fifth temperature. In this stage, switch the valve to the fully open state, turn on the exhaust function of the furnace body (1), and turn off its combustion heating function.
8. The method for atmosphere conditioning and cooling of an air-preheated lifting kiln according to claim 7, characterized in that, The first temperature is 700~900℃, the second temperature is 1200~1350℃, the highest sintering temperature is 1550~1650℃, the third temperature is 1100~1250℃, the fourth temperature is 700~900℃, and the fifth temperature is 250~400℃.
9. The method for atmosphere conditioning and cooling of an air-preheated lifting kiln according to claim 7, characterized in that, During the glue removal stage, the exhaust gas generated in the furnace (3) enters the furnace body (1) through the exhaust port (4) and the flue gas pipe, and is discharged after being burned and heated in the furnace body (1).
10. The method for atmosphere conditioning and cooling of an air-preheated lifting kiln according to claim 7, characterized in that, In the second controllable cooling stage, after the valve is fully opened, air enters the airflow channel (6) through the air inlet hole, is preheated by the airflow channel (6), flows from bottom to top through the furnace (3), and then enters the furnace body (1) through the exhaust port (4) and the flue gas pipe, and is discharged by the exhaust function of the furnace body (1).