A direct repair method and application for copper-impure degraded cathode materials
The hydrothermal-annealing method removes copper impurities from lithium-ion batteries, solving the cumbersome problem of copper impurity separation in lithium-ion battery recycling. It enables efficient repair and regeneration of cathode materials and is suitable for closed-loop recycling of lithium-ion batteries.
Patent Information
- Application Number
- CN202510600278.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-10
AI Technical Summary
In existing technologies, during the recycling of lithium-ion batteries, black powder containing copper impurities cannot be directly used for the repair and regeneration of cathode materials, leading to potential battery safety hazards. Furthermore, the separation process is cumbersome and cannot form a closed-loop recycling system.
The positive electrode material is repaired by using a hydrothermal-annealing method. After copper removal through pretreatment, copper impurities are removed by complexation reaction using ammonia/ammonium salt solution. Then, hydrothermal reaction and high-temperature sintering are carried out.
Without sacrificing nickel, cobalt, and manganese, the process is simplified, copper impurities are efficiently removed, and the performance of the cathode material is restored. This makes it suitable for large-scale promotion and is both economical and environmentally friendly.
Smart Images

Figure CN123073240A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of cathode material regeneration, specifically to a direct repair method and application for cathode materials containing copper impurities that have degraded. Background Technology
[0002] The overexploitation and irrational use of fossil fuels have caused severe environmental pollution and resource shortages. Finding more efficient, convenient, pollution-free, and safer energy sources is one of the most pressing energy issues to address. Lithium-ion batteries, due to their high volumetric energy density, high power output, and good cycle stability, are widely used in industries such as mobile phones and electric vehicles. However, lithium-ion batteries have a limited lifespan, and the number of retired lithium-ion batteries is constantly increasing. From an economic perspective, recycling lithium-ion batteries can significantly reduce their production costs (more than 20% of the cost of electric vehicles comes from cathode materials); from an environmental perspective, the flammable and toxic waste (such as organic solvents and heavy metals) generated by used batteries causes serious environmental pollution. Therefore, recycling and remanufacturing lithium-ion batteries to achieve sustainable energy storage is urgently needed.
[0003] Existing industrialized pyrometallurgical and hydrometallurgical recycling technologies both involve the crushing and dismantling of used batteries. This results in the recycled black powder containing not only waste positive electrode materials but also aluminum and copper fragments from both positive and negative electrode current collectors, conductive additives, binders, and graphite from the negative electrode. However, the presence of copper impurities in the black powder can easily cause short circuits in the battery, and may even lead to overheating, bulging, or even explosions. Therefore, black powder containing copper impurities cannot be directly used for positive electrode material repair and regeneration; the copper impurities must be removed before battery regeneration.
[0004] Currently, for black powder containing copper fragments, a multi-step screening process is generally used to separate the copper fragments from the black powder. First, a magnetic separator is used to separate magnetic materials containing a certain amount of copper, such as iron shells and caps. Then, the material is crushed and separated into lighter copper powders by an air-classification system. Finally, the particle size of the air-classified copper powder is controlled by a vibrating screen or a more advanced fine screening device. However, trace amounts of copper powder still remain in the final black powder. This process cannot completely separate the copper powder and does not consider subsequent battery regeneration, which is not conducive to forming a closed-loop recycling system for lithium-ion batteries.
[0005] Based on the above analysis, the present invention provides a direct repair method for copper-containing impurity-degraded cathode materials. The method can recover valuable metals without losing nickel, cobalt and manganese through two steps of hydrothermal annealing, and can also simplify the regeneration process, so that the cathode material can be restored to its initial state. Summary of the Invention
[0006] The purpose of this invention is to provide a direct repair method and application for copper-containing impurity-degraded cathode materials, which has the advantages of simple process, high efficiency, energy saving and environmental protection.
[0007] As the primary objective of this invention, it provides a method and application for directly repairing degraded cathode materials containing copper impurities. The direct repair method includes pretreatment to remove copper, followed by a hydrothermal annealing step to repair the degraded cathode material. Using the technical solution of this invention, copper impurities in the cathode material can be recovered, while the content of metals such as nickel in the cathode material remains almost unaffected.
[0008] Specifically, the direct repair method for the copper-containing impurity-degraded cathode material includes a copper removal-hydrothermal-annealing method; which includes mixing the degraded cathode material with copper powder and then performing a complexation reaction to remove copper; then adding lithium salt for a hydrothermal reaction, and finally annealing and repairing it by high-temperature sintering, thereby obtaining the repaired cathode material.
[0009] In a preferred embodiment, the complexation reaction includes adding a mixture of the decaying cathode material and copper powder to an ammonium ion solution, heating to carry out the reaction, and removing copper impurities from the decaying cathode material.
[0010] In a preferred embodiment, the copper impurity content in the decay cathode material is 0–6 wt%.
[0011] As a more preferred embodiment, the copper impurity content in the decaying cathode material is 0.5 to 3 wt%.
[0012] In a preferred embodiment, the ammonium ion solution is a mixed solution of ammonium salt and ammonia water.
[0013] In a preferred embodiment, the concentrations of both ammonium salt and ammonia water in the mixed solution are 0.05–0.2 M.
[0014] In a preferred embodiment, the molar ratio of ammonium salt to ammonia in the mixed solution is 1:1.
[0015] In a preferred embodiment, the conditions for the complexation reaction include a reaction temperature of 50–100°C.
[0016] Preferably, the reaction temperature is 60–90°C.
[0017] More preferably, the reaction temperature is 60°C.
[0018] As a preferred embodiment, the reaction time is 0.5 to 3 hours.
[0019] Preferably, the reaction time is 1 to 2 hours.
[0020] More preferably, the reaction time is 2 hours.
[0021] In a preferred embodiment, after the complexation reaction is completed, the material is centrifuged and dried to obtain a powdery substance, which is the copper-free decay cathode material.
[0022] In some specific embodiments, the drying temperature is 40–80°C.
[0023] In some specific embodiments, the drying time is 6 to 12 hours.
[0024] In a preferred embodiment, the hydrothermal reaction includes mixing the copper-removed decaying cathode material with a lithium salt solution and then adding the mixture to the solution to obtain a hydrothermal product.
[0025] In a preferred embodiment, the lithium salt includes lithium carbonate or lithium hydroxide.
[0026] In a preferred embodiment, the mass ratio of the decaying cathode material to the lithium salt is (50-55):1.
[0027] In a preferred embodiment, the hydrothermal reaction is carried out at a reaction temperature of 200–240°C for 1–6 hours.
[0028] In a preferred embodiment, the high-temperature sintering involves heating the hydrothermal product to 700-1000°C in an oxidizing gas atmosphere at a heating rate of 1-10°C / min for calcination, while holding at that temperature for 2-6 hours, and finally cooling to room temperature to obtain the repaired cathode material.
[0029] As another objective of the invention, the present invention also provides a cathode material prepared by the above-described direct repair method for cathode materials with copper impurities that have degraded.
[0030] Compared with the prior art, the technical effects of the present invention are as follows:
[0031] 1. The present invention provides a direct hydrothermal-annealing method for recovering copper-containing cathode materials. Without losing nickel, cobalt, and manganese, it effectively removes copper impurities by leaching with ammonia / ammonium salts and restores the properties of the regenerated cathode material to their initial state by adding lithium. It avoids the cumbersome steps of removing copper impurities and achieves multiple objectives through a simple two-step method. It has the advantages of simple process flow, low cost, and high return, and is economically efficient and suitable for large-scale promotion and application.
[0032] 2. This invention is based on the principle that copper ions can complex with ammonia molecules. It directly recovers copper-containing decaying cathode materials through hydrothermal annealing, and the content of copper impurities in the cathode material does not affect the copper removal effect. This greatly reduces the cumbersome pretreatment steps, meets the requirements of energy conservation and emission reduction, and has the advantages of energy saving and environmental protection.
[0033] 3. The technical solution of this invention uses a hydrothermal process in the liquid phase, and the hydrothermal lithium replenishment solution can be recycled, which can further reduce costs and has the advantages of being economical and environmentally friendly. Attached Figure Description
[0034] Figure 1 This is a schematic diagram of the regeneration method for lithium nickel cobalt manganese oxide cathode material containing copper impurities provided in Embodiment 1 of the present invention.
[0035] Figure 2 The copper dissolution effect is shown in the graphs at 0, 10, 30, 60, 90, 120 and 150 min when the concentration ratio of ammonium chloride and ammonia is 1:1.
[0036] Figure 3 Cold field scanning electron microscopy-X-ray energy dispersive spectroscopy (FSEM-XRD) of a commercially viable lithium nickel cobalt manganese oxide cathode material containing copper impurities.
[0037] Figure 4 Cold field scanning electron microscopy-X-ray energy dispersive spectroscopy (FSEM-XRD) image of the degraded lithium nickel cobalt manganese oxide cathode material containing copper impurities provided in Example 1 of this invention.
[0038] Figure 5 Cold field scanning electron microscopy-X-ray energy dispersive spectroscopy (FSEM-XRD) of hydrothermally heated lithium nickel cobalt manganese oxide after removing copper impurities with ammonium chloride and ammonia water, as provided in Example 1 of this invention.
[0039] Figure 6 Cold field scanning electron microscopy-X-ray energy dispersive spectroscopy (FSEM-XRD) image of lithium nickel cobalt manganese oxide repaired by removing copper impurities with ammonium chloride and ammonia water according to Example 1 of the present invention.
[0040] Figure 7 Comparison of X-ray diffraction results of lithium nickel cobalt manganese oxide before and after repair, as provided in Example 1 of the present invention.
[0041] Figure 8 This is a comparison chart of the charge-discharge curves of the lithium nickel cobalt manganese oxide cathode material before and after regeneration, as provided in Example 1 of the present invention.
[0042] Figure 9 This is a comparison chart of the low-rate cycling curves of the lithium nickel cobalt manganese oxide cathode material before and after regeneration, as provided in Example 1 of the present invention. Detailed Implementation
[0043] The specific technical solutions of the present invention will be described in detail below through specific embodiments. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. For the sake of brevity, this specification cannot provide a detailed description of all features of the actual embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0044] It should be noted that, unless otherwise defined, the technical or scientific terms used in this specification should be known to those skilled in the art described in this application.
[0045] The explanations of the abbreviations involved in the embodiments of this invention include:
[0046] Lithium nickel cobalt manganese oxide: NCM523
[0047] Degradation of lithium nickel cobalt manganese oxide: D-NCM523
[0048] Commercial lithium nickel cobalt manganese oxide: C-NCM523
[0049] Lithium nickel cobalt manganese oxide hydrothermally processed after removing copper impurities with ammonium chloride and ammonia:
[0050] NH4Cl + NH3·H2O - HT - NCM523
[0051] Lithium nickel cobalt manganese oxide repaired after removing copper impurities with ammonium chloride and ammonia:
[0052] NH4Cl + NH3·H2O - R - NCM523
[0053] This invention addresses the impact of varying copper impurity content on a hydrothermal-annealing direct recovery method. The method is based on the characteristics of cathode materials obtained during industrial production, particularly pyrometallurgical and hydrometallurgical methods for recovering copper impurities from black powder.
[0054] In some specific embodiments, taking NCM523, a typical power battery cathode material containing copper impurities, as an example, the degraded NCM material containing different copper impurities is first pretreated to remove the copper impurities, and then subjected to hydrothermal-annealing treatment to obtain the repaired cathode material.
[0055] Specifically, the direct repair method includes: removing copper impurities from degraded NCM materials containing different copper impurities by leaching with ammonia / ammonium salts, followed by hydrothermal reaction, and then brief high-temperature sintering. The sintered product is then washed and dried to obtain the repaired cathode material.
[0056] In some specific embodiments, electrochemical performance tests were conducted on the repaired cathode material. The results showed that, through the technical solution of the present invention, the degraded cathode material was successfully repaired by pretreatment to remove copper, followed by hydrothermal treatment and annealing. The method was effective and the repair was efficient.
[0057] In some specific embodiments, copper powder is mixed with the decaying cathode material to obtain simulated decaying cathode materials containing different amounts of copper impurities.
[0058] In some specific embodiments, copper is dissolved after complexing with ammonia molecules by adding an ammonium ion solution, thereby removing it from the decaying cathode material.
[0059] Using the technical solution of this invention, the copper content in the decaying cathode material can be 100% removed, even if it is as low as 0.5 wt%.
[0060] In particular, the technical solution of this invention does not affect the performance of the repaired cathode material.
[0061] However, it should be noted that this invention is not limited to NCM523 cathode material. It can be understood that this invention is applicable to lithium-ion battery cathode materials containing copper impurities.
[0062] The technical solution of the present invention will be described in detail below through specific embodiments.
[0063] Example 1
[0064] This embodiment provides a method for the direct regeneration of copper-containing decaying cathode materials (taking lithium nickel cobalt manganese oxide cathode material NCM523 as an example), see reference. Figure 1 The process flow diagram for directly repairing copper-containing degraded lithium nickel cobalt manganese oxide cathode material (D-NCM523) is as follows: The process includes mixing the degraded cathode material with copper powder to simulate copper-containing degraded cathode material (or, copper-containing degraded cathode material), adding ammonia solution for complexation reaction to remove copper, then washing and drying, and then adding lithium salt for hydrothermal reaction to replenish lithium, to obtain copper-removed and lithium-replenished cathode material HT-NCM523; then, high-temperature sintering to obtain the repaired cathode material (R-NCM523).
[0065] Specifically, the repair steps include:
[0066] (1) Material preparation: NCM523 cathode material with about 15% lithium deficiency was mixed with copper powder (the mass fraction of copper powder was 3%) to obtain copper-containing decay cathode material containing copper impurities.
[0067] (2) Copper removal process of copper-containing decaying cathode material: Add a mixed solution of ammonium chloride and ammonia (molar ratio of 1:1) to the decaying cathode material containing copper impurities provided in step (1) above, pour it into a glass bottle, heat at 50°C and stir for 120 minutes, centrifuge three times, and dry overnight at 50°C in a vacuum oven to obtain the decaying cathode material powder with copper impurities removed.
[0068] (3) The sample obtained in step (2) above was mixed with 4M lithium hydroxide solution and transferred to a hydrothermal reactor. The mixture was then subjected to hydrothermal reaction at 220°C for 4 hours in an oven. After the reaction was completed, the mixture was dried overnight at 50°C in a vacuum oven to obtain NCM523 material with supplemented lithium content.
[0069] (4) Sintering process: The hydrothermal products are transferred to a corundum boat and heated to 850°C in a tube furnace under an oxygen atmosphere at a heating rate of 5°C / min. The temperature is held for 4 hours and then cooled to room temperature. The repaired cathode material is obtained.
[0070] See Figure 3 Cold field scanning electron microscopy-X-ray energy dispersive spectroscopy image of commercial NCM523 cathode material. Figure 4 Cold field scanning electron microscopy-X-ray energy dispersive spectroscopy image of degraded NCM523 cathode material. Figure 5 This is a cold field scanning electron microscope-X-ray energy dispersive spectroscopy (SEM-XRD) image of the degraded cathode material after copper removal via ammonia solution complexation. Figure 6 This is a cold field scanning electron microscope-X-ray energy dispersive spectroscopy (SEM-XRD) image of the cathode material after final high-temperature sintering. Figures 3-6 The comparison shows that the single crystal particles of the degraded cathode material are of different sizes, and some particles have incomplete edges, while the surface of the repaired cathode material particles is smooth and consistent with the morphology of commercial materials.
[0071] See Figure 7 The figure shows a comparison of the X-ray diffraction results of commercial NCM523 cathode material and degraded NCM523 cathode material before and after repair. As can be seen from the figure, the diffraction peaks of the repaired cathode material are basically consistent with the standard card. Compared with the degraded material, the (003) peak at 18.783° shifts to the right, indicating that the lithium interlayer spacing is reduced. This method can successfully replenish lithium.
[0072] See Figure 8 and Figure 9 This is a comparison chart of the electrochemical performance of the cathode material before and after regeneration. Figure 8 This is a comparison chart of the cyclic curves. Figure 9 The graph shows a comparison of charge and discharge curves. As can be seen from the graph, the first discharge specific capacity of the regenerated battery (165mAh g) is... -1 ) is significantly higher than that of a degraded battery (148mAh g) -1 And after 80 cycles, the capacity retention rate was 87%.
[0073] Copper impurity removal rate / % = mass of dissolved copper / mass of copper powder. The copper impurity removal rate in this embodiment is shown in Table 1.
[0074] Example 2
[0075] This embodiment provides a method for the direct regeneration of copper-containing decaying cathode materials (taking lithium nickel cobalt manganese oxide cathode material NCM523 as an example), the specific steps of which include:
[0076] (1) Material preparation: NCM523 cathode material with about 15% lithium deficiency was mixed with copper powder (the mass fraction of copper powder was 3%) to obtain copper-containing decay cathode material containing copper impurities.
[0077] (2) Copper removal process of copper-containing decaying cathode material: Add a mixed solution of ammonium chloride and ammonia (molar ratio of 1:1) to the copper-containing decaying cathode material, pour it into a glass bottle, heat at 90°C and stir for 120 minutes, centrifuge three times, and dry overnight at 50°C in a vacuum oven to obtain decaying cathode material powder with copper impurities removed.
[0078] (3) The sample obtained in step 2 above was mixed with 4M lithium hydroxide solution and transferred to a hydrothermal reactor. The mixture was then subjected to hydrothermal reaction at 220°C for 4 hours in an oven. After the reaction was completed, the mixture was dried overnight at 50°C in a vacuum oven to obtain NCM523 material with supplemented lithium content.
[0079] (4) Sintering process: The hydrothermal products are transferred to the corundum boat and heated to 850°C in the tube furnace under an oxygen atmosphere at a heating rate of 5°C / min. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.
[0080] Example 3
[0081] This embodiment provides a method for the direct regeneration of copper-containing decaying cathode materials (taking lithium nickel cobalt manganese oxide cathode material NCM523 as an example), the specific steps of which include:
[0082] (1) Material preparation: NCM523 cathode material with about 15% lithium deficiency was mixed with copper powder (the mass fraction of copper powder was 3%) to obtain copper-containing decay cathode material containing copper impurities.
[0083] (2) Copper removal process of copper-containing decaying cathode material: Add a mixed solution of ammonium chloride and ammonia (molar ratio of 1:1) to the copper-containing decaying cathode material, pour it into a glass bottle, heat to 50 degrees and stir for 60 minutes, centrifuge three times, and dry overnight at 50 degrees in a vacuum oven to obtain decaying cathode material powder with copper impurities removed.
[0084] (3) The sample obtained in step 2 above was mixed with 4M lithium hydroxide solution and transferred to a hydrothermal reactor. The mixture was then subjected to hydrothermal reaction at 220°C for 4 hours in an oven. After the reaction was completed, the mixture was dried overnight at 50°C in a vacuum oven to obtain NCM523 material with supplemented lithium content.
[0085] (4) Sintering process: The hydrothermal products are transferred to an alumina boat and heated to 850°C in a tube furnace under an oxygen atmosphere at a heating rate of 5°C / min. The temperature is held for 4 hours, and finally cooled to room temperature. The repaired cathode material is obtained.
[0086] Example 4
[0087] This embodiment provides a method for the direct regeneration of copper-containing decaying cathode materials (taking lithium nickel cobalt manganese oxide cathode material NCM523 as an example), the specific steps of which include:
[0088] 1) Material preparation: NCM523 cathode material with about 15% lithium deficiency was mixed with copper powder (copper powder mass fraction of 3%) to obtain copper-containing decayed cathode material containing copper impurities.
[0089] (2) Copper removal process of copper-containing decaying cathode material: Add a mixed solution of ammonium chloride and ammonia (molar ratio of 1:1) to the copper-containing decaying cathode material, pour it into a glass bottle, heat at 50°C and stir for 150 minutes, centrifuge three times, and dry overnight at 50°C in a vacuum oven to obtain decaying cathode material powder with copper impurities removed.
[0090] (3) The sample obtained in step 2 above was mixed with 4M lithium hydroxide solution and transferred to a hydrothermal reactor. The mixture was then subjected to hydrothermal reaction at 220°C for 4 hours in an oven. After the reaction was completed, the mixture was dried overnight at 50°C in a vacuum oven to obtain NCM523 material with supplemented lithium content.
[0091] (4) Sintering process: The hydrothermal products are transferred to the corundum boat and heated to 850°C in the tube furnace under an oxygen atmosphere at a heating rate of 5°C / min. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.
[0092] Example 5
[0093] This embodiment provides a method for the direct regeneration of copper-containing decaying cathode materials (taking lithium nickel cobalt manganese oxide cathode material NCM523 as an example), the specific steps of which include:
[0094] 1) Material preparation: NCM523 cathode material with about 15% lithium deficiency was mixed with copper powder (copper powder mass fraction of 0.5%) to obtain copper-containing decayed cathode material containing copper impurities.
[0095] (2) Copper removal process of copper-containing decaying cathode material: Add a mixed solution of ammonium chloride and ammonia (molar ratio of 1:1) to the copper-containing decaying cathode material, pour it into a glass bottle, heat at 50°C and stir for 120 minutes, centrifuge three times, and dry overnight at 50°C in a vacuum oven to obtain decaying cathode material powder with copper impurities removed.
[0096] (3) The sample obtained in step 2 above was mixed with 4M lithium hydroxide solution and transferred to a hydrothermal reactor. The mixture was then subjected to hydrothermal reaction at 220°C for 4 hours in an oven. After the reaction was completed, the mixture was dried overnight at 50°C in a vacuum oven to obtain NCM523 material with supplemented lithium content.
[0097] (4) Sintering process: The hydrothermal products are transferred to the corundum boat and heated to 850°C in the tube furnace under an oxygen atmosphere at a heating rate of 5°C / min. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.
[0098] Example 6
[0099] This embodiment provides a method for the direct regeneration of copper-containing decaying cathode materials (taking lithium nickel cobalt manganese oxide cathode material NCM523 as an example), the specific steps of which include:
[0100] 1) Material preparation: NCM523 cathode material with about 15% lithium deficiency was mixed with copper powder (the mass fraction of copper powder was 6%) to obtain copper-containing decayed cathode material containing copper impurities.
[0101] (2) Copper removal process of copper-containing decaying cathode material: Add a mixed solution of ammonium chloride and ammonia (molar ratio of 1:1) to the copper-containing decaying cathode material, pour it into a glass bottle, heat at 50°C and stir for 120 minutes, centrifuge three times, and dry overnight at 50°C in a vacuum oven to obtain decaying cathode material powder with copper impurities removed.
[0102] (3) The sample obtained in step 2 above was mixed with 4M lithium hydroxide solution and transferred to a hydrothermal reactor. The mixture was then subjected to hydrothermal reaction at 220°C for 4 hours in an oven. After the reaction was completed, the mixture was dried overnight at 50°C in a vacuum oven to obtain NCM523 material with supplemented lithium content.
[0103] (4) Sintering process: The hydrothermal products are transferred to a corundum boat and heated to 850°C in a tube furnace under an oxygen atmosphere at a heating rate of 5°C / min. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.
[0104] Example 7
[0105] This embodiment provides a method for the direct regeneration of copper-containing decaying cathode materials (taking lithium nickel cobalt manganese oxide cathode material NCM523 as an example), the specific steps of which include:
[0106] 1) Copper removal process of copper-containing decaying cathode material: Add NCM523 decaying cathode material with about 15% lithium deficiency to a mixed solution of ammonium chloride and ammonia (molar ratio of the two is 1:1), pour into a glass bottle, heat at 50°C and stir for 120 minutes, centrifuge three times, and dry overnight at 50°C in a vacuum oven to obtain the soaked decaying cathode material powder.
[0107] 2) The sample obtained in step 1 was mixed with a 4M lithium hydroxide solution and transferred to a hydrothermal reactor. The mixture was then subjected to a hydrothermal reaction at 220°C for 4 hours in an oven. After the reaction was completed, the mixture was dried overnight at 50°C in a vacuum oven to obtain NCM523 material with supplemented lithium content.
[0108] 3) Sintering process: The hydrothermal products are transferred to the corundum boat and heated to 850°C in an oxygen atmosphere in a tube furnace at a heating rate of 5°C / min. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.
[0109] Comparative Example 1
[0110] This comparative example provides a method for the direct regeneration of copper-containing decaying cathode materials (taking lithium nickel cobalt manganese oxide cathode material NCM523 as an example), the specific steps of which include:
[0111] (1) Material preparation: NCM523 cathode material with about 15% lithium deficiency was mixed with copper powder (the mass fraction of copper powder was 3%) to obtain copper-containing decay cathode material containing copper impurities.
[0112] (2) Copper removal process of copper-containing decaying cathode material: Add a mixed solution of ammonium chloride and ammonia (molar ratio of 1:1) to the copper-containing decaying cathode material, pour it into a glass bottle, heat at 25°C and stir for 120 minutes, centrifuge three times, and dry overnight at 50°C in a vacuum oven to obtain decaying cathode material powder with copper impurities removed.
[0113] (3) The sample obtained in step 2 above was mixed with 4M lithium hydroxide solution and transferred to a hydrothermal reactor. The mixture was then subjected to hydrothermal reaction at 220°C for 4 hours in an oven. After the reaction was completed, the mixture was dried overnight at 50°C in a vacuum oven to obtain NCM523 material with supplemented lithium content.
[0114] (4) Sintering process: The hydrothermal products are transferred to the corundum boat and heated to 850°C in the tube furnace under an oxygen atmosphere at a heating rate of 5°C / min. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.
[0115] Comparative Example 2
[0116] This comparative example provides a method for the direct regeneration of copper-containing decaying cathode materials (taking lithium nickel cobalt manganese oxide cathode material NCM523 as an example), the specific steps of which include:
[0117] (1) Material preparation: NCM523 cathode material with about 15% lithium deficiency was mixed with copper powder (the mass fraction of copper powder was 3%) to obtain copper-containing decay cathode material containing copper impurities.
[0118] (2) Copper removal process of copper-containing decaying cathode material: Add a mixed solution of ammonium chloride and ammonia (molar ratio of 1:0.5) to the copper-containing decaying cathode material, pour it into a glass bottle, heat to 50 degrees and stir for 120 minutes, centrifuge three times, and dry overnight at 50 degrees in a vacuum oven to obtain decaying cathode material powder with copper impurities removed.
[0119] (3) The sample obtained in step 2 above was mixed with 4M lithium hydroxide solution and transferred to a hydrothermal reactor. The mixture was then subjected to hydrothermal reaction at 220°C for 4 hours in an oven. After the reaction was completed, the mixture was dried overnight at 50°C in a vacuum oven to obtain NCM523 material with supplemented lithium content.
[0120] (4) Sintering process: The hydrothermal products are transferred to the corundum boat and heated to 850°C in the tube furnace under an oxygen atmosphere at a heating rate of 5°C / min. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.
[0121] Comparative Example 3
[0122] This comparative example provides a method for the direct regeneration of copper-containing decaying cathode materials (taking lithium nickel cobalt manganese oxide cathode material NCM523 as an example), the specific steps of which include:
[0123] (1) Material preparation: NCM523 cathode material with about 15% lithium deficiency was mixed with copper powder (the mass fraction of copper powder was 3%) to obtain copper-containing decay cathode material containing copper impurities.
[0124] (2) Copper removal process of copper-containing decaying cathode material: Add a mixed solution of ammonium chloride and ammonia (molar ratio of 1:2) to the copper-containing decaying cathode material, pour it into a glass bottle, heat to 50 degrees and stir for 120 minutes, centrifuge three times, and dry overnight at 50 degrees in a vacuum oven to obtain decaying cathode material powder with copper impurities removed.
[0125] (3) The sample obtained in step 1 above was mixed with 4M lithium hydroxide solution and transferred to a hydrothermal reactor. The mixture was then subjected to hydrothermal reaction at 220°C for 4 hours in an oven. After the reaction was completed, the mixture was dried overnight at 50°C in a vacuum oven to obtain NCM523 material with supplemented lithium content.
[0126] (4) Sintering process: The hydrothermal products are transferred to the corundum boat and heated to 850°C in the tube furnace under an oxygen atmosphere at a heating rate of 5°C / min. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.
[0127] Comparative Example 4
[0128] This comparative example provides a method for the direct regeneration of copper-containing decaying cathode materials (taking lithium nickel cobalt manganese oxide cathode material NCM523 as an example), the specific steps of which include:
[0129] (1) Material preparation: NCM523 cathode material with about 15% lithium deficiency was mixed with copper powder (the mass fraction of copper powder was 6%) to obtain copper-containing decay cathode material containing copper impurities.
[0130] (2) Copper removal process of copper-containing decaying cathode material: Add a mixed solution of ammonium chloride and ammonia (molar ratio of 1:2) to the copper-containing decaying cathode material, pour it into a glass bottle, heat at 50°C and stir for 120 minutes, centrifuge three times, and dry overnight at 50°C in a vacuum oven to obtain decaying cathode material powder with copper impurities removed.
[0131] (3) The sample obtained in step 1 above was mixed with 4M lithium hydroxide solution and transferred to a hydrothermal reactor. The mixture was then subjected to hydrothermal reaction at 220°C for 4 hours in an oven. After the reaction was completed, the mixture was dried overnight at 50°C in a vacuum oven to obtain NCM523 material with supplemented lithium content.
[0132] (4) Sintering process: The hydrothermal products are transferred to the corundum boat and heated to 850°C in the tube furnace under an oxygen atmosphere at a heating rate of 5°C / min. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.
[0133] The copper removal rate and performance of the repaired cathode materials obtained in each embodiment and comparative example are shown in Table 1.
[0134] Table 1. Copper removal rate and performance of cathode materials in each embodiment and comparative example.
[0135]
[0136] When the ratio of ammonium salt to ammonia is 1:1, the temperature is 50 degrees Celsius, and the reaction time is 120 minutes, the removal rate of Cu impurities in the cathode material can reach 100%, and the initial capacity and capacity retention of the repair material are optimal. When the temperature is too low, the reaction rate is slow, and Cu impurities cannot be completely removed; when the temperature is too high, ammonia will evaporate, the pH will decrease, and Cu... 2+ Reprecipitation will occur, leading to a decrease in material capacity; if the reaction time is too short, Cu cannot be completely dissolved; if the time is too long, it does not affect Cu removal but reduces efficiency; if the ratio of ammonium salt to ammonia is too low, the pH is insufficient to form a copper-ammonia complex, thus failing to dissolve Cu; if the ratio is too high, the pH increases, leading to Cu... 2+ Secondary precipitation affects the electrochemical performance of the repair material. When the Cu content in the failed material is too low, it does not affect the Cu removal effect; however, when the Cu content is too high, the reaction kinetics are insufficient, and complete Cu removal cannot be achieved. A comparison of Examples 1 and 7 shows that the method of the present invention does not affect the performance of the cathode material and can completely remove copper impurities from the cathode material, achieving 100% removal even when the copper impurity content is as low as 0.5%.
[0137] The above are merely preferred embodiments of the present invention and do not limit the scope of protection of the present invention. For those skilled in the art, the present invention can have various modifications and variations. Any changes, modifications, substitutions, integrations, and parameter alterations to these embodiments within the spirit and principles of the present invention, achieved through conventional substitutions or by achieving the same function without departing from the principles and spirit of the present invention, fall within the scope of protection of the present invention.
Claims
1. A method for directly repairing copper-impure-containing degraded cathode materials, characterized in that, The direct repair method is a copper removal-hydrothermal-annealing method, which includes removing copper impurities from the degraded cathode material through a complexation reaction; then adding lithium salt for a hydrothermal reaction; and finally annealing the material after high-temperature sintering to obtain the repaired cathode material.
2. The direct repair method for copper-containing impurity-degraded cathode materials according to claim 1, characterized in that, The complexation reaction involves adding an ammonium ion solution to the decaying cathode material, heating it to carry out the reaction, and removing copper impurities from the decaying cathode material.
3. The direct repair method for copper-containing impurity-degraded cathode materials according to claim 2, characterized in that, The copper impurity content in the decaying cathode material is 0-6 wt%; preferably, the copper impurity content is 0.5-3 wt%.
4. The direct repair method for copper-containing impurity-degraded cathode materials according to claim 2, characterized in that, The ammonium ion solution is a mixed solution of ammonium salt and ammonia water; In the mixed solution, the concentrations of both ammonium salt and ammonia water are 0.05–0.2 M; the molar ratio of ammonium salt to ammonia water is 1:
1. The conditions for the complexation reaction include a reaction temperature of 50–100°C; preferably, the reaction temperature is 50–90°C; more preferably, the reaction temperature is 50°C. The reaction time is 0.5 to 3 hours; preferably, the reaction time is 1 to 2 hours; more preferably, the reaction time is 2 hours.
5. The direct repair method for copper-containing impurity-degraded cathode materials according to any one of claims 1-4, characterized in that, After the complexation reaction is completed, the material is centrifuged and dried to obtain a powdery substance, which is the copper-free decay cathode material. The drying temperature is 40–80°C; the drying time is 6–12 hours.
6. The direct repair method for copper-containing impurity-degraded cathode materials according to claim 1, characterized in that, The hydrothermal reaction involves mixing copper-free degraded cathode material with a lithium salt solution and then adding the mixture to the solution to produce a hydrothermal product.
7. The direct repair method for copper-containing impurity-degraded cathode materials according to claim 6, characterized in that, The lithium salt includes lithium carbonate or lithium hydroxide; The mass ratio of the decaying cathode material to the lithium salt is (50-55):
1.
8. The direct repair method for copper-containing impurity-degraded cathode materials according to claim 6, characterized in that, The hydrothermal reaction conditions are a reaction temperature of 200–240°C and a reaction time of 1–6 hours.
9. The direct repair method for copper-containing impurity-degraded cathode materials according to claim 1, characterized in that, The high-temperature sintering process involves heating the hydrothermal product to 700-1000°C in an oxidizing gas atmosphere at a heating rate of 1-10°C / min for calcination, while holding the temperature for 2-6 hours, and finally cooling it to room temperature to obtain the repaired cathode material.
10. A cathode material, prepared by the direct repair method for copper-containing impurity-degraded cathode materials according to any one of claims 1-9.