A graded packing system and method for xylene adsorptive separation apparatus
By utilizing a graded packing system and a three-dimensional graded topology of zeolite molecular sieve adsorbent, the problems of mass transfer kinetics, thermodynamics, and mechanical micro-leakage in the separation of para-xylene were solved, achieving efficient and stable para-xylene separation.
Patent Information
- Application Number
- CN202611250439.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-17
AI Technical Summary
Existing paraxylene separation technologies suffer from problems such as mass transfer kinetics and hydrodynamic pressure drop, uneven thermodynamic equilibrium, mechanical microleakage, and pore blockage caused by binders, which limit separation efficiency and product purity.
A graded packing system is adopted, including a distributed buffer layer, a core mass transfer layer and a support interception layer. Zeolite molecular sieve adsorbents with different particle sizes are used, and the packing is optimized by flexible porous interface isolation mesh and ultrasonic treatment to construct a three-dimensional graded topology.
This achieves deep decoupling of system pressure drop and mass transfer efficiency, reduces the heat release rate at the feed end, improves product purity and mechanical fault tolerance, reduces channel blockage, and enhances separation efficiency and stability.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of petrochemical separation engineering, and specifically relates to a graded packing system and method for a paraxylene adsorption separation unit. Background Technology
[0002] p-Xylene (PX) is an indispensable key basic chemical raw material. Industrially, p-xylene mainly comes from the C8 aromatic fraction of naphtha catalytic reforming or ethylene cracking gasoline. This fraction is usually composed of four isomers: p-xylene, m-xylene, o-xylene, and ethylbenzene. Because the physical boiling points of these isomers are extremely close, the distillation separation is extremely energy-intensive.
[0003] Currently, the industry widely adopts selective liquid-phase simulated moving bed (SMB) separation technology based on porous molecular sieves (such as barium-potassium exchange X-type molecular sieves). This technology utilizes the slight differences in steric hindrance and polarizability of molecular sieves for different C8 isomers to achieve highly selective physical adsorption. It is usually operated under isothermal conditions of 156~177℃ to obtain high-purity p-xylene.
[0004] Although simulated moving bed technology has been widely adopted, traditional homogeneous packing methods have revealed the following shortcomings: (1) Physical constraints of mass transfer kinetics and hydrodynamic pressure drop: According to the linear driving force (LDF) model, shortening the diffusion path inside the particles (i.e., reducing the adsorbent particle size) is an effective means to compress the mass transfer zone (MTZ) width and improve separation efficiency. However, according to the Ergun equation, the fluid friction pressure drop of the fixed bed is inversely proportional to the square of the adsorbent particle size. If the entire bed uses fine adsorbents, it will cause a significant increase in system pressure, which can easily lead to creep, crushing, and bed collapse of the bottom particles. Therefore, existing technologies often use adsorbents with a uniform particle size of 0.65~0.75 mm, which limits the improvement of separation efficiency.
[0005] (2) Adverse effects of thermodynamic equilibrium and jet distribution: Inside the industrial adsorption tower, the high-speed feed jet is prone to uneven kinetic energy distribution and axial backmixing. At the same time, the exothermic effect generated during the adsorption process will cause transient high temperature to be generated locally at the feed end. The temperature rise will lead to the saturation capacity and selectivity of the molecular sieve for the target component to decrease.
[0006] (3) Low tolerance for impurities caused by mechanical micro-leakage: Simulated moving beds rely on complex rotary valve or valve array systems. Under long-term operation, micro-leakage caused by wear on the sealing surface can lead to the mixed raw materials directly entering the extract flow path. Since traditional homogenized beds lack end-of-line interception mechanisms, micro-impurities can easily lead to substandard product purity.
[0007] (4) Pore blockage and desorption lag caused by binders: In the prior art, layered silicates such as kaolin are often used as molding binders for adsorbents. The layered structure of kaolin is prone to densification and accumulation during high-temperature calcination, which closes the pores of the molecular sieve, increases the diffusion resistance of heavy desorbents, and causes severe tailing of the desorption curve, increasing solvent consumption.
[0008] Therefore, there is an urgent need in this field to develop a novel adsorbent gradation packing system. Summary of the Invention
[0009] In order to overcome the above-mentioned shortcomings of the prior art, the purpose of this invention is to provide a graded packing system and method for a paraxylene adsorption and separation device.
[0010] The objective of this invention is achieved by at least one of the following technical solutions.
[0011] A graded packing system for a paraxylene adsorption and separation device is disclosed. The graded packing system is configured within an adsorption separation tower and comprises, in sequence according to the fluid flow direction: a distribution buffer layer, a core mass transfer layer, and a support interception layer. The average outer diameter of the first adsorbent filled in the distribution buffer layer is 0.75~0.90 mm. The average outer diameter of the second adsorbent filled in the core mass transfer layer is 0.40~0.55 mm. The average outer diameter of the third adsorbent filled in the support interception layer is 0.65~0.75 mm. All three adsorbents are zeolite molecular sieve adsorbents.
[0012] Furthermore, the fluid distribution buffer layer accounts for 15-25% of the effective filling height of the adsorption bed; the core mass transfer layer accounts for 50-70% of the effective filling height of the adsorption bed; and the support and interception layer accounts for 10-15% of the effective filling height of the adsorption bed.
[0013] Furthermore, the average outer diameter of the first adsorbent filled in the distribution buffer layer is 0.85 mm; the average outer diameter of the second adsorbent filled in the core mass transfer layer is 0.45 mm; and the average outer diameter of the third adsorbent filled in the support interception layer is 0.70 mm.
[0014] Furthermore, the distribution range of the first adsorbent matrix is 0.80~0.90 mm; the distribution range of the second adsorbent matrix is 0.40~0.55 mm; and the distribution range of the third adsorbent matrix is 0.65~0.75 mm.
[0015] Furthermore, the active components of the first adsorbent, the second adsorbent, and the third adsorbent are all octahedral zeolite X-type, and the silicon-aluminum molar ratio (SiO2 / Al2O3) of the octahedral zeolite X-type is 2.0~2.5.
[0016] Furthermore, the first adsorbent, the second adsorbent, and the third adsorbent all contain attapulgite, and the mass percentage of attapulgite in the raw materials for preparing the first adsorbent, the second adsorbent, and the third adsorbent is 5-15 wt%.
[0017] Furthermore, the first adsorbent, the second adsorbent, and the third adsorbent are all subjected to barium and potassium dual cation exchange treatment. The chemical composition of the first adsorbent, the second adsorbent, and the third adsorbent independently comprises, in terms of oxide weight percentage, 27.5~36.0 wt% barium content (BaO) and 0.5~2.0 wt% potassium content (K2O).
[0018] Furthermore, the chemical composition of the first adsorbent, in terms of oxide weight percentage, comprises: 27.5~30.0 wt% barium content (BaO), 0.5~2.0 wt% potassium content (K2O), and less than 1.2 wt% residual sodium content (Na2O).
[0019] More preferably, the chemical composition of the first adsorbent, in terms of oxide weight percentage, comprises: 30.0% barium content (BaO) and 1.0 wt% potassium content (K2O).
[0020] Furthermore, the chemical composition of the second adsorbent, in terms of oxide weight percentage, comprises: 30.5-34.0 wt% barium content (BaO) and 0.5-2.0 wt% potassium content (K2O).
[0021] More preferably, the chemical composition of the second adsorbent, in terms of oxide weight percentage, comprises: 34.0 wt% barium (BaO) and 1.0 wt% potassium (K2O).
[0022] Furthermore, the chemical composition of the third adsorbent, in terms of oxide weight percentage, comprises: 31.8~35.2 wt% barium content (BaO) and 0.5~2.0 wt% potassium content (K2O).
[0023] More preferably, the third adsorbent comprises, by weight percentage of oxides: 35.2 wt% barium (BaO), 1.0 wt% potassium (K2O), and less than 0.5 wt% residual sodium (Na2O).
[0024] Furthermore, the loss on ignition (LOI) of the first adsorbent, the second adsorbent, and the third adsorbent at 900°C is 3.5~6.7 wt%.
[0025] Furthermore, the loss on ignition (LOI) of the first, second, and third adsorbents at 900°C is 5.0~5.4 wt%. Furthermore, flexible porous interface isolation nets are provided at the first horizontal physical interface between the bottom surface of the distribution buffer layer and the top surface of the core mass transfer layer, and at the second horizontal physical interface between the bottom surface of the core mass transfer layer and the top surface of the support interception layer.
[0026] Furthermore, the flexible porous interface barrier is made of polytetrafluoroethylene (PTFE) or polyethersulfone (PES).
[0027] More preferably, the aperture of the flexible porous interface isolation mesh is ≤0.35mm, and the effective macroscopic physical opening cross-sectional area of the flexible porous interface isolation mesh accounts for ≥80% of the total area.
[0028] Furthermore, the preparation methods of the first adsorbent, the second adsorbent, and the third adsorbent specifically include the following steps: (1) A mixed dry powder is obtained by dry physical mixing of octahedral zeolite X type and attapulgite dry powder, wherein the silicon-aluminum molar ratio (SiO2 / Al2O3) of the octahedral zeolite X type is 2.0~2.5; and the amount of attapulgite added is 5~15 wt% of the total mass of the mixed dry powder. (2) Add a pore-forming agent to the mixed dry powder to obtain a mixed wet material, granulate the mixed wet material to obtain spherical particles; (3) The obtained spherical particles are continuously dried and dehydrated at 110~130 ℃ for 1~3 h, and then screened to obtain a first adsorbent matrix with an average particle outer diameter of 0.75~0.90 mm, a second adsorbent matrix with an average particle outer diameter of 0.40~0.55 mm, and a third adsorbent matrix with an average particle outer diameter of 0.65~0.75 mm; (4) The first adsorbent matrix, the second adsorbent matrix and the third adsorbent matrix are calcined at 500~650℃ for 2~4 h to obtain calcined particles of the first adsorbent matrix, calcined particles of the second adsorbent matrix and calcined particles of the third adsorbent matrix. (5) Liquid-phase ion exchange is performed on the first adsorbent matrix calcined particles, the second adsorbent matrix calcined particles, and the third adsorbent matrix calcined particles using aqueous solutions of barium and potassium salts, respectively, so that the chemical composition of the first adsorbent matrix calcined particles, in terms of oxide weight percentage, includes: barium content of 27.5~36.0 wt% (BaO) and potassium content of 0.5~2.0 wt% (K2O); the chemical composition of the second adsorbent matrix calcined particles, in terms of oxide weight percentage, includes: barium content of 27.5~36.0 wt% (BaO) and potassium content of 0.5~2.0 wt% (K2O); the chemical composition of the third adsorbent matrix calcined particles, in terms of oxide weight percentage, includes: barium content of 27.5~36.0 wt% (BaO) and potassium content of 0.5~2.0 wt% (K2O). (6) In an inert atmosphere, the calcined particles of the first adsorbent matrix, the calcined particles of the second adsorbent matrix, and the calcined particles of the third adsorbent matrix after ion exchange were dehydrated and activated at 200~300℃, respectively, until the loss on ignition at 900℃ was measured to be 3.5~6.7 wt%, and the first adsorbent, the second adsorbent, and the third adsorbent were obtained respectively.
[0029] Furthermore, in step (2), the pore-forming agent is a 3-10% aqueous solution of sodium carboxymethyl cellulose.
[0030] Furthermore, in step (4), the chemical composition of the first adsorbent matrix calcined particles, in terms of oxide weight percentage, includes: barium content of 27.5~30.0 wt% (BaO) and potassium content of 0.5~2.0 wt% (K2O).
[0031] Furthermore, in step (4), the chemical composition of the second adsorbent matrix calcined particles, in terms of oxide weight percentage, includes: barium content of 30.5~34.0 wt% (BaO) and potassium content of 0.5~2.0 wt% (K2O).
[0032] Furthermore, in step (4), the chemical composition of the third adsorbent matrix calcined particles, in terms of oxide weight percentage, includes: barium content of 31.8~35.2 wt% (BaO) and potassium content of 0.5~2.0 wt% (K2O).
[0033] The present invention also provides a method for filling a graded packing system for a xylene adsorption and separation device, specifically including the following steps: (1) Construction of the support and interception layer: On the support grid at the bottom of the adsorption separation tower, the third adsorbent is uniformly filled by gravity stacking until the third adsorbent accounts for 10 to 15% of the total effective filling height of the adsorption bed to form a support and interception layer. (2) Bottom interface isolation: A bottom flexible porous interface isolation mesh is horizontally laid on the top surface of the supporting interception layer; (3) Filling of the core mass transfer layer: Liquid aromatic solvent medium is injected into the adsorption separation tower to establish a buffer surface. The second adsorbent is then filled until it occupies 50-70% of the total effective filling height of the adsorption bed to form the core mass transfer layer. During the filling process, an ultrasonic wave generator array immersed in the liquid phase is used, with a transmission frequency of 20-40 kHz and a spatial power density of 1.0-2.5 W / cm². 2 Ultrasound; (4) Top-level interface isolation: A top-level flexible porous interface isolation mesh is horizontally laid on the top surface of the core mass transfer layer; (5) Assembly of the distribution buffer layer: On the top flexible porous interface isolation net, the first adsorbent is filled to 15-25% of the total effective filling height of the adsorption bed.
[0034] Furthermore, in step (3), the liquid-phase aromatic solvent medium is p-diethylbenzene.
[0035] Furthermore, in step (5), during the first adsorbent loading process, an ultrasonic wave generator array immersed in the liquid phase is used, with an emission frequency of 20~40 kHz and a spatial power density of 1.0~2.5 W / cm². 2 Ultrasound.
[0036] Furthermore, the flexible porous interface barrier is made of polytetrafluoroethylene (PTFE) or polyethersulfone (PES).
[0037] Furthermore, the aperture of the flexible porous interface isolation mesh is ≤0.35mm, and the effective macroscopic physical opening cross-sectional area of the flexible porous interface isolation mesh accounts for ≥80% of the total area.
[0038] The present invention also provides a method for adsorbing and separating p-xylene from mixed aromatics using the graded packing system described in any one of the above claims, specifically comprising the following steps: The C8 aromatic feed stream is fed into the graded packing system, the temperature of which is 120~180℃ and the back pressure of which is 8.0~25 bar. The p-xylene adsorbed in the solid phase is displaced and desorbed using a desorbent stream containing a desorbent agent. The volumetric flow rate ratio of the desorbent stream to the C8 aromatic feed stream is controlled to be 1.0~2.0. The extract rich in p-xylene and the raffinate rich in non-p-xylene isomers are collected separately.
[0039] Furthermore, the desorbent is p-diethylbenzene or toluene.
[0040] Furthermore, the temperature of the graded packing system is 175°C.
[0041] Furthermore, the apparent linear velocity of the fluid in the core mass transfer region is 0.5~2.5 cm / s.
[0042] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) This invention achieves deep decoupling of system pressure drop and mass transfer efficiency by constructing a three-dimensional graded topology structure consisting of a 15%-25% distribution buffer layer, a 50%-70% core mass transfer layer, and a 10%-15% support interception layer. The distribution buffer layer utilizes its large-particle coarse-pore gap network to effectively dissipate the jet non-uniform kinetic energy of the feed distributor, promoting the transformation of turbulent flow into laminar plug flow. The low-resistance large-particle sections at both ends release the pressure drop surplus, compensating for the surge in local resistance caused by the use of fine particles in the middle core mass transfer layer. Under the premise of maintaining the total fluid friction pressure drop at a safe threshold during steady-state operation, the theoretical width of the mass transfer zone is successfully compressed, significantly improving the single-pass yield of paraxylene.
[0043] (2) By setting a distributed buffer layer at the feed end, the present invention reduces the surface adsorption affinity in the initial contact stage and slows down the instantaneous heat release rate at the feed end. This allows the originally concentrated adsorption heat to be released gradually in the axial physical space, effectively reducing the maximum heat release temperature rise of transient adsorption at the feed end, and ensuring that the core mass transfer layer is always in a working state with a low temperature and high saturation capacity.
[0044] (3) The present invention sets a barium zeolite molecular sieve support interception layer with high ion exchange degree at the outlet end. When subjected to strong polar impurity pulse impact, the support interception layer uses electrostatic competitive repulsion and spatial steric hindrance effect to intercept impurities, avoid drastic fluctuations in product purity, and improve the mechanical fault tolerance and operational stability of industrial equipment.
[0045] (4) The present invention uses attapulgite as a molding binder, which improves the pore structure at the mesoscale: the unique one-dimensional needle-like crystals of attapulgite form an interpenetrating rigid support network during high-temperature calcination, which effectively suppresses the closed-pore effect during heat treatment and retains abundant macropores and mesopore channels; while maintaining the compressive strength of a single particle, it significantly reduces the diffusion steric hindrance of heavy desorbents deep in the pores and eliminates the desorption tailing phenomenon in the desorption stage. Detailed Implementation
[0046] The following examples further illustrate specific implementations of the present invention, but the implementation and protection of the present invention are not limited thereto. It should be noted that any processes not specifically described below are those that can be implemented or understood by those skilled in the art by referring to existing technology. Reagents or instruments whose manufacturers are not specified are considered to be conventional products that can be purchased commercially.
[0047] In this invention, the term "steady-state total fluid frictional pressure drop" refers to the static pressure difference between the inlet and outlet ends caused by the frictional resistance generated between the fluid and the surface, internal pore channels, and column wall of the adsorbent when the process fluid (including feed liquid or desorbent) flows through a packed bed of adsorbent under constant operating temperature, operating pressure, and feed linear velocity conditions.
[0048] In this invention, the term "theoretical mass transfer zone" refers to the longitudinal physical length of the packing layer in the adsorption column that is in an active adsorption state during dynamic adsorption. It represents the specific physical region occupied by the adsorbate (para-xylene) in the adsorption bed as the feed concentration decreases to the breakthrough concentration.
[0049] In this invention, the term "maximum exothermic temperature rise during transient adsorption at the feed end" refers to the peak increase in local temperature of the adsorption bed caused by the rapid release of adsorption heat when the feed fluid containing the target component (paraxylene) first contacts the front end of the adsorption bed during dynamic adsorption.
[0050] In this invention, the term "evolutionary rise rate of total system frictional pressure drop after 300 cycles" refers to the percentage increase in the total pressure drop of the system under steady-state operation relative to the initial steady-state pressure drop after the adsorption bed has undergone 300 step switching cycles of alternating hydraulic shock in a simulated moving bed (SMB) continuous separation evaluation system.
[0051] Example 1 (1) Weigh octahedral zeolite X-type (its silicon-aluminum molar ratio was determined to be 2.0 by X-ray fluorescence spectrometry) and attapulgite dry powder as dry powder matrix, and place them in a three-dimensional zero-gravity mixer for dry physical cross-linking. The amount of attapulgite added is 5 wt% of the total mass of the mixed dry powder. (2) A 3% sodium carboxymethyl cellulose aqueous solution was uniformly added to the dry powder matrix to obtain a mixed wet material. The mixed wet material was then transferred to a disc granulator for rolling granulation to obtain spherical particles. (3) The obtained spherical particles were continuously dried and dehydrated at 120℃ for 2 h, and then sent to a multi-layer vibrating screen for sieving to obtain a first adsorbent matrix with an average particle size of 0.85 mm (distribution range 0.80~0.90 mm), a second adsorbent matrix with an average particle size of 0.45 mm (distribution range 0.40~0.55 mm), and a third adsorbent matrix with an average particle size of 0.70 mm (distribution range 0.65~0.75 mm). (4) Place the three groups of substrates with different particle sizes in a muffle furnace and calcine them at 500°C in an oxygen-rich air atmosphere for 4 hours to burn off the organic pore-forming template agent carboxymethyl cellulose and promote the initial sintering and shaping of the binder. (5) Ion exchange and activation water control stage: Taking the first adsorbent matrix as the object, a mixed aqueous solution of barium chloride (BaCl2) and potassium chloride (KCl) with a concentration of 0.1 mol / L was used as the exchange liquid. Single-pass co-current exchange was carried out at 90℃. The exchange process continued until the solid phase after washing and drying was chemically analyzed. Based on oxides, the content of BaO was 28.0 wt%, the content of K2O was 0.5 wt%, and the residual Na2O content was controlled below 1.1 wt%. For the second adsorbent matrix, a mixed aqueous solution of barium chloride and potassium chloride with a concentration of 0.1 mol / L was used as the exchange liquid. Multi-stage countercurrent exchange was carried out at 90℃ so that the content of BaO in the modified matrix (after washing and drying, based on oxides) was 33.5 wt% and the content of K2O was 1.0 wt%. For the third adsorbent matrix, a mixed aqueous solution of barium chloride (BaCl2) and potassium chloride (KCl) with a concentration of 0.5 mol / L was used as the exchange liquid. BaCl2 was subjected to multi-stage countercurrent exchange at 100℃ to achieve a BaO content of 34.5 wt% and a K2O content of 0.5 wt% in the modified matrix (calculated on an oxide basis after washing and drying). After the matrix was washed with deionized water until neutral and free of free chloride ions, it was placed in an activation device, purged with dry nitrogen, and slowly dehydrated at 200℃ until the loss on ignition (LOI) of the finished product was maintained at 4.0 wt% ± 0.5 wt% according to Karl Fischer moisture analysis and 900℃ ignition test, yielding the first, second, and third adsorbents.
[0052] Example 2 The silica-alumina molar ratio of the octahedral zeolite X type is 2.2, and the amount of attapulgite added is 10 wt% of the total mass of the mixed dry powder; the calcination temperature in step (4) is 600℃, and the holding time is 3h; in step (5) the ion exchange stage, the first adsorbent matrix is calculated based on oxides, with BaO mass fraction of 30.0 wt% and K2O mass fraction of 1.0 wt%; the second adsorbent matrix is calculated based on oxides, with BaO mass fraction of 34.0 wt% and K2O mass fraction of 1.0 wt%; the third adsorbent matrix is calculated based on oxides, with BaO mass fraction of 35.2 wt% and K2O mass fraction of 1.0 wt%, and the residual Na2O is strictly less than 0.5 wt%; in step (5) the dehydration and activation stage, the activation temperature is set at 250℃, and the loss on ignition (LOI) is maintained at 5.2±0.2 wt%.
[0053] The remaining preparation process is the same as in Example 1. Example 3 The silica-alumina molar ratio of the octahedral zeolite X type is 2.5, and the amount of attapulgite added is 15 wt% of the total mass of the mixed dry powder; the calcination temperature in step (4) is 650℃, and the holding time is 2h; in step (5) the ion exchange stage, the first adsorbent matrix is calculated based on oxides, with BaO mass fraction of 27.5 wt% and K2O mass fraction of 2.0 wt%; the second adsorbent matrix is calculated based on oxides, with BaO mass fraction of 30.5 wt% and K2O mass fraction of 1.5 wt%; the third adsorbent matrix is calculated based on oxides, with BaO mass fraction of 31.8 wt% and K2O mass fraction of 1.0 wt%, and the residual Na2O is strictly less than 0.5 wt%; in step (5) the dehydration and activation stage, the activation temperature is set at 300℃, and the loss on ignition (LOI) is maintained at 6.5±0.5 wt%.
[0054] The remaining preparation process is the same as in Example 1. Comparative Example 1 The silicon-aluminum molar ratio of the octahedral zeolite X type is 2.2. 10 wt% layered kaolin is used to replace attapulgite as a binder. All granulated particles are cut and sieved into adsorbent matrix with an average particle size of 0.65 mm (distribution range 0.60~0.70 mm). The ion exchange and activation water control stages are the same as the third adsorbent matrix in Example 2. The rest of the preparation process is the same as in Example 2.
[0055] Comparative Example 2 All granulated particles were cut and sieved into adsorbent matrix with an average particle size of 0.45 mm (distribution range 0.40~0.50 mm). The ion exchange and activation water control stages were the same as the second adsorbent matrix in Example 2, and the rest of the preparation process was the same as in Example 2.
[0056] The physicochemical structure of the adsorbent particles located in the core mass transfer zone, specifically the second adsorbent particles of Examples 1-3 and the adsorbent particles of Comparative Example 1, were characterized using a multi-channel specific surface area and porosity analyzer (based on the N2 physical adsorption-desorption curve at 77K, with specific surface area calculated using the BET model and pore size distribution analyzed using the BJH model), a high-pressure mercury porosimeter (to measure the volume of macropores larger than 50 nm between and within particles), and a particle compressive strength tester. Experimental data are shown in Table 1.
[0057] Table 1. Physicochemical characteristics of particles in Examples 1-3 and comparative examples As shown in Table 1, provided that the compressive strength of a single particle meets industrial requirements (>10 N / particle), Examples 1-3, using attapulgite as the bonding system, exhibit significantly higher N2 adsorption specific surface area and open macropore volume (greater than 50 nm) than Comparative Example 1, which uses an equal amount of kaolin. The macropore volume in Example 2 reaches 0.18 cm³. 3 / g, approximately three times that of Comparative Example 1. This indicates that the needle-like crystals unique to attapulgite interpenetrate and form a three-dimensional support network during high-temperature calcination, effectively suppressing the dense stacking and closed-pore phenomenon of the lamellar structure. This abundant macroporous network can significantly reduce the mass transfer resistance between heavy desorbents and paraxylene molecules within the adsorbent, thereby increasing the diffusion rate.
[0058] Example 4 To systematically evaluate the macroscopic fluid dynamics and mass transfer thermodynamics effects of each physical section of the distribution system, a high-pressure thick-walled 316L stainless steel separation column with an inner diameter of 50 mm and an effective internal packing height calibrated to 700 mm was customized (this height-to-diameter ratio is sufficient to eliminate the non-plug flow effect caused by pipe wall flow).
[0059] (1) Construction of the support and interception layer: First, the third adsorbent (average particle size 0.70 mm) prepared in Example 1 was uniformly laid on the microporous stainless steel support grid at the bottom of the separation column by gravity filling to form a bottom support and interception zone with a height of 105 mm (accounting for 15% of the total filling height). Subsequently, a flexible polytetrafluoroethylene (PTFE) polymer mesh with a pore size of 0.30 mm and an effective porosity of 85% was laid on the surface of this layer.
[0060] (2) Packing of the core mass transfer layer: Pump liquid phase into the separation column to half the height of the separation column to establish a liquid phase buffer interface. In the wet suspension state, the second adsorbent prepared in Example 1 (average particle size of 0.45 mm) is continuously introduced. During the filling process, an ultrasonic amplitude transformer is used to inject a 20 kHz frequency and a power density of 1.5 W / cm³ into the liquid phase. 2 The ultrasonic waves utilize the ultrasonic cavitation effect to strip the adsorbed gas film on the particle surface, promoting the geometric rearrangement and densification of the particles until a core mass transfer zone with a height of 490 mm (accounting for 70% of the total filling height) is formed. (3) Construction of the distribution buffer layer: A flexible polytetrafluoroethylene (PTFE) polymer mesh with a pore size of 0.30 mm and an effective porosity of 85% is laid on the top of the core mass transfer zone; the first adsorbent (average particle size of 0.80 mm) prepared in Example 1 is continuously introduced under wet suspension. During the filling process, an ultrasonic amplitude transformer is used to inject a 20 kHz frequency and a power density of 1.5 W / cm³ into the liquid phase. 2 The ultrasonic waves utilize the ultrasonic cavitation effect to peel off the adsorbed gas film on the particle surface, promoting the geometric rearrangement and densification of the particles until a distributed buffer layer with a height of 105 mm (accounting for 15% of the total filling height) is formed. (4) Flange top tightening.
[0061] The gradation structure ratio of Example 4 is: 15% distributed buffer layer, 70% core mass transfer layer, and 15% support interception layer.
[0062] Example 5 Using the series of adsorbent materials from Example 2 and following the filling process of Example 4, a third adsorbent support and interception layer with a height of 140 mm (accounting for 20% of the total height), a second adsorbent core mass transfer layer with a height of 455 mm (accounting for 65%), and a first adsorbent fluid distribution buffer layer with a height of 105 mm (accounting for 15%) were sequentially established in the separation column; a PTFE flexible porous interface isolation mesh was laid between each layer.
[0063] The ultrasound frequency is 30 kHz.
[0064] The gradation structure ratio of Example 5 is: 15% distributed buffer layer, 65% core mass transfer layer, and 20% support and interception layer.
[0065] Example 6 Using the series of adsorbent materials from Example 3 and following the filling process of Example 4, a third adsorbent support and interception layer with a height of 175 mm (accounting for 25% of the total height), a second adsorbent core mass transfer layer with a height of 420 mm (accounting for 60%), and a first adsorbent fluid distribution buffer layer with a height of 105 mm (accounting for 15%) were sequentially established in the separation column; a PTFE flexible porous interface isolation mesh was laid between each layer.
[0066] The ultrasound frequency is 40 kHz.
[0067] The gradation structure ratio of Example 5 is: 25% distributed buffer layer, 60% core mass transfer layer, and 15% support interception layer.
[0068] Comparative Example 3 The separation column used the adsorbent prepared in Comparative Example 1 (average particle size 0.65 mm, with kaolin as binder).
[0069] Filling process: Gravity pouring is used to fill the effective filling height of 700mm; no flexible isolation net is laid inside the bed, and no acoustic cavitation is implemented during the filling process.
[0070] Comparative Example 4 The separation column used the adsorbent prepared in Comparative Example 2 (average particle size 0.45 mm).
[0071] Filling process: Gravity pouring is used to fill the effective filling height of 700mm; no flexible isolation net is laid inside the bed, and no acoustic cavitation is implemented during the filling process.
[0072] Comparative Example 5 The adsorbent material, the thickness ratio of each layer, and the filling process are the same as in Example 6, except that a flexible porous polytetrafluoroethylene (PTFE) isolation net is not laid between the three graded sections.
[0073] Effect verification To evaluate the dynamic separation performance of each adsorbent configuration in Examples 4-6 and Comparative Examples 3-5 under simulated industrial cracked gasoline conditions, the following evaluation system was established: Feed control: A high-pressure dual-plunger micro-stepping constant flow pump was used at the front end. The experimental feed was a multi-component mixed C8 aromatic hydrocarbon, with the following mass percentage composition: p-xylene (PX) 22%, m-xylene (MX) 45%, o-xylene (OX) 18%, and ethylbenzene (EB) 15%.
[0074] Elution conditions: The eluent used is 99.5% pure p-diethylbenzene (PDEB).
[0075] Operating parameters: The feed flow rate is constant at 120 mL / min (the apparent downward linear velocity of the fluid in the empty tower is approximately 1.0 cm / s). The system back pressure is maintained at 8.0 bar by a back pressure regulating valve, and the system temperature is controlled at 175°C by a thermal oil furnace jacket heater.
[0076] Data acquisition: The effluent concentration curve (breakthrough curve) and transient temperature rise at the feed end of the bed are continuously monitored using online gas chromatography and a high-frequency micro thermocouple array distributed along the bed.
[0077] Simulated mechanical microleakage and strong polar impurity pulse impact test: High-purity anhydrous methanol was selected as the polar impurity and pre-dissolved in p-diethylbenzene (PDEB) to prepare a pulse mother liquor with a concentration of 1000 mg / L. The pulse mother liquor was instantaneously injected into the main feed stream at a flow rate of 1.2 mL / min for 20 min to simulate the chemical impact caused by the strong polar impurity from the mechanical microleakage. The pulse injection was then stopped, and normal operation was resumed. The transient fluctuations in the purity of p-xylene in the effluent were continuously monitored and recorded.
[0078] Cyclic aging test: The system temperature was maintained at 175℃, and the reference back pressure was 8.0 bar. A mixed C8 aromatic hydrocarbon was used as the circulating medium, with a constant feed flow rate of 180 mL / min. An automated program controlled the outlet back pressure valve, generating a pressure jump of ±1.5 bar every 300 s to simulate the hydraulic shock during moving bed switching, and the system was continuously operated for 10,000 hours. After the test, the structure was dissected as follows: heating was stopped and the pressure was slowly released to atmospheric pressure to drain the residual liquid from the column; the separation column was vertically fixed, and sampling was performed layer by layer starting from the top flange using a micro-negative pressure suction device. The sampling step distance was set to 10 mm; the PTFE flexible mesh located at the gradation interface was removed, ultrasonically cleaned in ethanol, and then dried.
[0079] Table 2. Simulated industrial pyrolysis gasoline performance in Examples 4-6 As can be seen from the data comparison in Table 2, although Comparative Example 4 improved the mass transfer efficiency to some extent by using fine particles with an average particle size of 0.45 mm throughout the bed, according to the Ergun equation, the reduction in particle size will lead to a significant decrease in bed porosity and an increase in the fluid flow tortuosity factor, resulting in a nonlinear and sharp increase in the frictional resistance of the fluid passing through the bed. Specifically, the total pressure drop ΔP of the Comparative Example 4 system increased to 1.35 bar. In large-scale industrial adsorption towers, overpressure conditions can easily lead to safety accidents such as deformation of the support grid structure, flooding within the tower, and overall bed instability.
[0080] Examples 4-6 employ heterogeneous distribution, incorporating large particle buffer zones at both ends of the bed, accounting for 30-40% of the total height. Due to the higher external porosity of these regions, they effectively neutralize the local resistance generated by particles in the core mass transfer zone. The steady-state total pressure drop of the systems in Examples 4-6 is controlled at 0.41-0.45 bar, maintaining efficient mass transfer while achieving hydrodynamic loads comparable to Comparative Example 3 (traditional homogeneous bed).
[0081] Examples 4-6 utilize the fine particles in the core mass transfer region to shorten the radial diffusion path of the solute within the crystal. The theoretical width of the mass transfer region in Examples 4-6 is compressed to 35-39 mm, which is more than 60% smaller than that in Comparative Example 3, thus improving the bed utilization rate.
[0082] In Comparative Example 3, due to the uniform adsorption affinity throughout the entire bed, a violent transient adsorption exothermic reaction occurs at the feed end, resulting in a maximum temperature rise of up to ΔT as high as 12℃. According to the principle of adsorption thermodynamic equilibrium, the local temperature rise will cause the adsorption isotherm to shift towards the high-pressure side, thereby reducing the effective adsorption capacity of the adsorbent.
[0083] Examples 4-6 use a first adsorbent with low adsorption affinity as a distribution buffer layer, and control its macropore volume to ≥0.25 cm³. 3 / g, while maintaining a certain residual sodium ion content, effectively controlling the adsorption heat release rate. This layer can attenuate and dissipate the concentrated heat generated at the adsorption front in the axial direction, thereby stabilizing the maximum temperature rise in the bed inlet region at 4.8~5.5℃. After this temperature field optimization, the core mass transfer zone can maintain a near-isothermal environment, ensuring that the adsorbent always has a high saturation adsorption capacity.
[0084] In simulated mechanical microleakage-induced pulse shock tests of highly polar impurities, the purity of products in Comparative Examples 3-4 rapidly deteriorated, while the third adsorbent filled in the bottom layer in Examples 4-6 had an extremely high barium ion loading, constructing a strong electrostatic field within the crystal micropores. Based on the differences in polarizability of different xylene isomers, this electrostatic field selectively repels the more polarizable m-xylene and o-xylene through Coulomb interactions. Combined with the steric hindrance effect of the pores, this achieves highly efficient separation of para-xylene molecules. Ultimately, the purity of the exported para-xylene can be stably maintained within the range of 99.82%-99.90%.
[0085] Cyclic aging tests confirmed that, in the absence of a PTFE insulating mesh, Comparative Example 4 experienced interlayer mixing under alternating fluid pressure differentials. In contrast, Examples 4-6, through the mechanical restraint of a high-porosity PTFE flexible mesh, achieved physical locking of each functional zone, ensuring the structural integrity of the multi-layered structure during long-term operation.
[0086] Micro-simulated moving bed continuous purification experiment: The system is equipped with eight high-pressure, thick-walled 316L stainless steel separation columns with an inner diameter of 50 mm and an effective internal packing height of 700 mm.
[0087] All eight columns in the experimental group were filled with the same series of adsorbent materials, filling processes, and gradation structure ratios as described in Example 5.
[0088] The control group used the same adsorbent material and filling process as Comparative Example 3.
[0089] A 128-channel zero-dead-volume micro-solenoid valve array, controlled by a central industrial control PLC, is used to control the step time to achieve periodic switching of the feed port, desorbent port, extractor port, and raffinate port, simulating a countercurrent mass transfer process.
[0090] The system adopts the industrial 2-3-3 asymmetric physical partitioning logic: Zone I (Desorption Zone): Contains two columns (Column 1 and Column 2), which bear the highest fluid linear velocity and the main system pressure drop load.
[0091] Zone II (Refining Zone): Contains 3 columns (columns 3 to 5), responsible for the reflux refining of the target product.
[0092] Zone III (Adsorption Zone): Contains 3 columns (columns 6 to 8), responsible for the initial separation and extraction of raw materials.
[0093] The experiment simulated extreme industrial operating conditions, with a constant feed flow rate of 180 mL / min. The system back pressure was maintained at 15 bar by a back pressure regulating valve, and the system temperature was controlled at 175℃ by a heat transfer oil furnace jacket heater. The experimental feed was a multi-component mixed C8 aromatic hydrocarbon, with the following mass percentage composition: p-xylene (PX) 22%, m-xylene (MX) 45%, o-xylene (OX) 18%, and ethylbenzene (EB) 15%. The eluent used was 99.5% pure p-diethylbenzene (PDEB). The volumetric flow rate ratio of the desorbent to the feed liquid was set to 1.40. 300 switching cycles were performed continuously.
[0094] After the system is running stably, parallel sampling of each outflow stream is performed using multi-channel online gas chromatography.
[0095] Table 3 Results of continuous purification experiments using a micro-simulated moving bed As shown in Table 3, under simulated industrial extreme low-energy consumption conditions (desorbent / feed liquid ratio = 1.40), the experimental and control groups exhibited significant performance differences: the experimental group achieved a single-pass steady-state yield of 99.2% for xylene, with a product purity exceeding 99.95%. In contrast, the control group, using a uniform bed, under the same low solvent consumption conditions, suffered from a severe mass transfer tailing effect in the desorption zone due to insufficient macropore volume in the kaolin binder system, resulting in some target compounds failing to be effectively replaced. Consequently, the xylene yield was only 94.5%, and the purity was only 99.30%. This indicates that the porous structure based on needle-shaped attapulgite, combined with a core mass transfer layer of fine particles, significantly shortened the intracrystalline diffusion path, eliminated the diffusion lag of heavy desorbents at the mesoscopic depth, and ensured efficient replacement under high-speed valve-cutting cycles.
[0096] After 300 cycles, the fluid resistance of the control group system showed a continuous increase of 8.0%. Disassembly and inspection revealed that this was due to the lack of a pressure drop dissipation mechanism in the homogeneous bed, causing the bottom particles to mechanically pulverize and block the flow channels due to long-term alternating stress. The pressure fluctuation rate of the experimental group system was controlled within 1.5%, indicating that the isolation mesh and gradation structure effectively dissipated the hydraulic impact kinetic energy. The PTFE isolation mesh prevented interlayer mixing and secondary sedimentation between particles, maintaining the long-term integrity of the bed structure.
[0097] The above embodiments are merely preferred embodiments of the present invention and are only used to explain the present invention, not to limit the present invention. Any changes, substitutions, modifications, etc., made by those skilled in the art without departing from the spirit and essence of the present invention should be within the protection scope of the present invention.
Claims
1. A graded packing system for a para-xylene adsorption and separation device, characterized in that, The graded packing system is configured inside the adsorption separation tower. The graded packing system includes, in sequence according to the fluid flow direction: a distribution buffer layer, a core mass transfer layer, and a support interception layer. The average outer diameter of the first adsorbent filled in the distribution buffer layer is 0.75~0.90 mm. The average outer diameter of the second adsorbent filled in the core mass transfer layer is 0.40~0.55 mm. The average outer diameter of the third adsorbent filled in the support interception layer is 0.65~0.75 mm. The first, second, and third adsorbents are all zeolite molecular sieve adsorbents.
2. The graded packing system according to claim 1, characterized in that, The distributed buffer layer accounts for 15-25% of the effective filling height of the adsorption bed; the core mass transfer layer accounts for 50-70% of the effective filling height of the adsorption bed; and the support and interception layer accounts for 10-15% of the effective filling height of the adsorption bed.
3. The graded packing system according to claim 1, characterized in that, The average outer diameter of the first adsorbent filled in the distribution buffer layer is 0.85 mm; the average outer diameter of the second adsorbent filled in the core mass transfer layer is 0.45 mm; and the average outer diameter of the third adsorbent filled in the support interception layer is 0.70 mm.
4. The graded packing system according to claim 1, characterized in that, The active components of the first, second, and third adsorbents are all octahedral zeolite X-type, and the silicon-aluminum molar ratio of the octahedral zeolite X-type is 2.0~2.
5.
5. The graded packing system according to claim 1, characterized in that, The first, second, and third adsorbents all contain attapulgite, and the mass percentage of attapulgite in the raw materials for preparing the first, second, and third adsorbents is 5-15 wt%.
6. The graded packing system according to claim 1, characterized in that, The first, second, and third adsorbents are all subjected to barium and potassium dual cation exchange treatment. The chemical composition of the first, second, and third adsorbents, in terms of oxide weight percentage, independently includes: barium content of 27.5~36.0 wt% (BaO) and potassium content of 0.5~2.0 wt% (K2O).
7. The graded packing system according to claim 1, characterized in that, The loss on ignition of the first, second, and third adsorbents at 900°C is 3.5 to 6.7 wt%.
8. The graded packing system according to claim 1, characterized in that, Flexible porous interface isolation nets are provided at the first horizontal physical interface between the bottom surface of the distribution buffer layer and the top surface of the core mass transfer layer, and at the second horizontal physical interface between the bottom surface of the core mass transfer layer and the top surface of the support interception layer.
9. A method for filling a graded packing system in a paraxylene adsorption separation unit, characterized in that... Specifically, the following steps are included: (1) Construction of the support and interception layer: On the support grid at the bottom of the adsorption separation tower, the third adsorbent is uniformly filled by gravity stacking until the third adsorbent accounts for 10 to 15% of the total effective filling height of the adsorption bed to form a support and interception layer. (2) Bottom interface isolation: A bottom flexible porous interface isolation mesh is horizontally laid on the top surface of the supporting interception layer; (3) Filling of the core mass transfer layer: Liquid aromatic solvent medium is injected into the adsorption separation tower to establish a buffer surface. The second adsorbent is then filled until it occupies 50-70% of the total effective filling height of the adsorption bed to form the core mass transfer layer. During the filling process, an ultrasonic wave generator array immersed in the liquid phase is used, with a transmission frequency of 20-40 kHz and a spatial power density of 1.0-2.5 W / cm². 2 Ultrasound; (4) Top-level interface isolation: A top-level flexible porous interface isolation mesh is horizontally laid on the top surface of the core mass transfer layer; (5) Assembly of the distribution buffer layer: On the top flexible porous interface isolation net, the first adsorbent is filled to 15-25% of the total effective filling height of the adsorption bed.
10. A method for adsorbing and separating p-xylene from mixed aromatics using the graded packing system according to any one of claims 1-8, specifically comprising the following steps: The C8 aromatic feed stream is fed into the graded packing system. The temperature of the graded packing system is 120~180℃, and the back pressure of the graded packing system is 8.0~25 bar. The p-xylene adsorbed in the solid phase is displaced and desorbed using a desorbent stream containing a desorbent agent. The volumetric flow rate ratio of the desorbent stream to the C8 aromatic feed stream is controlled to be 1.0~2.
0. The extract rich in p-xylene and the raffinate rich in non-p-xylene isomers are collected separately.