Phase separation-induced core-shell structure flexible electromagnetic shielding composite membrane and its preparation method

By enabling low-melting-point alloy-based composite particles to spontaneously form a core-shell structure during solid-liquid phase transition, the complexity and stability issues in the preparation of existing core-shell structure materials have been resolved, achieving simplified preparation and superior performance of highly efficient electromagnetic protection materials.

CN123075883APending Publication Date: 2026-11-10BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611047285.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-15
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing core-shell structure materials have complex manufacturing processes, high costs, and insufficient structural controllability. Uneven distribution of functional phases in flexible composite systems leads to decreased electromagnetic performance and insufficient structural stability.

Method used

By utilizing the interfacial reconstruction behavior of low-melting-point alloy-based composite particles during solid-liquid phase transition, a core-shell heterostructure is spontaneously formed. The magnetic functional phase is fixed in the polymer matrix, enabling the structure to self-assemble, simplifying the fabrication process, and improving electromagnetic wave loss capability and structural stability.

Benefits of technology

A simple and low-cost preparation process was achieved, ensuring the structural stability and electromagnetic properties of the composite film. It possesses excellent tensile and bending mechanical properties, and the minimum reflection loss is less than 60 dB when the thickness is 2 mm, with an absorption bandwidth exceeding 7 GHz.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123075883A_ABST
    Figure CN123075883A_ABST
Patent Text Reader

Abstract

This invention discloses a flexible electromagnetic protective composite membrane with a phase separation-induced core-shell structure and its preparation method, belonging to the field of electromagnetic functional materials. The composite membrane comprises a flexible polymer matrix and a low-melting-point alloy-based magnetic composite filler dispersed therein. The low-melting-point alloy-based magnetic composite filler comprises a low-melting-point alloy matrix and magnetic functional phase powder. The low-melting-point alloy matrix has an internal compositional gradient structure including a core and an outer shell, with the core being a solid low-melting-point alloy matrix and the outer shell being a liquid low-melting-point alloy matrix. The magnetic functional phase powder is dispersed in the outer region of the outer shell. This invention utilizes the self-assembly behavior of component segregation and interfacial migration of the magnetic functional phase during the cooling process of the low-melting-point alloy to form a stable core-shell heterostructure, fixed by the flexible polymer matrix, without complex surface modification. It exhibits excellent flexibility, high mechanical strength, and no liquid metal leakage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electromagnetic functional materials technology, specifically to a phase-separated core-shell structure flexible composite and its preparation method, which is particularly suitable for electromagnetic protection fields such as microwave absorption and electromagnetic shielding. Background Technology

[0002] With the development of 5G communication, radar detection, and flexible electronic devices, higher demands are being placed on electromagnetic protection materials that combine flexibility, broadband absorption, and structural stability. Existing core-shell structure materials typically rely on complex surface modifications or multi-step synthesis methods, which suffer from complex processes, high costs, and insufficient structural controllability. Furthermore, uneven distribution of functional phases in flexible composite systems can lead to decreased electromagnetic performance and insufficient structural stability. Therefore, developing a flexible composite material that can achieve spontaneous formation of core-shell structures based on a simple fabrication process is of great significance. Summary of the Invention

[0003] Based on the above analysis, this invention provides a phase separation-induced core-shell structure flexible electromagnetic protection composite film and its preparation method. Through the interfacial reconstruction behavior of low-melting-point alloy-based composite particles during the solid-liquid phase transition, a stable enriched structure of magnetic functional phases is formed on the outer layer of the particles. This allows for self-assembly of the structure into a core-shell heterostructure without complex surface modifications or chemical plating, which is then fixed by a polymer matrix. This approach improves electromagnetic wave loss capability and structural stability while maintaining structural flexibility. The technical problems solved by this invention include: the complexity of traditional core-shell structure preparation processes; the uncontrollable distribution of functional phases; insufficient structural stability in flexible materials; and the reliance on a single electromagnetic loss mechanism.

[0004] This invention discloses a flexible electromagnetic protection composite membrane with a phase separation-induced core-shell structure, comprising a flexible polymer matrix and a low-melting-point alloy-based magnetic composite filler dispersed in the flexible polymer matrix; The low-melting-point alloy-based magnetic composite filler includes a low-melting-point alloy matrix and magnetic functional phase powder; the low-melting-point alloy matrix has an internal composition gradient structure including a core and an outer shell, the core is a solid low-melting-point alloy matrix, and the outer shell is a liquid low-melting-point alloy matrix; the magnetic functional phase powder is dispersed in the outer layer region of the outer shell.

[0005] Optionally, the low-melting-point alloy matrix is ​​a multi-metal system that can undergo component segregation during solidification or phase transformation.

[0006] Optionally, during cooling or structural evolution, or when using the flexible electromagnetic protection composite film, the core of the low-melting-point alloy matrix is ​​a solid low-melting-point alloy matrix, and the outer shell is a liquid low-melting-point alloy matrix.

[0007] Optionally, the flexible electromagnetic shielding composite film is used at room temperature.

[0008] Optionally, the mass ratio of the magnetic functional phase powder to the low melting point alloy matrix is ​​(2-8):100.

[0009] Optionally, the multi-metal system is one or more of Ga-based, In-based, Sn-based, or Bi-based multi-metal eutectic systems.

[0010] Optionally, the mass ratio of the low-melting-point alloy-based magnetic composite filler to the flexible polymer matrix is ​​(4-12):2.

[0011] Another aspect of the present invention discloses a method for preparing a flexible electromagnetic shielding composite film with a phase separation-induced core-shell structure as described above, comprising the following steps: Step 1: Heat and melt the low-melting-point alloy, then add magnetic functional phase powder, stir and disperse, and cool to obtain low-melting-point alloy-based magnetic composite filler; Step 2: Dissolve the flexible polymer matrix in a solvent, add the low melting point alloy-based magnetic composite filler obtained in Step 1, heat to above the melting point of the low melting point alloy to melt it, homogenize, and evaporate part of the solvent to obtain the composite slurry; Step 3: Place the composite slurry in a mold and cool it. During the cooling process, the low-melting-point alloy-based magnetic composite filler undergoes phase separation, and the magnetic functional phase powder accumulates in the outer layer region to form a core-shell structure. Demolding yields the flexible electromagnetic protection composite film.

[0012] Optionally, in step 2, the ratio of the flexible polymer matrix to the organic solvent is 5 to 10 mL of solvent per 1 g of flexible polymer matrix.

[0013] A third aspect of the present invention also discloses the application of the aforementioned flexible electromagnetic shielding composite film in microwave absorption and / or electromagnetic shielding.

[0014] Compared with the prior art, the present invention has at least the following beneficial effects: 1. Simple process, low cost, and easy to scale up production: This invention relies on the solid-liquid phase change separation self-assembly mechanism, which eliminates the need for complex surface modification, chemical plating and other treatment processes, greatly shortens the preparation cycle, simplifies the production process, effectively reduces the preparation cost, and is suitable for industrial mass production needs.

[0015] 2. No liquid metal leakage and excellent mechanical properties: The multi-layer core-shell structure constructed in this invention, combined with the surface anchoring effect of the magnetic functional phase, solves the leakage problem of low-melting-point liquid metal; at the same time, the core-shell heterostructure and the flexible polymer matrix are synergistically adapted, giving the composite film excellent tensile and bending mechanical properties and structural stability.

[0016] 3. In some embodiments, the matching and optimization of dielectric loss and magnetic loss are achieved through the synergistic effect of core-shell interface polarization loss, conductive loss, and magnetic loss. Typical samples exhibit excellent electromagnetic wave absorption performance at a thickness of 2 mm, with a minimum reflection loss lower than […]. With an effective absorption bandwidth of 60 dB and a maximum of over 7 GHz, it demonstrates the combined advantages of being ultra-thin, having a wide bandwidth, and strong absorption.

[0017] 4. High versatility and expandability: The low-melting-point alloy components, magnetic functional phase types, particle sizes, and polymer substrates used in this invention can all be flexibly adjusted and adapted. The formula can be adjusted according to the performance requirements of different electromagnetic protection scenarios, making it widely applicable and highly expandable. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the embodiments will be briefly introduced below. The features and advantages of the present invention can be more clearly understood by referring to the accompanying drawings. The accompanying drawings are schematic and should not be construed as limiting the present invention in any way. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 This is a flowchart illustrating the preparation process of the low-melting-point alloy-based magnetic composite filler of the present invention. Figure 2 This is a flowchart illustrating the preparation process of the phase separation-induced core-shell structure flexible electromagnetic protective composite membrane of the present invention. Figure 3 In Embodiment 1 of the present invention, Ga 40 In 60 Microwave absorption performance curve of Fe / SBS composite membrane. Detailed Implementation

[0020] To better understand the above-mentioned objectives, features, and advantages of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. It should be noted that, unless otherwise specified, the embodiments of the present invention and the features thereof can be combined with each other.

[0021] This invention employs a solid-liquid phase transition-induced structural construction strategy. During the cooling process of the low-melting-point alloy-based magnetic composite system, due to the differences in physical properties between the components and the influence of interfacial interactions, a non-uniform structure is formed inside the low-melting-point alloy-based composite particles. The magnetic functional phase exhibits an enriched distribution in the outer region of the particles and is eventually fixed in the polymer matrix, forming a core-shell structure.

[0022] A specific embodiment of the present invention, such as Figure 1-3As shown, a flexible electromagnetic protection composite membrane with a phase separation-induced core-shell structure is disclosed, which is composed of a flexible polymer matrix and a low-melting-point alloy-based magnetic composite filler.

[0023] Furthermore, the flexible polymer matrix includes one or more of thermoplastic elastomers, rubber polymers, or flexible film-forming resins, preferably SBS or SEBS.

[0024] Furthermore, the low-melting-point alloy-based magnetic composite filler is composed of a low-melting-point alloy matrix and magnetic functional phase powder dispersed therein. During cooling and structural evolution, and when the flexible electromagnetic protection composite film is used, the low-melting-point alloy matrix forms an internal compositional gradient structure, while the magnetic functional phase powder is enriched in the outer layer region of the low-melting-point alloy matrix under the action of the interface, thereby forming a multi-level heterogeneous structure.

[0025] Among them, the low melting point is no more than 300℃.

[0026] Furthermore, the flexible electromagnetic protection composite film is used at room temperature; the room temperature is 20-28°C; preferably, around 25°C.

[0027] The low-melting-point alloy matrix is ​​a multi-metal system with different component compatibility. During solidification or phase transformation, component segregation can occur, thereby forming a phase-separated structure in which enriched and depleted phases coexist. Such as one or more of Ga-based, In-based, Sn-based or Bi-based multi-element eutectic systems; preferably Ga-In, Ga-In-Sn or Ga-In-Sn-Bi systems.

[0028] The magnetic functional phase powder is a magnetic powder material with electromagnetic loss characteristics, including one or more of elemental metal powder, soft magnetic alloy powder, and ferrite powder; preferably one or more of Fe, carbonyl iron, FeSiAl, FeNi, FeCo, and ferrite.

[0029] For example, when the low-melting-point alloy matrix is ​​selected from Ga and In, and the magnetic functional phase powder is selected from Fe, under high-temperature processing conditions, the GaIn blend is in a liquid state, and the Fe particles are randomly distributed. After processing, a flexible electromagnetic protection composite is formed. When used at room temperature, the In core is solidified in the middle, followed by a liquid Ga layer, and Fe particles are attached to the outside of the Ga layer.

[0030] Furthermore, the magnetic functional phase powder has a particle size ranging from submicron to micron, preferably in the range of 0.5 to 4 μm.

[0031] Furthermore, the mass ratio of the magnetic functional phase powder to the low melting point alloy matrix is ​​(2-8):100.

[0032] Furthermore, the mass ratio of the solid low-melting-point alloy matrix to the liquid low-melting-point alloy matrix is ​​1:(0.2~6).

[0033] Furthermore, the particle size of the low-melting-point alloy-based magnetic composite filler is 10–30 μm.

[0034] Furthermore, in the flexible electromagnetic protection composite membrane system, the mass ratio of low melting point alloy-based magnetic composite filler to flexible polymer matrix is ​​(4-12):2.

[0035] This invention achieves a minimum reflection loss of less than -60dB with a thickness of approximately 2mm and an effective absorption bandwidth exceeding 7GHz, making it suitable for microwave absorption and electromagnetic shielding applications.

[0036] Another specific embodiment of the present invention discloses a method for preparing a phase separation-induced core-shell structure flexible electromagnetic protection composite film, comprising the following steps: Step 1. Preparation of low-melting-point alloy-based magnetic composite fillers; Specifically, under an inert atmosphere, low-melting-point alloys are added and melted in order of decreasing melting point to obtain a uniform multi-element low-melting-point alloy melt matrix. Subsequently, magnetic functional phase powders are added in the molten state and stirred at 500-1500 rpm for 3-5 min to ensure that the magnetic particles are uniformly distributed in the liquid alloy. After cooling to room temperature, a low-melting-point alloy-based magnetic composite filler is obtained.

[0037] Step 2. Preparation of composite slurry; The flexible polymer matrix is ​​dissolved in an organic solvent to form a homogeneous solution. The ratio is 5-10 mL of solvent for every 1 g of flexible polymer matrix. The solution is magnetically stirred for 1-5 h until completely dissolved. A low-melting-point alloy-based magnetic composite filler is added, and the mixture is heated above the melting point under inert gas protection to completely melt the alloy. The mixture is then mechanically homogenized at 5000-20000 rpm for 10-30 min. Part of the solvent is evaporated to obtain a viscous composite slurry.

[0038] The organic solvent is an organic solvent that can dissolve flexible polymer materials and does not react significantly with low-melting-point alloys, preferably one or more of ethyl acetate, toluene, xylene, cyclohexane, and petroleum ether.

[0039] Step 3. Composite film forming; The obtained composite slurry is poured into a polytetrafluoroethylene mold and dried at room temperature in an inert gas atmosphere for 12-24 hours. The drying method is not limited to natural static drying, but low-temperature negative pressure drying can also be used. During the cooling process, the low-melting-point alloy-based magnetic composite material in the viscous composite slurry undergoes phase separation. Magnetic elements (such as Fe) in the magnetic functional phase powder are enriched in the outer layer region of the particles, eventually forming a core-gradient transition layer-magnetically enriched outer layer. After cooling to room temperature, the material is demolded to obtain a flexible electromagnetic protective composite film with a phase separation-induced core-shell structure.

[0040] Example 1: Ga 40 In 60 -Fe / SBS flexible composite membrane 1. Under nitrogen protection, 0.6 mol of In was heated to 170 °C to melt, 0.4 mol of Ga was added, and the mixture was stirred at 500 rpm for 1 min. After cooling, Ga was obtained. 40 In 60 Binary alloy; 20 g Ga 40 In 60 A binary alloy is heated to above 90 °C, and 1 g of Fe particles (~1 μm) is added as a magnetic functional phase powder. The mixture is stirred and dispersed, and then cooled to obtain Ga. 40 In 60 -Fe ternary magnetic alloy; 2. Dissolve 2 g SBS in 15 mL ethyl acetate and stir for 2 h until the SBS is completely dissolved; add 7.5 g ternary magnetic alloy, heat to 90 ℃ to completely melt the alloy, and pulse homogenize at 10000 rpm for 20 min, during which some ethyl acetate evaporates to obtain a viscous composite slurry.

[0041] 3. The slurry was dried at room temperature for 24 hours under nitrogen protection in a mold, and then demolded to obtain Ga. 40 In 60 -Fe / SBS flexible composite membrane.

[0042] performance: SEM / EDS analysis results show that a "solid In-rich core-liquid Ga-rich shell" is formed, with the magnetic functional phase mainly distributed in the outer region of the particles, forming a core-shell structure. The elements are evenly distributed and there is no obvious agglomeration.

[0043] The tensile strength is 1.75 MPa, the elongation at break is 681%, and there is no leakage of liquid metal.

[0044] With a thickness of 1.7 mm, the minimum reflection loss is -68.6 dB, and with a thickness of 1.9 mm, the maximum effective absorption bandwidth is 7.3 GHz.

[0045] Example 2: Ga50 In 20 Sn 20 Bi 10 Preparation of Fe / SBS multi-element alloy flexible composite film 1. Under nitrogen protection, following the order of melting points from highest to lowest, 0.1 mol Bi was melted at 275 ℃, the temperature was maintained and the mixture was stirred. Then, 0.2 mol Sn was added, melted and stirred until homogeneous. The temperature was lowered to about 200 ℃, then 0.2 mol In was added, melted and stirred until homogeneous. Finally, 0.5 mol Ga was added, and the mixture was stirred for 1 min to achieve uniform mixing. The mixture was then cooled to room temperature to obtain Ga. 50 In 20 Sn 20 Bi 10 A multi-element alloy was prepared by heating 20 g of the alloy to 120 °C, adding 1 g of Fe particles (~1 μm) as a magnetic functional phase powder, stirring until uniformly dispersed, and cooling to room temperature to obtain Ga. 50 In 20 Sn 20 Bi 10 -Fe multi-element magnetic alloy.

[0046] 2. Dissolve 2 g SBS in 15 mL of ethyl acetate, then add 10 g Ga 50 In 20 Sn 20 Bi 10 -Fe magnetic multi-element alloy was heated to 120 ℃ to melt, and then pulsed at 10000 rpm for 20 min to obtain a composite slurry.

[0047] 3. The slurry was dried at room temperature for 24 hours under nitrogen protection in a mold, and then demolded to obtain Ga. 50 In 20 Sn 20 Bi 10 -Fe / SBS flexible composite membrane.

[0048] performance: The tensile strength is 1.8 MPa, the elongation at break is 620%, and there is no leakage of liquid metal; With a thickness of 3.2 mm, the minimum reflection loss is -77 dB, and with a thickness of 2.2 mm, the maximum effective absorption bandwidth is 7.8 GHz. The absorption performance is better than that of ternary magnetic alloy composite film, which confirms that the multi-element alloy phase separation strategy can further improve the absorption performance.

[0049] Comparative Example 1: Ga without phase separation 84 In 16 Preparation of Fe / SBS composite membrane Under nitrogen protection, 0.16 mol In was heated and melted, then 0.84 mol Ga was added, stirred until homogeneous, and cooled to room temperature to obtain Ga with eutectic composition. 84 In 16 A binary alloy (this composition cannot undergo phase separation); 1g of Fe particles (~1μm) were added as a magnetic functional phase powder, and the mixture was stirred and dispersed to obtain Ga. 84 In 16 -Fe alloy.

[0050] The composite slurry and composite membrane were prepared according to the method in Example 1 to obtain Ga 84 In 16 -Fe / SBS composite membrane.

[0051] Performance test results: The composite membrane exhibited significant liquid metal leakage under pressure (tensile strength was only 1.2 MPa, elongation at break was 450%, and mechanical properties were poor). At a thickness of 2.8 mm, the minimum reflection loss is only -10.8 dB and the maximum effective absorption bandwidth is 0.6 GHz, both of which fail to meet the performance indicators defined in the claims and are far lower than the performance of the embodiments of the present invention. The comparative results show that only when the conditions for phase separation-induced structure formation are met can the composite system form a stable core-shell structure and significantly improve electromagnetic absorption performance, further confirming the key role of the phase separation core-shell structure and the composition range defined in the present invention on the performance of the composite film.

[0052] All the above-mentioned optional technical solutions can be combined in any way to form optional embodiments of the present invention, and will not be described in detail here.

[0053] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be covered within the scope of the claims and specification of the present invention.

Claims

1. A flexible electromagnetic shielding composite membrane with a phase separation-induced core-shell structure, characterized in that, Includes a flexible polymer matrix and a low-melting-point alloy-based magnetic composite filler dispersed in the flexible polymer matrix; The low-melting-point alloy-based magnetic composite filler includes a low-melting-point alloy matrix and magnetic functional phase powder; the low-melting-point alloy matrix has an internal composition gradient structure including a core and an outer shell, the core is a solid low-melting-point alloy matrix, and the outer shell is a liquid low-melting-point alloy matrix; the magnetic functional phase powder is dispersed in the outer layer region of the outer shell.

2. The flexible electromagnetic protection composite film according to claim 1, characterized in that, The low-melting-point alloy matrix is ​​a multi-metal system that can undergo component segregation during solidification or phase transformation.

3. The flexible electromagnetic protection composite film according to claim 1, characterized in that, During cooling or structural evolution, or when using the flexible electromagnetic protection composite film, the core of the low-melting-point alloy matrix is ​​a solid low-melting-point alloy matrix, and the outer shell is a liquid low-melting-point alloy matrix.

4. The flexible electromagnetic protection composite film according to claim 3, characterized in that, The flexible electromagnetic protection composite film is used at room temperature.

5. The flexible electromagnetic protection composite film according to claim 1, characterized in that, The mass ratio of the magnetic functional phase powder to the low melting point alloy matrix is ​​(2-8):

100.

6. The flexible electromagnetic protection composite film according to claim 2, characterized in that, The multi-metal system is one or more of the following: Ga-based, In-based, Sn-based, or Bi-based multi-element eutectic systems.

7. The flexible electromagnetic protection composite film according to claim 1, characterized in that, The mass ratio of the low-melting-point alloy-based magnetic composite filler to the flexible polymer matrix is ​​(4-12):

2.

8. A method for preparing a flexible electromagnetic shielding composite membrane with a phase separation-induced core-shell structure according to any one of claims 1-7, characterized in that, Includes the following steps: Step 1: Heat and melt the low-melting-point alloy, then add magnetic functional phase powder, stir and disperse, and cool to obtain low-melting-point alloy-based magnetic composite filler; Step 2: Dissolve the flexible polymer matrix in a solvent, add the low melting point alloy-based magnetic composite filler obtained in Step 1, heat to above the melting point of the low melting point alloy to melt it, homogenize, and evaporate part of the solvent to obtain the composite slurry; Step 3: Place the composite slurry in a mold and cool it. During the cooling process, the low-melting-point alloy-based magnetic composite filler undergoes phase separation, and the magnetic functional phase powder accumulates in the outer layer region to form a core-shell structure. Demolding yields the flexible electromagnetic protection composite film.

9. The preparation method according to claim 8, characterized in that, In step 2, the ratio of the flexible polymer matrix to the organic solvent is 5 to 10 mL of solvent per 1 g of flexible polymer matrix.

10. The application of the flexible electromagnetic shielding composite film according to any one of claims 1-9 in microwave absorption and / or electromagnetic shielding.