A metal separator process for fabricating Micro-LED modules
The rotary wet etching process solved the problem of uneven etching caused by immersion etching, enabling stable production of large-size wafers and improving the production efficiency and yield of Micro-LED modules.
Patent Information
- Application Number
- CN202611343354.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-10
AI Technical Summary
In the existing Micro-LED module manufacturing process, the immersion wet etching process causes a difference in the renewal rate of the etching solution between the center and the edge of the wafer, resulting in uneven etching and lateral drilling problems, which makes it difficult to meet the production needs of large-size wafers.
The rotary wet etching process applies wet etching solution to the surface of the wafer during its rotation. Forced convection accelerates the renewal of the etching solution, ensuring the uniformity of the etching solution on the wafer surface. It is suitable for both small and large wafers.
It improves corrosion uniformity and process stability, making it suitable for large-size wafer production and enhancing the production efficiency and yield of Micro-LED modules.
Smart Images

Figure CN123076084A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor light-emitting device fabrication technology, and in particular to a metal separator process for fabricating Micro-LED modules. Background Technology
[0002] Micro-LED (micro-light-emitting diode) display technology is a novel display technology that integrates micron-scale LED light-emitting pixels onto a driving substrate. It boasts advantages such as self-illumination, high brightness, high contrast, high refresh rate, low power consumption, and long lifespan, and is widely considered one of the next-generation mainstream display technologies. In the fabrication process of Micro-LED modules, a mainstream technical route involves first growing an epitaxial layer on a substrate, then bonding the epitaxial layer to the driving substrate. After substrate removal, the epitaxial layer is patterned to form Micro-LED light-emitting pixels. To achieve independent driving of each Micro-LED pixel, the metal bonding layer must be isolated (i.e., metal etching). Current metal etching processes mainly include dry etching and wet etching. While dry etching is widely used, it suffers from drawbacks such as complex processes (requiring passivation layer deposition, photolithography, etc.), high costs (requiring high-precision equipment), and susceptibility to metal sputtering leading to pixel sidewall leakage, severely impacting yield and performance.
[0003] In contrast, while wet etching avoids the complexities of dry processes, it also has significant limitations. Conventional wet etching is prone to lateral drilling, making it difficult to control pixel size accuracy and resulting in poor etching uniformity. To address these issues, our research group proposed a self-aligned wet metal isolation process in a previously filed Chinese invention patent (publication number: CN120166827A). This process accelerates etching and prevents lateral drilling by controlling the metal layer thickness within a relatively thin range (20nm–120nm) and utilizing the porous structure and ultra-thin characteristics of the metal layer formed after epitaxial layer patterning.
[0004] However, subsequent research revealed the following shortcomings in the practical application of the technical solution disclosed in CN120166827A: Firstly, the improvement in corrosion uniformity relies on the porous structure formed after the metal layer is patterned in the epitaxial layer. For local areas in the metal layer where a porous structure is not formed, slow corrosion rates, uneven corrosion, and severe lateral drilling still occur, making it difficult to guarantee process stability. Secondly, this process employs conventional immersion wet etching. During immersion, due to the hydrodynamic characteristics of the etching solution, the renewal rate of the etching solution in the wafer edge region is higher than that in the center region, resulting in a faster corrosion rate in the edge region and poor corrosion uniformity on the wafer surface. Especially with the increase in wafer size, the difference in fluid exchange between the wafer center and edge further intensifies, leading to more significant uneven corrosion within the wafer. This size effect severely limits the production stability of the process, making it currently mainly suitable for small-sized wafers such as 2-inch wafers, and unable to meet the needs of the Micro-LED industry's development towards larger wafer sizes. Summary of the Invention
[0005] In view of this, the purpose of the present invention is to provide a metal separator process for preparing Micro-LED modules, so as to solve the problem of immersion wet etching in the prior art.
[0006] To achieve the above objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides a metal separator process for fabricating Micro-LED modules, comprising the following steps: S1. Provide a wafer, the wafer including a substrate and an epitaxial layer grown on the substrate; S2. Deposit a metal bonding layer across the entire surface of the epitaxial layer; S3. Provide a driving substrate and fabricate an array of metal bonding units on the driving substrate; S4. Bond the metal bonding layer to the metal bonding unit; S5, Remove substrate; S6. Pattern the epitaxial layer to divide it into multiple independent mesa arranged in an array, each mesa forming a Micro-LED light-emitting pixel; each Micro-LED light-emitting pixel corresponds to a metal bonding unit, and the area between adjacent Micro-LED light-emitting pixels exposes the metal bonding layer. S7. Rotate the wafer and apply a wet etching solution to the wafer surface during the wafer rotation process. The wet etching solution has high selectivity for the metal bonding layer relative to the epitaxial layer. It is used to remove the metal bonding layer between adjacent Micro-LED light-emitting pixels by wet etching, while retaining the Micro-LED light-emitting pixels, thereby achieving metal separation between adjacent Micro-LED light-emitting pixels.
[0007] The metal separation process for fabricating Micro-LED modules provided by this invention applies a wet etching solution to the wafer surface during wafer rotation. Forced convection accelerates the renewal and removal of the wet etching solution on the wafer surface, effectively overcoming the difference in etching solution renewal rate between the wafer edge and center caused by hydrodynamic characteristics in existing immersion wet etching processes. This results in a more uniform etching rate across the entire wafer surface. This improvement fundamentally enhances etching uniformity, ensuring consistent etching rates even in areas where the metal bonding layer lacks a porous structure. It avoids lateral drilling and uneven etching problems caused by localized lack of pores, thus improving process stability. Furthermore, the rotary wet etching method of this invention eliminates the uniformity degradation problem caused by size effects, is no longer limited by wafer size, and is suitable not only for small wafers but also for large wafers (2 inches and above), thereby improving the production efficiency and yield of Micro-LED modules.
[0008] Optionally, the wafer is rotated by a developing unit fixed to the spin coater; the wafer rotation speed range is 30 rpm to 150 rpm.
[0009] Optionally, the wet etching solution is applied to the wafer surface by spraying, and the spraying is achieved by the spraying robotic arm of the spin coater.
[0010] Optionally, the thickness of the metal bonding layer ranges from 20 nm to 100 nm.
[0011] Optionally, the epitaxial layer is a GaN-based epitaxial layer; the metal bonding layer is gold, a gold-containing alloy, or a metal stack with gold as the outermost layer.
[0012] Optionally, the metal bonding layer is a Ni / Au stack, wherein the thickness of Ni is 0.1nm to 0.5nm and the thickness of Au is 20nm to 60nm.
[0013] Optionally, the wet etching solution is an iodine-potassium iodide aqueous solution, wherein the mass ratio of iodine to potassium iodide is 1:(2-40).
[0014] Optionally, the temperature of the wet etching solution is 15℃~40℃, and the wet etching time in step S7 is 20s~300s.
[0015] Optionally, step S7 is followed by step S8: detecting the electrical connection status between adjacent Micro-LED light-emitting pixels to confirm that a metal separation is achieved between adjacent Micro-LED light-emitting pixels.
[0016] Secondly, the present invention also provides a Micro-LED module, which is manufactured using the metal separator process described above for preparing Micro-LED modules.
[0017] Additional aspects and advantages of the invention will be set forth in part in the description which follows, some of which will become clear as the description proceeds, and others will be learned by practicing the invention. Attached Figure Description
[0018] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments are briefly introduced below: Figure 1 This is a schematic diagram of the cross-sectional structure of a wafer provided in an embodiment of the present invention.
[0019] Figure 2 This is a schematic cross-sectional view of the metal bonding layer after it has been prepared in an embodiment of the present invention.
[0020] Figure 3 This is a schematic cross-sectional view of the structure after metal bonding units are fabricated on the driving substrate in an embodiment of the present invention.
[0021] Figure 4 This is a schematic cross-sectional view of the wafer and the driving substrate after bonding in an embodiment of the present invention.
[0022] Figure 5 This is a schematic cross-sectional view of the structure after removing the substrate in an embodiment of the present invention.
[0023] Figure 6 This is a schematic cross-sectional view of the epitaxial layer after patterning and etching in an embodiment of the present invention.
[0024] Figure 7 This is a schematic cross-sectional view of the metal partition after it has been completed in an embodiment of the present invention.
[0025] Figure 8 This is a schematic diagram of the wafer surface morphology after the metal partition is completed in an embodiment of the present invention.
[0026] Figure 9 This is a schematic diagram of the uneven surface morphology of the wafer edge region and the middle region after the metal partitioning is completed in Comparative Example 1.
[0027] Figure 10 This is a schematic diagram of the surface morphology of the light-emitting pixels connected due to photoresist residue at the "hole" after the metal partition was completed in Comparative Example 2.
[0028] In the figure: 100-substrate, 101-epitaxy layer, 102-metal bonding layer; 200-driving substrate, 201-top metal, 202-metal bonding unit. Detailed Implementation
[0029] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0030] This application provides a metal separator process for fabricating Micro-LED modules, such as... Figures 1-7 As shown, it includes the following steps: S1. A wafer is provided, the wafer including a substrate 100 and an epitaxial layer 101 grown on the substrate 100; S2. Deposit a metal bonding layer 102 over the entire surface of the epitaxial layer 101; S3. Provide a driving substrate 200, and fabricate an array of metal bonding units 202 on the driving substrate 200; S4. Bond the metal bonding layer 102 to the metal bonding unit 202; S5, Remove substrate 100; S6. Pattern etching is performed on the epitaxial layer 101 to divide the epitaxial layer 101 into multiple independent mesa arranged in an array, each mesa forming a Micro-LED light-emitting pixel; the Micro-LED light-emitting pixels correspond one-to-one with the metal bonding units 202, and the area between adjacent Micro-LED light-emitting pixels exposes the metal bonding layer 102. S7. Rotate the wafer and apply a wet etching solution to the wafer surface during the wafer rotation process. The wet etching solution has high selectivity for the metal bonding layer 102 relative to the epitaxial layer 101. It is used to remove the metal bonding layer 102 between adjacent Micro-LED light-emitting pixels by wet etching, while retaining the Micro-LED light-emitting pixels, thereby achieving metal separation between adjacent Micro-LED light-emitting pixels.
[0031] In one embodiment, the wafer is rotated via a developing unit fixed to a spin coater; the wafer rotation speed ranges from 30 rpm to 150 rpm. It should be noted that wafer rotation can be achieved using a spin coater commonly used in semiconductor manufacturing processes without adding additional equipment. By limiting the wafer rotation speed within the aforementioned range, the renewal and removal rate of the wet etching solution on the wafer surface can be controlled, thereby achieving uniform etching. If the rotation speed is less than 30 rpm, the wet etching solution renewal rate is inconsistent between the wafer edge and center, making uniform etching difficult to achieve; if the rotation speed is greater than 150 rpm, most of the wet etching solution will be rapidly ejected from the wafer surface, affecting the etching rate.
[0032] In one embodiment, the wet etching solution is applied to the wafer surface by spraying, which is achieved by the spraying robotic arm of the spin coater. It should be noted that using the spraying method can achieve uniform distribution of the wet etching solution on the wafer surface for wafers of various sizes. Furthermore, spraying and rotation can be achieved through different components of the same spin coater, without incurring additional costs.
[0033] In one embodiment, the thickness of the metal bonding layer 102 ranges from 20 nm to 100 nm. It should be noted that, due to the small size of Micro-LED light-emitting pixels and the small spacing between them, controlling the thickness of the metal bonding layer within the aforementioned range allows for controllable corrosion of the metal bonding layer.
[0034] In one embodiment, the epitaxial layer 101 is a GaN-based epitaxial layer; the metal bonding layer 102 is gold, a gold-containing alloy, or a metal stack with gold as the outermost layer. It should be noted that the gold-containing metal can be wet-etched using a gold etchant. The gold etchant hardly corrodes the GaN material, only etching the exposed metal bonding layer between the Micro-LED light-emitting pixels. The etched area is naturally self-aligned with the pixel area, eliminating the need for additional mask preparation or alignment, and allowing for a large process tolerance.
[0035] In one embodiment, the metal bonding layer 102 is a Ni / Au stack, wherein the thickness of Ni is 0.1 nm to 0.5 nm, and the thickness of Au is 20 nm to 60 nm. It should be noted that if the thickness of Au is less than 20 nm, continuous film formation is not possible; if the thickness of Au is greater than 60 nm, lateral etching can easily cause the GaN light-emitting pixels to detach.
[0036] In one embodiment, the wet etching solution is an iodine-potassium iodide aqueous solution, wherein the mass ratio of iodine to potassium iodide is 1:(2-40). It should be noted that the iodine-potassium iodide aqueous solution is a preferred gold etching solution, and controlling the mass ratio of iodine to potassium iodide within the above range can achieve uniform etching of the metal bonding layer.
[0037] In one embodiment, the temperature of the wet etching solution is 15℃~40℃, and the wet etching time in step S7 is 20s~300s. It should be noted that if the wet etching time is less than 20s, the time is too short and the metal bonding layer in some areas of the wafer will not be cleanly etched, and uniform etching cannot be achieved; if the wet etching time is greater than 300s, lateral etching will be severe, and the phenomenon of GaN light-emitting pixels falling off is likely to occur.
[0038] In one embodiment, step S7 is followed by step S8: detecting the electrical connection status between adjacent Micro-LED light-emitting pixels to confirm that a metallic barrier is achieved between adjacent Micro-LED light-emitting pixels. It should be noted that the complete isolation of the metallic bonding layer between adjacent light-emitting pixels is observed using an optical microscope or a scanning electron microscope.
[0039] This application also provides a Micro-LED module, which is manufactured using the metal separator process described above for preparing Micro-LED modules.
[0040] The following are some embodiments of this application, and the embodiments of the present invention will further describe the technical solution of the present invention in detail. Example 1
[0041] This embodiment provides a metal separator process for fabricating Micro-LED modules, including the following steps: Step S1: Provide the wafer. Please refer to [link / reference]. Figure 1 The wafer includes a substrate 100 and an epitaxial layer 101 grown on the substrate 100.
[0042] Specifically, a substrate 100 is provided, and an N-type layer, a multi-quantum-well light-emitting layer, and a P-type layer are sequentially grown on the substrate 100 using a metal-organic chemical vapor deposition (MOCVD) process. The substrate 100 is a silicon substrate, the N-type layer is an N-type GaN layer, the multi-quantum-well light-emitting layer is an InGaN / GaN multi-quantum-well structure, and the P-type layer is a P-type GaN layer. The N-type layer, the multi-quantum-well light-emitting layer, and the P-type layer form a transparent epitaxial layer.
[0043] Step S2: Deposit a metal bonding layer 102 over the entire surface of the epitaxial layer 101. (See [link to previous step]). Figure 2 .
[0044] Specifically, an electron beam evaporation process is used to deposit a 0.2 nm thick Ni and a 30 nm thick Au layer on the entire surface of the epitaxial layer 101, forming a Ni / Au stack. Due to the material and ultra-thin characteristics of the Ni / Au stack, the prepared metal bonding layer 102 is semi-transparent, which not only meets the requirements of subsequent wafer bonding but also has light transmittance, so it does not affect subsequent photolithography alignment.
[0045] Step S3: Provide a driving substrate 200, and fabricate an array of metal bonding units 202 on the driving substrate 200. Please refer to [link to relevant documentation]. Figure 3 .
[0046] Specifically, the driving substrate 200 is a CMOS driving substrate, on which an array of top metal 201 is provided. Metal bonding units 202 and photolithographic alignment marks are fabricated on the surface of the top metal 201. The metal bonding units 202 and the top metal 201 correspond one-to-one, and the material of the metal bonding units 202 is Au or AuSn alloy.
[0047] Step S4: Bond the metal bonding layer 102 to the metal bonding unit 202. Please refer to [link / reference]. Figure 4 .
[0048] Specifically, the wafer is thermo-bonded to the metal bonding unit 202 on the driving substrate 200 through the metal bonding layer 102. The bonding temperature is 180℃~360℃, the bonding pressure is 8MPa~20MPa, and the bonding time is 10min~60min.
[0049] Step S5, Remove substrate 100, please refer to Figure 5 .
[0050] Specifically, the substrate 100 (silicon substrate) is removed using a mechanical polishing and dry etching process, and the exposed epitaxial layer 101 surface is cleaned.
[0051] Step S6: Pattern the epitaxial layer 101 by etching to divide it into multiple independent mesa arranged in an array. Each mesa constitutes a Micro-LED light-emitting pixel. Please refer to [link to relevant documentation]. Figure 6 .
[0052] Specifically, a pixel pattern mask period is formed on the surface of the epitaxial layer 101 using photolithography. The epitaxial layer 101 is then etched using a phosphoric acid (H3PO4) wet etching process, with the etching depth penetrating the epitaxial layer 101 and stopping at the surface of the metal bonding layer 102. This divides the epitaxial layer 101 into multiple independent mesa arranged in an array, each mesa constituting a Micro-LED light-emitting pixel. Each Micro-LED light-emitting pixel corresponds one-to-one with a metal bonding unit 202. The Micro-LED light-emitting pixels are isolated from each other. The size of each Micro-LED light-emitting pixel is 0.5μm × 0.5μm, and the period between adjacent Micro-LED light-emitting pixels (i.e., the center-to-center distance between adjacent Micro-LED light-emitting pixels) is 1.5μm. The area between adjacent Micro-LED light-emitting pixels exposes the metal bonding layer 102. It should be noted that the wet etching in this step is only used to etch the epitaxial layer to form Micro-LED light-emitting pixels, and the photolithographic mask is formed on an epitaxial layer with a thickness on the micrometer scale and a continuously flat surface.
[0053] Step S7: Rotate the wafer. During wafer rotation, apply a wet etching solution to the wafer surface. The wet etching solution removes the metal bonding layer 102 between adjacent Micro-LED light-emitting pixels while retaining the Micro-LED light-emitting pixels, thus achieving metal separation between adjacent Micro-LED light-emitting pixels. Please refer to [link to relevant documentation]. Figure 7 .
[0054] Specifically, a gold etching solution (I2-KI aqueous solution) was prepared as a wet etching solution, with an I2:KI:water ratio of 6g:120g:1L. The wafer, after completing step S6, was fixed in the rotating chuck of a spin coater and rotated at 120 rpm. Simultaneously, during wafer rotation, an I2-KI gold etching solution was sprayed onto the wafer surface via a spraying robotic arm. Under the rotational action, the I2-KI gold etching solution was evenly distributed on the wafer surface. The I2-KI gold etching solution only etches away the metal bonding layer 102 between adjacent Micro-LED light-emitting pixels, with minimal corrosion of the GaN material (Micro-LED light-emitting pixels). Therefore, the metal bonding layer 102 between adjacent Micro-LED light-emitting pixels was removed, while the Micro-LED light-emitting pixels were retained, achieving metal separation between adjacent Micro-LED light-emitting pixels. The etching time was 30 seconds, and the temperature of the sprayed I2-KI gold etching solution was 23°C. After etching, the process switches to spraying deionized water to clean the wafer, and finally the rotation speed is increased to 2000 rpm for spin drying. Rotary wet etching accelerates the renewal and discharge of the etching solution through centrifugal force, resulting in better etching uniformity. Furthermore, etching, cleaning, and drying can be completed continuously in the same equipment, further shortening the process time.
[0055] Step S8: Observe under an optical microscope the lack of connection in the metal bonding layer 102 between adjacent Micro-LED light-emitting pixels to confirm that there is no electrical conduction between adjacent GaN light-emitting pixels, thus completing the metal separation. Please refer to... Figure 8 Upon full inspection with an optical microscope, no metal connection was found between adjacent GaN light-emitting pixels in the Micro-LED display module prepared in this embodiment. Example 2
[0056] This embodiment provides a metal separator process for fabricating Micro-LED modules. Compared with Embodiment 1, the Micro-LED light-emitting pixels in this embodiment have larger sizes and larger spacing between adjacent Micro-LED light-emitting pixels, and include the following steps: Step S1: Provide the wafer. Please refer to [link / reference]. Figure 1 The wafer includes a substrate 100 and an epitaxial layer 101 grown on the substrate 100.
[0057] Specifically, a substrate 100 is provided, and an N-type layer, a multi-quantum-well light-emitting layer, and a P-type layer are sequentially grown on the substrate 100 using a metal-organic chemical vapor deposition (MOCVD) process. The substrate 100 is a silicon substrate, the N-type layer is an N-type GaN layer, the multi-quantum-well light-emitting layer is an InGaN / GaN multi-quantum-well structure, and the P-type layer is a P-type GaN layer. The N-type layer, the multi-quantum-well light-emitting layer, and the P-type layer form a transparent epitaxial layer.
[0058] Step S2: Deposit a metal bonding layer 102 over the entire surface of the epitaxial layer 101. (See [link to previous step]). Figure 2 .
[0059] Specifically, an electron beam evaporation process is used to deposit a 0.5 nm thick Ni and a 50 nm thick Au layer on the entire surface of the epitaxial layer 101, forming a Ni / Au stack. Due to the material and ultra-thin characteristics of the Ni / Au stack, the prepared metal bonding layer 102 is semi-transparent, which not only meets the requirements of subsequent wafer bonding but also has light transmittance, so it does not affect subsequent photolithography alignment.
[0060] Step S3: Provide a driving substrate 200, and fabricate an array of metal bonding units 202 on the driving substrate 200. Please refer to [link to relevant documentation]. Figure 3 .
[0061] Specifically, the driving substrate 200 is a CMOS driving substrate, on which an array of top metal 201 is provided. Metal bonding units 202 and photolithographic alignment marks are fabricated on the surface of the top metal 201. The metal bonding units 202 and the top metal 201 correspond one-to-one, and the material of the metal bonding units 202 is Au or AuSn alloy.
[0062] Step S4: Bond the metal bonding layer 102 to the metal bonding unit 202. Please refer to [link / reference]. Figure 4 .
[0063] Specifically, the wafer is thermo-bonded to the metal bonding unit 202 on the driving substrate 200 through the metal bonding layer 102. The bonding temperature is 180℃~360℃, the bonding pressure is 8MPa~20MPa, and the bonding time is 10min~60min.
[0064] Step S5, Remove substrate 100, please refer to Figure 5 .
[0065] Specifically, the substrate 100 (silicon substrate) is removed using a mechanical polishing and dry etching process, and the exposed epitaxial layer 101 surface is cleaned.
[0066] Step S6: Pattern the epitaxial layer 101 by etching to divide it into multiple independent mesa arranged in an array. Each mesa constitutes a Micro-LED light-emitting pixel. Please refer to [link to relevant documentation]. Figure 6 .
[0067] Specifically, a pixel pattern mask is formed on the surface of the epitaxial layer 101 using photolithography. The epitaxial layer 101 is then etched using a phosphoric acid (H3PO4) wet etching process, with the etching depth penetrating the epitaxial layer 101 and stopping at the surface of the metal bonding layer 102. This divides the epitaxial layer 101 into multiple independent mesas arranged in an array, each mesas constituting a Micro-LED light-emitting pixel. Each Micro-LED light-emitting pixel corresponds one-to-one with a metal bonding unit 202. The Micro-LED light-emitting pixels are isolated from each other, with a size of 1μm × 1μm and a period of 4μm between adjacent Micro-LED light-emitting pixels. The area between adjacent Micro-LED light-emitting pixels exposes the metal bonding layer 102. It should be noted that the wet etching in this step is only used to etch the epitaxial layer to form the Micro-LED light-emitting pixels, and the photolithographic mask is formed on an epitaxial layer with a thickness on the micrometer scale and a continuously flat surface.
[0068] Step S7: Rotate the wafer. During wafer rotation, apply a wet etching solution to the wafer surface. The wet etching solution removes the metal bonding layer 102 between adjacent Micro-LED light-emitting pixels while retaining the Micro-LED light-emitting pixels, thus achieving metal separation between adjacent Micro-LED light-emitting pixels. Please refer to [link to relevant documentation]. Figure 7 .
[0069] Specifically, a gold etching solution (I2-KI aqueous solution) was prepared as a wet etching solution, with an I2:KI:water ratio of 6g:120g:10L. The wafer, after completing step S6, was fixed in the rotating chuck of a spin coater and rotated at 120 rpm. Simultaneously, during wafer rotation, an I2-KI gold etching solution was sprayed onto the wafer surface via a spraying robotic arm. Under the rotational action, the I2-KI gold etching solution was evenly distributed on the wafer surface. The I2-KI gold etching solution only etches away the metal bonding layer 102 between adjacent Micro-LED light-emitting pixels, with minimal corrosion of the GaN material (Micro-LED light-emitting pixels). Therefore, the metal bonding layer 102 between adjacent Micro-LED light-emitting pixels was removed, while the Micro-LED light-emitting pixels were retained, achieving metal separation between adjacent Micro-LED light-emitting pixels. The etching time was 200 s, and the temperature of the sprayed I2-KI gold etching solution was 23°C. After etching, the process switches to spraying deionized water to clean the wafer, and finally the rotation speed is increased to 2000 rpm for spin drying. Rotary wet etching accelerates the renewal and discharge of the etching solution through centrifugal force, resulting in better etching uniformity. Furthermore, etching, cleaning, and drying can be completed continuously in the same equipment, further shortening the process time.
[0070] Step S8: Observe under an optical microscope to check for any connection in the metal bonding layer 102 between adjacent Micro-LED light-emitting pixels, confirming that there is no electrical conduction between adjacent GaN light-emitting pixels, and that the metal separation is complete. A full inspection under an optical microscope also showed no metal connections between adjacent GaN light-emitting pixels in the Micro-LED display module prepared in this embodiment. Comparative Example 1
[0071] Please combine Figures 1 to 6 as well as Figure 9 This comparative example uses the same steps S1 to S6 as in Example 1, except that step S7 is changed to an immersion wet etching route: the wafer after step S6 is immersed in a gold etching solution and etched at 23°C for 100 seconds. Using Micro-LED light-emitting pixels as a mask, the exposed metal bonding layer 102 between adjacent Micro-LED light-emitting pixels is completely etched away. The wafer is then removed, rinsed with deionized water for 5 minutes, and then dried with nitrogen. Figure 9 As shown, in immersion wet etching, the etchant renewal rate in the wafer edge region is higher than that in the middle region, resulting in a faster etching rate in the edge region than in the middle region. This occurs when the metal bonding layer in the wafer edge region has been completely etched away. Figure 9 (Right image) The metal bonding layer in the center region of the wafer has not been completely etched. Figure 9 (See left image) This results in uneven etching across the entire wafer, making it difficult to guarantee production stability. Comparative Example 2
[0072] Please combine Figures 1 to 6 as well as Figure 10 This comparative example uses the same steps S1 to S6 as in Example 1, except that step S7 is changed to a photolithography + plasma dry etching route: Photoresist is spin-coated onto the wafer surface. Because the metal bonding layer 102, with a thickness of only 30.2 nm, is prone to random "holes" during the aforementioned process, the "hole" areas exhibit abnormal resist uniformity (too thick resist or voids). After exposure and development, photoresist remains in these areas. This residual, non-removable photoresist blocks the underlying metal bonding layer 102 during plasma etching. After etching and resist removal, the remaining metal bonding layer 102 in these areas is as follows: Figure 10 As shown, this causes adjacent Micro-LED light-emitting pixels to connect, resulting in a display defect where adjacent Micro-LED light-emitting pixels light up simultaneously during the lighting test.
[0073] As can be seen from the comparison of Examples 1, 2, 1, and 2, this invention uses a rotary wet etching process instead of an immersion wet etching process or a dry etching process to isolate the metal bonding layer, effectively improving the etching uniformity. This process does not involve a photolithography step, completely avoiding the pixel overlap problem caused by dry etching, and eliminating all processes such as photoresist coating, exposure, development, plasma etching, and resist removal in the isolation process. Furthermore, this invention does not rely on the metal bonding layer to form a porous structure and is applicable to semi-transparent metal bonding layers in the thickness range of 20nm to 60nm. It can cover both conventional pitch modules and ultra-small pitch modules with pixel periods of 0.1 to 10μm, greatly improving the wafer fabrication efficiency and yield.
[0074] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. For example, in addition to I2-KI aqueous solution, other etching solutions that are capable of corroding the metal bonding layer but not the epitaxial layer can be used in the wet etching process; the material, thickness, and spacing of the metal bonding units can be set according to the specifications of the driving substrate; the substrate can also be a silicon substrate, sapphire substrate, or other substrates suitable for epitaxial layer growth; the shape, size, and arrangement of the Micro-LED light-emitting pixels can be set according to the specifications of the display module. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
[0075] It should also be noted that, in this application, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that an article or device that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such an article or device. Without further limitations, an element defined by the phrase "comprising..." does not exclude the presence of other identical elements in an article or device that includes the aforementioned elements.
Claims
1. A metal separator process for fabricating Micro-LED modules, characterized in that, Includes the following steps: S1. A wafer is provided, the wafer comprising a substrate and an epitaxial layer grown on the substrate; S2. A metal bonding layer is deposited over the entire surface of the epitaxial layer; S3. Provide a driving substrate, and fabricate an array of metal bonding units on the driving substrate; S4. Bond the metal bonding layer to the metal bonding unit; S5. Remove the substrate; S6. The epitaxial layer is patterned and etched to divide the epitaxial layer into multiple independent mesa arranged in an array, each mesa constituting a Micro-LED light-emitting pixel; the Micro-LED light-emitting pixel corresponds one-to-one with the metal bonding unit, and the area between adjacent Micro-LED light-emitting pixels exposes the metal bonding layer. S7. Rotate the wafer and apply a wet etching solution to the surface of the wafer during the rotation process. The wet etching solution has high selectivity for the metal bonding layer relative to the epitaxial layer and is used to wet-etch away the metal bonding layer between adjacent Micro-LED light-emitting pixels while retaining the Micro-LED light-emitting pixels, thereby achieving metal separation between adjacent Micro-LED light-emitting pixels.
2. The metal separator process for fabricating Micro-LED modules according to claim 1, characterized in that: The wafer is rotated by a developing unit fixed to a spin coater; the rotation speed of the wafer is in the range of 30 rpm to 150 rpm.
3. The metal separator process for fabricating Micro-LED modules according to claim 1, characterized in that: The wet etching solution is applied to the wafer surface by spraying, and the spraying is achieved by the spraying robotic arm of the spin coater.
4. The metal separator process for fabricating Micro-LED modules according to claim 1, characterized in that: The thickness of the metal bonding layer ranges from 20 nm to 100 nm.
5. The metal separator process for fabricating Micro-LED modules according to claim 1, characterized in that: The epitaxial layer is a GaN-based epitaxial layer; the metal bonding layer is gold, a gold-containing alloy, or a metal stack with gold as the outermost layer.
6. The metal separator process for fabricating Micro-LED modules according to claim 5, characterized in that: The metal bonding layer is a Ni / Au stack, wherein the thickness of Ni is 0.1nm to 0.5nm and the thickness of Au is 20nm to 60nm.
7. The metal separator process for fabricating Micro-LED modules according to claim 5, characterized in that: The wet etching solution is an iodine-potassium iodide aqueous solution, wherein the mass ratio of iodine to potassium iodide is 1:(2-40).
8. The metal separator process for fabricating Micro-LED modules according to claim 7, characterized in that: The temperature of the wet etching solution is 15℃~40℃, and the wet etching time in step S7 is 20s~300s.
9. The metal separator process for fabricating Micro-LED modules according to claim 1, characterized in that, Step S7 is followed by step S8: detecting the electrical connection status between adjacent Micro-LED light-emitting pixels to confirm that the metal separation is achieved between adjacent Micro-LED light-emitting pixels.
10. A Micro-LED module, characterized in that, It is prepared using the metal separator process for preparing Micro-LED modules as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Self-alignment metal wet isolation process for ultra-small spacing GaN-based Micro LED module
CN120166827A