A cross-linked polyether block polyamide membrane, its preparation method and application

By using 2,4-toluene diisocyanate crosslinked polyether block polyamide membranes, the problems of easy swelling and insufficient separation selectivity of polyether block polyamide membranes were solved, and a crosslinked PEBA/PSf composite membrane with better swelling resistance and stability was prepared for pervaporation separation of aromatics and alkanes.

CN123102162APending Publication Date: 2026-11-17CHINA INST FOR RADIATION PROTECTION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611204964.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polyether block polyamide membranes are prone to swelling and have poor stability during the separation of aromatic and alkane hydrocarbons, resulting in low separation selectivity.

Method used

Crosslinked polyether block polyamide membranes were prepared by spin coating using 2,4-toluene diisocyanate as a crosslinking agent. The crosslinking effect was used to inhibit chain segment mobility and strengthen the hydrogen bond interaction between chain segments to prepare crosslinked PEBA/PSf composite membranes.

Benefits of technology

It improves the membrane's resistance to swelling and stability, enhances the solubility selectivity for aromatics, and achieves excellent performance in the separation of aromatics and alkanes by pervaporation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102162A_ABST
    Figure CN123102162A_ABST
Patent Text Reader

Abstract

This invention discloses a crosslinked polyether block polyamide membrane, its preparation method, and its applications, addressing the problems of poor swelling resistance and stability, and insufficient selectivity for aromatic hydrocarbon dissolution, in existing polyether block polyamide membranes. This application uses 2,4-toluene diisocyanate as a crosslinking agent. The polyether block polyamide membrane obtained by spin coating is immersed in a hexane solution of 2,4-toluene diisocyanate to prepare the crosslinked polyether block polyamide membrane. The crosslinked polyether block polyamide membrane of this invention exhibits excellent swelling resistance and stability during the pervaporation separation of aromatics and alkanes, and shows better selectivity for aromatic hydrocarbon dissolution compared to existing technologies, making it applicable to the pervaporation separation of aromatics and alkanes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of membrane separation materials technology, and particularly relates to a cross-linked polyether block polyamide membrane, its preparation method and application. Background Technology

[0002] With the increasing demand for various petroleum products driven by human economic and social development and the growing scarcity of petroleum resources worldwide, the molecular-oriented management and utilization of petroleum fractions has gradually attracted widespread attention in the petrochemical industry. Naphtha is a light fraction of crude oil or coal tar, ranging from its initial boiling point at atmospheric distillation to 200°C. Its main components are n-alkanes, isoalkanes, cycloalkanes, and aromatics, with carbon atoms ranging from 4 to 10. The downstream industries of naphtha have complementary demands for its hydrocarbon composition. Alkanes have low aromatics correlation index (BMCI) values, resulting in high yields when used for ethylene production via cracking. Therefore, alkanes are high-quality feedstocks for ethylene production via cracking, while oil products with high cycloalkanes and aromatics content are high-quality feedstocks for aromatics production via catalytic reforming. When naphtha is used as a feedstock for ethylene production via steam cracking, the 10-25% aromatics it contains cannot be cracked into olefins, leading to a significant increase in the process's heat load. Aromatics also cause coking in the ethylene cracking furnace, shortening the operating cycle of the ethylene unit and significantly increasing production costs. Furthermore, aromatics, as a basic raw material in the petrochemical industry, are widely used in the synthesis of resins, fibers, rubber, dyes, and pharmaceuticals, and have high economic benefits from recycling. Therefore, reducing the aromatic content in naphtha and recovering it can improve the utilization rate of naphtha resources and is of great significance to the sustainable development of modern petrochemicals.

[0003] Polyether-block polyamide (PEBA) is a block copolymer composed of rigid polyamide segments and flexible polyether segments, prepared by catalytic polycondensation of dicarboxylic acid polyamide and polyether glycol under vacuum and high temperature conditions. The crystalline rigid polyamide segments act as crosslinking sites, endowing PEBA with excellent mechanical properties and thermoplasticity, while the amorphous soft polyether segments exhibit rubbery and elastic properties. PEBA exhibits good selective permeability to aromatic compounds, with a solubility parameter of 19.51 (J / cm³). 3 ) 1 / 2 It is close to that of benzene, a common aromatic compound (18.6 (J / cm). 3 ) 1 / 2 ), Toluene (18.2 (J / cm) 3 ) 1 / 2 Its solubility parameter, combined with its excellent mechanical stability and resistance to organic solvents, makes it a potential membrane material for pervaporation separation of aromatics and alkanes.

[0004] Currently, the use of polyether block polyamide membranes in the separation of aromatics and alkanes still faces the following problems. First, the membrane is prone to swelling in the feed solution. Although the block polymerization strategy endows polyether block polyamide membranes with a certain degree of swelling resistance, when the content of flexible polyether segments is too high, the high mobility of the polyether block polyamide segments allows permeate molecules to enter the membrane, increasing the intersegmental spacing and reducing the intersegmental interaction forces, leading to decreased membrane stability. Second, the membrane separation selectivity is low. Because the carbonyl and amide polar groups contained in the polyether block polyamide segments can interact with the π bonds of aromatic compounds but not with aliphatic compounds, they promote the preferential adsorption and permeation of aromatic compounds within the membrane. However, the highly mobile segments are difficult to interact strongly with aromatic compounds, resulting in low selectivity for aromatic separation in polyether block polyamide membranes. Therefore, there is an urgent need to provide a cross-linked polyether block polyamide membrane separation material that combines excellent swelling resistance and selectivity for aromatic dissolution. Summary of the Invention

[0005] In view of this, this application aims to provide a crosslinked polyether block polyamide membrane, its preparation method, and its application, to solve the problems of poor swelling resistance and stability, and insufficient selectivity for aromatic hydrocarbon dissolution in existing polyether block polyamide membranes. This application uses 2,4-toluene diisocyanate as a crosslinking agent, immersing a polyether block polyamide membrane obtained by spin coating in a hexane solution of 2,4-toluene diisocyanate, thereby preparing the crosslinked polyether block polyamide membrane. The crosslinked polyether block polyamide membrane of this invention exhibits excellent swelling resistance and stability during the pervaporation separation of aromatics and alkanes, and has better solubility selectivity for aromatics compared to existing technologies, thus it can be applied to the pervaporation separation of aromatics and alkanes.

[0006] To achieve the aforementioned objectives, the technical solution of this application is implemented as follows: In a first aspect, this application provides a method for preparing a crosslinked polyether block polyamide film, comprising the following steps: S1. Preparation of casting solution Polyether block polyamide (PEBA) and n-butanol were placed in a reactor and heated in a water bath to dissolve PEBA in the n-butanol solution. After filtration, settling and degassing, the PEBA casting solution was obtained. S2. Composite membrane preparation The casting solution was spin-coated onto the surface of a polysulfone (PSf) base film, and after heat treatment, a PEBA / PSf composite film was obtained. S3. Composite membrane crosslinking The PEBA / PSf composite membrane was immersed in a hexane solution containing 2,4-toluene diisocyanate and heated to carry out a crosslinking reaction. After the reaction was completed, the composite membrane was removed and dried to obtain a crosslinked PEBA / PSf composite membrane.

[0007] Furthermore, in step S1, the mass fraction of PEBA in the casting solution is 5~20wt%.

[0008] Furthermore, in step S1, the water bath heating conditions are as follows: mechanical stirring in a water bath at 50~100℃ for 1~5 hours.

[0009] Furthermore, in step S1, the conditions for filtration, settling, and degassing are as follows: after filtering the solution with a 200-1000 mesh filter cloth, it is settling and degassing at room temperature for 0.5-2.5 hours.

[0010] Furthermore, in step S2, the spin coating conditions are as follows: the casting solution is poured onto the surface of the PSf base film, and spin-coated at a speed of 200~1000 rpm for 10~60 seconds.

[0011] Furthermore, in step S2, the heat treatment conditions are as follows: heating at 60~100℃ for 6~24h.

[0012] Furthermore, in step S3, the volume fraction of 2,4-toluene diisocyanate in the hexane solution is 1~6 vol.

[0013] Furthermore, in step S3, the crosslinking reaction is carried out under the condition of heating at 30~60°C for 1~6 hours.

[0014] Secondly, this application also provides a cross-linked polyether block polyamide membrane, which is obtained by the cross-linked polyether block polyamide membrane preparation method of the first aspect of this application.

[0015] Thirdly, this application also provides an application of a cross-linked polyether block polyamide membrane in the separation of organic solvents. The cross-linked polyether block polyamide membrane is obtained by the cross-linked polyether block polyamide membrane preparation method of the first aspect of this application. The cross-linked polyether block polyamide membrane is used for the separation of aromatic hydrocarbons and alkanes by pervaporation.

[0016] This application discloses a crosslinked polyether block polyamide film, its preparation method, and its application. Compared with the prior art, this application has at least the following advantages: This application uses 2,4-toluene diisocyanate as a crosslinking agent. A PEBA / PSf composite membrane obtained by spin coating is immersed in a hexane solution containing 2,4-toluene diisocyanate to prepare a crosslinked PEBA / PSf composite membrane. This application utilizes toluene diisocyanate to covalently crosslink PEBA segments. The crosslinking effectively inhibits segment mobility and shortens the intersegmental spacing, strengthening the hydrogen bonding interactions between segments, thereby improving the swelling resistance and stability of the PEBA / PSf composite membrane in separation processes. The regular and dense packing structure of the PEBA segments in this application strengthens the interaction between the polar groups of the segments and aromatic hydrocarbons, thereby improving the solubility selectivity of the crosslinked PEBA / PSf composite membrane for aromatic hydrocarbons. This achieves synergistic optimization of the solubility selectivity and stability of the crosslinked PEBA / PSf composite membrane for aromatic hydrocarbons, making it suitable for pervaporation separation processes of aromatic hydrocarbons and alkanes.

[0017] The cross-linked polyether block polyamide membrane preparation method of this application is simple, universal, highly controllable, and has a high degree of process maturity. The cross-linked PEBA / PSf composite membrane prepared in this way exhibits excellent anti-swelling properties and separation selectivity for the pervaporation separation of toluene / n-heptane. Attached Figure Description

[0018] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 The image shows the microstructure of the cross-section of the cross-linked PEBA / PSf composite membrane from Example 1, characterized by SEM. Figure 2 The image shows the microstructure of the cross-section of the cross-linked PEBA / PSf composite membrane from Example 2, characterized by SEM. Figure 3 The image shows the microstructure of the cross-section of the cross-linked PEBA / PSf composite membrane in Example 3, characterized by SEM. Figure 4 The image shows the microstructure of the cross-section of the PEBA / PSf composite membrane in Comparative Example 1, characterized by SEM. Detailed Implementation

[0020] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.

[0021] Unless otherwise specified, all temperatures mentioned herein are in degrees Celsius, and the preferred embodiments can be freely combined as needed. Those skilled in the art will understand that the data and parameters described in the examples are merely exemplary and do not constitute a limitation of the invention. All components used in the following examples and comparative examples are compounds known in the art, and all equipment used is equipment publicly known in the art. All components and equipment used in this invention can be obtained commercially or prepared using known techniques.

[0022] In a first aspect, this application provides a method for preparing a crosslinked polyether block polyamide film, comprising the following steps: S1. Preparation of casting solution Polyether block polyamide (PEBA) and n-butanol are placed in a reactor, and the reactor is heated in a water bath to dissolve PEBA in the n-butanol solution. After filtration, settling, and degassing, a PEBA casting solution is obtained. The preferred mass fraction of PEBA in the casting solution of this application is 5~20wt%.

[0023] The polyether block polyamide used in this application may be at least one of Pebax 1657, Pebax 2533, Pebax 3533, Pebax 4033, and Pebax 4533. Preferably, the mass ratio of PEBA to n-butanol is 1:4 to 19.

[0024] As an optional embodiment, PEBA particles and n-butanol are mixed in a 50-150 mL three-necked flask, sealed with a PTFE tape, and then mechanically stirred in a water bath at 50-100°C for 1-5 hours. This application does not specifically limit the water bath heating conditions; the purpose of high-temperature water bath stirring is to dissolve the solid PEBA polymer particles in n-butanol to prepare the casting solution. As an optional embodiment, to remove solid impurities from the n-butanol solution, the filtration, settling, and degassing process conditions in this step are as follows: the solution after water bath heating is filtered using a 200-1000 mesh filter cloth, and then allowed to stand at room temperature for degassing for 0.5-2.5 hours.

[0025] S2. Composite membrane preparation A casting solution is spin-coated onto the surface of a polysulfone (PSf) base film, followed by heat treatment to obtain a PEBA / PSf composite film. The preferred spin-coating conditions in this step are: fixing the PSf base film onto a glass plate, pouring the casting solution onto the PSf base film surface, and spin-coating at 200-1000 rpm for 10-60 seconds. The preferred heat treatment conditions in this step are: heating the spin-coated PSf base film at 60-100°C for 6-24 hours to obtain the PEBA / PSf composite film. This heat treatment promotes thermal crosslinking of PEBA, causing the solvent n-butanol to evaporate and form a dense porous structure within the PEBA layer.

[0026] As an optional implementation, in order to remove impurities present in the PSf base film during production and transportation to prevent membrane pore blockage, the PSf base film can be soaked in deionized water beforehand, and then hung to air dry naturally for later use.

[0027] S3. Composite membrane crosslinking The PEBA / PSf composite membrane was immersed in a hexane solution containing 2,4-toluene diisocyanate and heated to carry out a crosslinking reaction. After the reaction was completed, the composite membrane was removed and dried to obtain a crosslinked PEBA / PSf composite membrane. In this step, the volume fraction of 2,4-toluene diisocyanate in the hexane solution is preferably 1~6 vol%.

[0028] As an optional implementation, the crosslinking reaction in this step is carried out under the following conditions: heating at 30-60°C for 1-6 hours, thereby accelerating the crosslinking reaction of 2,4-toluene diisocyanate and PEBA.

[0029] As an optional implementation, after the reaction is complete, the composite membrane can be rinsed with a large amount of deionized water to remove any residual solution, then soaked in deionized water for 12-24 hours to remove any residual solution inside the composite membrane, and finally dried to obtain the crosslinked PEBA / PSf composite membrane. This application does not have specific limitations on the drying process, as long as it can remove residual moisture from the composite membrane. Optionally, the composite membrane can be dried in a vacuum oven at 60-100°C for 6-24 hours.

[0030] Secondly, this application also provides a cross-linked polyether block polyamide membrane, which is obtained by the cross-linked polyether block polyamide membrane preparation method of the first aspect of this application.

[0031] Thirdly, this application also provides an application of a cross-linked polyether block polyamide membrane in the separation of organic solvents. The cross-linked polyether block polyamide membrane is obtained by the cross-linked polyether block polyamide membrane preparation method of the first aspect of this application. The cross-linked polyether block polyamide membrane is used for the separation of aromatic hydrocarbons and alkanes by pervaporation.

[0032] The preparation method of the cross-linked PEBA / PSf composite membrane in this application is simple, universal, and highly controllable. The prepared cross-linked polyether block polyamide PEBA / PSf composite membrane exhibits excellent anti-swelling properties and separation selectivity when used for pervaporation separation of toluene / n-heptane.

[0033] The present invention will now be described in more detail with reference to exemplary embodiments. The following embodiments or experimental data are intended to illustrate the present invention by way of example, and those skilled in the art should understand that the present invention is not limited to these embodiments or experimental data.

[0034] Example 1 The preparation of crosslinked polyether block polyamide membranes includes the following steps: S1. Preparation of casting solution Weigh 16g of Pebax2533 polymer particles and 90g of n-butanol and mix them in a 150mL three-necked flask. After sealing the flask with a polytetrafluoroethylene tape, fix it in an 80℃ water bath and stir mechanically for 3h to dissolve Pebax2533 in n-butanol to form a solution. Filter the solution obtained after water bath heating using a 600-mesh filter cloth. After filtration, let it stand at room temperature for 1.5h to degas, and obtain a Pebax2533 casting solution with a mass fraction of approximately 15 wt%. S2. Composite membrane preparation A polysulfone (PSf) base film was fixed on a glass plate, and Pebax 2533 casting solution was poured onto the surface of the PSf base film. The film was then spin-coated at 500 rpm for 30 seconds. The spin-coated PSf base film was then thermally crosslinked at 80℃ for 15 hours to obtain a PEBA / PSf composite film.

[0035] S3. Composite membrane crosslinking The PEBA / PSf composite membrane was immersed in a 4 vol% n-hexane solution of 2,4-toluene diisocyanate and heat-treated in an oven at 45°C for 3 hours. After the membrane was removed, the surface of the composite membrane was rinsed with a large amount of deionized water, then immersed in deionized water for 18 hours, and then dried in a vacuum oven at 80°C for 15 hours to obtain the crosslinked PEBA / PSf composite membrane.

[0036] The cross-sectional microstructure of the cross-linked PEBA / PSf composite film prepared in this embodiment was characterized using scanning electron microscopy (SEM), and the results are as follows: Figure 1 As shown.

[0037] Example 2 The preparation of crosslinked polyether block polyamide membranes includes the following steps: S1. Preparation of casting solution Weigh 23g of Pebax2533 polymer particles and 90g of n-butanol and mix them in a 150mL three-necked flask. After sealing the flask with a polytetrafluoroethylene tape, fix it in a 100℃ water bath and stir mechanically for 1h to dissolve Pebax2533 in n-butanol to form a solution. Filter the solution obtained after water bath heating using a 1000-mesh filter cloth. After filtration, let it stand at room temperature for 2.5h to remove bubbles, and obtain a Pebax2533 casting solution with a mass fraction of approximately 20 wt%. S2. Composite membrane preparation A polysulfone (PSf) base film was fixed on a glass plate, and Pebax 2533 casting solution was poured onto the surface of the PSf base film. The film was then spin-coated at 1000 rpm for 60 seconds. The spin-coated PSf base film was then thermally crosslinked at 100℃ for 6 hours to obtain a PEBA / PSf composite film.

[0038] S3. Composite membrane crosslinking The PEBA / PSf composite membrane was immersed in a 6 vol% n-hexane solution of 2,4-toluene diisocyanate and heat-treated in an oven at 60°C for 1 hour. After the membrane was removed, the surface of the composite membrane was rinsed with a large amount of deionized water, then immersed in deionized water for 24 hours, and then dried in a vacuum oven at 100°C for 24 hours to obtain the crosslinked PEBA / PSf composite membrane.

[0039] The cross-sectional microstructure of the cross-linked PEBA / PSf composite membrane prepared in this embodiment was characterized using SEM, and the results are as follows: Figure 2 As shown.

[0040] Example 3 The preparation of crosslinked polyether block polyamide membranes includes the following steps: S1. Preparation of casting solution Weigh 5g of Pebax2533 polymer particles and 90g of n-butanol and mix them in a 150mL three-necked flask. After sealing the flask with a polytetrafluoroethylene tape, fix it in a 50℃ water bath and mechanically stir for 5h to dissolve Pebax2533 in n-butanol to form a solution. Filter the solution obtained after water bath heating using a 200-mesh filter cloth. After filtration, let it stand at room temperature for 0.5h to remove bubbles, and obtain a Pebax2533 casting solution with a mass fraction of 5 wt%. S2. Composite membrane preparation A polysulfone (PSf) base film was fixed on a glass plate, and Pebax 2533 casting solution was poured onto the surface of the PSf base film. The film was then spin-coated at 200 rpm for 10 seconds. The spin-coated PSf base film was then thermally crosslinked at 60℃ for 24 hours to obtain a PEBA / PSf composite film. S3. Composite membrane crosslinking The PEBA / PSf composite membrane was immersed in a 2 vol% n-hexane solution of 2,4-toluene diisocyanate and heat-treated in an oven at 30°C for 6 hours. After the membrane was removed, the surface of the composite membrane was rinsed with a large amount of deionized water, then immersed in deionized water for 12 hours, and then dried in a vacuum oven at 60°C for 6 hours to obtain the crosslinked PEBA / PSf composite membrane.

[0041] The cross-sectional microstructure of the cross-linked PEBA / PSf composite membrane prepared in this embodiment was characterized using SEM, and the results are as follows: Figure 3 As shown.

[0042] Comparative Example 1 The preparation process of the polyether block polyamide membrane is exactly the same as that in Example 1, except that step 3 in Example 1 is not performed. The specific preparation method includes the following steps: S1. Preparation of casting solution Weigh 16g of Pebax2533 polymer particles and 90g of n-butanol and mix them in a 150mL three-necked flask. After sealing the flask with a polytetrafluoroethylene tape, fix it in an 80℃ water bath and stir mechanically for 3h to dissolve Pebax2533 in n-butanol to form a solution. Filter the solution obtained after water bath heating using a 600-mesh filter cloth. After filtration, let it stand at room temperature for 1.5h to degas, and obtain a Pebax2533 casting solution with a mass fraction of approximately 15 wt%. S2. Composite membrane preparation A polysulfone (PSf) base film was fixed on a glass plate, and Pebax 2533 casting solution was poured onto the surface of the PSf base film. The film was then spin-coated at 500 rpm for 30 seconds. The spin-coated PSf base film was then thermally crosslinked at 80℃ for 15 hours to obtain a PEBA / PSf composite film.

[0043] The cross-sectional microstructure of the PEBA / PSf composite membrane prepared in this comparative example was characterized using SEM, and the results are as follows: Figure 4 As shown.

[0044] Tests on the separation performance and anti-swelling properties of pervaporation of aromatics and alkanes 1. Performance test of pervaporation for separating aromatic and alkane hydrocarbons The cross-linked PEBA / PSf composite membranes prepared in Examples 1-3 and the PEBA / PSf composite membrane prepared in Comparative Example 1 were cut, assembled into membrane modules, and fixed in a pervaporation apparatus. A 50 wt% toluene / n-heptane feed solution was added to the feed tank, and the feed solution was controlled at a flow rate of 10 L / h using a temperature and flow rate control device. -1The flow rate was circulated, and the feed liquid in the feed tank was heated to 40°C. An empty collector was weighed to its initial mass and fixed downstream of the membrane module. The vacuum pump was turned on, and the vacuum gauge reading was observed to check the airtightness of the downstream system. When the vacuum level dropped to 0.1 kPa, the fixed collector was immersed in a thermos containing liquid nitrogen, and timing began. After 15 minutes, the collector was removed, sealed, and immersed in room temperature water. After all the permeate had liquefied, a sample was taken using a microsyringe. The sample in the syringe was analyzed by gas chromatography to obtain the composition and mass fraction of the permeate, and the separation factor α was calculated according to the following formula: , Among them, F A and P A The mass fraction (wt%) of toluene in the feed solution and permeate solution are respectively. B and P B The values ​​represent the mass fraction (wt%) of n-heptane in the feed solution and permeate, respectively.

[0045] 2. Anti-swelling performance test The cross-linked PEBA / PSf composite membranes prepared in Examples 1-3 and the PEBA / PSf composite membrane prepared in Comparative Example 1 were immersed in a feed solution under performance evaluation conditions to test the anti-swelling performance of the membrane materials in the feed solution.

[0046] The specific experimental procedure was as follows: The cross-linked PEBA / PSf composite membranes prepared in Examples 1-3 and the PEBA / PSf composite membrane prepared in Comparative Example 1 were dried in a vacuum oven at 60°C for 24 hours. The mass W1 (g) of the membrane was weighed and then immersed in a sufficient amount of 50 wt% toluene / n-heptane mixed feed solution. The scintillation bottle was sealed and placed in an oven at 40°C for 72 hours to allow the solvent molecules to fully penetrate into the membrane. The membrane was then removed and the excess feed solution on the membrane surface was wiped dry with filter paper. The mass W2 (g) of the membrane was quickly weighed. The membrane swelling degree SD... W (%) is calculated using the following formula: .

[0047] The cross-linked PEBA / PSf composite membranes of Examples 1-3 and the PEBA / PSf composite membrane of Comparative Example 1 were tested and calculated using the above-described performance testing methods. The results are shown in Table 1. Table 1 shows that the cross-linked PEBA / PSf composite membranes prepared according to the methods of Examples 1-3 of this application exhibit higher separation factors and superior anti-swelling properties compared to the PEBA / PSf composite membrane prepared according to the method of Comparative Example 1. This demonstrates the excellent application of cross-linked polyether block polyamide membranes in the separation of aromatics / alkanes through pervaporation, especially in the separation of toluene / n-heptane through pervaporation.

[0048] Table 1. Separation factors and swelling degrees of the composite membranes in Examples 1-3 and Comparative Example 1

[0049] As shown in Table 1, the preparation method of this application, which crosslinks the polyether block polyamide composite membrane with toluene diisocyanate, significantly improves the separation factor and swelling resistance of the crosslinked PEBA / PSf composite membrane compared to the pure PEBA / PSf composite membrane. This is because the crosslinking effectively inhibits chain segment mobility, shortens the intersegmental spacing, and strengthens the hydrogen bond interactions between chains, thereby improving the swelling resistance and stability of the PEBA membrane in the pervaporation separation process of aromatics / alkanes. Figures 1-3 It can be observed that the cross-linked polyether block polyamide composite membrane exhibits a regular and dense stacked structure of internal segments, significantly enhancing the interaction between the polar groups of the segments and aromatic hydrocarbons. This improves the solubility selectivity of the cross-linked PEBA composite membrane for aromatic hydrocarbons, thereby achieving synergistic optimization of the composite membrane's selectivity and stability. For Comparative Example 1, which did not use the cross-linking agent 2,4-toluene diisocyanate, from... Figure 4 It can be observed that the chain segments in the polyether block polyamide composite film are loosely and irregularly arranged, and the interaction between the polar groups of the chain segments and the aromatic hydrocarbons is weakened, resulting in the PEBA composite film having lower selectivity for dissolving aromatic hydrocarbons, worse stability, and higher swelling degree.

[0050] All materials used in this invention are commercially available and can be purchased from retail sources.

[0051] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a cross-linked polyether block polyamide film, characterized in that, The preparation method includes the following steps: S1. Preparation of casting solution Polyether block polyamide (PEBA) and n-butanol were placed in a reactor and heated in a water bath to dissolve PEBA in the n-butanol solution. After filtration, settling and degassing, the PEBA casting solution was obtained. S2. Composite membrane preparation The casting solution was spin-coated onto the surface of a polysulfone (PSf) base film, and after heat treatment, a PEBA / PSf composite film was obtained. S3. Composite membrane crosslinking The PEBA / PSf composite membrane was immersed in a hexane solution containing 2,4-toluene diisocyanate and heated to carry out a crosslinking reaction. After the reaction was completed, the composite membrane was removed and dried to obtain a crosslinked PEBA / PSf composite membrane.

2. The method for preparing a crosslinked polyether block polyamide membrane according to claim 1, characterized in that, In step S1, the mass fraction of PEBA in the casting solution is 5~20wt%.

3. The method for preparing a crosslinked polyether block polyamide membrane according to claim 1, characterized in that, In step S1, the water bath heating conditions are as follows: mechanical stirring in a water bath at 50~100℃ for 1~5 hours.

4. The method for preparing a crosslinked polyether block polyamide membrane according to claim 1, characterized in that, In step S1, the conditions for filtration, settling, and degassing are as follows: after filtering the solution with a 200-1000 mesh filter cloth, it is settling and degassing at room temperature for 0.5-2.5 hours.

5. The method for preparing a crosslinked polyether block polyamide membrane according to claim 1, characterized in that, In step S2, the spin coating conditions are as follows: the casting solution is poured onto the surface of the PSf base film, and spin-coated at a speed of 200~1000 rpm for 10~60 seconds.

6. The method for preparing a crosslinked polyether block polyamide membrane according to claim 1, characterized in that, In step S2, the heat treatment conditions are: heating at 60~100℃ for 6~24h.

7. The method for preparing a crosslinked polyether block polyamide membrane according to claim 1, characterized in that, In step S3, the volume fraction of 2,4-toluene diisocyanate in the hexane solution is 1-6 vol.

8. The method for preparing a cross-linked polyether block polyamide membrane according to claim 1, characterized in that, In step S3, the crosslinking reaction is carried out under the condition of heating at 30~60℃ for 1~6 hours.

9. A cross-linked polyether block polyamide film, characterized in that, The cross-linked polyether block polyamide membrane is obtained by the cross-linked polyether block polyamide membrane preparation method according to any one of claims 1-8.

10. An application of a cross-linked polyether block polyamide membrane in organic solvent separation, characterized in that, The cross-linked polyether block polyamide membrane is obtained by the cross-linked polyether block polyamide membrane preparation method according to any one of claims 1-8, and the cross-linked polyether block polyamide membrane is used for the separation of aromatic hydrocarbons and alkanes by pervaporation.