Semiconductor Components and Their Fabrication Methods
By forming shallow trenches and epitaxial layers between transistor regions, and using high dielectric constant dielectric layers and work function metal layers, the problem of poor electrical performance during the fabrication of metal gate transistors is solved, thereby improving the device's driving capability and overall efficiency.
Patent Information
- Application Number
- CN202510645955.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2025-05-20
- Publication Date
- 2026-11-10
AI Technical Summary
During the fabrication of metal gate transistors, the input/output region and the core region suffer from poor electrical performance due to the pre-set gate dielectric layer thickness, and the wet cleaning process may cause problems such as epitaxial layer loss and void formation.
Shallow trenches are formed between transistor regions, and epitaxial layers are formed therebetween. Epitaxial growth processes are used to form epitaxial layers around the transistor regions, followed by metal gate replacement. High dielectric constant dielectric layers and work function metal layers are used to improve electrical performance.
By forming shallow trenches and epitaxial layers between transistor regions, the electrical performance of metal gate transistors is improved, epitaxial layer loss and void formation are avoided, and the driving capability and overall performance of the device are enhanced.
Smart Images

Figure CN123075997A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for fabricating a semiconductor device, and more particularly to a method for forming trenches in shallow trench isolation between epitaxial layers of different transistor regions. Background Technology
[0002] In the current semiconductor industry, polysilicon is widely used in semiconductor devices such as metal-oxide-semiconductor (MOS) transistors as the standard gate fill material. However, as the size of MOS transistors continues to shrink, traditional polysilicon gates suffer from problems such as reduced device performance due to the boron penetration effect and the unavoidable depletion effect. This leads to an increase in the equivalent gate dielectric layer thickness, a decrease in gate capacitance, and consequently, a decline in device drive capability. Therefore, the semiconductor industry is also exploring new gate fill materials, such as work function metals, to replace traditional polysilicon gates as control electrodes to match high-k gate dielectric layers.
[0003] However, in current metal gate transistor fabrication processes, particularly in the input / output (I / O) region and core region, the electrical performance is suboptimal due to the pre-defined gate dielectric layer thickness. For example, during the hollowing-out of the polysilicon gate in these two regions, the epitaxial layer often erodes, resulting in voids, due to the wet cleaning process. Therefore, improving current metal gate fabrication processes to address this issue is a crucial research topic. Summary of the Invention
[0004] An embodiment of the present invention discloses a method for fabricating a semiconductor device, which mainly involves first providing a substrate including a first transistor region and a second transistor region, then forming a shallow trench isolation surrounding the first transistor region and the second transistor region, forming a gate structure extending from the first transistor region to the second transistor region, forming a first epitaxial layer next to the gate structure of the first transistor region and a second epitaxial layer next to the gate structure of the second transistor region, and then forming a trench within the shallow trench isolation between the first epitaxial layer and the second epitaxial layer.
[0005] Another embodiment of the present invention discloses a semiconductor device, which mainly includes a substrate including a first transistor region and a second transistor region, a shallow trench isolation surrounding the first transistor region and the second transistor region, a gate structure extending from the first transistor region to the second transistor region, a first epitaxial layer disposed next to the gate structure of the first transistor region, a second epitaxial layer disposed next to the gate structure of the second transistor region, and a trench disposed within the shallow trench isolation between the first epitaxial layer and the second epitaxial layer.
[0006] Another embodiment of the present invention discloses a semiconductor device, which mainly includes a substrate including a first transistor region and a second transistor region, a shallow trench isolation surrounding the first transistor region and the second transistor region, and a gate structure extending from the first transistor region to the second transistor region, wherein the bottom surface of the gate structure directly above the shallow trench isolation between the first transistor region and the second transistor region includes a protrusion. Attached Figure Description
[0007] Figures 1 to 7 This is a schematic diagram of a method for fabricating a semiconductor device according to an embodiment of the present invention;
[0008] Figure 8 This is a schematic diagram of the structure of a semiconductor device according to an embodiment of the present invention;
[0009] Figure 9 According to an embodiment of the present invention Figures 1 to 7 A schematic diagram of the structure of a semiconductor device fabricated using the manufacturing process.
[0010] Symbol explanation:
[0011] 12: Base
[0012] 14: PMOS region
[0013] 16: NMOS region
[0014] 20: Fin-like structure
[0015] 22: Shallow trench isolation
[0016] 24: Gate Structure
[0017] 26: Gate Structure
[0018] 28: Gate Structure
[0019] 30: Gate dielectric layer
[0020] 32: Gate material layer
[0021] 34: Spacer wall
[0022] 36: Source / Drain Region
[0023] 38: Epitaxial layer
[0024] 40: Epitaxial layer
[0025] 42: Opening
[0026] 44: Trench
[0027] 46: Flat surface
[0028] 48: Inclined sidewall
[0029] 54: Contact hole etching stop layer
[0030] 56: Interlayer dielectric layer
[0031] 58: Groove
[0032] 60: Gate dielectric layer
[0033] 62: High dielectric constant dielectric layer
[0034] 64: Work function metal layer
[0035] 66: Low-resistivity metal layer
[0036] 68: Hard Mask
[0037] 70: Metal gate
[0038] 72: Contact plug
[0039] 74: Contact plug
[0040] 76: Contact plug
[0041] 78: Interlayer dielectric layer
[0042] 80: Protrusion
[0043] 82: Protrusion
[0044] 84: Groove Detailed Implementation
[0045] Please refer to Figures 1 to 7 , Figures 1 to 7 This is a schematic diagram of a method for fabricating a semiconductor device according to an embodiment of the present invention, wherein... Figures 1 to 7 The upper half is a top view of a semiconductor device fabricated according to an embodiment of the present invention. Figures 1 to 8 The lower half is a cross-sectional view showing the semiconductor device fabricated along the X1, X2, X3, and Y directions from the upper half. For example... Figure 1As shown, a substrate 12 is first provided, such as a silicon substrate or a silicon-on-insulator (SOI) substrate, and a first transistor region and a second transistor region are defined on the substrate 12. In this embodiment, the first transistor region and the second transistor region are preferably transistor regions with different conductivity types. For example, the first transistor region may be a PMOS region 14 used to fabricate a PMOS transistor, and the second transistor region may be an NMOS region 16 used to fabricate an NMOS transistor, but it is not limited to this. Both the PMOS region 14 and the NMOS region 16 of the substrate 12 have at least one fin structure 20, wherein the bottom of the fin structure 20 is covered by an insulating material such as silicon oxide to form a shallow trench isolation (STI) 22. It should be noted that although this embodiment takes the fabrication of a non-planar field-effect transistor such as a fin structure as an example, it is not limited to this. The present invention can also be applied to general planar field-effect transistors, and this embodiment is also within the scope of the present invention.
[0046] According to one embodiment of the present invention, the fin structure 20 can be fabricated using sidewall image transfer (SIT) technology. The procedure generally includes: providing a layout pattern to a computer system and performing appropriate calculations to define the corresponding pattern in a photomask. Subsequently, multiple equidistant and equally wide patterned sacrificial layers are formed on a substrate using photolithography and etching processes, giving each layer a strip-like appearance. Then, deposition and etching processes are sequentially performed to form spacers on the sidewalls of the patterned sacrificial layers. The patterned sacrificial layers are then removed, and etching is performed under the cover of the spacers, transferring the pattern formed by the spacers into the substrate. Finally, a fin cut process is performed to obtain the desired patterned structure, such as a strip-shaped patterned fin structure.
[0047] In addition, the formation of the fin structure 20 may also include first forming a patterned mask (not shown) on the substrate 12, and then transferring the pattern of the patterned mask to the substrate 12 through an etching process to form the fin structure 20. Alternatively, the fin structure 20 may be formed by first fabricating a patterned hard mask layer (not shown) on the substrate 12, and then using an epitaxial fabrication process to grow a semiconductor layer, such as silicon-germanium, on the substrate 12 exposed above the patterned hard mask layer. This semiconductor layer can then serve as the corresponding fin structure 20. These embodiments of forming the fin structure 20 are all within the scope of this invention.
[0048] Then as Figure 2As shown, gate structures 24, 26, and 28, or dummy gates, can be formed on the substrate 12 of the PMOS region 14 and the NMOS region 16, respectively. In this embodiment, the gate structures 24, 26, and 28 are preferably formed by sequentially forming a gate dielectric layer 30, a gate material layer 32, and a selective hard mask (not shown) on the substrate 12, and using a patterned photoresist (not shown) as a mask for a pattern transfer fabrication process. A single etching or sequential etching step is used to remove a portion of the gate material layer 32 and a portion of the gate dielectric layer 30, and then the patterned photoresist is stripped off, so that at least one gate structure 24, 26, or 28 composed of a patterned gate dielectric layer 30 and a patterned gate material layer 32 is formed on the fin structure 20 of the PMOS region 14 and the NMOS region 16, respectively. In this embodiment, the gate dielectric layer 30 may contain silicon oxide and the gate material layer 32 may contain polysilicon, but is not limited thereto.
[0049] Then as Figure 3 As shown, at least one spacer wall 34 is formed on the sidewalls of each gate structure 24, 26, 28. A source / drain region 36 and / or epitaxial layers 38, 40 are formed in the fin structures 20 and / or the substrate 12 on both sides of the spacer wall 34. A metal silicide (not shown) is selectively formed on the surface of the source / drain region 36 and / or the epitaxial layers 38, 40. In this embodiment, the spacer wall 34 can be a single spacer wall or a composite spacer wall. For example, it may include a bias spacer wall (not shown) and a main spacer wall (not shown). The spacer wall 34 can be selected from the group consisting of silicon oxide, silicon nitride, silicon oxynitride, and silicon carbide, but is not limited thereto. The source / drain region 36 and the epitaxial layers 38, 40 may contain different dopants or different materials depending on the conductivity type of the transistor being disposed. For example, the source / drain region 36 of the PMOS region 14 may contain P-type dopants and the epitaxial layer 38 may contain silicon germanide (SiGe), while the source / drain region 36 of the NMOS region 16 may contain N-type dopants and the epitaxial layer 40 may contain silicon phosphide (SiP).
[0050] In detail, during the formation of epitaxial layers 38 and 40 in PMOS region 14 and NMOS region 16, a patterned mask (not shown) is preferably formed first. For example, the patterned photoresist covers most of the area between PMOS region 14 and NMOS region 16, and the patterned mask has two openings 42 to expose the area. Figure 3In the top view of the upper half, the fin structures 20 and gate structures 24, 26, and 28 located in the PMOS region 14 and the fin structures 20 and gate structures 24, 26, and 28 located in the NMOS region 16 are shown. Then, using a patterned mask as a mask, one or more etching processes are performed to remove the fin structures 20 on both sides of the gate structures 24, 26, and 28 in the PMOS region 14 and the fin structures 20 on both sides of the gate structures 24, 26, and 28 in the NMOS region 16 to form grooves 84. Then, using one or more epitaxial growth processes, an epitaxial layer 38 is formed in the PMOS region 14 and an epitaxial layer 40 is formed in the NMOS region 16, respectively. The epitaxial layer 38 in the PMOS region 14 preferably contains silicon germanide, while the epitaxial layer 40 in the NMOS region 16 preferably contains silicon phosphide.
[0051] It is worth noting that, due to the masking effect of the patterned mask and the addition of the shadow effect, in this embodiment, when removing the partial fin structures 20 on both sides of the gate structures 24, 26, and 28 inside the opening 42 by the above etching, it is also preferable to remove the partial gate structures 24, 26, and 28 inside the opening 42 but not the gate structures 24, 26, and 28 outside the opening 42. In this way, the top surfaces of the gate structures 24, 26, and 28 in the X1 and X2 directions are slightly lower than the top surfaces of the gate structures 24, 26, and 28 in the X3 direction.
[0052] Furthermore, when etching away the fin structures 20 on both sides of the gate structures 24, 26, and 28 within the opening 42, it is preferable to also remove the shallow trench isolation 22 outside the opening 42, particularly between the PMOS region 14 and the NMOS region 16, to form a trench 44. Figure 3 Viewed along the X3 and Y directions, the trench 44 is preferably formed such that, in the X3 direction, the top surface of the shallow trench isolation 22 on both sides of the gate structures 24, 26, 28 is slightly lower than the top surface of the shallow trench isolation 22 directly below the gate structures 24, 26, 28. In the Y direction, the top surface of the shallow trench isolation 22 is slightly lower than the bottom surface of the epitaxial layers 38, 40 on both sides or the top surface of the shallow trench isolation 22 below the epitaxial layers 38, 40. In detail, the top surface of the shallow trench isolation 22 directly below the trench 44, being slightly recessed, can have a flat surface 46 and two inclined sidewalls 48 extending from both sides to the epitaxial layers 38, 40 of the PMOS region 14 and the NMOS region 16, respectively.
[0053] Then as Figure 4As shown, a contact etch stop layer (CESL) 54 made of silicon nitride can be selectively formed on the substrate 12 to cover the gate structures 24, 26, and 28. Then, an interlayer dielectric layer 56 is formed on the contact etch stop layer 54. Next, a planarization process is performed, for example, by using chemical mechanical polishing (CMP) to remove part of the interlayer dielectric layer 56 and part of the contact etch stop layer 54, exposing the gate material layer 32 made of polysilicon, so that the upper surface of the gate material layer 32 of the PMOS region 14 and the NMOS region 16 is flush with the upper surface of the interlayer dielectric layer 36.
[0054] Subsequently, as Figure 5 As shown, a metal gate replacement (RMG) fabrication process is performed to convert each gate structure 24, 26, and 28 into a metal gate 70. For example, a selective dry etching or wet etching process can be performed first, such as using an etching solution such as ammonia hydroxide (NH4OH) or tetramethylammonium hydroxide (TMAH) to remove the gate material layer 32 and the gate dielectric layer 30 in the gate structures 24, 26, and 28 of the PMOS region 14 and the NMOS region 16, so as to form a groove 58 in the interlayer dielectric layer 56.
[0055] like Figure 6 As shown, an oxide growth process, such as a rapid thermal oxidation (RTO) process or an in-situ steam generation (ISSG) process, is then performed to form a gate dielectric layer 60 made of silicon oxide in the recesses 38 of the PMOS region 14 and the NMOS region 16, respectively. Subsequently, a high dielectric constant dielectric layer 62, a work function metal layer 64, and a low impedance metal layer 66 are sequentially formed in the recesses. Then, a planarization process is performed, for example, by using CMP to remove part of the low impedance metal layer 66, part of the work function metal layer 64, and part of the high dielectric constant dielectric layer 62 to form the metal gate 70.
[0056] In this embodiment, the high dielectric constant dielectric layer 62 comprises a dielectric material with a dielectric constant greater than 4, such as hafnium oxide (HfO2), hafnium silicon oxide (HfSiO4), hafnium silicon oxynitride (HfSiON), aluminum oxide (Al2O3), lanthanum oxide (La2O3), tantalum oxide (Ta2O5), yttrium oxide (Y2O3), zirconium oxide (ZrO2), strontium titanate oxide (SrTiO3), zirconium silicon oxide (ZrSiO4), hafnium zirconium oxide (HfZrO4), and strontium bismuth tantalum oxide. lead zirconate titanate (SrBi₂Ta₂O₉, SBT) and lead zirconate titanate (PbZr) x Ti 1-x O3, PZT), barium strontium titanate (Ba x Sr 1- x The group consisting of TiO3, BST, or combinations thereof.
[0057] The work function metal layer 64 is preferably used to adjust the work function of the metal gate to make it suitable for N-type transistors (NMOS) or P-type transistors (PMOS). If the transistor is an N-type transistor, the work function metal layer 64 can be made of a metal material with a work function of 3.9 electron volts (eV) to 4.3 eV, such as titanium aluminide (TiAl), zirconium aluminide (ZrAl), tungsten aluminide (WAl), tantalum aluminide (TaAl), hafnium aluminide (HfAl), or titanium aluminum carbide (TiAlC), but is not limited thereto; if the transistor is a P-type transistor, the work function metal layer 64 can be made of a metal material with a work function of 4.8 eV to 5.2 eV, such as titanium nitride (TiN), tantalum nitride (TaN), or tantalum carbide (TaC), but is not limited thereto. Another barrier layer (not shown) may be included between the work function metal layer 64 and the low impedance metal layer 66. The material of the barrier layer may include titanium (Ti), titanium nitride (TiN), tantalum (Ta), tantalum nitride (TaN), etc. The low impedance metal layer 66 may be selected from low resistance materials such as copper (Cu), aluminum (Al), tungsten (W), titanium-aluminum alloy (TiAl), cobalt-tungsten phosphide (CoWP), or combinations thereof.
[0058] Next, a portion of the high dielectric constant dielectric layer 62, a portion of the work function metal layer 64, and a portion of the low impedance metal layer 66 can be removed to form a groove (not shown). Then, a hard mask 68 is filled into the groove and made flush with the surface of the interlayer dielectric layer 56. The hard mask 68 can be selected from the group consisting of silicon oxide, silicon nitride, silicon oxynitride, and silicon carbide.
[0059] Subsequently, as Figure 7As shown, a contact plug fabrication process can be performed to form contact plugs 72, 74, and 76 that are electrically connected to the source / drain regions 36 of the PMOS region 14 and the NMOS region 16, respectively. The contact plugs 72 and 74 in the X1 and X2 directions preferably contact the source / drain regions 36 or the epitaxial layers 38 and 40, while the contact plug 76 in the X3 direction contacts the contact hole etch stop layer 54. In this embodiment, the contact plugs 72, 74, and 76 can be formed by first forming another interlayer dielectric layer 78 on the interlayer dielectric layer 56, removing a portion of the interlayer dielectric layer 78, a portion of the interlayer dielectric layer 56, and a portion of the contact hole etch stop layer 54 to form a contact hole (not shown), and then sequentially depositing a barrier layer (not shown) and a metal layer (not shown) on the substrate 12 to fill the contact hole. Next, a planarization process, such as CMP, is used to remove part of the metal layer, part of the barrier layer, and even part of the interlayer dielectric layer 78 to form contact plugs 72, 74, and 76 in the contact holes. The upper surfaces of the contact plugs 72, 74, and 76 are preferably flush with the upper surface of the interlayer dielectric layer 78. In this embodiment, the barrier layer is preferably selected from the group consisting of titanium, tantalum, titanium nitride, tantalum nitride, and tungsten nitride; the metal layer is preferably selected from the group consisting of aluminum, titanium, tantalum, tungsten, niobium, molybdenum, and copper; and the stop layer 66 preferably contains an oxide such as tetraethyl orthosilicate (TEOS), but is not limited thereto.
[0060] Please refer to the following at the same time: Figure 7 and Figure 8 , Figure 7 and Figure 8 According to an embodiment of the present invention Figures 1 to 7 A schematic diagram of the structure of a semiconductor device fabricated using the manufacturing process, wherein... Figure 8 The right half is a top view of the semiconductor device. Figure 8 The left half is a cross-sectional view showing the fabrication of a semiconductor device along the Y1 and Y2 directions in the right half. It should be noted that, for the sake of simplicity, Figure 8 The gate structure 26 along the Y2 direction preferably omits some components in the metal gate 70, such as the high dielectric constant dielectric layer 62, the work function metal layer 64, the low impedance metal layer 66, and the hard mask 68.
[0061] like Figure 7 and Figure 8As shown, the semiconductor device mainly includes a shallow trench isolation 22 surrounding the PMOS region 14 and the MMOS region 16, gate structures 24, 26, and 28 extending from the PMOS region 14 to the NMOS region 16, an epitaxial layer 38 disposed beside the gate structures 24, 26, and 28 of the PMOS region 14, an epitaxial layer 40 disposed beside the gate structures 24, 26, and 28 of the NMOS region 16, a trench 44 disposed within the shallow trench isolation 22 between the epitaxial layer 38 and the epitaxial layer 40, a contact plug 72 disposed on one side of the gate structure 26 of the PMOS region 14, a contact plug 74 disposed on one side of the gate structure 26 of the MMOS region 16, and a contact plug 76 disposed on the other side of the gate structure 26 and extending from the PMOS region 14 to the NMOS region 16.
[0062] from Figure 7 upper half or Figure 8 From the top view of the right half, contact plugs 72 and 74 may have the same length, and the length of contact plug 72 or contact plug 74 is less than the length of contact plug 76. From the cross-section in the Y1 direction, the epitaxial layers 38 and 40 have a height Y1a, the flat surface 46 of the trench 44 of the shallow trench isolation 22 to the top surface of the fin structure 20 or the bottom surface of the epitaxial layers 38 and 40 has a height Y1b, the bottom surface of the shallow trench isolation 22 to the flat surface 46 of the trench 44 includes a height Y1c, and the bottom of the contact plug 76 includes a protrusion 80 located directly above the trench 44, wherein the bottom surface of the protrusion 80 has the same contour as the trench 44. In this embodiment, Y1a is preferably between 400 and 500 angstroms or more preferably about 450 angstroms, Y1b is preferably between 200 and 300 angstroms or more preferably about 250 angstroms, and Y1c is preferably between 450 and 550 angstroms or more preferably about 500 angstroms. The width of the bottom surface of the protrusion 80 at the bottom of the contact plug 76 is preferably one, two, three, four, or even five times greater than the width of each epitaxial layer 38 and 40. These are all within the scope of this invention.
[0063] Furthermore, looking at the cross-section along the Y2 direction, the bottom surface of the gate structure 26 directly above the shallow trench isolation 22 between the PMOS region 14 and the NMOS region 16 also includes a protrusion 82. The surface of the substrate 12 on both sides of the protrusion 82 to the top surface of the fin structure 20 has a height Y2a. The overall depth of the protrusion 82 or the depth from the bottom surface of the protrusion 82 to the surface of the shallow trench isolation 22 on both sides of the protrusion has a height Y2b. The depth from the bottom surface of the shallow trench isolation 22 to the flat surface 46 of the protrusion 82 or the trench 44 includes a height Y2c. In this embodiment, Y2a is preferably between 400 and 500 angstroms or more preferably about 450 angstroms, Y2b is preferably between 50 and 150 angstroms or more preferably about 100 angstroms, and Y2c is preferably between 600 and 700 angstroms or more preferably about 650 angstroms. Similar to the protrusion 80 at the bottom of the contact plug 76, the bottom surface width of the protrusion 82 at the bottom of the gate structure 26 or the metal gate 70 is preferably one, two, three, four, five, or even ten times greater than the width of each epitaxial layer 38, 40 or fin structure 20, all of which fall within the scope of this invention.
[0064] Please continue to refer to Figure 9 , Figure 9 According to an embodiment of the present invention Figures 1 to 7 A schematic diagram of the structure of a semiconductor device fabricated using the manufacturing process, wherein... Figure 9 The upper half is a top view of a semiconductor device fabricated according to an embodiment of the present invention. Figure 9 The lower half is a cross-sectional view showing the semiconductor device fabricated along the X3 and Y directions of the upper half. For example... Figure 9 As shown, compared to the previous embodiment where the bottom of the contact plug 76 extending from the PMOS region 14 to the NMOS region 16 directly contacts the contact hole etch stop layer 54, the present invention can also retain part of the interlayer dielectric layer 56 in the trench 44 during the preparation of the contact plug 76 and make the top surface of the interlayer dielectric layer 56 approximately flush with the surfaces of the substrate 12 on both sides. In this way, after the contact plug 76 is formed, the contact plug 76 can be suspended between the two gate structures 26 and 28 as shown in the X3 direction, and the bottom surface and two sidewalls of the contact plug 76 are surrounded by the interlayer dielectric layer 56, or it can be as shown in the Y direction, with its bottom contacting the interlayer dielectric layer 56 and the contact hole etch stop layer 54. These are all within the scope of the present invention.
[0065] In summary, this invention primarily involves first forming a gate structure in the PMOS and NMOS regions, then forming a patterned mask covering most of the area between the PMOS region 14 and the NMOS region 16. Next, the patterned mask is used to remove portions of the substrate on both sides of the gate structure, forming grooves, and simultaneously forming trenches 44 on the shallow trench isolation 22 between the PMOS region 14 and the NMOS region 16. Subsequently, epitaxial growth processes are used to form epitaxial layers 40 in the PMOS region 14 and the NMOS region 16, respectively. According to a preferred embodiment of this invention, the trenches formed at the boundary between the two transistors using this method can have a lower depth, thereby improving the overall process window and preventing the subsequently formed metal interconnects from being too close to the substrate and affecting the overall device performance.
[0066] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made in accordance with the claims of the present invention should be included within the scope of the present invention.
Claims
1. A method for manufacturing a semiconductor device, characterized in that, Include: The substrate includes a first transistor region and a second transistor region; A shallow trench is formed to isolate the first transistor region and the second transistor region; A gate structure is formed that extends from the first transistor region to the second transistor region; A first epitaxial layer is formed next to the gate structure of the first transistor region, and a second epitaxial layer is formed next to the gate structure of the second transistor region; as well as A trench is formed within the shallow trench isolation between the first epitaxial layer and the second epitaxial layer.
2. The method of claim 1, further comprising: A first groove is formed next to the gate structure of the first transistor region and a second groove is formed next to the gate structure of the second transistor region; The first epitaxial layer is formed in the first groove and the second epitaxial layer is formed in the second groove; An interlayer dielectric layer is formed around the gate structure; and The gate structure is converted into a metal gate by a metal gate replacement fabrication process.
3. The method of claim 2, further comprising: A first contact plug is formed on the metal gate side of the first transistor region; A second contact plug is formed on the metal gate side of the second transistor region; and A third contact plug is formed on the other side of the metal gate and extends from the first transistor region to the second transistor region.
4. The method of claim 3, wherein the bottom surface of the third contact plug includes a protrusion located directly above the groove.
5. The method of claim 3, wherein the length of the first contact plug is less than the length of the third contact plug.
6. The method of claim 1, wherein the trench depth is less than the height of the first epitaxial layer.
7. A semiconductor element, characterized in that, Include: The substrate includes a first transistor region and a second transistor region; Shallow trench isolation surrounds the first transistor region and the second transistor region; A gate structure extends from the first transistor region to the second transistor region; A first epitaxial layer is disposed next to the gate structure of the first transistor region; A second epitaxial layer is disposed adjacent to the gate structure of the second transistor region; and A trench is provided within the shallow trench isolation between the first epitaxial layer and the second epitaxial layer.
8. The semiconductor element of claim 7, further comprising: A first contact plug is disposed on the metal gate side of the first transistor region; A second contact plug is disposed on the metal gate side of the second transistor region; and The third contact plug is located on the other side of the metal gate and extends from the first transistor region to the second transistor region.
9. The semiconductor element of claim 8, wherein the bottom surface of the third contact plug includes a protrusion located directly above the trench.
10. The semiconductor element of claim 8, wherein the length of the first contact plug is less than the length of the third contact plug.
11. The semiconductor device of claim 7, wherein the trench depth is less than the height of the first epitaxial layer.
12. A semiconductor element, characterized in that, Include: The substrate includes a first transistor region and a second transistor region; Shallow trench isolation surrounds the first transistor region and the second transistor region; as well as A gate structure extending from the first transistor region to the second transistor region, wherein the bottom surface of the gate structure directly above the shallow trench isolation between the first transistor region and the second transistor region includes a protrusion.
13. The semiconductor element of claim 12, further comprising: A first fin junction is disposed in the first transistor region; A second fin-shaped junction is disposed in the second transistor region; and The gate structure is disposed on the first fin structure and the second fin structure.
14. The semiconductor element of claim 13, wherein the protrusion is disposed between the first fin structure and the second fin structure.
15. The semiconductor device of claim 12, further comprising a trench disposed within a shallow trench isolation between the first transistor region and the second transistor region.
16. The semiconductor element of claim 15, wherein the protrusion is located directly above the trench.
17. The semiconductor device of claim 12, wherein the gate structure comprises a metal gate.