A method for standardizing and quickly determining the cause of surface scale fold defects of hot-rolled stainless steel

By adopting a standardized process of sample preparation, observation, classification, and judgment, and combining macroscopic morphology, microscopic morphology, and energy dispersive spectroscopy composition detection, the problem of rapid and accurate determination of scaly defects on the surface of hot-rolled stainless steel is solved, improving the standardization and consistency of detection. It is applicable to the detection of stainless steel in the entire process of hot rolling, pickling, and cold rolling.

CN123065841APending Publication Date: 2026-11-10BAOSTEEL DESHENG STAINLESS STEEL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611323105.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies make it difficult to quickly and accurately determine the essential type of surface flaking defects in hot-rolled stainless steel, resulting in unclear directions for process rectification and troubleshooting, and long processing cycles for quality objections.

Method used

A standardized process of sample preparation, observation, typing, and judgment was adopted. Combining macroscopic morphology screening, microscopic morphology typing, and energy dispersive spectroscopy (EDS) micro-area component detection, a unified numerical threshold standard was established to distinguish the three types of defects: central mountain scale, line scale, and stripe scale through dual verification of microscopic morphology and component data.

Benefits of technology

It enables rapid and accurate identification of scale-like defects, reduces reliance on personal experience, improves the consistency and efficiency of testing, clarifies the direction of process rectification, and is applicable to the full-process testing of BN series Cr-Mn-N and 300 series austenitic hot-rolled stainless steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123065841A_ABST
    Figure CN123065841A_ABST
Patent Text Reader

Abstract

The application discloses a kind of standardization fast judging method of hot-rolled stainless steel surface scale fold type defects causes, it can accurately distinguish middle mountain scale, line scale, strip scale three essentially different defects by double verification of micro morphology and composition data, further subdivides two kinds of foreign matter sources of mould flux, refractory, gives clear process investigation priority, provides clear direction for process rectification.The judging method is clear and fixed in sample preparation, observation, typing, determination steps, single sample detection process is controllable, can quickly output standardization detection conclusion, meets the demand of on-site quality objection quick response.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of stainless steel smelting, and in particular to a standardized and rapid method for determining the causes of surface flaking defects in hot-rolled stainless steel. Background Technology

[0002] Scale-like defects (including line scales, mountain scales, edge scales, central mountain scales, and strip scales) are common surface quality defects in the hot-rolled stainless steel production process, directly affecting the surface grade and downstream performance of the product. These defects are often the result of the coupled effects of multiple processes such as heating, pickling, and rolling. They have a high degree of similarity in macroscopic morphology, making it difficult to distinguish their underlying causes by visual inspection alone.

[0003] Currently, there are two main methods for determining this type of defect on-site: manual visual inspection and inspection using scanning electron microscopy (SEM) and energy dispersive spectroscopy (EDS). Manual visual inspection can only distinguish macroscopic morphology and cannot accurately identify the essential type of defect. Inspection using SEM involves personnel observing the morphology under an SEM and then selecting points in the defect area based on their personal experience to perform EDS analysis. Based on the peaks in the EDS spectrum, they determine whether a certain element is present (e.g., the presence of O, Mg, Al, Si, Ca, F, etc.). This method relies entirely on the subjective judgment of the inspector, combining morphology and element peaks, without a unified numerical threshold. For example, a high O peak might classify it as an oxidation defect, while the presence of Mg / Ca / F peaks might classify it as a foreign matter defect. However, there is no unified quantitative standard for determining "what content constitutes enrichment and a certain type of defect," leading to significant differences in judgment criteria among different personnel.

[0004] Given that existing methods are insufficient for quickly and accurately identifying scale-like defects, resulting in unclear directions for process rectification and troubleshooting, and long processing cycles for quality disputes, there is an urgent need to develop a standardized testing method that can quickly identify the essential type of scale-like defects and accurately investigate their core causes. This method would have significant engineering application value in improving production line quality testing efficiency and shortening the response cycle for quality issues. Summary of the Invention

[0005] The purpose of this invention is to provide a standardized and rapid method for determining the causes of surface flaking defects in hot-rolled stainless steel.

[0006] The technical solution to achieve the objective of this invention is: a standardized and rapid method for determining the causes of scaling defects on the surface of hot-rolled stainless steel, comprising the following steps: 1) Sample preparation: Cut a sample containing the target defect. Clean the regular and flat sample to obtain the test sample. For the sample with irregular peeling or uneven defects, directional embedding and fixation are performed. Only the edge of the sample is subjected to gradient grinding treatment so that the core area of ​​the defect avoids contact with the abrasive to obtain the test sample. 2) Initial screening of macroscopic morphology: Visual observation or observation using microscopic morphology observation equipment to confirm defect distribution, rolling direction extension characteristics, and core abnormal areas. Macroscopic morphology classification is performed by comparing the morphological characteristics of central mountain scales, line scales, and strip scales, and macroscopic micro-area detection points are marked in the areas where macroscopic morphology classification has been performed. Among them, central mountain scales are wide strip-shaped morphology extending along the rolling direction, with a large and continuous defect band, a rough and uneven surface, and a clear transition boundary with the surrounding flat substrate, showing a typical "mountain-shaped" peeling / protrusion morphology; line scales extend along the rolling direction as narrow / discontinuous thin lines, with narrow defect width, mostly discontinuous distribution, some accompanied by slight edge curling, a delicate overall morphology, and a sharp boundary with the substrate; strip scales are uniformly distributed as strips along the rolling direction, with a width between central mountain scales and line scales, a relatively flat surface, no obvious unevenness or peeling, a dark gray tone that forms a color difference with the substrate, and straight boundaries; 3) Microscopic Morphology Classification: The macroscopic micro-area detection points marked in step 2) are magnified step by step, and the microstructure of the test sample within these macroscopic micro-area detection points is observed. The microscopic morphology characteristics of the central mountain scale, line scale, and strip scale are compared to further perform microscopic morphology classification, and microscopic micro-area detection points are marked in the areas where microscopic morphology classification has been performed. Among them, the defect area of ​​the central mountain scale exhibits large-area intergranular cracking characteristics, with extensive development and interconnection of microcracks at the grain boundaries, and a large number of grains discontinuously detaching along the grain boundaries to form irregular concave areas. The pits and rough surfaces show no obvious heterogeneous clusters or layered oxides, and the damage is mainly due to the deformation and detachment of matrix grains. In the defects of the linear scales, chain-like and clustered heterogeneous fillers can be seen in the gaps / depressions, distributed along the defect direction. The interface between the heterogeneous area and the matrix is ​​clear, and the surrounding matrix is ​​accompanied by local grain deformation and micro-detachment traces. The defect area of ​​the strip scales is a dense lamellar / granular oxide structure with a smooth surface, no intergranular cracks or grain detachment pits, and the interface between the oxide layer and the matrix is ​​straight. The overall shape is a continuous film / strip with an indentation. 4) Micro-area composition detection using energy dispersive spectroscopy: The elemental composition, content and distribution characteristics within the micro-area detection sites in step 3) are obtained by using a combination of energy dispersive spectroscopy semi-quantitative point scanning and elemental surface scanning. 5) Combining the micro-morphology classification results from step 3) with the micro-area composition detection results from step 4) and the composition threshold standards, determine the essential type of the defect and provide the corresponding direction for investigation and tracing of the production line process; when there is a conflict between morphology and composition detection, the composition detection results shall prevail. Among them, when the main detected elements are Fe, Cr and Mn, the total mass fraction of foreign characteristic elements is generally less than 1.0%, and the oxygen element signal mass fraction is less than 6% with no obvious enrichment, it is judged as a defect in the central mountain scale. When O, Mg, Al, Si, Ca, and F are detected, and the total mass fraction of foreign characteristic elements Mg, Al, Si, Ca, and F is ≥25%, the determination threshold is that the main elements in the matrix region are Fe and Cr, and the defect is determined to be a linear scale defect. When the main elements are Fe, Cr, and O, and the oxygen mass fraction is about 24%, and no foreign characteristic elements such as Mg, Al, Ca, and F are detected, it belongs to a relatively thick secondary iron oxide scale layer, which still meets the judgment threshold of oxygen mass fraction > 6%. The oxygen content of iron oxide scale of different thicknesses is usually distributed in the range of 6% to 30%, which is judged as a stripe scale defect.

[0007] Furthermore, the directional embedding fixation in step 1) is performed by epoxy resin cold embedding directional fixation.

[0008] Furthermore, the microscopic morphology observation device mentioned in step 2) is a scanning electron microscope, and the magnification of the scanning electron microscope is limited to the extent that it can completely encompass the entire defect area.

[0009] Furthermore, in step 3), a field emission scanning electron microscope is used to observe the microstructure of the sample to be tested within the macroscopic micro-area detection point.

[0010] Furthermore, if step 5) determines that the sample defect is a central mountain scale defect, the investigation direction is the hot rolling process matching process, the heating furnace grain boundary oxidation process, or the pickling surface corrosion process.

[0011] Furthermore, in step 5), if the sample defect is determined to be a linear scale defect and F element is detected, the investigation direction is continuous casting protective slag entrapment. If the sample defect is determined to be a linear scale defect and does not contain F element, the investigation direction is heating furnace refractory material or foreign object falling from the roller conveyor.

[0012] Furthermore, if step 5) determines that the sample defect is a stripe scale defect, the investigation direction is the oxidation control of the heating furnace and the descaling process of rough rolling.

[0013] Compared with the prior art, the present invention has the following beneficial effects: (1) High degree of standardization and reduced reliance on experience: A complete standardized process of “sample preparation-observation-classification-judgment” has been established. Inspection personnel can complete the identification of defect types by following the process, get rid of reliance on personal experience, and significantly improve the consistency of inspection by different personnel.

[0014] (2) High accuracy in identification and strong targeting in investigation: The macroscopic morphology screening, microscopic morphology classification, and composition threshold are all empirical standardized judgment conditions based on a large amount of on-site sample data from the production line. Through the dual verification of microscopic morphology and composition data, the three types of defects with different essential characteristics, namely, mountain scale, line scale, and strip scale, can be accurately distinguished, providing a clear direction for process rectification. Among them, the microscopic observation in the microscopic morphology classification step is to accurately lock the typical characteristic area of ​​the defect (such as the center of heterogeneous clusters, dense layer of iron oxide scale, and grain shedding section) within the macroscopic range, ensuring that the energy dispersive spectrometer data directly hits the essence of the defect and ensures accurate composition judgment. For samples with extremely typical morphological characteristics (such as clear intergranular grain shedding and typical cracked iron oxide scale), the classification can be roughly completed through microscopic observation. The composition detection step only requires a small number of point verifications and does not require large-area blind testing. If microscopic observation is skipped and composition detection is relied upon, all samples need to be confirmed by a large number of points, and the overall detection time will be longer.

[0015] (3) The testing process is standardized and efficient: the steps of sample preparation, observation, classification and judgment are clear and fixed, the single sample testing process is controllable, and standardized test conclusions can be output quickly to meet the needs of rapid response to on-site quality objections.

[0016] (4) Applicable scenarios are in line with on-site production: This method is developed for the scale-like defects of BN series Cr-Mn-N and 300 series austenitic hot-rolled stainless steel, covering samples of all processes of hot rolling, pickling and cold rolling, and can be directly incorporated into the standardized testing specifications of the laboratory. Attached Figure Description

[0017] Figure 1 This is a 47x SEM image of the central mountain scale defect described in Embodiment 1 of the present invention; Figure 2 This is a 500x SEM image of the central mountain scale defect described in Embodiment 1 of the present invention; Figure 3 This is a 200x SEM image of the linear scale defect described in Embodiment 2 of the present invention; Figure 4 This is a 1000x EDS elemental surface scan distribution map of the line scale defect described in Embodiment 2 of the present invention; Figure 5 The distribution of O element enrichment in the SEM morphology of foreign object embedded defects at 1000x magnification; Figure 6 The SEM image shows the Fe enrichment distribution of foreign object embedded defects at 1000x magnification. Figure 7 The SEM morphology of foreign object embedded defects at 1000x magnification shows the enrichment and distribution of Ca elements. Figure 8The Si element enrichment distribution in the SEM morphology of foreign object embedded defects at 1000x magnification; Figure 9 The SEM image shows the Cr enrichment distribution of foreign object embedded defects at 1000x magnification. Figure 10 The SEM morphology of foreign object embedded defects at 1000x magnification shows the enrichment distribution of element F. Figure 11 The SEM morphology of foreign object embedded defects at 1000x magnification shows the enrichment and distribution of Al elements. Figure 12 The SEM image shows the enrichment and distribution of Mg in foreign matter embedded defects at 1000x magnification. Figure 13 This is a 200x SEM image of the stripe scale defect described in Embodiment 3 of the present invention; Figure 14 This is the energy spectrum detection correspondence diagram of Example 1, where... Figure 14-1 For detecting point spectrum Figure 4 SEM morphology image; Figure 14-2 For detecting point spectrum Figure 4 The corresponding EDS spectrum; Figure 14-3 For detecting point spectrum Figure 9 SEM morphology image; Figure 14-4 For detecting point spectrum Figure 9 The corresponding EDS spectrum; Figure 15 The energy spectrum detection correspondence diagram for Example 2 is shown below. Figure 15-1 SEM topography of the detection points; Figure 15-2 For detecting point spectrum Figure 14 EDS energy spectrum corresponding to the location; Figure 15-3 For detecting point spectrum Figure 15 EDS energy spectrum corresponding to the location; Figure 15-4 For detecting point spectrum Figure 16 EDS energy spectrum; Figure 16 This is the energy spectrum detection correspondence diagram for Example 3, where... Figure 16-1 SEM topography of the detection points; Figure 16-2 For detecting point spectrum Figure 15 EDS energy spectrum corresponding to the location; Figure 16-3 For detecting point spectrum Figure 16 EDS energy spectrum corresponding to the location; Figure 16-4 For detecting point spectrum Figure 18 EDS energy spectrum; Figure 17 This is a 200x SEM image of the line scale defect described in Embodiment 4 of the present invention; Figure 18This is a 1000x SEM image of the line scale defect described in Embodiment 4 of the present invention; Figure 19 This is the energy spectrum detection correspondence diagram for Example 4, where... Figure 19-1 To obtain the SEM topography of the detection points, Figure 19-2 For the score Figure 1 The corresponding EDS spectrum of the point; where Figure 19-3 For the score Figure 2 The corresponding EDS spectrum of the point; where Figure 19-4 For detecting point spectrum Figure 4 The EDS energy spectrum. Detailed Implementation

[0018] The preferred embodiments of the present invention will be described in detail below. Example 1

[0019] This embodiment uses BN1D4 cold-rolled white coils with scaly or folded defects as the inspection object, and employs the method of this invention for detection and judgment. The specific steps are as follows: 1) Sample preparation: A 10mm×10mm sample was cut from the defect roll, with the defect located at the center of the sample; since the defect is relatively flat, it was directly observed under an electron microscope after being cleaned with alcohol and ultrasonically.

[0020] 2) Initial screening of macroscopic morphology: The test samples obtained in step 1) are observed under low magnification using a scanning electron microscope to confirm the defect distribution, rolling direction extension characteristics, and core abnormal areas. Macroscopic morphology classification is performed by comparing the morphological characteristics of the central mountain scale, line scale, and strip scale, and macroscopic micro-area detection points are marked within the macroscopic morphology classification areas; the morphology at 47x magnification is as follows... Figure 1 As shown, the defects exhibit a wide, strip-shaped, mountain-scale morphology extending along the rolling direction. The defect bands are wide and continuously distributed, with a rough and uneven surface. There is a clear transition boundary between the defect bands and the surrounding flat matrix area, which allows for a direct visual identification of the overall distribution range of the defects and the core abnormal area. Further observation at 100x magnification reveals a large area of ​​uneven morphology within the defect bands, widespread grain spalling marks, a clear boundary between the defect bands and the normal matrix, and a complete grain outline and relatively flat surface in the matrix area. The macroscopic morphology conforms to the characteristics of the mountain-scale morphology in the central part of the matrix. 3) Microscopic morphology classification was performed using field emission scanning electron microscopy: The macroscopic micro-area detection points marked in step 2) were magnified step by step, and the microstructure of the test sample within these macroscopic micro-area detection points was observed. The microscopic morphology was further classified by comparing it with the microscopic morphology characteristics of the central mountain scale, line scale, and strip scale. Microscopic micro-area detection points were marked within the areas where microscopic morphology classification was performed. At 200x magnification, typical large-area intergranular cracking characteristics were observed within the defect zone. Microcracks were widely developed at grain boundaries and interconnected. A large number of grains discontinuously detached along the grain boundaries, forming a continuous rough, uneven surface. The grain outlines of the normal matrix regions on both sides of the defect zone were complete, and the boundaries with the defect region were clearly distinguishable. At 500x magnification, the morphology was observed as follows... Figure 2 As shown: in the defect area, the grain boundaries are fully exposed, and microcracks preferentially initiate at the grain boundary and penetrate each other; local grains peel off along the grain boundaries, forming dense irregular pits, and the overall surface has a porous and rough morphology; in the intact matrix area, the grain boundaries are clear and the surface is relatively flat; the micromorphology is consistent with the characteristics of the central mountain scale morphology. 4) Micro-area composition detection using energy dispersive spectroscopy: A semi-quantitative point scanning combined with elemental surface scanning method was used to detect three points in the core defect region, obtaining the elemental composition, content, and distribution characteristics of the defect region; the detection results are as follows: Figure 14 As shown in Table 1; Table 1. Microstructural regions of the detection points in the micro-area, measured at the locations, and the components measured by energy dispersive spectroscopy.

[0021] Depend on Figure 14 As shown in Table 1, for the three points (spectral density) in the core defect region Figure 14 Spectrum Figure 9 The main elements detected were Fe, Cr, and Mn. The oxygen element signal was below the detection limit and there was no obvious enrichment. No foreign characteristic elements such as Mg, Al, Si, Ca, and F were detected, which meets the threshold requirements for the determination of scale insects in central mountainous areas.

[0022] 5) Combining the micro-morphology classification results from step 3) with the micro-area composition detection results and composition threshold standards from step 4), determine the essential type of the defect and provide the corresponding investigation and tracing direction for the production line process: Combining morphological characteristics (large-area intergranular cracking, grain shedding to form a continuous rough and uneven surface) and compositional data (containing only matrix elements, low oxygen content, and no enrichment of foreign characteristic elements), it meets the criteria for judging the central mountain scale defect. The final damage of this type of defect is formed during the rolling deformation process. The main investigation direction is the tension matching between hot rolling mill stands and the roll gap control. At the same time, it is necessary to combine the heating system of the heating furnace and the pickling process to investigate the pre-grain boundary weakening causes.

[0023] Example 2 This embodiment uses BN1D4 cold-rolled white coils with flaking defects as the inspection object, and employs the method of the present invention for detection and judgment: 1) Sample preparation: Cut a 10mm×10mm sample with smooth defects, clean it directly with alcohol and then test it.

[0024] 2) Initial screening of macroscopic morphology: The test sample obtained in step 1) was observed in low magnification mode of scanning electron microscope to confirm the defect distribution, rolling direction extension characteristics and core abnormal area. The macroscopic morphology was classified by comparing the morphological characteristics of the central mountain scale, line scale and strip scale, and the macroscopic micro-area detection points were marked in the area where the macroscopic morphology was classified. Among them, the morphology of 74x low magnification electron microscope showed that the defect was a continuous narrow strip line scale morphology extending along the rolling direction, and the whole was continuously distributed. The surface of the defect area was rough and uneven, showing a fine and uneven morphology, and there was a relatively clear morphological transition boundary with the surrounding normal matrix area. The macroscopic morphology is consistent with the morphological characteristics of line scale.

[0025] 3) Microscopic morphology classification using field emission scanning electron microscopy: The macroscopic micro-area detection points marked in step 2) are magnified step by step, and the microstructure of the test sample within these points is observed. Microscopic morphology classification is further performed by comparing the microscopic morphology characteristics of the central mountain scale, line scale, and stripe scale, and microscopic micro-area detection points are marked within the areas where microscopic morphology classification has been performed; the morphology at 200x magnification is as follows... Figure 3 As shown: The defect zone exhibits typical intergranular separation characteristics, with fine pits and traces of grain detachment in micro-regions. The surface is rough and uneven, with locally visible clusters of heterogeneous material, and a clear interface with the matrix. At 500x magnification, extensive microcracks are observed at the grain boundaries within the defect zone, with some grains discontinuously detaching along the grain boundaries, forming irregular pit-like morphologies. The heterogeneous cluster regions exhibit a loose and porous morphology, significantly different from the matrix grain morphology. At 1000x magnification, the morphology is as follows... Figures 4-12 As shown, the grain boundaries in the defect region are fully exposed, and microcracks preferentially initiate and interconnect at the grain boundary locations. The interior of the heterogeneous cluster exhibits the characteristics of glassy fine particle aggregation; the micromorphology conforms to the characteristics of line scale defects. 4) Micro-area composition detection using energy dispersive spectroscopy: A semi-quantitative point scanning combined with elemental surface scanning method was used to detect three points in the core defect region, obtaining the elemental composition, content, and distribution characteristics of the defect region; the detection results are as follows: Figure 15 As shown in Table 2; Table 2. Microstructural regions of the detection points in the micro-area, measured at the locations, and the components measured by energy dispersive spectroscopy.

[0026] Depend on Figure 15 As shown in Table 2, three points (spectral density) in the central region of the defective heterogeneous clusters Figure 14-16O, Mg, Al, Si, Ca, and F were detected. The total mass fraction of foreign characteristic elements Mg, Al, Si, Ca, and F was about 30%, which is ≥25%, meeting the threshold requirements for line scale determination. The main elements in the matrix region were Fe and Cr.

[0027] Surface scan analysis: such as Figure 5-12 The defect region shown exhibits a clear enrichment distribution of O, Mg, Al, Si, Ca, and F elements, which corresponds perfectly to the defect location.

[0028] 5) Combining the microscopic morphology classification results from step 3) with the micro-area composition detection results and composition threshold standards from step 4), determine the essential type of the defect and provide the corresponding investigation and tracing direction for the production line process: Combining morphological characteristics (clustered heterogeneous substances exist in the defect area, with a clear interface with the matrix) and composition data (multi-element synergistic enrichment of O, F, Mg, Al, Si, and Ca, with the total mass fraction of characteristic elements meeting the judgment threshold), it meets the judgment standard for foreign matter embedding. This defect is caused by the mold flux from the continuous casting stage being rolled into the surface of the billet, and then pressed and extended during the subsequent rolling process to form a linear scale morphology. The main tracing direction is the fluctuation of the liquid level in the continuous casting mold and the control of mold flux slag entrainment.

[0029] Example 3 This embodiment uses 304 cold-rolled white steel coils with flaking or scaly defects as the inspection object, and employs the method of this invention for detection and judgment: 1) Sample preparation: Cut a 10mm×10mm sample, clean it with alcohol and then observe it directly under an electron microscope.

[0030] 2) Initial screening of macroscopic morphology: The test sample obtained in step 1) is observed under the 50x low magnification mode of a scanning electron microscope to confirm the defect distribution, rolling direction extension characteristics and core abnormal area. The macroscopic morphology is classified by comparing the morphological characteristics of the central mountain scale, line scale and strip scale, and the macroscopic micro-area detection points are marked in the area where the macroscopic morphology has been classified. At this magnification, the defect appears as a dark gray strip extending along the rolling direction, the surface is relatively flat without obvious peeling, and the boundary with the normal matrix area is clearly distinguishable.

[0031] 3) Microscopic morphology classification using field emission scanning electron microscopy: The macroscopic micro-area detection points marked in step 2) are magnified step by step, and the microstructure of the test sample within these macroscopic micro-area detection points is observed. Microscopic morphology classification is further performed by comparing the microscopic morphology characteristics of the central mountain scale, line scale, and stripe scale, and microscopic micro-area detection points are marked within the areas where microscopic morphology classification has been performed; the morphology observed at 200x magnification is as follows... Figure 13As shown: the defect is a dense lamellar structure extending along the surface of the matrix, with a flat and regular interface, and no large-area intergranular cracking or grain shedding; at 500x magnification: the defect area is an aggregate of fine oxide particles with a dense structure that is tightly bonded to the matrix. There are fine cracks at the interface, but no heterogeneous clusters or porous morphology.

[0032] 4) Micro-area composition detection using energy dispersive spectroscopy: A semi-quantitative point scanning combined with elemental surface scanning method was used to detect three points in the core defect region, obtaining the elemental composition, content, and distribution characteristics of the defect region; the detection results are as follows: Figure 16 As shown in Table 3: Table 3. Microstructural regions of the detection points, measurement locations, and components measured by energy dispersive spectroscopy.

[0033] Depend on Figure 16 As shown in Table 3, the three points in the core defect region (spectral density) Figure 15-18 The test results showed that the main elements were Fe, Cr, and O, with an oxygen mass fraction of about 24%. No foreign characteristic elements such as Mg, Al, Ca, and F were detected. It belongs to a relatively thick secondary iron oxide scale layer, which still meets the judgment threshold of oxygen mass fraction > 6%. The oxygen content of iron oxide scale of different thicknesses is usually distributed in the range of 6% to 30%, which all meet the judgment rule.

[0034] 5) Combining the microscopic morphology classification results from step 3) with the micro-area composition detection results and composition threshold standards from step 4), determine the essential type of the defect and provide the corresponding investigation and tracing direction for the production line process: Based on the lamellar indentation morphology and the compositional characteristics dominated by Fe-Cr-O, it meets the criteria for scale defects. This defect is caused by incomplete descaling of secondary iron oxide scale generated in the heating furnace, which is then indented into the substrate surface during the rolling process. The main tracing direction is the control of the heating atmosphere in the heating furnace and the efficiency of the rough rolling descaling process.

[0035] Example 4 This embodiment uses a 439 hot-rolled stainless steel black coil with surface stripe defects as the test object, and uses the method of the present invention for detection and classification to verify the judgment rules when the morphology and conclusion conflict.

[0036] 1) Sample preparation: A 10mm×10mm sample was cut from the defect roll. The defect was located in the center of the sample. The sample was gently cleaned with alcohol and ultrasonically, preserving the original surface defect morphology. After cleaning, the sample was directly observed under an electron microscope.

[0037] 2) Initial screening of macroscopic morphology: Macroscopic morphology classification was performed by visual observation and comparison with the morphological characteristics of the central mountain scale, line scale and strip scale, and macroscopic micro-area detection points were marked in the area where macroscopic morphology classification was performed; According to visual observation, the defect is a wide strip extending along the rolling direction, with a rough and uneven surface, accompanied by local scaly uplift, and a clear boundary with the surrounding black skin matrix; Based on the macroscopic morphology alone, it is highly similar to the appearance characteristics of the iron oxide scale pressed into the strip scale, and the initial judgment is prone to deviation based on low magnification morphology alone.

[0038] 3) Microscopic morphology classification using field emission scanning electron microscopy: The macroscopic micro-area detection points marked in step 2) are magnified step by step, and the microstructure of the test sample within these points is observed. The microscopic morphology is further classified by comparing it with the microscopic morphology characteristics of the central mountain scale, line scale, and stripe scale. Microscopic micro-area detection points are marked within the areas where microscopic morphology classification has been performed. The morphology of the defect area at 200x magnification is shown below. Figure 17 As shown, the defect surface is generally rough, with a granular accumulation pattern and obvious undulations. It has a high degree of similarity to the typical surface morphology of iron oxide scale indentation defects. Based solely on the morphological characteristics at this magnification, it is easy to preliminarily classify it as iron oxide scale indentation type stripe scale.

[0039] The magnified morphology of the defect core region at 1000x magnification is as follows: Figure 18 As shown, high-magnification observation reveals that the interior of the defect is filled with clustered, unevenly sized particles, which still have a high degree of similarity to the particle aggregation morphology of thick iron oxide scale. It is impossible to clearly distinguish whether it is the iron oxide scale itself or foreign foreign inclusions based solely on microscopic morphological characteristics, making it difficult to achieve accurate classification.

[0040] 4) Micro-area composition detection using energy dispersive spectroscopy: A semi-quantitative point scanning combined with elemental surface scanning method was used to detect three points in the core defect region, obtaining the elemental composition, content, and distribution characteristics of the defect region; the detection results are as follows: Figure 19 As shown in Table 4: Table 4. Microstructural regions of the detection points, measurement locations, and components measured by energy dispersive spectroscopy.

[0041] Depend on Figure 19 As shown in Table 4, the elements detected in the defect area mainly include O, Mg, Al, Si, Ca, and F, with a small amount of Ti and Zr as associated elements (not included in the statistics for the determination of foreign characteristic elements); the total mass fractions of foreign characteristic elements Mg, Al, Si, Ca, and F at the three sites are approximately 28%, 44%, and 53%, respectively. The composition of heterogeneous clusters at different locations of the defect varies to some extent, but all meet the threshold of ≥25% for the determination of foreign matter embedded defects; the main elements in the matrix control area are Fe and Cr, and the total mass fraction of foreign characteristic elements is less than 1%.

[0042] 5) Combining the microscopic morphology classification results from step 3) with the micro-area composition detection results and composition threshold standards from step 4), the essential type of the defect is determined, and the corresponding direction for investigation and tracing of the production line process is given: In this embodiment, the macroscopic appearance and low-magnification microscopic morphology of the defect are highly similar to the iron oxide scale indentation type, and misjudgment is easily made based solely on morphological observation; however, the EDS composition detection results meet the judgment criteria for foreign object embedded type defects. According to the judgment rule of this invention, when the morphological characteristics and composition detection results are inconsistent, the EDS micro-area composition detection results are used as the final classification basis, and the defect is finally determined to be a foreign object embedded type scale defect, verifying the accuracy and necessity of the "composition priority" judgment rule of this method.

[0043] Comparison of empirical tests without standardized rules Twenty groups of samples with known origins of scale-like defects, covering three categories—grain detachment and peeling type, foreign object embedding type, and iron oxide scale indentation type—were selected and examined by two personnel with more than five years of experience in electron microscopy. (1) Conventional empirical testing: Self-observation of SEM morphology and qualitative judgment of energy spectrum composition. There is no unified classification standard and composition threshold. The results of the two people's judgments overlap by about 70%. The main confusion is between iron oxide scale indentation and foreign object embedding defects. The testing process and output conclusion form are quite different. (2) The standardized method of this invention: the judgment is made strictly in accordance with the unified morphology classification standard and composition threshold rules. The overlap of the judgment results of two people is more than 95%, there is no misjudgment across major categories, and all results can be reproduced and traced through SEM morphology map and EDS energy spectrum map. The detection stability and consistency between personnel are significantly improved.

[0044] In step 2) of the initial screening of macroscopic morphology, the "low-magnification mode" is mainly used to fully observe the overall distribution of defects, the direction of rolling extension, and the marking of abnormal areas. This mode is generally tens to 100 times magnification. The operator can flexibly select the mode based on the size of the defects on the sample, as long as it can completely encompass the entire defect area; there is no fixed single-magnification limit. Step 3) Microscopic morphology classification using a field emission scanning electron microscope employs a progressive magnification mode. First, a low-magnification field of view is established, and then the magnification is gradually increased. The main classification observation range is 200-800 times; for local fine features (such as grain detachment, peeling, etc.), further magnification to 1000-1500 times can be used for observation.

[0045] The above are the core characteristics for judging each type of defect. Meeting the core characteristics is sufficient to complete the initial morphological judgment. The details described in the examples are the complete representation of typical samples. Actual defects may present some differences in detail due to the degree of development and the sampling location, but this does not affect the classification.

[0046] The microstructure grading standard and composition determination threshold described in this invention are based on the statistical analysis of 57 samples of scale-like defects verified through process traceability in the production site. All samples cover mainstream stainless steel grades such as BN1D4, 304, 430, 439, and 443, and include various typical process states such as hot-rolled black skin, pickled white skin, and cold-rolled white skin. Furthermore, the final defect type of each sample has been confirmed through subsequent production process verification and defect traceability, demonstrating sufficient representativeness of the field.

[0047] By statistically analyzing the distribution of oxygen mass fraction and total mass fraction of foreign characteristic elements in the full sample, the results show that the core component indicators of the three types of defects exhibit significant interval differentiation characteristics: 1. The oxygen content in the central mountain scale (grain peeling and flaking type) defects is generally less than 5%, and the total mass fraction of foreign characteristic elements is generally less than 1.0%. 2. The total mass fraction of foreign characteristic elements Mg, Al, Si, Ca, and F in linear scale (foreign object embedded type) defects is higher than 25%, which is significantly different in magnitude from the previous two types of defects. 3. The oxygen mass fraction of streak (iron oxide scale indentation) defects is concentrated in the range of 6% to 30%, and the total mass fraction of foreign characteristic elements is generally less than 2.0%; Based on the above statistical distribution patterns, this invention selects an oxygen mass fraction of 6% and a total mass fraction of foreign characteristic elements of 25% as the classification threshold. Verification through full-sample backtesting shows that this threshold system achieves an accuracy rate of over 95% in classifying the three types of defects, demonstrating standardized judgment value for engineering applications. Specific sample statistics are shown in the table below:

[0048] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent process transformations made using the content of the present invention specification, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.

Claims

1. A standardized and rapid method for determining the causes of scaling defects on the surface of hot-rolled stainless steel, characterized in that: It includes the following steps: 1) Sample preparation: Cut a sample containing the target defect. Clean the regular and flat sample to obtain the test sample. For the sample with irregular peeling or uneven defects, directional embedding and fixation are performed. Only the edge of the sample is subjected to gradient grinding treatment so that the core area of ​​the defect avoids contact with the abrasive to obtain the test sample. 2) Initial screening of macroscopic morphology: Visual observation or observation using microscopic morphology observation equipment to confirm defect distribution, rolling direction extension characteristics, and core abnormal areas. Macroscopic morphology classification is performed by comparing the morphological characteristics of central mountain scales, line scales, and strip scales, and macroscopic micro-area detection points are marked in the areas where macroscopic morphology classification has been performed. Among them, central mountain scales are wide strip-shaped morphology extending along the rolling direction, with a large and continuous defect band, a rough and uneven surface, and a clear transition boundary with the surrounding flat substrate, showing a typical "mountain-shaped" peeling / protrusion morphology; line scales extend along the rolling direction as narrow / discontinuous thin lines, with narrow defect width, mostly discontinuous distribution, some accompanied by slight edge curling, a delicate overall morphology, and a sharp boundary with the substrate; strip scales are uniformly distributed as strips along the rolling direction, with a width between central mountain scales and line scales, a relatively flat surface, no obvious unevenness or peeling, a dark gray tone that forms a color difference with the substrate, and straight boundaries; 3) Microscopic Morphology Classification: The macroscopic micro-area detection points marked in step 2) are magnified step by step, and the microstructure of the test sample within these macroscopic micro-area detection points is observed. The microscopic morphology characteristics of the central mountain scale, line scale, and strip scale are compared to further perform microscopic morphology classification, and microscopic micro-area detection points are marked in the areas where microscopic morphology classification has been performed. Among them, the defect area of ​​the central mountain scale exhibits large-area intergranular cracking characteristics, with extensive development and interconnection of microcracks at the grain boundaries, and a large number of grains discontinuously detaching along the grain boundaries to form irregular concave areas. The pits and rough surfaces show no obvious heterogeneous clusters or layered oxides, and the damage is mainly due to the deformation and detachment of matrix grains. In the defects of the linear scales, chain-like and clustered heterogeneous fillers can be seen in the gaps / depressions, distributed along the defect direction. The interface between the heterogeneous area and the matrix is ​​clear, and the surrounding matrix is ​​accompanied by local grain deformation and micro-detachment traces. The defect area of ​​the strip scales is a dense lamellar / granular oxide structure with a smooth surface, no intergranular cracks or grain detachment pits, and the interface between the oxide layer and the matrix is ​​straight. The overall shape is a continuous film / strip with an indentation. 4) Micro-area composition detection using energy dispersive spectroscopy: The elemental composition, content and distribution characteristics within the micro-area detection sites in step 3) are obtained by using a combination of energy dispersive spectroscopy semi-quantitative point scanning and elemental surface scanning. 5) Combining the micromorphological classification results from step 3) with the micro-area composition detection results from step 4) and the composition threshold standards, determine the essential type of the defect and provide the corresponding direction for investigation and tracing of the production line process; when there is a conflict between the morphological and composition detection results, the composition detection results shall prevail. Among them, when the main detected elements are Fe, Cr and Mn, the total mass fraction of foreign characteristic elements is generally less than 1.0%, and the oxygen element signal mass fraction is less than 6% with no obvious enrichment, it is judged as a defect in the central mountain scale. When O, Mg, Al, Si, Ca, and F are detected, and the total mass fraction of foreign characteristic elements Mg, Al, Si, Ca, and F is ≥25%, the determination threshold is that the main elements in the matrix region are Fe and Cr, and the defect is determined to be a linear scale defect. When the main elements are Fe, Cr, and O, and the oxygen mass fraction is about 24%, and no foreign characteristic elements such as Mg, Al, Ca, and F are detected, it belongs to a relatively thick secondary iron oxide scale layer, which still meets the judgment threshold of oxygen mass fraction > 6%. The oxygen content of iron oxide scale of different thicknesses is usually distributed in the range of 6% to 30%, which is judged as a stripe scale defect.

2. The standardized rapid determination method for the causes of surface scaling defects in hot-rolled stainless steel according to claim 1, characterized in that: The directional embedding fixation in step 1) is achieved by using epoxy resin cold embedding for directional fixation.

3. The standardized rapid determination method for the causes of scaling and flaking defects on the surface of hot-rolled stainless steel according to claim 1, characterized in that: The microscopic morphology observation device mentioned in step 2) is a scanning electron microscope (SEM), and the magnification of the SEM is limited to the extent that it can completely encompass the entire defect area.

4. The standardized rapid determination method for the causes of surface scaling defects in hot-rolled stainless steel according to claim 1, characterized in that: Step 3) involves using a field emission scanning electron microscope to observe the microstructure of the sample to be tested within the macro-micro area detection point.

5. The standardized rapid determination method for the causes of surface scaling defects in hot-rolled stainless steel according to claim 1, characterized in that: If step 5) determines that the sample defect is a central mountain scale defect, the investigation direction is the hot rolling process matching process, the heating furnace grain boundary oxidation process, or the pickling surface corrosion process.

6. The standardized rapid determination method for the causes of surface scaling defects in hot-rolled stainless steel according to claim 1, characterized in that: In step 5), if the sample defect is determined to be a linear scale defect and F element is detected, the investigation direction is continuous casting protective slag entrapment. If the sample defect is determined to be a linear scale defect and does not contain F element, the investigation direction is heating furnace refractory material or foreign object falling from the roller conveyor.

7. The standardized rapid determination method for the causes of surface scaling defects in hot-rolled stainless steel according to claim 1, characterized in that: If step 5) determines that the sample defect is a stripe scale defect, the investigation direction is the oxidation control of the heating furnace and the descaling process of rough rolling.