Preparation method of ultraviolet transmission blazed grating master
By using flexible imprint templates and staged reactive ion etching, the problem of limited groove shape in ultraviolet transmission blazed grating master templates was solved, enabling flexible adjustment of groove shape parameters and improving the flexibility and controllability of grating master template fabrication.
Patent Information
- Application Number
- CN202611569777.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-10
AI Technical Summary
In the existing process of preparing ultraviolet transmission blazed grating master, when using the original blazed grating master for nanoimprint replication, the resulting grating groove shape is limited by the existing groove shape of the original blazed grating master, and it is difficult to adjust the aspect ratio, groove depth, blaze angle and anti-blaze angle separately, making it difficult to obtain grating master with different groove parameters.
The method employs a flexible imprint template and a staged reactive ion etching process. First, the aspect ratio and trench depth of the photomask are adjusted by O2 reactive ion etching. Then, the blaze angle and anti-blaze angle are adjusted on the silicon substrate using an etching gas system containing CHF3, SF6, Ar and O2, and the trench shape parameters are adjusted in stages.
This invention enables flexible adjustment of the groove shape parameters of the ultraviolet transmission blazed grating master while keeping the original master unchanged, reducing dependence on the original master and improving the flexibility and controllability of groove shape adjustment.
Smart Images

Figure CN123066904A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of diffraction grating manufacturing technology, specifically to a method for preparing an ultraviolet transmission blazed grating master. Background Technology
[0002] Diffraction gratings are crucial dispersive elements in spectral analysis, spectral imaging, and related optical systems. Ultraviolet (UV) transmission gratings enable beam splitting and dispersion in the UV band. To improve energy utilization of the target diffraction orders, the grating groove shape is typically designed as an asymmetric structure with blazed and anti-blazed surfaces, concentrating more incident light energy at the predetermined diffraction orders. Therefore, parameters such as the fill power, groove depth, blaze angle, and anti-blaze angle of the blazed grating directly affect its optical performance. Obtaining a stable groove shape that meets design requirements is a critical issue in the manufacturing process of UV transmission blazed gratings.
[0003] Existing blazed grating master sheets can typically be manufactured using methods such as mechanical scribing, holographic lithography combined with ion beam etching, etc. Mechanical scribing can directly form periodic grooves with a certain blaze angle on the substrate surface, but it has high requirements for high-precision scribing equipment, cutting tools, and motion control accuracy, resulting in high manufacturing costs in the production of large-area, high-consistency gratings. Holographic lithography combined with ion beam etching can first form a periodic mask, and then obtain asymmetric grooves through etching processes, but the process involves more steps, and the groove morphology is easily affected by etching conditions, deposition state, and sidewall evolution, making stable control of the blaze angle, anti-blaze angle, and groove depth quite difficult.
[0004] With the development of micro-nano fabrication technology, nanoimprinting has gradually been used for the replication of grating structures. Nanoimprinting can replicate micro- and nano-scale periodic structures into the imprinting adhesive layer using an existing master template. Compared to re-forming periodic structures using mechanical scribing or holographic exposure, it has certain advantages in terms of reproducibility and reduced master template replication costs. However, nanoimprinting essentially replicates existing structures. Once the period and groove shape of the original blazed grating master template are determined, the directly imprinted adhesive structure usually inherits the groove shape characteristics corresponding to the original master template. If it is necessary to obtain another grating master template with different aspect ratios, groove depths, blaze angles, or anti-blaze angles, it is difficult to complete the corresponding groove shape adjustment solely through imprinting replication.
[0005] On the other hand, to obtain a hard grating structure that can be used as a master for subsequent replication, it is usually necessary to further transfer the grating pattern formed in the imprinted resist layer to the substrate. Reactive ion etching (RIE) can change the etching state of the resist mask and substrate materials by adjusting process conditions such as etching gas composition, gas flow rate, RF power, and cavity pressure, and therefore can be used for the transfer of imprinted patterns and the formation of grating grooves. However, during the pattern transfer process, factors such as the consumption of the resist mask, the etching rate of the substrate material, the passivation state of the groove sidewalls, and the degree of anisotropic etching are interdependent. If RIE is used only as a process to directly transfer the resist mask pattern to the substrate, the groove shape finally formed on the substrate is easily limited by the initial groove shape of the resist mask. If multiple groove parameters such as the aspect ratio, groove depth, blaze angle, and anti-blaze angle are adjusted simultaneously in the same etching stage, different etching actions are easily coupled with each other, making it difficult to adjust each groove parameter separately according to the target structure, thereby increasing the processing control difficulty of different target groove master shapes.
[0006] Therefore, for original blazed grating masters with specific periods and groove shapes, there is still room for improvement in how to further reduce the dependence of the final ultraviolet transmission blazed grating master on the existing groove shape of the original master, and how to make different groove parameters adjustable in different processing stages, based on the realization of periodic structure repetition using nanoimprinting. Summary of the Invention
[0007] The present invention aims to solve the problem that in the existing process of preparing ultraviolet transmission blazed grating masters, when using the original blazed grating master for nanoimprint replication, the resulting grating groove shape is limited by the existing groove shape of the original blazed grating master. Furthermore, it is difficult to adjust the grating's aspect ratio, groove depth, blaze angle, and anti-blaze angle separately during the subsequent pattern transfer process. As a result, it is difficult to obtain ultraviolet transmission blazed grating masters with different groove shape parameters based on the same original blazed grating master.
[0008] To address the above problems, this invention provides a method for preparing an ultraviolet transmission blazed grating master, comprising the following steps:
[0009] S1. Prepare a flexible imprint template with a blazed grating array structure corresponding to the original blazed grating master template;
[0010] S2. An imprinting adhesive layer is formed on the surface of a silicon substrate. The flexible imprinting template is used to perform nanoimprinting on the imprinting adhesive layer, so that the blazed grating array structure on the flexible imprinting template is transferred to the imprinting adhesive layer, and an adhesive mask is formed in the imprinting adhesive layer.
[0011] S3. The first stage of shaping of the adhesive mask is performed by O2 reactive ion etching, adjusting the aspect ratio and groove depth of the adhesive mask to obtain the shaped adhesive mask;
[0012] S4. A second-stage reactive ion etching process is performed using an etching gas system containing CHF3, SF6, Ar and O2. The modified photomask is used as the etching mask, and the pattern of the modified photomask is transferred to the silicon substrate. During the pattern transfer process, the blaze angle and anti-blaze angle of the blaze groove formed on the silicon substrate are adjusted to obtain an ultraviolet transmission blaze grating master.
[0013] Furthermore, the flexible imprinting template is obtained by replicating the original blazed grating master. A template adhesive layer is formed on the surface of the original blazed grating master. The PET soft film is then bonded to the template adhesive layer and subjected to ultraviolet nanoimprinting. After curing, the PET soft film is separated from the original blazed grating master, so that the template adhesive layer forms a cured template adhesive grating structure on the surface of the PET soft film corresponding to the original blazed grating master. The PET soft film serves as a support layer to support the cured template adhesive grating structure, and the cured template adhesive grating structure serves as the main body for subsequently replicating the blazed grating array structure onto the imprinting adhesive layer.
[0014] Furthermore, before forming the imprinting adhesive layer on the silicon substrate surface, an tackifier layer is first formed on the silicon substrate surface, and then the imprinting adhesive layer is formed on the tackifier layer; before performing nanoimprinting using the flexible imprinting template, a release agent is applied to the surface of the flexible imprinting template to improve the bonding state between the imprinting adhesive layer and the silicon substrate, as well as the separation state between the flexible imprinting template and the imprinting adhesive layer after imprinting.
[0015] Furthermore, in the first stage of reactive ion etching, O2 is used as the etching gas to modify the resist mask formed by nanoimprinting. The O2 reactive ion etching consumes the resist mask material, causing changes in the aspect ratio and trench depth of the resist mask. This adjusts the trench shape of the imprinted resist mask from its initial shape to a shape suitable for subsequent silicon substrate pattern transfer. Once the resist mask reaches the target aspect ratio and trench depth, the first stage of reactive ion etching is switched to the second stage of reactive ion etching.
[0016] Further, the aspect ratio of the modified photomask is 0.7–0.8. Optionally, electromagnetic field simulation can be performed on the transmission characteristics of ultraviolet transmission blazed gratings under different aspect ratios to compare the changes in the -1st order transmission efficiency corresponding to different aspect ratios in the 200nm–500nm wavelength range, and 0.7–0.8 can be used as a preferred adjustment range for the photomask aspect ratio to determine the modification target of the first-stage reactive ion etching.
[0017] Furthermore, the second stage of reactive ion etching employs an etching gas system containing CHF3, SF6, Ar, and O2. The modified photomask obtained in the first stage is used as the etching mask, allowing the groove pattern of the modified photomask to be transferred to the silicon substrate. During the pattern transfer process, the blaze groove shape formed on the silicon substrate is further altered. The first stage of reactive ion etching primarily focuses on modifying the aspect ratio and groove depth of the photomask, while the second stage focuses on adjusting the transfer of the photomask pattern to the silicon substrate and the formation of blaze and anti-blaze angles on the silicon substrate. This allows the two etching stages to have different processing targets and control focuses.
[0018] Furthermore, in the second stage of reactive ion etching, SF6 is used to adjust the etching rate of the silicon substrate, CHF3 is used to passivate the sidewalls of the groove during etching, O2 is used to adjust the loss rate of the resist mask and the etching depth of the silicon substrate, and Ar is used to adjust the anisotropic depth etching process of the silicon substrate. By adjusting the gas flow rates of CHF3, SF6, Ar, and O2 respectively, the resist mask consumption, silicon substrate etching, sidewall passivation, and anisotropic depth etching are coordinated to adjust the blaze angle, anti-blaze angle, and groove depth formed during the pattern transfer process.
[0019] Furthermore, in the second stage of reactive ion etching, the etching rate of the silicon substrate is increased by increasing the flow rate of SF6, the passivation effect on the sidewalls of the groove is adjusted by decreasing the flow rate of CHF3, and the flashing groove formed during the transfer of the modified photomask to the silicon substrate is brought to the target state by adjusting the flow rate of O2 on the loss rate of the photomask and the etching depth of the silicon substrate, and adjusting the flow rate of Ar on the anisotropic depth etching process.
[0020] Furthermore, the first-stage reactive ion etching and the second-stage reactive ion etching respectively adjust the etching state of the corresponding stage by regulating at least one of the etching gas flow rate, RF power, and cavity pressure. Specifically, the first stage controls the degree of mask shaping by changing the corresponding reactive ion etching conditions to adjust the mask's aspect ratio and trench depth; the second stage adjusts the etching state of the shaped mask during pattern transfer to the silicon substrate by changing the gas flow rates of CHF3, SF6, Ar, and O2, as well as the RF power and cavity pressure, thereby changing the blaze angle, anti-blaze angle, and trench depth of the final trench shape formed on the silicon substrate.
[0021] Furthermore, for a flexible imprint template obtained from the same original blazed grating master, while keeping the original blazed grating master and its periodic structure unchanged, the mask shaping conditions of the first stage reactive ion etching and the silicon substrate etching conditions of the second stage reactive ion etching can be adjusted according to different target groove shapes. By changing the aspect ratio and groove depth of the mask in the first stage, and by changing the blaze angle and anti-blaze angle formed during the transfer of the shaped mask to the silicon substrate in the second stage, at least one of the aspect ratio, groove depth, blaze angle, and anti-blaze angle of the final ultraviolet transmission blazed grating master is different from the corresponding groove shape parameters of the original blazed grating master. Thus, ultraviolet transmission blazed grating masters with different groove shape parameters can be prepared based on the same original blazed grating master.
[0022] Compared to existing technologies that directly replicate the groove shape of the original blazed grating master using nanoimprinting or simultaneously adjust multiple groove parameters in a single etching stage, this invention divides the subsequent etching process after forming the resist mask using nanoimprinting into two reactive ion etching stages with different processing targets and control focuses: resist mask reshaping and silicon substrate pattern transfer. First, O2 reactive ion etching is used to pre-adjust the area ratio and groove depth of the resist mask. Then, an etching gas system containing CHF3, SF6, Ar, and O2 is used to transfer the reshaped resist mask pattern to the silicon substrate, with further adjustments made during the pattern transfer process. The blaze angle and anti-blaze angle enable the adjustment of the fill factor, groove depth, blaze angle, and anti-blaze angle to be performed in stages, reducing the mutual coupling when multiple groove parameters are concentrated in a single etching stage. At the same time, by changing the reactive ion etching conditions of the first and second stages, ultraviolet transmission blazed grating masters with different groove parameters can be obtained while keeping the original blazed grating master unchanged. This reduces the need to remake the original blazed grating master for different target groove shapes, improves the utilization of the original blazed grating master, and enhances the flexibility and controllability of the groove shape adjustment of the ultraviolet transmission blazed grating master. Attached Figure Description
[0023] Figure 1 This is a schematic diagram illustrating the main fabrication process of the ultraviolet transmission blazed grating master of the present invention;
[0024] Figure 2 This is a schematic diagram of the simulated groove shape within one period of the ultraviolet transmission blazed grating of the present invention;
[0025] Figure 3 The simulated transmission efficiency curves of the ultraviolet transmission blazed grating at the -1st order under different duty cycles of the present invention are shown.
[0026] Figure 4 This is a SEM cross-section and groove parameter illustration of the ultraviolet transmission blazed grating master formed by reactive ion etching according to the present invention.
[0027] In the figure: 1. Flexible embossing template; 2. Imprinting adhesive layer; 3. Silicon substrate; 4. Adhesive mask; 5. Reshaped adhesive mask; 6. Ultraviolet transmission blazed grating master. Detailed Implementation
[0028] The specific embodiments of the present invention will be further described below with reference to the accompanying drawings. For process conditions not specifically described, they can be selected or adjusted according to the processing equipment, imprinting material, silicon substrate specifications, and target grating groove shape used.
[0029] like Figure 1 As shown, the flexible imprint template 1 used in this invention can be obtained by replicating a pre-engraved blazed grating master. The surface of the pre-engraved blazed grating master has a pre-formed periodic blazed grating array structure. This array structure can have asymmetrical grooves within one period, forming corresponding blazed and anti-blazed surfaces. The pre-engraved blazed grating master can be prepared using mechanical scribing, photolithography combined with etching, or other existing micro / nano fabrication methods capable of forming blazed grating grooves. The periodic grooves formed on its surface are used for subsequent flexible template replication. In one embodiment, the pre-engraved blazed grating master can be placed on the suction cup of a spin coater, and template adhesive can be spin-coated onto the side with the grating grooves, so that the template adhesive covers the micro / nano grooved surface of the pre-engraved blazed grating master. In one embodiment, the spin-coating speed of the template adhesive can be 2000 r / min; the spin-coating speed can also be adjusted according to the viscosity of the template adhesive, the area of the pre-engraved blazed grating master, and the target template adhesive thickness.
[0030] After the template adhesive is formed, the original blazed grating master can be placed in an ultraviolet nanoimprinting device, so that the PET soft film is bonded to the side of the original blazed grating master with the template adhesive. Existing nanoimprinting auxiliary components such as adhesive rollers can be used to ensure full contact between the PET soft film and the template adhesive layer. Through ultraviolet nanoimprinting, the template adhesive replicates the micro-nano grooves on the original blazed grating master and completes curing. After imprinting and curing, the PET soft film is separated from the original blazed grating master. The cured template adhesive grating structure remains on the surface of the PET soft film, which serves as a support layer, thus forming a flexible imprinting template 1. The cured template adhesive grating structure has a blazed grating array structure corresponding to the original blazed grating master and serves as the main body for subsequently imprinting the adhesive layer 2 onto the surface of the silicon substrate 3 to replicate this array structure. Using the above method, nanoimprinting can be repeatedly performed through the flexible imprinting template 1, and the groove shape formed by imprinting can be further adjusted during subsequent etching processes, providing a basis for preparing ultraviolet transmission blazed grating masters with different groove parameters based on the same original blazed grating master.
[0031] After obtaining the flexible imprinting template 1, a silicon substrate 3 can be provided as a rigid substrate for subsequently forming a UV transmission blazed grating master. In this embodiment, the silicon substrate 3 can be a silicon wafer. Before applying the adhesive, the silicon wafer can be cleaned and dried according to existing techniques in the art to reduce the influence of surface contaminants on adhesive layer adhesion and pattern transfer. Optionally, an tackifier layer can be formed on the surface of the silicon substrate 3 first, and then an imprinting adhesive layer 2 can be formed on the tackifier layer. The tackifier can be an existing tackifier material compatible with the selected imprinting adhesive and the silicon substrate to improve the bonding state of the imprinting adhesive layer 2 on the surface of the silicon substrate 3. The imprinting adhesive layer 2 can be formed by spin coating. In one embodiment, the silicon wafer can be placed on the suction cup of a spin coater, and the etched imprinting adhesive can be spin-coated at a speed of 2500 r / min to obtain a relatively uniform imprinting adhesive layer 2. The spin coating speed can be adjusted according to the viscosity of the imprinting adhesive, the target adhesive layer thickness, and the spin coating equipment used. Before nanoimprinting, a release agent can be applied to the side of the flexible imprinting template 1 with the grating array structure. The release agent can be used to reduce the adhesion resistance when the flexible imprinting template 1 separates from the imprinting adhesive layer 2 after imprinting. The release agent can be a commonly used release material in the field of nanoimprinting, and the application method is determined according to the materials of the flexible imprinting template 1 and the imprinting adhesive layer 2.
[0032] Subsequently, the side of the flexible imprinting template 1 with the blazed grating array structure can be aligned with the imprinting adhesive layer 2 on the silicon substrate 3, and the two can be bonded together using an ultraviolet nanoimprinting device, allowing the periodic grooves on the flexible imprinting template 1 to enter the imprinting adhesive layer 2. In one embodiment, a roller can be used to ensure full contact between the flexible imprinting template 1 and the imprinting adhesive layer 2, so that the periodic micro / nano structure on the template surface can be replicated relatively completely to the imprinting adhesive layer 2. After the corresponding imprinting adhesive has cured, the flexible imprinting template 1 and the imprinting adhesive layer 2 can be separated, thereby obtaining an adhesive mask 4 with periodic grooves on the surface of the silicon substrate 3. At this time, the grooves of the adhesive mask 4 mainly originate from the flexible imprinting template 1, which in turn originates from the original blazed grating master. Therefore, if pattern transfer is directly performed on the silicon substrate 3 in this state, the final groove shape of the silicon substrate is likely to inherit the initial groove shape defined by the original blazed grating master to a large extent. After nanoimprinting is completed, the first stage reactive ion etching is performed on the photomask 4 to modify its structure before it is used as an etching mask for the silicon substrate. Then, the modified photomask 5 is used for subsequent silicon substrate pattern transfer.
[0033] Specifically, O2 reactive ion etching can be used to modify the shape of the adhesive mask 4. The O2 reactive ion etching primarily targets the imprinting adhesive material, causing the material of the adhesive mask 4 to be consumed under the action of reactive ions, thereby changing the lateral dimensions and longitudinal groove shape of the adhesive mask 4. For example... Figure 2As shown, the fill power ratio f = A / T, where A is the lateral width of the protrusion structure along the periodic direction within one grating period, and T is the grating period. Therefore, with the grating period remaining essentially constant, changing the lateral dimension of the resist mask 4 through O2 reactive ion etching can correspondingly alter its fill power ratio. Simultaneously, as the resist material is gradually removed along the thickness direction, the groove depth and shape of the resist mask 4 can also change accordingly. By controlling the degree of O2 reactive ion etching, the resist mask 4 formed after nanoimprinting can be gradually transformed from its initial groove shape into a groove shape more suitable for subsequent silicon substrate pattern transfer, forming a modified resist mask 5. For example, when the fill power ratio of the resist mask 4 formed by nanoimprinting is greater than the target fill power ratio, the resist mask material can be gradually removed through O2 reactive ion etching to reduce the corresponding lateral structure size, and the process can be stopped or switched after reaching the target fill power ratio. The O2 flow rate, RF power, cavity pressure, and processing time can be selected based on the imprinting adhesive material, initial adhesive layer thickness, initial groove shape, and target groove shape to achieve controllable shaping of the adhesive mask 4 and maintain its structural integrity as a subsequent silicon etching mask.
[0034] In one specific embodiment, the first-stage reactive ion etching uses O2 as the etching gas. The chamber pressure can be set to 1.5 Pa, the RF power to 100 W, the O2 flow rate to 60 sccm, and the etching time to 40 s. Under these process conditions, the aspect ratio of the resist mask 4 can be adjusted from 1 to 0.76, thereby allowing the aspect ratio of the modified resist mask 5 to fall within the preferred range of 0.7 to 0.8. In other embodiments, the above process parameters can be adjusted accordingly based on the imprinting resist material, the initial groove shape, and the target aspect ratio.
[0035] In the first stage of reactive ion etching, O2 is used to modify the resist mask 4, adjusting its aspect ratio and trench depth before pattern transfer to the silicon substrate 3, forming a modified resist mask 5. Subsequently, the modified resist mask 5 is used as the etching mask for the second stage of reactive ion etching, transferring its trench pattern to the silicon substrate 3. Thus, the trench shape actually involved in the pattern transfer to the silicon substrate 3 is different from the initial trench shape of the resist mask 4 after nanoimprinting. This means that the final UV-Vis blazed grating master 6 is no longer completely limited by the existing trench shape of the original blazed grating master, providing a basis for obtaining UV-Vis blazed grating masters with different trench parameters based on the same original blazed grating master.
[0036] like Figure 2 As shown, the asymmetric slot shape within one grating period can be determined by the fill factor, slot depth, and blaze angle. and anti-flare angle The structural parameters are characterized, including the blaze angle. The angle between the blazing plane and the reference plane is called the anti-blazing angle. The angle between the anti-blaze surface and the reference plane. For a given period of grating, given other structural parameters and incident conditions, the effect of changing the fill factor on the transmission efficiency of the target diffraction order can be analyzed, and the target fill factor range suitable for subsequent mask shaping can be determined accordingly.
[0037] like Figure 3 As shown, to determine the suitable target aspect ratio for the ultraviolet transmission blazed grating, a simulation model can be established for the quartz ultraviolet transmission blazed grating structure subsequently replicated using the aforementioned ultraviolet transmission blazed grating master. In this embodiment, the grating period T is 1.9 μm, and the blaze angle is... The anti-flare angle is 25°. The angle is 120°, the grating material is quartz, and the incident light is perpendicular to the grating surface, without distinguishing polarization states. While keeping these conditions constant, the -1st order transmission efficiency corresponding to different duty cycles is calculated. Within the wavelength range of 200nm to 500nm, the transmission efficiency distribution varies for different duty cycles. Based on the simulation results and the efficiency requirements of the target operating wavelength band, 0.7–0.8 can be considered a preferred target duty cycle range. Accordingly, the process conditions for the first-stage O2 reactive ion etching are adjusted to ensure that the modified photomask 5 achieves a groove shape suitable for subsequent silicon substrate pattern transfer.
[0038] An aspect ratio of 0.7 to 0.8 is a preferred range under the above optical design conditions. When the target working band, diffraction order or other grating structure parameters change, the target aspect ratio can be determined according to the corresponding optical design results, and the degree of modification of the photomask can be adjusted accordingly.
[0039] After the modified photomask 5 reaches the desired state, the first stage of O2 reactive ion etching can be ended, and the process can switch to the second stage of reactive ion etching targeting the silicon substrate 3. The second stage uses an etching gas system containing CHF3, SF6, Ar, and O2, and uses the modified photomask 5 as the etching mask to transfer its periodic groove pattern to the silicon substrate 3. The modified photomask 5 not only defines the etching area on the surface of the silicon substrate 3, but also uses the area ratio, groove depth, and sidewall state formed in the first stage as the initial structural boundary for the pattern transfer in the second stage. Therefore, the first stage of photomask modification and the second stage of silicon substrate pattern transfer constitute a continuous processing procedure. By changing the groove shape of the photomask formed in the first stage and the etching conditions in the second stage, the groove shape can undergo further controllable evolution during the transfer to the silicon substrate 3, thereby forming an ultraviolet transmission blazed grating master 6 with groove parameters different from the original blazed grating master.
[0040] The etching gases used in the second stage play different regulatory roles during the etching process. SF6 primarily affects the etching rate of the silicon substrate 3. When other process conditions are appropriately coordinated, increasing the SF6 flow rate can increase the etching rate of the silicon material, allowing the exposed silicon material to be removed more quickly. Therefore, the formation process of the silicon substrate groove in the depth direction can be influenced by adjusting the SF6 flow rate. CHF3 can produce sidewall passivation during etching. The sidewall passivation state affects the removal of lateral material in the groove and the retention of the groove sidewalls. Therefore, CHF3 can influence the formation of the final blaze and anti-blaze surfaces. In one embodiment, the passivation effect on the groove sidewalls can be altered by reducing the CHF3 flow rate, and this can be combined with the silicon etching effect produced by SF6 to adjust the evolution state of the silicon substrate groove sidewalls. The blaze angle and anti-blaze angle are jointly regulated by the combined effects of silicon material etching, sidewall passivation, mask consumption, and anisotropic etching. Changes in these interactions affect the evolution state of the two sides of the groove during the pattern transfer process. For example, if the relative relationship between the silicon material removal rate and the sidewall passivation effect changes when the initial groove shape of the adhesive mask 5 is the same, the development ratio of the silicon groove shape along the depth direction and the lateral direction will also change accordingly, which may cause the final asymmetric groove shape to differ from the groove shape of the adhesive mask 5 itself.
[0041] In the second stage, O2 can further influence the loss rate of the modified photomask 5 and the achievable etching depth of the silicon substrate 3. Since the modified photomask 5 is continuously subjected to plasma during silicon substrate etching, its effective thickness and shielding ability change with the etching process. Therefore, changing the O2 flow rate can affect the consumption state of the photomask material, thereby influencing the effective pattern retention time and the achievable silicon etching depth. Ar can be used to influence the anisotropic depth etching process, making the etching process more conducive to forming a groove with a certain depth along a specific direction. CHF3, SF6, Ar, and O2 work together in the second stage of reactive ion etching to jointly influence silicon material removal, groove sidewall retention, photomask consumption, and depth-direction etching, thereby achieving adjustment of the final groove shape. The specific flow rates and ratios of CHF3, SF6, Ar, and O2 can be adjusted according to the reactive ion etching equipment, the structural state of the modified photomask 5, and the target groove shape, so that the etching rate of the silicon substrate 3, sidewall passivation, photomask loss, and anisotropic etching process are coordinated with each other.
[0042] In one specific embodiment, the chamber pressure of the second-stage reactive ion etching can be set to 5 Pa, the radio frequency power can be set to 150 W, the SF6 flow rate can be set to 13 sccm, the CHF3 flow rate can be set to 45 sccm, the Ar flow rate can be set to 10 sccm, and the O2 flow rate can be set to 5 sccm. Under the above conditions, the etching rate of the silicon substrate 3 is about 50 nm / min, and the etching time can be set to 9.8 min.
[0043] Besides the process gas flow rate, the first and second stages of reactive ion etching can also be controlled by adjusting the radio frequency (RF) power and cavity pressure to regulate the etching state. RF power affects the plasma's interaction with the material to be etched, while cavity pressure affects the transport and reaction processes of reactive gases and charged particles within the etching cavity. Therefore, the gas flow rate, RF power, and cavity pressure can be adjusted in conjunction with the material and structural state of the resist mask 4, the etching characteristics of the silicon substrate 3, and the target trench shape. The first stage primarily controls the degree of modification of the resist mask 4 by adjusting the O2 reactive ion etching conditions, ensuring its aspect ratio and trench depth meet the requirements for subsequent pattern transfer. The second stage controls the silicon material etching, sidewall passivation, resist mask loss, and anisotropic etching state during the transfer of the modified resist mask 5 to the silicon substrate 3 by adjusting the gas flow rates of CHF3, SF6, Ar, and O2, as well as the corresponding RF power and cavity pressure. These process conditions can be adjusted to match the performance of the reactive ion etching equipment used and the target trench shape.
[0044] Through the two-stage reactive ion etching described above, the resist mask reshaping and silicon substrate pattern transfer can each undertake different trench shape adjustment tasks. The first stage directly acts on the resist mask 4, changing its aspect ratio and trench depth through O2 reactive ion etching to obtain the reshaped resist mask 5. In the second stage, the reshaped resist mask 5 is used as the etching mask, and a gas system of CHF3, SF6, Ar, and O2 is used to perform reactive ion etching on the silicon substrate 3. While completing the pattern transfer, the blaze angle and anti-blaze angle formed on the silicon substrate 3 are further adjusted. Thus, the resist mask trench shape formed in the first stage can serve as the structural basis for the silicon substrate etching in the second stage. This allows the pre-adjustment of the aspect ratio and trench depth, along with the further adjustment of the blaze angle and anti-blaze angle, to be completed sequentially according to the processing order, thereby reducing the mutual influence that occurs when multiple trench shape parameters are adjusted in the same etching stage.
[0045] When using the same original blazed grating master, a flexible imprint template 1 obtained by replicating it can be used to form a resist mask 4 with the same initial periodic structure in the imprint resist layer 2 of at least two silicon substrates 3. Then, the reactive ion etching conditions of the first and second stages can be adjusted according to different target groove shapes. For example, by changing the degree of O2 reactive ion etching in the first stage, different resist masks 4 can form different aspect ratios or groove depths. Subsequently, the gas flow rates of CHF3, SF6, Ar, and O2 in the second stage, as well as the RF power and cavity pressure, can be adjusted according to the corresponding target groove shape to change the pattern transfer and sidewall formation state on the silicon substrate 3 accordingly. In this way, different ultraviolet transmission blazed grating masters 6 obtained from the same original blazed grating master can have differences in at least one of aspect ratio, groove depth, blaze angle, and anti-blaze angle, without having to re-fabricate the original blazed grating master for each target groove shape.
[0046] After the second stage of reactive ion etching is completed, the residual photoresist mask on the surface of the silicon substrate 3 can be removed as needed, and the silicon substrate 3 can be cleaned and its morphology inspected. The above post-processing can be implemented using existing techniques in the field. For example... Figure 4 As shown, under the aforementioned second-stage reactive ion etching conditions, a periodic asymmetric blazed groove is formed on the surface of the silicon substrate 3, thereby obtaining the ultraviolet transmission blazed grating master 6. According to Figure 4 The SEM profile shown was used to measure the groove shape parameters, and the obtained groove depth is approximately 491.3 nm; where the angle between the blazing surface and the reference surface is the blazing angle. The angle between the anti-flare surface and the reference plane is the anti-flare angle. .
[0047] Using the above-described fabrication method, the original blazed grating master is mainly used to provide the initial periodic structure. The flexible imprinting template 1 is used to transfer this periodic structure to the imprinting adhesive layer 2, and the adhesive mask 4 serves as an intermediate structure for subsequent groove shape adjustment. The adhesive mask 4 is shaped by O2 reactive ion etching in the first stage, and the shaped adhesive mask 5 is transferred to the silicon substrate 3 in the second stage using a gas system of CHF3, SF6, Ar, and O2. This allows for further adjustment of the aspect ratio, groove depth, blaze angle, and anti-blaze angle of the final ultraviolet transmission blazed grating master 6 while keeping the original blazed grating master unchanged. This enables the fabrication of ultraviolet transmission blazed grating masters with different groove shape parameters based on the same original blazed grating master.
[0048] Template materials, tackifiers, release agents, substrate cleaning methods, and spin coating, UV nanoimprinting, and reactive ion etching equipment can be selected from existing technologies in this field according to actual process requirements.
Claims
1. A method for preparing an ultraviolet transmission blazed grating master, characterized in that, Includes the following steps: S1. A flexible imprint template with a corresponding blazed grating array structure is prepared based on the original blazed grating master plate (1); S2. An imprinting adhesive layer (2) is formed on the surface of a silicon substrate (3), and a flexible imprinting template (1) is used for nanoimprinting to form an adhesive mask (4) in the imprinting adhesive layer (2). S3. The first stage of shaping of the adhesive mask (4) is performed by O2 reactive ion etching. The aspect ratio and groove depth of the adhesive mask (4) are adjusted to obtain the shaped adhesive mask (5). S4. The second stage of reactive ion etching is carried out using an etching gas system containing CHF3, SF6, Ar and O2. The pattern of the modified photomask (5) is transferred to the silicon substrate (3), and the blaze angle and anti-blaze angle of the groove formed on the silicon substrate (3) are adjusted to obtain the ultraviolet transmission blaze grating master (6). The aspect ratio, groove depth, blaze angle and anti-blaze angle of the ultraviolet transmission blazed grating master (6) are different from the corresponding parameters of the original blazed grating master.
2. The method for preparing an ultraviolet transmission blazed grating master according to claim 1, characterized in that, In step S1: A template adhesive layer is formed on the surface of the original blazed grating master. The PET soft film is then bonded to the template adhesive layer and subjected to ultraviolet nanoimprinting. After curing, the PET soft film is separated from the original blazed grating master, so that the template adhesive layer forms a cured template adhesive grating structure with a blazed grating array structure on the surface of the PET soft film. The PET soft film serves as a support layer to support the cured template adhesive grating structure, thereby forming the flexible imprinting template (1).
3. The method for preparing an ultraviolet transmission blazed grating master according to claim 1, characterized in that, In step S2: An tackifier layer and an imprinting adhesive layer (2) are sequentially formed on the surface of the silicon substrate (3), and a release agent is applied to the surface of the flexible imprinting template (1) before nanoimprinting is performed using the flexible imprinting template (1).
4. The method for preparing an ultraviolet transmission blazed grating master according to claim 1, characterized in that, In step S3: The aspect ratio of the adhesive mask (4) is adjusted by O2 reactive ion etching, and the aspect ratio of the modified adhesive mask (5) is 0.7 to 0.
8.
5. The method for preparing an ultraviolet transmission blazed grating master according to claim 1, characterized in that, In step S4: The gas flow rates of CHF3, SF6, Ar, and O2 were adjusted respectively, among which, The etching rate of the silicon substrate (3) can be increased by adjusting the flow rate of SF6; The passivation effect on the sidewalls during the etching process can be adjusted by regulating the flow rate of CHF3.
6. The method for preparing an ultraviolet transmission blazed grating master according to claim 5, characterized in that, In step S4: The loss rate of the modified photomask (5) and the etching depth of the silicon substrate (3) are adjusted by regulating the flow rate of O2. The anisotropic etching degree of the silicon substrate (3) is adjusted by regulating the flow rate of Ar.
7. The method for preparing an ultraviolet transmission blazed grating master according to claim 1, characterized in that: In step S3, the degree of shaping of the adhesive mask (4) is controlled by adjusting at least one of the following: O2 gas flow rate, radio frequency power, and cavity pressure; In step S4, the etching state of the silicon substrate (3) is controlled by adjusting at least one of the gas flow rates of CHF3, SF6, Ar and O2, the radio frequency power and the cavity pressure.
8. The method for preparing an ultraviolet transmission blazed grating master according to claim 7, characterized in that: Step S3 ends the first stage of reactive ion etching after the adhesive mask (4) reaches the target aspect ratio and trench depth, and uses the modified adhesive mask (5) as the etching mask for the second stage of reactive ion etching in step S4.
9. The method for preparing an ultraviolet transmission blazed grating master according to claim 8, characterized in that: A flexible imprint template (1) obtained from the same original blazed grating master is used to form a photomask (4) in the imprint adhesive layer (2) of at least two silicon substrates (3). Different first-stage reactive ion etching conditions and / or second-stage reactive ion etching conditions are set for different silicon substrates (3) to obtain ultraviolet transmission blazed grating master templates (6) with different groove parameters.
10. The method for preparing an ultraviolet transmission blazed grating master according to claim 9, characterized in that: The flexible embossing template (1) includes a PET soft film support layer and a cured template adhesive grating structure formed on the surface of the PET soft film support layer. The cured template adhesive grating structure is used to perform nanoimprinting on the embossing adhesive layer (2). The surface of the silicon substrate (3) is sequentially provided with an adhesive layer and an imprinting adhesive layer (2); Nanoimprinting is performed after applying a release agent to the surface of the flexible imprinting template (1); The first stage reactive ion etching makes the aspect ratio of the modified photomask (5) 0.7 to 0.
8. The second stage reactive ion etching adjusts the groove shape of the ultraviolet transmission blazed grating master (6) by adjusting the flow rates of SF6, CHF3, O2 and Ar.