Glass through-hole encapsulation structure with high-fidelity ultrasonic penetration window and its preparation method

By employing techniques such as femtosecond laser modification, hydrofluoric acid etching, and partitioned mask electroplating of a three-layer composite glass substrate, a glass through-hole encapsulation structure for high-fidelity ultrasonic transmission windows was fabricated. This solved the performance and cost challenges of existing miniature ultrasonic sensor devices, enabling low-loss, high-fidelity transmission and large-scale mass production.

CN123076262APending Publication Date: 2026-11-10BEIJING ZIYIXIN INTEGRATED CIRCUIT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611235788.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing pMUT packaging technology cannot simultaneously achieve miniaturized vertical electrical interconnection, low-loss and high-fidelity ultrasonic transmission, and low-cost mass production, thus limiting the performance improvement and large-scale commercial application of miniature ultrasonic sensors.

Method used

Using a three-layer composite glass substrate, a glass through-hole encapsulation structure with a high-fidelity ultrasonic penetration window is prepared through femtosecond laser modification, hydrofluoric acid selective etching, partitioned mask electroplating, and nanoscale polishing technology. This ensures that there is no metal residue in the central penetration window area and reduces surface roughness. Encapsulation is achieved by combining low-temperature hybrid hot-pressing eutectic bonding.

Benefits of technology

It achieves low vertical transmission loss and no waveform distortion in ultrasound, improves the accuracy of ultrasound detection and the signal-to-noise ratio of imaging, and has high product yield and batch consistency, making it suitable for the large-scale mass production needs of consumer products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076262A_ABST
    Figure CN123076262A_ABST
Patent Text Reader

Abstract

This invention discloses a glass through-hole packaging structure and its fabrication method with a high-fidelity ultrasonic transmission window. It employs a three-layer composite glass substrate with a centrally located, metal-free ultrasonic transmission window that undergoes nanoscale mirror polishing. Metallized glass through-holes surround the central layer for vertical electrical interconnection. A pMUT chip is flip-chip bonded to the upper surface of the substrate, with its ultrasonic emission axis precisely aligned with the geometric center of the transmission window, forming a highly airtight ultrasonic transmission cavity. The fabrication method involves six major processes: femtosecond laser modification of the strike-free zone, hydrofluoric acid selective etching, partitioned mask electroplating, nanoscale mirror polishing, high-precision visual alignment, and low-temperature bonding, strictly achieving zero metal residue in the transmission window. This invention simultaneously satisfies the requirements of high-density vertical interconnection, low-loss, high-fidelity ultrasonic transmission, and high process reliability, effectively reducing mass production costs. It is widely applicable to the packaging needs of pMUT devices in scenarios such as micro-ultrasonic sensing and ultrasonic fingerprint recognition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor advanced packaging and microelectromechanical systems (MEMS) device packaging technology, specifically relating to a through-glass via (TGV) substrate packaging structure with ultrasonic transmission window and its preparation method. Background Technology

[0002] A piezoelectric micromachined ultrasonic transducer (pMUT) is a miniature MEMS device that uses the vibration of a piezoelectric thin film to transmit and receive ultrasonic waves. Compared to traditional capacitive ultrasonic transducers and bulk ultrasonic probes, it has advantages such as small size, low power consumption, and ease of monolithic integration, making it a core chip solution in the current field of miniature ultrasonic sensing. As miniature ultrasonic devices develop towards miniaturization, high precision, and low power consumption, the packaging structure needs to simultaneously meet multiple requirements such as high-density vertical electrical interconnection, low-loss and high-fidelity ultrasonic transmission, high process reliability, and low-cost mass production.

[0003] Currently, the mainstream packaging solutions for pMUTs are mainly divided into three categories: PCB substrate packaging, through-silicon via (TSV) packaging, and glass through-hole packaging. Each of these solutions has obvious technical shortcomings. 1. PCB substrate packaging: The substrate contains a copper foil wiring layer. The metal copper layer below the ultrasonic emission area will reflect ultrasonic waves significantly, causing signal attenuation and waveform distortion, making it impossible to achieve high-fidelity ultrasonic transmission. If the metal layer of the emission area is removed by opening a window, the acoustic impedance of the PCB resin substrate is poorly matched with air and piezoelectric chips, resulting in high ultrasonic interface loss and making it difficult to guarantee detection accuracy.

[0004] 2. TSV (Through Silicon Via) Packaging: Silicon substrates have extremely high absorption loss of ultrasonic waves, so an additional acoustic matching film must be attached, which increases the number of packaging layers and process costs; at the same time, the TSV processing flow is complex and the manufacturing cost per wafer is high, making it difficult to meet the large-scale mass production needs of consumer products.

[0005] 3. Existing glass through-hole packaging: Although it uses low-ultrasonic-loss glass as the substrate, its metallization process lacks zoned control. Metal wiring and through-hole metal layers easily extend into the ultrasonic transmission window area. Residual metal films and burrs in the window severely interfere with ultrasonic wave propagation. Furthermore, conventional glass surfaces only undergo ordinary grinding, resulting in high surface roughness and easily causing diffuse ultrasonic wave reflection, leading to waveform distortion. In addition, existing processes lack standardized zoned metallization procedures, making it difficult to ensure that the transmission window area is completely free of metal residue, resulting in low mass production yield and poor product consistency.

[0006] In summary, existing pMUT packaging technology cannot simultaneously achieve miniaturized vertical electrical interconnection, low-loss and high-fidelity ultrasonic transmission, and low-cost mass production, becoming a key technological bottleneck restricting the performance improvement and large-scale commercial application of miniature ultrasonic sensors. Summary of the Invention

[0007] The purpose of this invention is to provide a glass through-hole packaging structure with a high-fidelity ultrasonic transmission window and its preparation method. On the one hand, the structure design eliminates the interference of metal shielding and surface diffuse reflection on ultrasonic waves, achieving high-fidelity and low-loss ultrasonic transmission. On the other hand, the three-layer composite carrier improves the thermal reliability of the substrate, and the standardized partitioned preparation process enables low-cost mass production, solving the pain point that existing packaging solutions cannot simultaneously meet the requirements of performance, size and cost.

[0008] The objective of this invention is achieved through the following technical solution: A method for fabricating a glass through-hole encapsulation structure with a high-fidelity ultrasonic penetration window includes the following steps: S1. Femtosecond laser modification of holes in three-layer composite glass substrate: The central penetration window area of ​​the three-layer composite glass substrate is set as a program-restricted area. Femtosecond laser is used to modify the lattice of TGV points surrounding the central penetration window only. After modification, the substrate is cleaned and dried. S2, Hydrofluoric Acid Selective Etching to Form TGV: Hydrofluoric acid etching solution is used to etch the modified three-layer composite glass substrate, so that only the laser-modified area is etched to form through holes, while the original glass plane of the central penetrating window area is completely preserved. S3, TGV metallization partition mask electroplating: The central penetration window area is completely covered by a photolithographic mask, and a conductive metal layer is deposited only on the inner wall of the through hole and the upper and lower electrode pad areas of the substrate, so as to achieve zero metal residue in the central penetration window area. S4. Nanoscale precision mirror polishing of the penetration window area: All electrode pad areas are masked, and only the central penetration window area is polished with nanoscale mirror polishing to reduce surface roughness. S5, pMUT chip metal microbump high-precision visual alignment: visually align the metal microbumps of the pMUT chip with the electrode pads on the upper surface of the three-layer composite glass substrate, so that the ultrasonic emission axis of the pMUT chip is precisely aligned with the central penetration window area. S6. Low-temperature hybrid hot pressing / eutectic bonding completes the encapsulation and bonding: The metallurgical bonding of microbumps and electrode pads is achieved through a low-temperature bonding process, and a sealed ultrasonic transmission cavity is formed by the encapsulation layer to complete the encapsulation.

[0009] As a further improvement of the present invention, in step S1, the femtosecond laser pulse width is 150~300fs, the single-point laser energy is 0.4~0.8μJ, and the processing alignment accuracy is ≤±0.3μm; the processing environment is a Class 1000 cleanroom with an ambient temperature of 22±2℃ and a relative humidity of 40%~60%RH.

[0010] As a further improvement of the present invention, in step S2, the etching solution is 4%~8% diluted hydrofluoric acid with a buffer corrosion aid, the etching temperature is 28±1℃, and the etching time is 12~25min; the verticality of the formed through hole is ≤2°, and the hole diameter tolerance is ±2μm.

[0011] As a further improvement of the present invention, in step S3, a titanium-copper seed layer is first deposited by PVD process, and then the central penetration window area is shielded by photolithography mask, and copper pillars in the through hole and copper conductive layer, nickel barrier layer and gold protective layer of electrode pad are formed by step electroplating; wherein the copper conductive layer has a thickness of 1.5~2.5μm, the nickel barrier layer has a thickness of 40~60nm, the gold protective layer has a thickness of 0.08~0.12μm, and the temperature of the electroplating solution is maintained at 25±1℃ throughout the process.

[0012] As a further improvement of the present invention, in step S4, a silica suspension polishing slurry with a particle size of 10~30nm is used, the polishing pressure is 0.02~0.05MPa, the polishing speed is 300~600r / min, and the polishing time is 4~8min; In step S6, bonding is carried out in a cavity with a vacuum degree ≤5×10⁻³Pa, a bonding temperature of 120~220℃, a bonding pressure of 0.4~1.2MPa, and is held at the temperature and pressure for 40~90s, followed by a gradient cooling at a rate of ≤5℃ / min.

[0013] A glass through-hole encapsulation structure with a high-fidelity ultrasonic penetration window is prepared by the above-mentioned method, comprising a three-layer composite glass substrate, a pMUT chip, and an encapsulation layer. The three-layer composite glass carrier consists of an upper composite buffer layer, a glass core layer, and a lower composite buffer layer from top to bottom, forming a symmetrical stacked structure. The central area of ​​the three-layer composite glass carrier is a central penetration window area without metal residue, and the surface of the central penetration window area is treated with nano-level mirror polishing. The three-layer composite glass substrate has several vertically penetrating through holes arranged around the central penetrating window area. The inner wall of the through holes is provided with a composite metal conductive layer, which includes a titanium-copper seed layer that adheres to the inner wall of the through holes and copper pillars that fill the through holes. The upper and lower surfaces of the three-layer composite glass substrate are provided with electrode pads that are electrically connected to the composite metal conductive layer. The electrode pads are stacked with a copper conductive layer, a nickel barrier layer and a gold protective layer from the inside to the outside. The copper conductive layer is electrically connected to the copper pillar. The pMUT chip is disposed on the top of the three-layer composite glass substrate. The bottom surface of the pMUT chip is provided with metal microbumps. The metal microbumps are bonded and fixed to the electrode pads on the upper surface of the three-layer composite glass substrate. The ultrasonic emission axis of the pMUT chip is perpendicular to the geometric center of the central penetration window area. The encapsulation layer surrounds the pMUT chip and together with the three-layer composite glass substrate and the pMUT chip, forms a sealed ultrasonic transmission cavity.

[0014] As a further improvement of the present invention, the glass core layer is made of borosilicate glass or aluminosilicate glass with a thickness of 0.3~1.0 mm and an acoustic attenuation coefficient ≤0.02dB / mm.

[0015] As a further improvement of the present invention, both the upper composite buffer layer and the lower composite buffer layer are made of organic-inorganic composite materials with low thermal expansion coefficients, and the thickness of a single layer is 10~30μm; the upper composite buffer layer and the lower composite buffer layer only have avoidance holes at the corresponding positions of the through holes, and the buffer layer in the central penetration window area is complete and continuous.

[0016] As a further improvement of the present invention, the central penetrating window area is a native glass structure of uniform thickness, without groove thinning, and the surface roughness Ra≤0.01μm.

[0017] As a further improvement of the present invention, the conductivity between the metal conductive layer and the electrode pad corresponding to a single through-hole is ≤0.08Ω, and the resistance consistency deviation of the substrate is ≤0.01Ω; the airtightness of the sealed ultrasonic transmission cavity is ≤1×10 -9 Pa m³ / s.

[0018] The above technical solution has the following beneficial effects: 1. Excellent ultrasonic transmission performance: The central penetration window adopts a native glass structure with zero metal residue, combined with nano-level mirror polishing to eliminate diffuse reflection. The vertical transmission loss of ultrasonic waves is as low as 0.12dB, and the waveform is distortion-free, which can significantly improve the accuracy of ultrasonic detection and the signal-to-noise ratio of imaging.

[0019] 2. High structural reliability: The three-layer symmetrical composite structure buffers thermal stress through an organic-inorganic buffer layer, preventing cracking of the glass core layer and ensuring the continuity of the ultrasonic medium; the encapsulated cavity has high airtightness and can withstand thousands of high and low temperature cycles, with long-term stable electrical performance.

[0020] 3. High process yield and consistency: Through standardized zone control of laser no-drill zone design, selective etching, and zoned mask electroplating, metal residue in the penetration window is strictly eliminated, and the consistency deviation of TGV conduction resistance is ≤0.01Ω, significantly improving product yield and batch consistency.

[0021] 4. The process flow is standardized, the processing time of a single piece is controllable, there is no need to attach an additional acoustic matching film, the number of encapsulation layers and processes are simplified, the manufacturing cost is effectively reduced, and it is suitable for the large-scale mass production needs of consumer-grade ultrasonic devices. Attached Figure Description

[0022] To more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings in the following description are merely exemplary, and those skilled in the art can derive other embodiments based on the provided drawings without creative effort.

[0023] The structures, proportions, sizes, etc. shown in this specification are only used to complement the content disclosed in the specification for those skilled in the art to understand and read, and are not intended to limit the conditions under which the present invention can be implemented. Therefore, they have no substantial technical significance. Any modifications to the structure, changes in the proportional relationships, or adjustments to the size, without affecting the effects and objectives that the present invention can produce, should still fall within the scope of the technical content disclosed in the present invention.

[0024] Figure 1 This is a schematic diagram of the preparation method provided by the present invention.

[0025] Figure 2 This is a schematic diagram of the structure provided in step 1 of the present invention.

[0026] Figure 3 This is a schematic diagram of the preparation process in step 2 of the present invention.

[0027] Figure 4 This is a schematic diagram of the horizontal processing structure for removing photoresist through double-sided PVD photolithography in step 3 of the present invention.

[0028] Figure 5 This is a schematic diagram of the double-sided electroplating process performed vertically in step 3 of the present invention.

[0029] Figure 6 This is a schematic diagram of the product structure prepared in step 3 of the present invention.

[0030] Figure 7 This is a schematic diagram of the structure prepared in step 4 of the present invention.

[0031] Figure 8 This is a schematic diagram of the structure prepared in step 5 of the present invention.

[0032] Figure 9 This is a schematic diagram of the structure prepared in step 6 of the present invention.

[0033] In the picture: 1. Three-layer composite glass carrier plate; 11. Positioning reference angle; 12. Programmable no-drill zone; 13. Through hole; 2. Vacuum adsorption stage; 21. Titanium-copper seed layer; 22. Copper conductive layer; 23. Nickel barrier layer; 24. Gold protective layer; 25. Copper pillar; 3. Polishing pad; 31. Positioning fixture; 4. pMUT chip; 5. Packaging layer; 61. Carrier; 62. Etching tank. Detailed Implementation

[0034] In this invention, unless otherwise stated, directional terms such as "upper," "lower," "top," and "bottom" are generally used in relation to the direction shown in the accompanying drawings, or in relation to the vertical, perpendicular, or gravitational direction of the component itself; similarly, for ease of understanding and description, "inner" and "outer" refer to the inner and outer contours of each component itself, but the above directional terms are not intended to limit this invention.

[0035] like Figure 1 As shown, a method for fabricating a glass through-hole encapsulation structure with a high-fidelity ultrasonic penetration window includes the following steps: Step 1: Femtosecond laser modification of holes in a three-layer composite glass substrate Local lattice modification is performed at the pre-set TGV via locations on the three-layer composite glass substrate, allowing the modified area to be selectively etched by hydrofluoric acid, while ensuring that the central penetration window area is free from laser damage and internal defects throughout the process.

[0036] like Figure 2 As shown, the three-layer composite glass substrate 1 (hereinafter referred to as the substrate) consists of an upper composite buffer layer, a glass core layer and a lower composite buffer layer from top to bottom, forming a symmetrical stacked structure. The substrate is loaded and fixed on the vacuum adsorption stage 2, and the shape of the substrate and the positioning reference angle 11 are scanned by the CCD vision system, and the substrate batch traceability code is recorded. Then, the substrate is fixed by vacuum adsorption, the laser focal length and processing coordinates are calibrated, and the preset TGV array coordinate processing program is loaded.

[0037] The central penetration window region of the three-layer composite glass substrate 1 is designated as the program-restricted area 12. Femtosecond infrared lasers are used to perform lattice modification point-by-point on the TGV modification points surrounding the central penetration window region. The laser pulse width is controlled between 150 and 300 fs, the laser energy per point is 0.4 to 0.8 μJ, and the processing alignment accuracy is ≤ ±0.3 μm. At this time, the laser will form clearance holes on the upper and lower composite buffer layers.

[0038] After all TGV points on the substrate have been modified, all modified points are re-inspected using a CCD to confirm that there are no missed or misaligned points. The substrate is then transferred to a pure water pre-cleaning station, using a water with a resistivity ≥18.2MΩ. The surface laser dust is removed with pure water (cm), and after drying, it flows into the next process.

[0039] This process must be carried out in a Class 1000 cleanroom, with the ambient temperature controlled at 22±2℃ and the relative humidity at 40%~60%RH. The substrate processing cycle time is ≤90s / piece. The finished product quality requirements are: TGV modification point coordinate deviation ≤±0.5μm, no laser burning or internal micro-cracks in the program no-drill zone 12, no laser debris or scratches on the substrate surface, roughness Ra≤0.05μm, and complete and identifiable substrate traceability code with batch information binding.

[0040] Step 2: Selective etching with hydrofluoric acid to form TGV Only the glass in the laser-modified area is corroded and penetrated to form a through hole 13 that vertically penetrates the three-layer composite glass carrier plate 1, thus completely preserving the original plane of the glass penetration window that is undamaged and uncorroded.

[0041] like Figure 3 As shown, the laser-modified substrate is inserted into a special corrosion-resistant PTFE carrier 61 to avoid scratching the substrate surface. The substrate is then immersed in deionized water for 30 seconds to eliminate surface bubbles. After pre-wetting, the carrier 61 is immersed in the etching solution of the etching tank 62. The etching solution is prepared by diluting 4% to 8% hydrofluoric acid with a buffer corrosion aid. It is soaked at a constant temperature of 28±1℃ for 12 to 25 minutes to dissolve the glass core layer of the modified area to form glass through holes. The verticality of the glass through holes is controlled to be ≤2°. The glass through holes, together with the clearance holes on the upper composite buffer layer and the clearance holes on the lower composite buffer layer, form through holes 13 that vertically penetrate the three-layer composite glass carrier plate 1.

[0042] After etching, the substrate is rinsed in three stages of pure water countercurrent to remove hydrofluoric acid residue from the substrate surface. Then, it is immersed in a weak alkaline neutralizing solution for 5 minutes to completely neutralize the residual acid radicals on the surface. Finally, it is dried with hot air at 60°C and 15L / min nitrogen flow rate. After optical inspection to ensure that the diameter and perpendicularity of the through hole 13 are qualified, it is transferred to the next process.

[0043] This process requires continuous negative pressure suction of workshop exhaust gas, and unified collection, neutralization and discharge of etching waste liquid after meeting standards; the finished product quality requirements are that all through holes 13 (TGV) are fully open, with no blind holes or semi-through holes, the inner wall of through holes 13 is smooth without steps or burrs, the hole diameter tolerance is ±2μm, the surface of the central penetration window area is free of corrosion pits, pitting and lattice damage, the substrate surface is free of acid residue, and the surface resistance after water washing is ≥10¹²Ω.

[0044] Step 3: TGV metallization partitioned mask electroplating Conductive metal layers are deposited only on the inner wall of the TGV and in the upper and lower electrode pad areas of the substrate. The central penetration window area is completely covered by a photolithography mask, which isolates metal ions from the central penetration window area throughout the process, achieving zero metal residue.

[0045] like Figure 4 As shown, the product prepared in step 2 is first subjected to double-sided PVD photolithography to remove photoresist and remove surface organic impurities to improve photoresist adhesion. Then, a titanium-copper seed layer 21 is deposited by PVD process. After the seed layer is prepared, a positive photoresist with a thickness of 3~5μm is spin-coated and pre-baked at 90℃ for 3min to remove the solvent in the photoresist. Then, a photomask is used to precisely cover the central penetration window area, exposing only the via 13 and the electrode pad area. After alignment exposure, development and fixing, the excess photoresist outside the central penetration window area is peeled off to form an electroplating protective shielding layer.

[0046] Subsequently, as Figure 5 The process involves double-sided electroplating performed vertically in steps. First, copper is electroplated inside the through-hole 13 to form copper pillars 25. The combination of the titanium-copper seed layer 21 inside the through-hole 13 and the copper pillars 25 forms a conductive metal layer. Then, the electrode pads are electroplated, sequentially with a copper conductive layer 22, a nickel barrier layer 23, and a gold protective layer 24. Specifically, the copper conductive layer 22 is electrically connected to the copper pillars 25, with a film thickness controlled at 1.5~2.5μm and a current density of 1.2A / dm². The nickel barrier layer 23 has a film thickness of 40~60nm and a current density of 0.8A / dm². The gold protective layer 24 has a film thickness of 0.08~0.12μm and a current density of 0.5A / dm². The electroplating bath temperature is maintained at 25±1℃ throughout the process.

[0047] After electroplating, the photomask is stripped, excess titanium-copper seed layer is etched away, and the product is ultrasonically cleaned with pure water and dried. The metal film thickness and via conductivity are then measured. The resulting product structure is as follows: Figure 6 As shown.

[0048] The finished product quality requirements for this process are: no metal film, metal particles, or electroplating burrs remaining in the central penetration window area; the metal layer on the inner wall of the TGV must be complete and continuous, without any missed plating, breaks, or pinholes; the metal film thickness must be uniform, with a thickness deviation of ≤±0.1μm for the same substrate; the metal layer on the electrode pads must be flat, with no overflow plating to the edge of the penetration window; all TGVs must be electrically conductive without any open circuits; the conductivity resistance between the metal conductive layer and the electrode pad corresponding to a single through-hole must be ≤0.08Ω, and the resistance consistency deviation must be ≤0.01Ω.

[0049] Step 4: Nanoscale precision mirror polishing of the penetration window area Reduce the surface roughness of the glass in the central penetration window area to eliminate diffuse ultrasonic reflection and form a natural acoustic matching interface, while ensuring that the electrode pads at the TGV are not damaged during the polishing process.

[0050] like Figure 7 As shown, a positioning fixture 31 is used to shield all electrode pad areas, exposing only the central penetration window area. Then, a polishing pad 3 is attached to the surface of the central penetration window area, and a silica suspension polishing slurry with a particle size of 10-30 nm is supplied to the polishing pad 3 at a uniform rate. Segmented low-speed mirror polishing is performed for 4-8 minutes under polishing pressure of 0.02-0.05 MPa and polishing speed of 300-600 r / min, with surface roughness monitored in real time. After polishing, the positioning fixture is removed, and ultrasonic waves with a frequency of 40 kHz and a resistivity of 18.2 MΩ are used. The surface is thoroughly cleaned with pure water (cm) through multiple stages to completely remove polishing powder. After being dried with hot air, the surface roughness is tested and found to be qualified before flowing into the next process.

[0051] The quality requirements for the finished product in this process are as follows: the surface roughness Ra of the central penetration window area is ≤0.01μm; the mirror surface is free of scratches and pits; the polished area has clear boundaries and no polishing fluid erosion of the TGV electrode pads; the thickness of the penetration window is consistent with the original thickness of the glass core layer and there is no local thinning; the substrate surface has no polishing powder residue and uniform light transmission without haze.

[0052] Step 5: High-precision visual alignment of pMUT chip metal microbumps The metal microbumps on the bottom of the pMUT chip (miniature piezoelectric ultrasonic transducer) correspond one-to-one with the electrode pads on the top of the TGV, ensuring complete electrical connection without misalignment after bonding, while also ensuring precise alignment of the ultrasonic emission axis with the penetration window where the program's no-hit zone is located.

[0053] During the operation, the incoming inspection of pMUT chip 4 is completed first. The height and flatness of the gold-tin or copper-palladium microbumps on the bottom are checked. pMUT chip 4 with missing or deformed microbumps are rejected. The height of qualified microbumps is controlled between 5 and 15 μm.

[0054] The substrate was then fixed to the bonding machine base, and the processing reference was established by scanning the electrode pad coordinates with a CCD. The pMUT chip 4 was picked up with a vacuum nozzle with a vacuum negative pressure of -0.06~-0.09MPa, and the coordinates of the microbump array of the pMUT chip 4 were acquired by looking up with a CCD.

[0055] like Figure 8 As shown, the system automatically matches the coordinates of the microbumps and electrode pads, automatically compensates for the XYθ three-axis offset, and the pMUT chip 4 positioning rotation compensation range is ±3°. The final visual alignment accuracy is ≤±0.5μm. After the coordinate matching is completed, the alignment image is manually re-inspected. After confirming that there is no offset or misalignment, the alignment coordinates are latched.

[0056] This process must be carried out in a Class 100 cleanroom to avoid coordinate drift caused by airflow disturbance; the finished product quality requirements are that all microbumps are completely aligned with the corresponding electrode pads, with no single-sided offset or pad crossing issues, the ultrasonic emission axis of the pMUT chip is completely aligned with the geometric center of the central penetration window area, and the coaxiality is ≤±1μm, the pMUT chip is free from warping, edge chipping, and piezoelectric film damage, and the bumps are free from oxidation and foreign matter adhesion.

[0057] Step 6: Low-temperature mixing hot pressing / eutectic bonding completes the encapsulation and bonding process. A permanent metallurgical bond is achieved between the microbumps of the pMUT chip and the electrode pads, forming a sealed, airtight cavity to isolate moisture and dust, thus completing the final encapsulation and bonding.

[0058] During the process, the aligned substrate and pMUT chip 4 are simultaneously fed into the bonding vacuum chamber. The chamber is first evacuated to a vacuum level of ≤5×10. -3 Pa is used to eliminate air bubbles at the bonding interface; then, the temperature is gradually increased to the bonding temperature, while a constant pressure is applied and held for 40-90 seconds. The bonding temperature range is 120-220℃ (the gold-tin eutectic bonding temperature is controlled at 170-190℃, and the copper-palladium hot-press bonding temperature is controlled at 120-160℃), and the bonding pressure is controlled at 0.4-1.2MPa. After the holding and pressure is completed, the temperature is gradually reduced in stages at a rate of ≤5℃ / min to avoid substrate cracking caused by thermal stress. After cooling, the vacuum chamber is broken and the encapsulated semi-finished product is removed. The area where the microbumps and electrode pads are located is encapsulated with epoxy sealant to form encapsulation layer 5. The above encapsulation layer 5 does not contact the central penetration window area and forms a sealed cavity along the central penetration window area for use in ultrasonic wave transmission. After external cleaning, it enters the comprehensive performance testing stage. The structure of the prepared product is as follows. Figure 9 As shown.

[0059] The finished product quality requirements for this process are complete metallurgical bonding between the microbumps and electrode pads, free from defects such as incomplete soldering, cold soldering, and bridging; and an airtightness of ≤1×10⁻⁶ for the sealed cavity formed between the pMUT chip 4 and the three-layer composite glass substrate 1.-9 Pa m³ / s, the three-layer composite glass substrate 1 showed no cracking, delamination, or warping, the ultrasonic emission surface of the pMUT chip 4 showed no extrusion damage, and after 25 sets of high and low temperature cycles, the bonding interface showed no delamination or open circuit failure.

[0060] like Figure 9 As shown, a glass through-hole encapsulation structure with a high-fidelity ultrasonic penetration window is manufactured using the above-mentioned preparation method. It includes a three-layer composite glass carrier plate 1, which consists of an upper composite buffer layer, a glass core layer, and a lower composite buffer layer from top to bottom, forming a symmetrical stacked structure.

[0061] The central penetration window area of ​​the three-layer composite glass substrate 1 is the effective area for ultrasonic transmission, and the surface of this area is subjected to nanoscale mirror polishing. A plurality of through holes 13 are arranged around the periphery of the central penetration window area on the three-layer composite glass substrate 1. A composite metal conductive layer is electroplated on the inner wall of each through hole 13. This composite metal conductive layer consists of a titanium-copper seed layer 21 and copper pillars 25, with the titanium-copper seed layer 21 adhering to the inner wall of the through hole 13. Electrode pads electrically connected to the composite metal conductive layer are respectively provided at the upper and lower ends of the three-layer composite glass substrate 1. These electrode pads are composed of a copper conductive layer 22, a nickel barrier layer 23, and a gold protective layer 24 stacked sequentially, with the copper conductive layer 22 located on the inner side and electrically connected to the copper pillars 25.

[0062] A pMUT chip 4 is disposed on the top of the three-layer composite glass substrate 1. Metal microbumps are prepared on the bottom surface of the pMUT chip 4 and are bonded and fixed to the electrode pads on the upper surface of the three-layer composite glass substrate 1 by a low-temperature hybrid bonding process. The ultrasonic emission axis of the pMUT chip 4 is vertically aligned with the central penetration window area below.

[0063] The above structure enables vertical downward interconnection of the electrodes of the pMUT chip 4. Electrical signals are conducted through the copper pillar 25 to the electrode pads on the lower surface of the three-layer composite glass substrate 1, thereby achieving connection with external circuits.

[0064] Furthermore, the glass core layer uses borosilicate glass or aluminosilicate glass with low ultrasonic attenuation, a thickness of 0.3~1.0mm, and an acoustic attenuation coefficient ≤0.02dB / mm, serving as the core medium for ultrasonic transmission and the main support structure for the substrate. The upper and lower composite buffer layers are made of organic-inorganic composite materials with low thermal expansion coefficients, and the thickness of a single layer is 10~30μm. Through the application of the upper and lower composite buffer layers, the thermal stress generated by high-temperature bonding and reflow soldering processes is buffered to avoid cracking of the glass core layer, while ensuring the continuity of the ultrasonic transmission medium and reducing sound wave scattering loss. Example

[0065] This embodiment describes a glass through-hole packaging structure adapted to a 4-channel miniature ultrasonic biosensor pMUT chip, including the following structural design: Three-layer composite glass carrier plate 1: The core glass layer is made of aluminosilicate glass with a thickness of 0.6 mm and an acoustic attenuation coefficient of 0.015 dB / mm; the upper and lower composite buffer layers are both 20 μm thick with a thermal expansion coefficient of 1.2 ppm / ℃. A clearance hole is only opened at the glass through-hole position, and the upper and lower composite buffer layers in the central penetration window area are completely continuous.

[0066] Through-hole structure: A total of 12 through holes are arranged in an array around the central square penetration window area, with a through hole diameter of 50μm; a metal conductive layer is set inside the through hole, and the electrode pads on both sides are electroplated from the inside to the outside with a 2μm copper conductive layer, a 50nm nickel barrier layer and a 0.1μm gold protective layer. The conduction resistance between the metal conductive layer and the electrode pad in a single through hole is 0.06Ω; the electroplating process uses a photolithography mask to fully cover the penetration window area, so that there is no metal residue in the penetration window area.

[0067] Square penetrating window: 1.2mm×1.2mm in size, with a surface roughness Ra=0.008μm after nano-polishing. It is made of original glass of uniform thickness without grooving or thinning.

[0068] pMUT chip bonding structure: A 10μm high gold-tin microbump is fabricated on the bottom of the pMUT chip, with a flip-chip alignment accuracy of ±0.3μm; after bonding, a sealed cavity is formed between the pMUT chip and the three-layer composite glass substrate, with an airtightness ≤1×10 -9 Pa m³ / s.

[0069] Its preparation process is as follows: Femtosecond laser modification: A femtosecond infrared laser with a pulse width of 200 fs is used, with a single-point laser energy of 0.6 μJ and a processing alignment accuracy of ±0.3 μm. Lattice modification is performed on 12 via points in a Class 1000 cleanroom environment, with the central penetration window set as a no-drill zone in the program. After processing, the point deviation is ≤±0.5 μm and there is no laser damage to the penetration window.

[0070] Selective etching: Using 6% diluted hydrofluoric acid with a buffer corrosion aid, etching is performed at a constant temperature of 28℃ for 18 minutes to form through holes with a verticality of ≤2°; after rinsing with three levels of pure water, neutralization, and drying with nitrogen at 60℃, the through holes are found to be completely through, and there are no corrosion pits on the surface of the penetration window.

[0071] Partial electroplating: After PVD deposition of a titanium-copper seed layer on the substrate, a 4μm thick positive photoresist is spin-coated and pre-baked at 90℃ for 3 min; after the through-hole is masked by a mask, it is exposed and developed. First, copper is electroplated in the through-hole to form copper pillars, and then the electrode pads are electroplated. A 2μm copper conductive layer, a 50nm nickel barrier layer, and a 0.1μm gold protective layer are electroplated in sequence at a temperature of 25℃; after the photoresist is stripped and the seed layer is etched, the through-hole on-resistance consistency deviation is checked to be ≤0.01Ω, and there is no metal residue in the through-hole.

[0072] Mirror polishing: The electrode pads were shielded using a tooling, and polishing was performed for 6 minutes at a pressure of 0.03 MPa and a speed of 450 r / min using 20 nm silicon dioxide polishing slurry. After polishing, the surface was cleaned and dried, and the surface roughness of the penetration window was measured to be Ra=0.008 μm, with no reduction in window thickness.

[0073] Visual alignment: In a Class 100 cleanroom, a visual alignment system is used to achieve precise alignment between microbumps and electrode pads with an alignment accuracy of ±0.5μm. The coaxiality between the pMUT chip's emitter axis and the center of the penetration window is ≤±1μm.

[0074] Eutectic bonding: The vacuum chamber is evacuated to 5×10⁻³Pa, heated to 180℃, pressure of 0.8MPa is applied, and the temperature is held for 60s; then the temperature is gradually reduced at a rate of 3℃ / min; after bonding, the airtightness of the cavity is tested and found to be up to standard, and the three-layer composite glass substrate is free from cracks and delamination.

[0075] Performance testing The finished ultrasonic center frequency is 2MHz, the vertical transmission loss is ≤0.12dB, and the waveform is without distortion. After 1000 cycles of high and low temperature (-40℃~125℃), the three-layer composite glass substrate shows no cracking, no open circuits in the through holes, and stable electrical performance. Example

[0076] This embodiment describes a glass through-hole packaging structure adapted to ultrasonic fingerprint recognition pMUT chips for consumer electronics, including the following structural design: Three-layer composite glass substrate: The core glass layer is made of borosilicate glass with a thickness of 0.4 mm and an acoustic attenuation coefficient of 0.018 dB / mm; the upper and lower composite buffer layers are both 15 μm thick.

[0077] Through-hole structure: A total of 8 glass through-holes are arranged around the central circular penetration window, with a through-hole diameter of 30μm; the conduction resistance between the metal conductive layer and the electrode pad corresponding to a single through-hole is 0.07Ω.

[0078] Circular penetrating window: The window diameter is 0.8mm, and the surface roughness Ra=0.01μm after nano-polishing. It is made of original glass of uniform thickness.

[0079] pMUT chip bonding structure: Copper-palladium microbumps with a height of 8μm are prepared on the bottom of the pMUT chip, and a sealed cavity is formed after hot pressing and bonding.

[0080] Its preparation process Femtosecond laser modification: A femtosecond laser with a pulse width of 180 fs and a single-point energy of 0.5 μJ is used to modify 8 through-hole points. The center penetration window is not allowed to be drilled. After processing, the points are inspected and found to be qualified, and the penetration window is undamaged.

[0081] Selective etching: Using 5% diluted hydrofluoric acid, etching was performed at a constant temperature of 28℃ for 14 minutes to form through holes; after rinsing and drying, the morphology of the through holes was found to be qualified, and there was no pitting corrosion in the penetration window.

[0082] Zoned electroplating: Zoned mask electroplating is completed according to the process, the through-hole conductivity meets the standard, and there is no metal residue in the penetration window.

[0083] Mirror polishing: Using 15nm silica polishing slurry, polishing was performed for 5 minutes under a pressure of 0.025MPa. The surface roughness after polishing was Ra=0.01μm.

[0084] Visual alignment: Achieve precise alignment between copper-palladium microbumps and pads, and ensure the coaxiality of the axis meets the standard.

[0085] Hot-press bonding: Hot-press bonding is performed at 150℃ and 0.6MPa for 50s, followed by gradient cooling to complete the encapsulation.

[0086] Performance testing The finished product has an ultrasonic vertical transmission loss of ≤0.15dB, and the signal-to-noise ratio of near-field fingerprint imaging is improved by 32%; the overall thickness of the package is only 0.48mm, making it suitable for ultra-thin terminal devices.

[0087] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments according to this application. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0088] It should be noted that the terms "first," "second," etc., used in the specification, claims, and accompanying drawings of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of this application described herein can be implemented in sequences other than those illustrated or described herein.

[0089] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for fabricating a glass through-hole encapsulation structure with a high-fidelity ultrasonic penetration window, comprising the following steps: S1. Femtosecond laser modification of holes in three-layer composite glass substrate: The central penetration window area of ​​the three-layer composite glass substrate (1) is set as the program-inactive zone (12). Femtosecond laser is used to modify the lattice of the TGV points surrounding the central penetration window only. After the modification is completed, the substrate is cleaned and dried. S2, Hydrofluoric acid selective etching to form TGV: Hydrofluoric acid etching solution is used to etch the modified three-layer composite glass substrate (1), so that only the laser modified area is etched to form through holes (13), and the original glass plane of the central penetrating window area is completely preserved. S3, TGV metallization partition mask electroplating: The central penetration window area is completely covered by a photolithographic mask, and a conductive metal layer is deposited only on the inner wall of the through hole (13) and the upper and lower electrode pad areas of the substrate, so as to achieve zero metal residue in the central penetration window area. S4. Nanoscale precision mirror polishing of the penetration window area: All electrode pad areas are masked, and only the central penetration window area is polished with nanoscale mirror polishing to reduce surface roughness. S5, High-precision visual alignment of pMUT chip metal microbumps: Visually align the metal microbumps of pMUT chip (4) with the upper surface electrode pads of the three-layer composite glass substrate (1) so that the ultrasonic emission axis of pMUT chip (4) is precisely aligned with the central penetration window area. S6. Low-temperature mixed hot pressing / eutectic bonding completes the encapsulation and bonding: the metallurgical bonding of microbumps and electrode pads is achieved through low-temperature bonding process, and the encapsulation layer (5) is used to form a sealed ultrasonic transmission cavity to complete the encapsulation.

2. The preparation method according to claim 1, characterized in that, In step S1, the femtosecond laser pulse width is 150~300fs, the single-point laser energy is 0.4~0.8μJ, and the processing alignment accuracy is ≤±0.3μm; the processing environment is a Class 1000 cleanroom with an ambient temperature of 22±2℃ and a relative humidity of 40%~60%RH.

3. The preparation method according to claim 1, characterized in that, In step S2, the etching solution is 4%~8% diluted hydrofluoric acid with a buffer corrosion aid, the etching temperature is 28±1℃, and the etching time is 12~25min; the verticality of the formed through hole (13) is ≤2° and the hole diameter tolerance is ±2μm.

4. The preparation method according to claim 1, characterized in that, In step S3, a titanium-copper seed layer (21) is first deposited by PVD process, and then the central penetration window area is shielded by photolithography mask. The copper pillar (25) in the through hole and the copper conductive layer (22), nickel barrier layer (23) and gold protective layer (24) of the electrode pad are formed by step electroplating. The copper conductive layer (22) has a film thickness of 1.5~2.5μm, the nickel barrier layer (23) has a film thickness of 40~60nm, and the gold protective layer (24) has a film thickness of 0.08~0.12μm. The temperature of the electroplating solution is maintained at 25±1℃ throughout the process.

5. The preparation method according to claim 1, characterized in that, In step S4, a silica suspension polishing slurry with a particle size of 10~30nm is used, the polishing pressure is 0.02~0.05MPa, the polishing speed is 300~600r / min, and the polishing time is 4~8min; In step S6, bonding is carried out in a cavity with a vacuum degree ≤5×10⁻³Pa, a bonding temperature of 120~220℃, a bonding pressure of 0.4~1.2MPa, and is held at the temperature and pressure for 40~90s, followed by a gradient cooling at a rate of ≤5℃ / min.

6. A glass through-hole encapsulation structure with a high-fidelity ultrasonic penetration window, prepared by the method described in any one of claims 1 to 5, characterized in that, It includes a three-layer composite glass substrate (1), a pMUT chip (4), and a packaging layer (5); The three-layer composite glass carrier plate (1) consists of an upper composite buffer layer, a glass core layer and a lower composite buffer layer from top to bottom, forming a symmetrical stacked structure; the central area of ​​the three-layer composite glass carrier plate (1) is a central penetration window area without metal residue, and the surface of the central penetration window area is treated with nano-level mirror polishing. The three-layer composite glass substrate (1) has several vertically penetrating through holes (13) arranged around the central penetration window area. The inner wall of the through hole (13) is provided with a composite metal conductive layer, which includes a titanium-copper seed layer (21) that adheres to the inner wall of the through hole (13) and copper pillars (25) that fill the through hole (13). The upper and lower surfaces of the three-layer composite glass substrate (1) are provided with electrode pads that are electrically connected to the composite metal conductive layer. The electrode pads are stacked with a copper conductive layer (22), a nickel barrier layer (23) and a gold protective layer (24) from the inside to the outside. The copper conductive layer (22) and the copper pillar (25) are electrically connected. The pMUT chip (4) is disposed above the three-layer composite glass substrate (1). The bottom surface of the pMUT chip (4) is provided with metal microbumps. The metal microbumps are bonded and fixed to the electrode pads on the upper surface of the three-layer composite glass substrate (1). The ultrasonic emission axis of the pMUT chip (4) is perpendicular to the geometric center of the central penetration window area. The encapsulation layer (5) surrounds the pMUT chip (4) and together with the three-layer composite glass substrate (1) and the pMUT chip (4) form a sealed ultrasonic transmission cavity.

7. The glass through-hole encapsulation structure with a high-fidelity ultrasonic penetration window according to claim 6, characterized in that, The glass core layer is made of borosilicate glass or aluminosilicate glass with a thickness of 0.3~1.0mm and an acoustic attenuation coefficient ≤0.02dB / mm.

8. The glass through-hole encapsulation structure with a high-fidelity ultrasonic penetration window according to claim 6, characterized in that, Both the upper and lower composite buffer layers are made of organic-inorganic composite materials with low thermal expansion coefficients, and the thickness of a single layer is 10~30μm. The upper and lower composite buffer layers only have clearance holes at the corresponding positions of the through holes (13), and the buffer layer in the central penetration window area is complete and continuous.

9. The glass through-hole encapsulation structure with a high-fidelity ultrasonic penetration window according to claim 6, characterized in that, The central penetration window area is a native glass structure of uniform thickness, without groove thinning, and has a surface roughness Ra≤0.01μm.

10. The glass through-hole encapsulation structure with a high-fidelity ultrasonic penetration window according to claim 6, characterized in that, The conduction resistance between the metal conductive layer and the electrode pad corresponding to a single through-hole (13) is ≤0.08Ω, and the resistance consistency deviation of the substrate is ≤0.01Ω; the airtightness of the sealed ultrasonic transmission cavity is ≤1×10 -9 Pa m³ / s.