Use of artesunate or artesunate-supported matrices in preventing the attachment of large marine fouling organisms.
By combining artesunate with acrylic silicone resin or organosilicon resin, a slow-release antifouling coating is constructed, which solves the ecotoxicity and non-degradability problems of existing marine antifouling coatings and achieves a long-lasting and environmentally friendly antifouling effect.
Patent Information
- Application Number
- CN202611130416.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing marine antifouling coatings have ecotoxicity and non-biodegradability issues, making it difficult to achieve long-lasting and environmentally friendly antifouling effects.
Artesunate is combined with acrylic silicone resin, organosilicon resin or acrylic silicone coating to form a stable antifouling matrix through a slow-release mechanism. The antioxidant and antibacterial properties of artesunate are utilized to construct a long-lasting antifouling coating in combination with inorganic fillers.
Artesunate achieves sustained release and long-lasting antifouling, avoiding the ecotoxicity risks of traditional antifouling agents. It also has good water solubility and bioavailability, making it suitable for preventing large marine fouling organisms.
Smart Images

Figure CN123100644A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of marine antifouling materials technology, specifically relating to the use of artesunate or a matrix loaded with artesunate in preventing the attachment of large marine fouling organisms. Background Technology
[0002] Marine biofouling refers to structural and functional damage to underwater surfaces caused by the attachment of marine organisms. More than 4,000 species of biofouling organisms have been recorded in global oceans. The synergistic attachment of different biological communities exacerbates the complexity and difficulty of remediation of biofouling. Therefore, developing efficient antifouling strategies is of significant economic and strategic importance. Using chemical antifouling coatings to protect the surfaces of ships and other facilities is currently the most widely used, convenient, and efficient technical method.
[0003] Marine antifouling coating technology has undergone three main development stages: the traditional high-toxicity coating stage, the tributyltin (TBT) self-polishing coating stage, and the environmentally friendly coating stage. Early antifouling coatings used hot asphalt and grease as bases, compounded with heavy metal fillers such as mercury oxide; these were phased out due to their excessive toxicity. In the 1970s, TBT compounds were widely used due to their highly efficient and broad-spectrum antifouling properties. This technology utilizes the hydrolysis of acrylate resins in weakly alkaline seawater to gradually release TBT to exert its antifouling activity, while the coating surface is continuously renewed, thus achieving long-term fouling control. However, TBT has persistent bioaccumulation and high ecotoxicity, leading to deformities and deaths in various marine organisms. The International Maritime Organization (IMO) banned the use of TBT-containing antifouling coatings on commercial vessels worldwide from January 1, 2008. Since then, research on marine antifouling coatings has not only focused on ensuring antifouling efficiency but also on environmental friendliness as a core design principle.
[0004] Biofouling refers to the dynamic process by which microorganisms, plants, or animals attach to and grow on material surfaces, gradually forming a biofilm. This phenomenon is particularly prominent in marine environments, accelerating hull corrosion, increasing drag, and boosting fuel consumption, thus imposing a significant economic burden on the global shipping industry. The biofouling process follows a clear temporal sequence. When a material surface comes into contact with water, macromolecules such as proteins and polysaccharides in the water are almost immediately adsorbed onto the surface, forming a "conditioned film." This film provides a substrate for subsequent microbial attachment. Subsequently, microorganisms such as bacteria and algal spores gradually colonize and secrete extracellular polymers, eventually forming a structurally stable biofilm. On this basis, larger fouling organisms such as barnacles and shellfish further attach and grow, significantly exacerbating the degree of fouling.
[0005] From a control strategy perspective, suppressing the initial stages of fouling—namely, conditioned film formation and primary microbial adhesion—is considered the most effective intervention window. Polymer coatings play a crucial role in preventing direct contact between microorganisms and material surfaces. However, while many synthetic antifouling coatings (such as those containing copper ions or organic biocides) offer significant short-term effects, their non-biodegradability and potential ecotoxicity are facing increasingly stringent regulatory restrictions. Therefore, developing alternative materials that combine excellent antifouling performance with environmental friendliness has become a current research hotspot. Summary of the Invention
[0006] In view of this, and to solve the aforementioned technical problems, the purpose of this invention is to provide the use of artesunate or a matrix loaded with artesunate in preventing the attachment of large marine fouling organisms. The artemisinin derivative is derived from the extract of the traditional Chinese medicine Artemisia annua, possessing both environmental friendliness and highly efficient, broad-spectrum antifouling activity. By blending artesunate into an acrylic silicone resin matrix, an organosilicon resin matrix, or an acrylic silicone coating, the slow-release and long-lasting antifouling effect of artesunate is achieved.
[0007] The technical solution adopted is as follows:
[0008] Use of artesunate or artesunate-loaded matrix in preventing the attachment of large marine fouling organisms.
[0009] Furthermore, the matrix loaded with artesunate is an acrylic silicone resin loaded with artesunate, an acrylic silicone coating loaded with artesunate, or an organosilicon coating loaded with artesunate.
[0010] Furthermore, the large marine fouling organisms are mussels and / or barnacles.
[0011] Furthermore, the artesunate-loaded silicone acrylate resin comprises artesunate and a silicone acrylate matrix. The raw materials for preparing the silicone acrylate matrix include methyl methacrylate, triisopropyl methacrylate, 2-methoxyethyl acrylate, azobisisobutyronitrile, benzoyl peroxide, and xylene. By mass ratio, the ratio of methyl methacrylate: triisopropyl methacrylate: artesunate: 2-methoxyethyl acrylate: azobisisobutyronitrile: benzoyl peroxide: xylene is 35-55: 35-60: 10-50: 0.5-10: 0.5-2: 0.5-1.5: 90-110.
[0012] Further, the preparation method of the artesunate-loaded silicone acrylate resin includes the following steps: In a reaction vessel equipped with a stirrer, thermometer, and reflux condenser, xylene is added according to the specified ratio, and the mixture is heated to 90°C under nitrogen protection. Then, methyl methacrylate, triisopropyl methacrylate, and 2-methoxyethyl acrylate are added. Azobisisobutyronitrile and benzoyl peroxide are slowly added dropwise as initiators, and the reaction is maintained at this temperature for 6-8 hours. After the reaction is completed, the mixture is cooled to room temperature to obtain a silicone acrylate prepolymer. Artesunate is dissolved in anhydrous ethanol and added to the prepolymer under stirring to obtain the artesunate-loaded silicone acrylate resin. The obtained artesunate-loaded silicone acrylate resin can be directly used for brushing or spraying, and forms an antifouling coating after curing at room temperature for 7 days.
[0013] Furthermore, the organosilicon resin loaded with artesunate comprises artesunate and an organosilicon resin matrix. The raw materials for making the organosilicon resin matrix include tetraethyl orthosilicate, n-octyltriethoxysilane, hydrochloric acid, and isopropanol. By mass ratio, the ratio of tetraethyl orthosilicate: n-octyltriethoxysilane: artesunate: hydrochloric acid: isopropanol is 9-11:12-14:5-20:15-25:6-8.
[0014] Further, the preparation method of the artesunate-loaded organosilicon resin includes the following steps: at room temperature, tetraethyl orthosilicate, n-octyltriethoxysilane, and isopropanol are added sequentially to a reaction vessel, stirred for 30 minutes, and then 0.1 mol / L hydrochloric acid is slowly added dropwise. After the addition is complete, stirring is continued for 24 hours to allow the system to fully hydrolyze and condense, forming a uniform sol to obtain an organosilicon resin prepolymer; artesunate is dissolved in anhydrous ethanol and added to the organosilicon resin prepolymer to obtain the artesunate-loaded organosilicon resin. The obtained sol is coated onto the surface of a substrate and cured at room temperature for 7 days to form an antifouling coating.
[0015] Furthermore, the artesunate-loaded acrylic silicone coating comprises artesunate and an acrylic silicone coating. The raw materials for making the acrylic silicone coating include acrylic silicone resin, pigment, desparon, talc, bentonite, barium sulfate, plasticizer, compound antifouling component, and organic solvent. By mass ratio, the ratio of acrylic silicone resin: pigment: desparon: talc: bentonite: barium sulfate: plasticizer: artesunate: compound antifouling component: organic solvent is 45-55: 2-4: 1-3: 4-6: 0.5-1.5: 0.5-2: 0.5-2.5: 10-30: 0.5-20: 10-20.
[0016] Furthermore, the antifouling components are zinc oxide and / or titanium dioxide.
[0017] Furthermore, the organic solvent is xylene and / or propylene glycol methyl ether.
[0018] Furthermore, the pigment is iron oxide red.
[0019] Furthermore, the plasticizer is chlorinated paraffin.
[0020] Furthermore, the method for preparing the acrylic silicone coating loaded with artesunate includes the following steps:
[0021] (1) Add xylene, propylene glycol methyl ether, antifouling components, bentonite, pigment, talc, desparon, plasticizer and barium sulfate to a dispersion container according to the formula. Stir at 800-1200 r / min for 10-15 minutes to make the components initially mixed evenly. Then increase the speed to 2500-3500 r / min and stir for 20-40 minutes to make the pigment and filler fully dispersed to the required fineness (it can be tested with a scraper fineness gauge, or by brushing the material obtained in step (1) onto filter paper and checking that no obvious particles enter the next step).
[0022] (2) Add acrylic silicone resin and artesunate to the material obtained in step (1), stir at a speed of 1500-2500 r / min for 40-60 seconds, repeat stirring twice until completely mixed, and the acrylic silicone coating coating loaded with artesunate is obtained.
[0023] Grind the substrate to be coated until the surface is rough, apply a layer of bonding paint evenly with a roller or brush, and let it dry at room temperature for 2-4 hours. Then brush or spray the acrylic silicone coating with artesunate loaded in step (2) onto the substrate surface coated with bonding paint. It can be used after curing at room temperature for 7 days.
[0024] In the above technical solutions,
[0025] Artesunate is an artemisinin derivative extracted from Artemisia annua L., a plant in the Asteraceae family. It is a sesquiterpene lactone compound with good water solubility and bioavailability. As a classic antimalarial drug, artesunate has been shown in recent years to possess a wide range of pharmacological activities, including anti-inflammatory, immunomodulatory, antioxidant, antibacterial, antifibrotic, and organ-protective effects. Artesunate is a weakly acidic drug, and its transport in vivo is mainly via simple diffusion, making it relatively easy to cross biological membranes.
[0026] In the field of antifouling, artesunate, as a functional molecule of natural origin, has antifouling application value. Its mechanism of action mainly includes the following aspects: (1) by activating the Nrf2 / HO-1 signaling pathway, inhibiting the production of reactive oxygen species (ROS), regulating the expression of oxidative stress-related genes and proteins, thereby exerting an antioxidant effect; (2) by inducing oxidative stress and membrane structure damage in microorganisms or fouled organisms, achieving contact antibacterial or antialgal activity; (3) by regulating cell autophagy, apoptosis and metabolic homeostasis, inhibiting the formation and development of biofilms.
[0027] The structural formula of artesunate is as follows:
[0028] ,
[0029] The molecular formula is C 19 H 28 O8 has a molecular weight of 384.42.
[0030] However, artesunate faces challenges in controlling its dissolution behavior and maintaining long-term release when used directly for antifouling. Therefore, it requires rational matrix design, cross-linking modification, or formulation with other antifouling agents to improve the matrix stability and antifouling durability. Based on the above analysis, this invention uses artesunate as a natural antifouling active component, combined with suitable film-forming materials and cross-linking strategies, to construct a matrix material with stable performance, environmental friendliness, and long-term antifouling capability. Artesunate is incorporated as an antifouling agent during the preparation of the antifouling matrix material, which is used to prevent the attachment of large marine fouling organisms.
[0031] The matrix material includes an acrylic silicone resin loaded with artesunate, an acrylic silicone coating loaded with artesunate, or an organosilicon coating loaded with artesunate.
[0032] The artesunate-loaded silicone resin is produced by blending artesunate with methyl methacrylate and triisopropyl methacrylate copolymer to form a sea-island-like loading system. In seawater, the siloxane segments on the resin surface slowly hydrolyze, allowing the artesunate loaded on the surface to be gradually released. At the same time, the artesunate inside continuously migrates to the surface due to the concentration gradient, thus achieving a stable release period of several months.
[0033] The acrylic silicone coating loaded with artesunate uses tetraethyl orthosilicate and n-octyltriethoxysilane as precursors, forming a three-dimensional cross-linked network structure under acid catalysis. During gelation, artesunate is in situ encapsulated within the hydrophobic siloxane pores. The matrix itself has extremely low surface energy, endowing the coating with excellent fouling desorption physical properties (low surface tension makes it difficult for fouling organisms to adhere firmly), which, combined with the gradual release of artesunate, results in antifouling durability.
[0034] The organosilicon coating loaded with artesunate introduces zinc oxide and / or titanium dioxide as antifouling components, forming microcouples or photocatalytic active sites in the coating. This complements the organic antifouling mechanism of artesunate, expanding the antifouling spectrum. At the same time, the steric hindrance effect of inorganic fillers is used to further regulate the dissolution path of artesunate, avoiding burst release and achieving long-lasting antifouling.
[0035] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0036] The artesunate used in this invention is a sesquiterpene lactone derivative obtained through semi-synthesis from artemisinin extracted from the traditional Chinese medicine Artemisia annua L. It belongs to the category of green antifouling active substances derived from natural products, possessing good water solubility and bioavailability, and readily permeating biofilms. When used as an antifouling active ingredient, the matrix contains no added heavy metals such as copper, tin, or DDT, nor any persistent organic pollutants. It has no long-term ecotoxicity to marine waters, sediments, or non-target organisms, and can gradually degrade into low-toxicity or non-toxic small molecules in seawater environments. This effectively avoids the risks of bioaccumulation and transmission in the food chain associated with traditional antifouling agents, providing a feasible path to achieve the eco-friendly goal of marine antifouling. Loading artesunate onto stable matrices, including acrylic silicone resins, organosilicon resins, or acrylic silicone coatings, achieves sustained release of artesunate, resulting in long-lasting antifouling effects. Attached Figure Description
[0037] Figure 1 Photographs showing the effects of artesunate on the adhesion behavior and growth and development of the glandular larvae of Amphibalanus amphitrite in Example 1 of the invention.
[0038] Figure 2 The bar chart shows the concentration-effect of artesunate obtained in Example 2 on the inhibition of adhesion behavior in mytilus edulis.
[0039] Figure 3 A bar chart illustrating the effect of artesunate-loaded acrylic silicone resin on the formation of byssal discs in mussels in Example 3 of the invention.
[0040] Figure 4 A bar chart showing the effect of artesunate-loaded silicone resin on the formation of byssal discs in mussels in Example 4 of the invention.
[0041] Figure 5 Photographs showing the antifouling effect of the acrylic silicone coating loaded with artesunate in marine areas in Example 5 of the invention.
[0042] Figure 6 Photographs showing the antifouling effect of artesunate-loaded organosilicon resin in marine environments in Example 6 of the invention. Detailed Implementation
[0043] The present invention will be described in detail below through specific embodiments. However, the uses and purposes of these exemplary embodiments are only for illustrating the present invention and do not constitute any limitation on the actual protection scope of the present invention, nor are they intended to limit the protection scope of the present invention to this.
[0044] Example 1: Effects of artesunate on adhesion behavior of barnacle gland larvae
[0045] Take a clean 6-well plate, add 7 ml of artificial seawater to each well, add 7 μL of solvent to each of the three wells of the control group, add 7 μL of artesunate solution to each of the three wells of the experimental group, add 10 adenocarcinoma larvae to each well, and observe after incubation at room temperature for 48 hours.
[0046] Figure 1 The image shows a microscopic image of the adenocarcinoma larvae obtained in Example 1. After being exposed to a seawater system containing artesunate for 48 hours, the adenocarcinoma larvae in the control group could freely extend and retract their first antennae and six pairs of thoracic limbs, and had the ability to swim and explore the substrate. The adenocarcinoma larvae in the experimental group lost their ability to move, and their first antennae and six pairs of thoracic limbs everted out and stretched out rigidly, completely losing their ability to swim, explore the substrate, and attach and metamorphose.
[0047] Example 2: Effect of artesunate on the adhesion behavior of mussels
[0048] Acquisition of purple mussels: Adult purple mussels were collected from the waters off Dalian, cultured in the laboratory, and selected from those with abundant byssal secretion (shell length about 3cm). The byssal secretions were gently cut off, and the mussels were cleaned and set aside for use.
[0049] Artesunate was dissolved in anhydrous ethanol, and experimental groups were set at 25, 50, 75, and 100 mg / L. -1 A control group consisting of artificial seawater (blank) and a control group consisting of artificial seawater solution in 4‰ anhydrous ethanol (solvent) were set up. Each group had three replicates. A 3L water tank was used; 1L of artificial seawater was added to the tank, followed by 10mL of the prepared solution. Six mussels were gently placed into each tank. After standing for 72 hours, the mussels were removed, and the number of byssal discs in each hole was observed and recorded.
[0050] Figure 2 This is a concentration-effect bar chart showing the inhibition of mussel adhesion behavior by artesunate obtained in Example 2. The half-maximal inhibitory concentration (EC50) was calculated. 50 It is 56.49 mg·L -1 Artesunate was confirmed to have a good inhibitory effect on the secretion of byssal threads in purple violets.
[0051] Example 3: Test on the effect of artesunate-loaded acrylic silicone resin on inhibiting mussel adhesion.
[0052] In this embodiment, an acrylic silicone resin loaded with artesunate is prepared, and the weight parts of each raw material in its components are as follows:
[0053] 45 parts by weight of methyl methacrylate;
[0054] 50 parts by weight of triisopropyl methacrylate;
[0055] An ethanol solution containing artesunate at a concentration of 0.1 g / mL;
[0056] 5 parts by weight of 2-methoxyethyl acrylate;
[0057] 1 part by weight of azobisisobutyronitrile;
[0058] Benzoyl peroxide 0.5 parts by weight;
[0059] 100 parts by weight of xylene.
[0060] The specific preparation method includes the following steps: In a reaction vessel equipped with a stirrer, thermometer, and reflux condenser, xylene is first heated to 90°C under nitrogen protection, then methyl methacrylate, triisopropyl methacrylate, and 2-methoxyethyl acrylate are added, followed by the slow dropwise addition of azobisisobutyronitrile and benzoyl peroxide. The reaction is maintained at this temperature for 6-8 hours. After the reaction is completed, the mixture is cooled to room temperature to obtain an acrylic silicone ester prepolymer. Artesunate is dissolved in anhydrous ethanol to form an ethanol solution containing artesunate. Then, the ethanol solution containing artesunate is added to the acrylic silicone resin prepolymer at different mass ratios to obtain an acrylic silicone resin loaded with artesunate.
[0061] 15*18.5cm 2 After ultrasonic cleaning, a layer of acrylic silicone resin loaded with artesunate was evenly brushed onto the glass slides, which were then cured at room temperature for one week before use. Mussels with abundant byssal secretion were selected, their byssal threads were gently cut off, and the slides were cleaned and set aside. Three replicates were set up for each group. A 3L water tank was prepared, with the glass slide placed at the bottom, followed by 1L of artificial seawater. The experimental groups used acrylic silicone resin slides loaded with artesunate (artesunate content was 20%, 30%, and 40% by mass), while the control groups used both glass slides and acrylic silicone resin slides. Four mussels (shell length approximately 5cm) were evenly placed in the tank. After standing for 72 hours, the glass slides were removed, and the number of byssal discs was counted.
[0062] Depend on Figure 3 It can be seen that the inhibitory effect of the acrylic silicone resin sheet loaded with artesunate on the formation of byssal discs of mussels in Example 3 increases with the increase of loading concentration. When the loading reaches 40%, the formation rate of byssal discs is zero, achieving complete inhibition.
[0063] Example 4: Test on the effect of organosilicon resin loaded with artesunate on inhibiting mussel adhesion.
[0064] In this embodiment, an organosilicon resin loaded with artesunate is prepared, and the weight parts of each raw material in its components are as follows:
[0065] 10 parts by weight of tetraethyl orthosilicate;
[0066] 14 parts by weight of n-octyltriethoxysilane;
[0067] An ethanol solution containing artesunate at a concentration of 0.1 g / mL;
[0068] 20 parts by weight of isopropanol;
[0069] 7 parts by weight of hydrochloric acid.
[0070] The specific preparation method includes the following steps: At room temperature, tetraethyl orthosilicate, n-octyltriethoxysilane, and isopropanol are added sequentially to a reaction vessel. After stirring for 10 minutes, 0.1 mol / L hydrochloric acid is slowly added dropwise. After the addition is complete, stirring continues for 24 hours to allow the system to fully hydrolyze and condense, forming a homogeneous sol to obtain an organosilicon resin prepolymer. Artesunate is dissolved in anhydrous ethanol to form an ethanol solution containing artesunate. Then, the ethanol solution containing artesunate is added to the organosilicon resin prepolymer at different mass ratios to obtain an organosilicon resin loaded with artesunate.
[0071] 15*18.5cm 2 After ultrasonic cleaning, a layer of artesunate-loaded silicone resin was evenly brushed onto the glass slides, which were then cured at room temperature for one week before use. Mussels with abundant byssal secretion were selected, their byssal threads were gently cut off, and the slides were cleaned and set aside. Three replicates were set up for each group. A 3L water tank was prepared. The glass slides were placed at the bottom of the tank, and 1L of artificial seawater was added. The experimental groups used silicone resin slides loaded with artesunate (artesunate mass contents of 20%, 30%, and 40%, respectively), while the control groups used both glass slides and silicone resin slides. Four mussels (shell length approximately 5cm) were evenly placed in the tank. After standing for 72 hours, the glass slides were removed, and the number of byssal discs was counted.
[0072] Depend on Figure 4 It can be seen that the organosilicon resin sheet loaded with artesunate in Example 4 has an excellent inhibitory effect on the byssal discs of mussels. Within the loading range of 20% to 40%, the resin sheet can reduce the byssal disc formation rate to zero, indicating that when the loading is not less than 20%, the formation of byssal discs can be completely inhibited.
[0073] Example 5: Testing the antifouling effect of artesunate-loaded acrylic silicone coating in marine areas
[0074] In this embodiment, an acrylic silicone coating loaded with artesunate is prepared, and the weight ratio of each raw material in its components is as follows:
[0075] 40 parts by weight of acrylic silicone resin;
[0076] 4 parts by weight of artesunate;
[0077] 15 parts by weight of xylene;
[0078] 15 parts by weight of zinc oxide;
[0079] 5 parts by weight of talc;
[0080] 4 parts by weight of titanium dioxide;
[0081] 3 parts by weight of propylene glycol methyl ether;
[0082] Iron oxide red 3 parts by weight;
[0083] 2 parts by weight of Desparon;
[0084] 1.5 parts by weight of chlorinated paraffin;
[0085] 1 part by weight of barium sulfate;
[0086] 0.5 parts by weight of bentonite.
[0087] The specific preparation method includes the following steps:
[0088] (1) Add xylene, zinc oxide, titanium dioxide, propylene glycol methyl ether, bentonite, iron oxide red, talc, dispora, chlorinated paraffin and barium sulfate to a container in proportion. First adjust the speed to 1000 r / min and stir for 10 min. Then increase the speed to 3000 r / min and stir for 30 min.
[0089] (2) Use a brush to apply the material obtained in step (1) onto filter paper. It can be used only if there are no obvious particles.
[0090] (3) Add acrylic silicone resin and artesunate to the material obtained in step (1), set the program to speed 2000r / min and time 50s, and stir twice until the mixture is uniform; thus, the acrylic silicone coating loaded with artesunate is obtained.
[0091] Sand the epoxy board until the surface is rough, apply the bonding paint evenly with a roller, let it dry at room temperature, then brush the material obtained in step (3) onto the epoxy board coated with the bonding paint, and use it after curing at room temperature for 7 days.
[0092] The preparation method of the acrylic silicone resin is the same as in Example 3, except that artesunate is not added. Specifically, it includes the following steps: In a reaction vessel equipped with a stirrer, thermometer, and reflux condenser, xylene is added, and the temperature is raised to 90°C under nitrogen protection. Then, methyl methacrylate, triisopropyl methacrylate, and 2-methoxyethyl acrylate are added, and the mixture is stirred thoroughly. Azobisisobutyronitrile and benzoyl peroxide are slowly added dropwise, and the reaction is maintained at this temperature for 6-8 hours. After the reaction is complete, the mixture is cooled to room temperature to obtain the acrylic silicone resin.
[0093] The antifouling performance of the artesunate-loaded acrylic silicone coating was tested as follows:
[0094] The shallow-sea siding was tested in the Huacai Haikou Bay waters of Meilan District, Haikou City, Hainan Province, in accordance with the national standard GB / T 5370-2007. Figure 5 As shown, after 3 months of sea area plastering, the paint film was intact, with no peeling or blistering. Only a small amount of large fouling organisms adhered to the coating surface of the experimental group.
[0095] Example 6: Testing the antifouling effect of artesunate-loaded organosilicon resin in marine areas
[0096] The organosilicon resin loaded with artesunate from Example 3 was brushed onto an epoxy board coated with bonding paint and used after curing at room temperature for 7 days.
[0097] The antifouling performance of the organosilicon resin loaded with artesunate in Example 3 is tested as follows:
[0098] The shallow-sea siding was tested in the Huacai Haikou Bay waters of Meilan District, Haikou City, Hainan Province, in accordance with the national standard GB / T 5370-2007. Figure 6 As shown, after 3 months of sea area plastering, the paint film was intact, with no peeling or blistering. Only a small amount of large fouling organisms adhered to the coating surface of the experimental group.
[0099] The detailed descriptions listed above are merely specific illustrations of feasible embodiments of the present invention and are not intended to limit the scope of protection of the present invention. All equivalent embodiments or modifications made without departing from the spirit of the present invention should be included within the scope of protection of the present invention.
Claims
1. Use of artesunate or artesunate-loaded matrix in preventing the attachment of large marine fouling organisms.
2. Use according to claim 1, characterized in that, The substrate loaded with artesunate is an acrylic silicone resin loaded with artesunate, an organosilicon resin loaded with artesunate, or an acrylic silicone coating loaded with artesunate.
3. Use according to claim 1, characterized in that, The large marine fouling organisms mentioned are mussels and / or barnacles.
4. Use according to claim 2, characterized in that, The artesunate-loaded silicone acrylate resin comprises artesunate and a silicone acrylate matrix. The raw materials for making the silicone acrylate matrix include methyl methacrylate, triisopropyl methacrylate, 2-methoxyethyl acrylate, azobisisobutyronitrile, benzoyl peroxide, and xylene. By mass ratio, the ratio of methyl methacrylate: triisopropyl methacrylate: artesunate: 2-methoxyethyl acrylate: azobisisobutyronitrile: benzoyl peroxide: xylene is 35-55: 35-60: 10-50: 0.5-10: 0.5-2: 0.5-1.5: 90-110.
5. Use according to claim 4, characterized in that, The method for preparing the artesunate-loaded silicone acrylate resin includes the following steps: In a reaction vessel equipped with a stirrer, thermometer, and reflux condenser, xylene is added according to the specified ratio, and the mixture is heated to 90°C under nitrogen protection. Then, methyl methacrylate, triisopropyl methacrylate, and 2-methoxyethyl acrylate are added. Azobisisobutyronitrile and benzoyl peroxide are slowly added dropwise as initiators, and the reaction is maintained at this temperature for 6-8 hours. After the reaction is completed, the mixture is cooled to room temperature to obtain a silicone acrylate prepolymer. Artesunate is dissolved in anhydrous ethanol and added to the prepolymer and stirred to obtain the artesunate-loaded silicone acrylate resin.
6. Use according to claim 2, characterized in that, The organosilicon resin loaded with artesunate comprises artesunate and an organosilicon resin matrix. The raw materials for making the organosilicon resin matrix include tetraethyl orthosilicate, n-octyltriethoxysilane, hydrochloric acid and isopropanol. By mass ratio, the ratio of tetraethyl orthosilicate: n-octyltriethoxysilane: artesunate: hydrochloric acid: isopropanol is 9-11:12-14:5-20:15-25:6-8.
7. Use according to claim 6, characterized in that, The method for preparing the artesunate-loaded organosilicon resin includes the following steps: at room temperature, tetraethyl orthosilicate, n-octyltriethoxysilane, and isopropanol are added sequentially to a reaction vessel and stirred for 30 minutes. Then, 0.1 mol / L hydrochloric acid is slowly added dropwise. After the addition is complete, stirring is continued for 24 hours to allow the system to fully hydrolyze and condense, forming a uniform sol and obtaining an organosilicon resin prepolymer. Artesunate is dissolved in anhydrous ethanol and added to the organosilicon resin prepolymer to obtain the artesunate-loaded organosilicon resin.
8. Use according to claim 2, characterized in that, The artesunate-loaded acrylic silicone coating comprises artesunate and an acrylic silicone coating. The raw materials for making the acrylic silicone coating include acrylic silicone resin, pigment, desparon, talc, bentonite, barium sulfate, plasticizer, compound antifouling component, and organic solvent. By mass ratio, the ratio of acrylic silicone resin: pigment: desparon: talc: bentonite: barium sulfate: plasticizer: artesunate: compound antifouling component: organic solvent is 45-55: 2-4: 1-3: 4-6: 0.5-1.5: 0.5-2: 0.5-2.5: 10-30: 0.5-20: 10-20.
9. Use according to claim 8, characterized in that, The method for preparing the acrylic silicone coating loaded with artesunate includes the following steps: (1) Add xylene, propylene glycol methyl ether, antifouling components, bentonite, pigment, talc, desparon, plasticizer and barium sulfate to a dispersion container according to the formula. First, stir at 800-1200 r / min for 10-15 minutes to make the components initially mixed evenly. Then increase the speed to 2500-3500 r / min and stir for 20-40 minutes to make the pigment and filler fully dispersed to the qualified fineness. (2) Add acrylic silicone resin and artesunate to the material obtained in step (1), stir at a speed of 1500-2500 r / min for 40-60 seconds, repeat stirring twice until completely mixed, and the acrylic silicone coating coating loaded with artesunate is obtained.
10. Use according to claim 8, characterized in that, The antifouling component is zinc oxide and / or titanium dioxide; and / or, the organic solvent is xylene and / or propylene glycol methyl ether; and / or, the pigment is iron oxide red; and / or, the plasticizer is chlorinated paraffin.